Nickel-based bimetallic phosphide catalyst as well as preparation method and application thereof

The preparation of nickel-based bimetallic phosphide catalysts through co-precipitation method and phosphating calcination technology has solved the problem of low conversion efficiency and insufficient stability in the preparation of benzoic acid by electrochemical oxidation of benzyl alcohol, and achieved efficient conversion and structural stability, suitable for industrial electrocatalytic applications.

CN118957652APending Publication Date: 2024-11-15CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410950535.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing Ni-based catalysts have problems of low conversion efficiency and insufficient stability in the process of electrochemical oxidation of benzoic acid, and the process is complex and the kinetics are slow.

Method used

The nickel-based bimetallic layered hydroxide precursor was synthesized by co-precipitation method and converted into a nickel-based bimetallic phosphide catalyst through phosphating calcination. A catalyst with a crystal-amorphous interfacial coupling structure was prepared, and it was applied to Electrocatalytic benzyl alcohol for preparation of benzoic acid.

Benefits of technology

It achieves high efficiency conversion and high yield of benzyl alcohol at high current density, and the catalyst has excellent structural stability and kinetic characteristics, which is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957652A_ABST
    Figure CN118957652A_ABST
Patent Text Reader

Abstract

The invention discloses a series of nickel-based bimetallic phosphide catalysts as well as a preparation method and application thereof. The invention relates to the technical field of catalysts. The preparation method comprises the following steps: firstly, synthesizing a nickel-based bimetallic layered hydroxide precursor by adopting a coprecipitation method, and then topologically converting the precursor into the nickel-based bimetallic phosphide catalyst in a phosphating and calcining manner. The working electrode of the nickel-based bimetallic phosphide catalyst is applied to preparation of benzoic acid by electro-catalysis of benzyl alcohol. The nickel-vanadium bimetallic phosphide catalyst prepared by the preparation method disclosed by the invention not only retains a nano lamellar structure of a precursor, but also has an obvious crystalline-amorphous interface coupling structure in a microscopic form; the surface chemical structure is adjusted while the metal characteristics are maintained, so that the material has rich active sites and better dynamic characteristics; and high-efficiency conversion and high yield of preparing benzoic acid from benzyl alcohol through electro-catalysis are realized under high current density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a nickel-based bimetallic phosphide catalyst and a preparation method and application thereof. Background Art

[0002] As an important chemical raw material, benzoic acid is widely used in food, medicine, chemical industry and other fields. In traditional industrial synthesis, benzoic acid is usually synthesized from toluene and air under high temperature and high pressure conditions. The process conditions are harsh (temperature 150-170℃, pressure 1MPa) and the process is complex. Electrochemical oxidation of benzyl alcohol to prepare benzoic acid is a green, sustainable and efficient way to produce high-value chemicals. Electrochemical methods can promote chemical synthesis under more environmentally friendly and milder conditions, and have significant advantages in the synthesis of benzoic acid. A notable feature of this method is that it produces highly active free radicals under green and mild conditions through electrochemical reactions to participate in the activation and functionalization of CH bonds, replacing traditional oxidants (O2, H2O2, etc.), and the electrochemical reaction system is easy to achieve separation between products and catalysts. The electrochemical oxidation of benzyl alcohol to produce benzoic acid in an alkaline medium is a 4-electron-proton coupled transfer process, which can be described as PH-CH2OH+4OH-→PH-COOH+3H2O+4e-, which involves multiple CH bond breaks (Csp 2 - and Csp 3 -H bond) and C-OH generation process. At present, related electrocatalysts generally have problems such as cumbersome synthesis process and slow kinetics. Therefore, the development of low-cost, easy to synthesize, directional catalysis, high activity and excellent stability of efficient electrocatalysts is the key to achieve the efficient preparation of benzoic acid by electrochemical oxidation of benzyl alcohol. At present, nickel (Ni)-based catalysts are the most widely studied areas for C-H bond activation and functionalization due to their low cost and excellent conductivity and d electron adjustability. Existing Ni-based catalysts (h-Ni(OH)2, Hp-Ni, Ni@NC-280, etc.) have been preliminarily explored in the field of electrochemical oxidation of benzyl alcohol to prepare benzoic acid, but there are still problems such as low conversion efficiency and stability to be improved. Summary of the invention

[0003] The purpose of the present invention is to provide a series of nickel-based bimetallic phosphide catalysts and preparation methods and applications thereof in view of the above-mentioned deficiencies in the prior art.

[0004] The present invention discloses a method for preparing a nickel-based bimetallic phosphide catalyst. The method comprises the following steps: firstly, synthesizing a nickel-based bimetallic layered hydroxide precursor by a coprecipitation method, and then topologically converting the precursor into a nickel-based bimetallic phosphide catalyst by phosphating and calcining. The other metal M in the bimetallic is one or more of V, Mn, Fe, and Co.

[0005] Furthermore, nickel nitrate is used as a Ni source, and vanadium chloride, manganese nitrate, iron nitrate, and cobalt nitrate are used as V, Mn, Fe, and Co sources, respectively.

[0006] Furthermore, the phosphating calcination method is specifically as follows: a phosphorus source is placed upstream of a tubular furnace, a nickel-based bimetallic layered hydroxide precursor is placed downstream of the tubular furnace, a protective gas flows from the upstream to the downstream of the tubular furnace, and after calcination, the temperature is naturally cooled to room temperature to obtain a nickel-based bimetallic phosphide catalyst.

[0007] Furthermore, the calcination mechanism is as follows: the heating rate is 1-5°C / min, the temperature is raised to 250-450°C and kept warm for 60-180min; the protective gas is argon.

[0008] Furthermore, the phosphorus source is sodium hypophosphite; the molar ratio of sodium hypophosphite to the nickel-based bimetallic layered hydroxide precursor is 10:1.

[0009] Furthermore, the specific preparation method of the co-precipitation method for synthesizing a nickel-based bimetallic layered hydroxide precursor is as follows: the soluble metal salt Ni(NO3)2·6H2O is dissolved in deionized water with one or more of VCl3, Mn(NO3)2·4H2O, Fe(NO3)3·9H2O, and Co(NO3)2·6H2O in a certain molar ratio to form a mixed salt solution; the growth inhibitor formamide is dissolved in NaNO3 solution to form a base liquid, and the pH of the base liquid is adjusted to 10 with a NaOH solution; in an 80°C water bath environment, the mixed salt solution is added dropwise to the base liquid, and the pH of the system is maintained at 10 with a NaOH solution; the entire dropping process is completed within 10 minutes, and the reaction solution obtained after the reaction is fully washed with deionized water until the pH of the supernatant is between 7 and 8, and then dried under vacuum conditions to obtain a nickel-based bimetallic layered hydroxide precursor.

[0010] Furthermore, in the nickel-based bimetallic layered hydroxide precursor, the molar ratio of Ni to M is 3:1.

[0011] A nickel-vanadium bimetallic phosphide catalyst prepared by the above-mentioned preparation method is characterized by having a crystalline-amorphous interface coupling structure.

[0012] An application of the nickel-based bimetallic phosphide catalyst as described above is to dissolve the nickel-based bimetallic phosphide catalyst and Nafion membrane solution in ethanol, and form a uniformly dispersed slurry after ultrasonic treatment; transfer the dispersed slurry and drop it on a conductive substrate nickel foam; and dry it under vacuum conditions to obtain a working electrode of the nickel-based bimetallic phosphide catalyst.

[0013] A working electrode of the nickel-based bimetallic phosphide catalyst as described above is used for electrocatalytic preparation of benzoic acid from benzyl alcohol.

[0014] The present invention uses a phosphating and calcining method to topologically convert a nickel-based bimetallic layered hydroxide precursor into a nickel-based bimetallic phosphide catalyst, and applies it to the electrocatalytic reaction of preparing benzoic acid from benzyl alcohol. The nickel-based bimetallic phosphide catalyst adjusts the surface chemical structure while maintaining the metal properties, so that it has abundant active sites and better kinetic properties.

[0015] Nickel-vanadium bimetallic phosphide (NiV-P) catalyst can be used at high current density (200mA / cm 2 ) to achieve efficient conversion (~100%) and high yield (167 mM g -1 h -1 ), and the product collection was achieved, which has industrial application prospects. Nickel-vanadium bimetallic phosphide (NiV-P) catalyst has excellent structural stability during long-term operation.

[0016] The nickel-vanadium layered double hydroxide precursor prepared by the present invention has an irregularly wrinkled nanosheet structure with a sheet thickness of about 5 to 10 nm. The prepared nickel-vanadium bimetallic phosphide catalyst not only retains the nanosheet structure of the precursor, but also has an obvious crystalline-amorphous interface coupling structure in microscopic morphology, and the size of the crystalline nanoparticles is about 2 to 5 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 XRD patterns of nickel-based bimetallic layered hydroxide (NiM-LDHs) precursor and nickel-based bimetallic phosphide (NiM-P);

[0018] Figure 2 For high current density (200mA / cm 2 ) schematic diagram of the catalytic results of the nickel-based bimetallic phosphide (NiM-P) catalyst electrode in the electrocatalytic reaction of benzyl alcohol to prepare benzoic acid;

[0019] Figure 3 SEM images of nickel-vanadium layered double hydroxide (NiV-LDHs) precursor and nickel-vanadium bimetallic phosphide (NiV-P) catalyst;

[0020] Figure 4 TEM images of nickel-vanadium bimetallic phosphide (NiV-P) catalyst before and after reaction;

[0021] Figure 5 The electrochemical performance diagram of nickel-vanadium bimetallic phosphide (NiV-P) catalyst under different current densities for long-term stable operation;

[0022] Figure 6 The figure and XRD diagram of the product benzoic acid. DETAILED DESCRIPTION

[0023] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0024] Embodiment 1:

[0025] In this embodiment, a coprecipitation method is used to prepare a nickel-vanadium layered double hydroxide precursor.

[0026] 0.003 mol Ni(NO3)2·6H2O and 0.001 mol VCl3 were dissolved in 10 mL of deionized water to form a mixed salt solution; the growth inhibitor formamide was dissolved in 10 mL of 1 mol / L NaNO3 solution to form a base solution, and the pH of the base solution was adjusted to 10 using 0.75 mol / L NaOH solution; in an 80°C water bath environment, the mixed salt solution was added dropwise to the base solution, and 0.75 mol / L NaOH solution was used to maintain the pH of the system at 10. The entire dropwise addition process was completed within 10 minutes, and the reaction solution obtained after the reaction was fully washed with deionized water until the pH of the supernatant was 7-8, and then dried at 60°C under vacuum conditions for 6 hours to obtain a nickel-vanadium layered double hydroxide (NiV-LDHs) precursor.

[0027] This embodiment uses phosphating and calcining to convert the precursor topology into a nickel-vanadium bimetallic phosphide catalyst.

[0028] 2.64g of sodium hypophosphite (NaH2PO2) was placed upstream of the tube furnace as a phosphorus source, and then 0.391g of NiV-LDHs precursor was placed downstream of the tube furnace. The heating time was 165min, from room temperature to 350℃ and kept warm for 120min. After the reaction was completed, the tube furnace was cooled naturally to room temperature to obtain the nickel-vanadium bimetallic phosphide (NiV-P) catalyst.

[0029] Embodiment 2:

[0030] In this embodiment, a coprecipitation method is used to prepare a nickel-manganese layered double hydroxide precursor.

[0031] 0.003 mol Ni(NO3)2·6H2O and 0.001 mol Mn(NO3)2·4H2O were dissolved in 10 mL of deionized water to form a mixed salt solution; the growth inhibitor formamide was dissolved in 10 mL of 1 mol / L NaNO3 solution to form a base solution, and the pH of the base solution was adjusted to 10 using 0.75 mol / L NaOH solution; the mixed salt solution was added dropwise to the base solution in an 80°C water bath environment, and the pH of the system was maintained at 10 using 0.75 mol / L NaOH solution. The entire dropwise addition process was completed within 10 minutes, and the reaction solution obtained after the reaction was fully washed with deionized water until the pH of the supernatant was 7-8, and then dried at 60°C under vacuum conditions for 6 hours to obtain a nickel-manganese layered double hydroxide (NiMn-LDHs) precursor.

[0032] This embodiment uses phosphating and calcining to convert the precursor topology into a nickel-manganese bimetallic phosphide catalyst.

[0033] 2.64g of sodium hypophosphite (NaH2PO2) was placed upstream of the tube furnace as a phosphorus source, and then 0.397g of NiMn-LDHs precursor was placed downstream of the tube furnace. The heating time was 165min, from room temperature to 350℃ and kept warm for 120min. After the reaction was completed, the tube furnace was cooled naturally to room temperature to obtain a nickel-manganese bimetallic phosphide (NiMn-P) catalyst.

[0034] Embodiment 3:

[0035] In this embodiment, a coprecipitation method is used to prepare a nickel-iron layered double hydroxide precursor.

[0036] 0.003 mol Ni(NO3)2·6H2O and 0.001 mol Fe(NO3)3·9H2O were dissolved in 10 mL of deionized water to form a mixed salt solution; the growth inhibitor formamide was dissolved in 10 mL of 1 mol / L NaNO3 solution to form a base solution, and the pH of the base solution was adjusted to 10 using 0.75 mol / L NaOH solution; in an 80°C water bath environment, the mixed salt solution was added dropwise to the base solution, and 0.75 mol / L NaOH solution was used to maintain the pH of the system at 10. The entire dropwise addition process was completed within 10 minutes, and the reaction solution obtained after the reaction was fully washed with deionized water until the pH of the supernatant was 7-8, and then dried at 60°C under vacuum conditions for 6 hours to obtain a nickel-iron layered double hydroxide (NiFe-LDHs) precursor.

[0037] This embodiment uses phosphating and calcining to convert the precursor topology into a nickel-iron bimetallic phosphide catalyst.

[0038] 2.64g of sodium hypophosphite (NaH2PO2) was placed upstream of the tube furnace as a phosphorus source, and then 0.429g of NiFe-LDHs precursor was placed downstream of the tube furnace. The heating time was 165min, from room temperature to 350℃ and kept warm for 120min. After the reaction was completed, the tube furnace was cooled naturally to room temperature to obtain the nickel-iron bimetallic phosphide (NiFe-P) catalyst.

[0039] Embodiment 4:

[0040] In this embodiment, a coprecipitation method is used to prepare a nickel-cobalt layered double hydroxide precursor.

[0041] 0.003 mol Ni(NO3)2·6H2O and 0.001 mol Co(NO3)2·6H2O were dissolved in 10 mL of deionized water to form a mixed salt solution; the growth inhibitor formamide was dissolved in 10 mL of 1 mol / L NaNO3 solution to form a base solution, and the pH of the base solution was adjusted to 10 using 0.75 mol / L NaOH solution; the mixed salt solution was added dropwise to the base solution in an 80°C water bath environment, and the pH of the system was maintained at 10 using 0.75 mol / L NaOH solution. The entire dropwise addition process was completed within 10 minutes, and the reaction solution obtained after the reaction was fully washed with deionized water until the pH of the supernatant was 7-8, and then dried at 60°C under vacuum conditions for 6 hours to obtain a nickel-cobalt layered double hydroxide (NiCo-LDHs) precursor.

[0042] This embodiment uses phosphating and calcining to convert the precursor topology into a nickel-cobalt bimetallic phosphide catalyst.

[0043] 2.64g of sodium hypophosphite (NaH2PO2) was placed upstream of the tube furnace as a phosphorus source, and then 0.441g of NiCo-LDHs precursor was placed downstream of the tube furnace. The heating time was 165min, from room temperature to 350℃ and kept warm for 120min. After the reaction was completed, the tube furnace was cooled naturally to room temperature to obtain the nickel-cobalt bimetallic phosphide (NiCo-P) catalyst.

[0044] Comparative Example 1:

[0045] In this comparative example, a coprecipitation method was used to prepare a nickel-chromium layered double hydroxide precursor.

[0046] 0.003 mol Ni(NO3)2·6H2O and 0.001 mol Cr(NO3)3·9H2O were dissolved in 10 mL of deionized water to form a mixed salt solution; the growth inhibitor formamide was dissolved in 10 mL of 1 mol / L NaNO3 solution to form a base solution, and the pH of the base solution was adjusted to 10 using 0.75 mol / L NaOH solution; the mixed salt solution was added dropwise to the base solution in an 80°C water bath environment, and the pH of the system was maintained at 10 using 0.75 mol / L NaOH solution. The entire dropwise addition process was completed within 10 minutes, and the reaction solution obtained after the reaction was fully washed with deionized water until the pH of the supernatant was 7-8, and then dried at 60°C under vacuum conditions for 6 hours to obtain a nickel-chromium layered double hydroxide (NiCr-LDHs) precursor.

[0047] This embodiment uses phosphating and calcining to convert the precursor topology into a nickel-chromium bimetallic phosphide catalyst.

[0048] 2.64g of sodium hypophosphite (NaH2PO2) was placed upstream of the tube furnace as a phosphorus source, and then 0.423g of NiCr-LDHs precursor was placed downstream of the tube furnace. The heating time was 165min, from room temperature to 350℃ and kept warm for 120min. After the reaction was completed, the tube furnace was cooled naturally to room temperature to obtain a nickel-chromium bimetallic phosphide (NiCr-P) catalyst.

[0049] Application Testing

[0050] In this embodiment, nickel foam is used as a substrate to prepare a working electrode for the electrocatalytic reaction of benzyl alcohol to prepare benzoic acid.

[0051] Take 20 mg of the nickel-based bimetallic phosphide (NiM-P, M=V, Cr, Mn, Fe, Co) catalyst prepared in Example 1-5 and 10 μL of Nafion membrane solution and dissolve them in 2 mL of ethanol. After ultrasonic treatment for 30 min, a uniformly dispersed slurry is formed; use a pipette to take 200 μL of the dispersed slurry and drop it on a conductive substrate nickel foam with a specification of 1 cm×1 cm; dry it at 60°C under vacuum conditions for 6 h to obtain a working electrode of the nickel-based bimetallic phosphide (NiM-P) catalyst.

[0052] In this example, the electrocatalytic reaction of benzyl alcohol to produce benzoic acid was carried out in an H-type electrolytic cell.

[0053] The electrocatalytic reaction of benzyl alcohol to benzoic acid was carried out in an H-type electrolytic cell, and the two electrolytic cells were separated by a proton exchange membrane. The reaction system was a three-electrode system, with a platinum mesh as the counter electrode and a silver chloride electrode as the reference electrode. The electrocatalytic reaction of benzyl alcohol to benzoic acid was carried out in the anode electrolytic cell, with an electrolyte of 1 mol / L potassium hydroxide and a concentration of 10 mmol / L of the reactant benzyl alcohol; 1 mol / L potassium hydroxide was used as the electrolyte in the cathode electrolytic cell, and hydrogen evolution occurred at the cathode during the electrocatalytic reaction. The content of phenolic compounds was detected by high performance liquid chromatography (Agilent 1260), and the detection conditions were as follows: a Diamonsil C18 (2) type liquid chromatography column was used, the detection column temperature was 35 °C; the mobile phase was acetonitrile and formic acid aqueous solution (0.02 mol / L) (ratio of 3:7), the flow rate was 1 ml / min; a VWD ultraviolet detector was used, and the detection wavelength was 260 nm.

[0054] Under industrial production conditions (current density of 200 mA / cm 2 ), the catalytic results of the electrocatalytic reaction of benzyl alcohol to benzoic acid over nickel-based bimetallic phosphide catalysts are shown in Table 1. Among them, the nickel-vanadium bimetallic phosphide (NiV-P) catalyst has obvious performance advantages. Benzyl alcohol achieves nearly 100% conversion within 3 h, and the yield of benzoic acid reaches 167 mM g -1 h -1 1 mol / L HCl was added dropwise to the solution after the reaction to adjust the pH of the solution. After the reaction product was gradually precipitated, the product benzoic acid was finally collected by centrifugation, washing and drying.

[0055] Table 1 Catalytic results of the electrocatalytic reaction of benzyl alcohol to benzoic acid over nickel-based bimetallic phosphide catalysts

[0056]

[0057] Figure 1 XRD patterns of nickel-based bimetallic layered hydroxide (NiM-LDHs, M=V, Cr, Mn, Fe, Co) precursor and nickel-based bimetallic phosphide (NiV-P) catalyst; it can be seen from the figure that NiM-LDHs has typical characteristic diffraction peaks of layered double hydroxides (LDHs), such as (003), (006), (009), (015), (110), etc., indicating that the NiM-LDHs precursor has been successfully synthesized; after phosphating and calcining, the nickel-based bimetallic layered hydroxide is topologically transformed into a nickel-based bimetallic phosphide, and the crystal structure of NiM-P is consistent with Ni2P, indicating that NiM-P is dominated by Ni2P and M atoms replace some Ni atoms in Ni2P.

[0058] Figure 2 For high current density (200mA / cm2 Schematic diagram of the catalytic results of nickel-based bimetallic phosphides in the electrocatalytic reaction of benzyl alcohol to benzoic acid; Among them, the nickel-vanadium bimetallic phosphide (NiV-P) catalyst has obvious performance advantages, and benzyl alcohol achieves nearly 100% conversion within 3 hours, and the yield of benzoic acid reaches 167mM g -1 h -1 .

[0059] Figure 3 The SEM images of the nickel-vanadium layered double hydroxide (NiV-LDHs) precursor and the nickel-vanadium bimetallic phosphide (NiV-P) catalyst show that the NiV-LDHs precursor has an irregularly wrinkled nanosheet structure with a sheet thickness of about 5 to 10 nm. After phosphating and calcining, NiV-P retains the nanosheet structure of the precursor. The sheet structure is conducive to the contact between the catalyst and the reactants and the electron transfer during the reaction, accelerating the reaction kinetics.

[0060] Figure 4 TEM images of the nickel-vanadium bimetallic phosphide (NiV-P) catalyst before and after the reaction; it can be seen from the figure that NiV-P has a clear crystalline-amorphous interface coupling structure, and the size of the crystalline nanoparticles is about 2 to 5 nm ( Figure 4 a); After the catalytic reaction is completed, NiV-P still maintains the crystalline-amorphous interface coupling structure ( Figure 4 b), indicating that the NiV-P catalyst has excellent structural stability.

[0061] The bimetallic synergistic strategy is an effective way to regulate the electronic structure of catalysts, which can induce the formation of active species and overcome the problem of slow kinetics. In the NiV bimetallic phosphide catalyst, the transition metal vanadium (V) containing empty orbitals and half-filled orbitals will achieve a significant d-electron complementary effect with Ni (unsaturated d electrons on the 3d orbital), thereby regulating the electronic structure of the Ni-based catalyst and promoting the catalytic reaction.

[0062] Figure 5 This is the electrochemical performance diagram of the nickel-vanadium bimetallic phosphide (NiV-P) catalyst operating stably for a long time at different current densities; it can be seen from the figure that the NiV-P catalyst has excellent electrochemical stability during long-term operation.

[0063] Figure 6 The physical picture and XRD diagram of the product benzoic acid are shown in Figure 1. After acidification, centrifugation, washing and drying, the product benzoic acid is finally collected.

[0064] For matters not mentioned above, the prior art applies.

[0065] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the described specific embodiments or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above implementations based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a nickel-based bimetallic phosphide catalyst, characterized in that: First, a nickel-based bimetallic layered hydroxide precursor is synthesized by a coprecipitation method, and then the precursor is topologically converted into a nickel-based bimetallic phosphide catalyst by phosphating and calcining; the other metal M in the bimetallic is one or more of V, Mn, Fe, and Co.

2. The preparation method according to claim 1, characterized in that: Nickel nitrate was used as the Ni source, and vanadium chloride, manganese nitrate, iron nitrate and cobalt nitrate were used as the V, Mn, Fe and Co sources respectively.

3. The preparation method according to claim 1, characterized in that: The specific method of phosphating calcination is: placing a phosphorus source upstream of a tubular furnace, placing a nickel-based bimetallic layered hydroxide precursor downstream of the tubular furnace, and allowing a protective gas to flow from the upstream to the downstream of the tubular furnace. After calcination, the mixture is naturally cooled to room temperature to obtain a nickel-based bimetallic phosphide catalyst.

4. The preparation method according to claim 3, characterized in that: The calcination mechanism is as follows: the heating rate is 1-5°C / min, the temperature is raised to 250-450°C and kept warm for 60-180min; the protective gas is argon.

5. The preparation method according to claim 1, characterized in that: The phosphorus source is sodium hypophosphite; the molar ratio of sodium hypophosphite to the nickel-based bimetallic layered hydroxide precursor is 10:

1.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The specific preparation method of the co-precipitation method for synthesizing a nickel-based bimetallic layered hydroxide precursor is as follows: dissolving the soluble metal salt Ni(NO3)2·6H2O and one or more of VCl3, Mn(NO3)2·4H2O, Fe(NO3)3·9H2O, and Co(NO3)2·6H2O in a certain molar ratio in deionized water to form a mixed salt solution; dissolving the growth inhibitor formamide in a NaNO3 solution to form a base liquid, and using a NaOH solution to adjust the pH of the base liquid to 10; in an 80°C water bath environment, adding the mixed salt solution dropwise to the base liquid, and using a NaOH solution to maintain the pH of the system at 10; the entire dropping process is completed within 10 minutes, and the reaction solution obtained after the reaction is fully washed with deionized water until the pH of the supernatant is between 7 and 8, and then dried under vacuum conditions to obtain a nickel-based bimetallic layered hydroxide precursor.

7. The preparation method according to claim 6, characterized in that: In the nickel-based bimetallic layered hydroxide precursor, the molar ratio of Ni to M is 3:

1.

8. A nickel-vanadium bimetallic phosphide catalyst prepared by the preparation method according to any one of claims 1 to 7, characterized in that: It has a crystalline-amorphous interface coupling structure.

9. Use of the nickel-based bimetallic phosphide catalyst as claimed in claim 8, characterized in that: The nickel-based bimetallic phosphide catalyst and Nafion membrane solution are dissolved in ethanol, and a uniformly dispersed slurry is formed after ultrasonic treatment; the dispersed slurry is transferred and dripped on the conductive substrate nickel foam; and the working electrode of the nickel-based bimetallic phosphide catalyst is obtained by drying under vacuum conditions.

10. A working electrode of the nickel-based bimetallic phosphide catalyst as claimed in claim 9 is used for electrocatalytic production of benzoic acid from benzyl alcohol.

Citation Information

Cited By

  • Catalytic material, preparation method thereof and application of catalytic material in electro-catalysis alcohol selective oxidation assisted hydrogen production

    CN119824472A

  • A catalytic material, a preparation method thereof and application thereof in electrocatalytic selective oxidation of alcohols assisted hydrogen production

    CN119824472B