Nickel and cerium loaded bimetallic sulfide catalyst as well as preparation method and application thereof

By using dithiooxalamide as the sulfur source, a supported nickel and cerium bimetallic sulfide catalyst was prepared, which solved the problem of easy corrosion of precious metal catalysts and insufficient sulfur source of nickel sulfide catalysts, and achieved efficient hydrolysis and hydrogen production catalysis, with excellent Catalytic activity and stability.

CN118957658APending Publication Date: 2024-11-15INNER MONGOLIA UNIV OF SCI & TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411012513.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Precious metal catalysts are susceptible to corrosion and oxidation in electrochemical water decomposition, resulting in unstable catalytic activity. There are few researches on the sulfur source of traditional nickel sulfide catalysts, which affects their application in industry.

Method used

Dithiooxalamide is used as the sulfur source to prepare nickel and cerium bimetallic sulfide catalysts by electrodeposition and vulcanization treatment, replacing traditional thiourea to improve catalytic activity and cycle stability.

Benefits of technology

The prepared nickel and cerium bimetallic sulfide catalysts have good catalytic activity and cycle stability. They are suitable for hydrolysis hydrogen production, optimized overpotential and taffel slope, with the largest capacitance of the double layer, the smallest impedance, and the best catalytic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957658A_ABST
    Figure CN118957658A_ABST
Patent Text Reader

Abstract

The invention provides a nickel and cerium loaded bimetallic sulfide catalyst and a preparation method and application thereof, and belongs to the technical field of hydrogen production.The nickel and cerium loaded bimetallic sulfide catalyst is prepared by taking a stainless steel mesh as a substrate and adopting an electrodeposition method and a vulcanization method, and the nickel and cerium loaded bimetallic sulfide catalyst is used for hydrogen production through water electrolysis and is high in catalytic activity and good in catalytic performance. And the impedance is small and the stability is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogen production, and in particular relates to a nickel-cerium loaded bimetallic sulfide catalyst and a preparation method and application thereof. Background Art

[0002] With the progress and development of society and the improvement of economic life, after the industrial revolution, economic development is accompanied by certain environmental damage. Environmental damage and energy shortages have attracted more and more attention. Therefore, the study of sustainable energy that can replace fossil fuels and is economical, efficient, cheap, clean and sustainable has become the research direction of most scientists today. Hydrogen energy is an existing secondary energy source and an environmentally friendly "green energy" with high energy density. Therefore, people generally recognize that hydrogen energy is a new energy source that can solve the environmental and energy crisis and replace fossil fuels. Nowadays, the methods of hydrogen production are mainly divided into fossil energy hydrogen production, water electrolysis hydrogen production, chemical by-product hydrogen production, biological hydrogen production, and solar hydrogen production. The electrocatalytic water decomposition hydrogen production technology has the advantages of pure products, efficient reaction, abundant raw materials, no pollution, simple process and easy control, and has attracted widespread attention from researchers.

[0003] Precious metal materials are excellent catalysts with high catalytic activity in electrochemical water splitting. However, in addition to being rare and expensive, precious metals are easily corroded or oxidized in solutions, which leads to decreased activity and unstable performance, seriously affecting their application and development in industry.

[0004] Transition metal sulfides are considered to be an excellent class of hydrogen evolution electrocatalysts due to their structural characteristics similar to hydrogenases. Commonly used transition metals include Ni, Co, Fe, Mn, etc. Among them, Ni has the best catalytic activity among single-atom transition metals in alkaline electrolytes. However, thiourea and elemental sulfur are commonly used as sulfur sources in the preparation of nickel sulfide catalysts, and there are few studies on other sulfur sources. Therefore, it is of great significance to develop novel structural sulfur sources to enhance the hydrogen evolution activity of nickel sulfide. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a supported nickel and cerium bimetallic sulfide catalyst and its preparation method and application, and for the first time uses dithiooxamide as a sulfur source to replace traditional sulfur sources such as thiourea. The supported nickel and cerium bimetallic sulfide catalyst of the present invention can be used for hydrolysis to produce hydrogen, and has the characteristics of good catalytic activity and good cycle stability.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention:

[0008] The present invention provides a preparation method of a loaded nickel and cerium bimetallic sulfide catalyst, which uses a stainless steel mesh as a substrate, firstly loads the nickel and cerium bimetallic by an electrodeposition method, and then performs a sulfidation treatment to prepare the loaded nickel and cerium bimetallic sulfide catalyst;

[0009] The electrodeposition solution in the electrodeposition process is nickel nitrate hexahydrate, cerium nitrate hexahydrate, sodium chloride and water;

[0010] The sulfur source in the sulfurization treatment is dithiooxamide.

[0011] The present invention adopts dithiooxamide to replace the traditional sulfur source (such as sulfur, thiourea) to prepare the loaded nickel and cerium bimetallic sulfide catalyst. The molar ratio of C:N:S in dithiooxamide (C2N2S2H4) is 1:1:1, which has a higher sulfur content and a more balanced sulfur ratio relative to the thiourea (CN2SH4) molecule.

[0012] Furthermore, the stainless steel mesh was pretreated before electrodeposition: the stainless steel mesh was cut into 1 cm×2.5 cm, its surface was polished with sandpaper, the polished stainless steel mesh was placed in hydrochloric acid, ultrasonicated for 30 minutes, the hydrochloric acid was poured out and washed with water, and then ultrasonicated with acetone, anhydrous ethanol and water for 10 minutes respectively, and finally dried.

[0013] Furthermore, the stainless steel mesh is 316 stainless steel mesh (1400 mesh).

[0014] Furthermore, the concentration of the hydrochloric acid is 3 mol·L -1 .

[0015] Furthermore, the molar ratio of nickel nitrate hexahydrate, cerium nitrate hexahydrate and sodium chloride in the electrodeposition solution is 8:5:10.

[0016] Furthermore, the process of the electrodeposition method is: using a three-electrode system, immersing three electrodes in an electrodeposition solution, and performing electrodeposition on the stainless steel mesh using cyclic voltammetry.

[0017] Furthermore, the number of turns of the electrodeposition is 14 to 42 turns (cv), preferably 14 cv, 28 cv, 35 cv or 42 cv, and more preferably 28 cv.

[0018] Furthermore, the voltage of the cyclic voltammetry is -1.2V to -0.6V.

[0019] Furthermore, the process of the electrodeposition method is: using a three-electrode system, with a pretreated stainless steel base as a working electrode, a platinum sheet as a counter electrode, and a silver-silver chloride electrode as a reference electrode, 2.3264g (8mmol) of nickel nitrate hexahydrate, 0.2171g (5mmol) of cerium nitrate hexahydrate and 0.5844g (10mmol) of sodium chloride are dissolved in 100mL of water, and the stainless steel mesh is electrodeposited using cyclic voltammetry, scanning 28CV between -1.2V and -0.6V, and then washed with deionized water and placed in an oven for drying.

[0020] Furthermore, the process of the sulfurization treatment is: using a sulfur source to perform a sulfurization treatment on the stainless steel mesh after electrodeposition under high temperature calcination conditions.

[0021] Furthermore, the molar ratio of dithiooxamide to nickel nitrate hexahydrate is 1:20.

[0022] Furthermore, the high temperature calcination temperature is 250-550° C., preferably 350° C., and the time is 1-4 hours, preferably 2 hours.

[0023] Furthermore, the process of the sulfurization treatment is as follows: using dithiooxamide as a non-metallic sulfur source, weighing 0.05328g (0.4mmol) of dithiooxamide and the stainless steel mesh after electrodeposition are respectively placed in a porcelain boat, and then the porcelain boat containing dithiooxamide is placed above the air inlet, and finally pistons are placed at both ends of the tube (i.e., both ends of the tubular furnace). After passing argon for 15 minutes, the argon is adjusted to a rate of one bubble per minute, and then the tubular furnace is opened and set to 350°C for calcination for 2h.

[0024] The second technical solution of the present invention:

[0025] The present invention also provides a supported nickel and cerium bimetallic sulfide catalyst prepared by the above method.

[0026] The third technical solution of the present invention:

[0027] The present invention also provides application of the supported nickel and cerium bimetallic sulfide catalyst in hydrogen production by electrohydrolysis.

[0028] Compared with the prior art, the present invention has the following advantages and technical effects:

[0029] The prepared nickel and cerium bimetallic sulfide catalyst is in the form of small spheres, has good catalytic activity, and good cycle stability. Electrochemical measurements show that the overpotentials are 124.6 mV, 77.6 mV, 160.6 mV, and 129.6 mV at 14, 28, 35, and 42 cycles; the Tafel slope is 70.9 mV·dec -1、53.8mV·dec -1 、175.4mV·dec -1 、72.3mV·dec -1 ; Double layer capacitance C dl 62.8mF·cm-2, 67.5mF·cm -2 、52.3mF·cm -2 、59.7mF·cm -2 ; When the tube furnace sintering temperature is 250℃, 350℃, 450℃, and 550℃, the overpotential is 284.6mV, 77.6mV, 147.6mV, and 98.6mV; the Tafel slope is 216mV·dec -1 、42.6mV·dec -1 、155mV·dec -1 、99mV·dec -1 ; Double layer capacitance C dl 11.4mF·cm -2 、67.5mF·cm -2 、14.5mF·cm -2 、29.4mF·cm -2 When the sintering time is 1h, 2h, 3h, and 4h, the overpotential is 125.6mV, 77.6mV, 224.6mV, and 228.6mV; the Tafel slope is 73.9mV·dec -1 、46mV·dec -1 、178mV·dec -1 、190mV·dec -1 ; Double layer capacitance C dl 41.1mF·cm -2 、67.5mF·cm -2 、30.9mF·cm -2 、20mF·cm -2 It can be concluded that the overpotential is 77.6mV and the Tafel slope is 42.6mV·dec at 28cv, 350℃ and 2h. -1 , double layer capacitance C dl 67.5mF cm -2 The impedance is minimal and stable. Under this condition, the bimetallic sulfide catalyst loaded with nickel and cerium has the highest efficiency and the best catalytic effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0031] Figure 1 This is a SEM image of the nickel and cerium bimetallic sulfide catalyst loaded in Example 1;

[0032] Figure 2 This is the SEM energy spectrum of the nickel and cerium bimetallic sulfide catalyst in Example 1;

[0033] Figure 3 is the XRD spectrum of the nickel and cerium bimetallic sulfide catalyst in Example 1;

[0034] Figure 4 This is the full XPS spectrum of the nickel and cerium bimetallic sulfide catalyst in Example 1;

[0035] Figure 5 High-resolution spectra of C1s (a), Ni2p (b), Ce3d (c), and S2p (d) of the nickel-cerium bimetallic sulfide catalyst in Example 1;

[0036] Figure 6 LSV (a) and Tafel (b) of the nickel and cerium bimetallic sulfide catalysts loaded with different numbers of modifications;

[0037] Figure 7 The electrochemical active areas of the modified nickel-cerium bimetallic sulfide catalysts at different numbers of cycles: 14 cycles (a), 28 cycles (b), 35 cycles (c), and 42 cycles (d);

[0038] Figure 8 is the double-layer capacitance C of the loaded nickel and cerium bimetallic sulfide catalysts at different CV cycles dl (a) and Ac(b);

[0039] Fig. 9 LSV (a) and Tafel (b) of the supported nickel and cerium bimetallic sulfide catalysts with different sintering times;

[0040] Fig.10 The prepared catalysts with nickel and cerium bimetallic sulfide after sintering for different times of 1 hour (a), 2 hours (b), 3 hours (c), and 4 hours (d) at a scanning rate of 10-50 mV·s -1 Plotted active area;

[0041] Fig.11 is the double layer capacitance C of the supported nickel and cerium bimetallic sulfide catalysts with different sintering times dl (a) and Ac(b);

[0042] Fig.12 LSV (a) and Tafel (b) of the nickel-cerium bimetallic sulfide catalyst modified at different sintering temperatures;

[0043] Fig.13 The electrodes were modified at different sintering temperatures of 250℃ (a), 350℃ (b), 450℃ (c), and 550℃ (d) at a scanning rate of 10 to 50 mV·s -1 The active area;

[0044] Fig.14 is the double layer capacitance C of the supported nickel and cerium bimetallic sulfide catalysts at different sintering temperatures dl (a) and Ac(b);

[0045] Fig.15 This is the constant current stability test curve of the nickel and cerium bimetallic sulfide catalyst loaded in Example 1. DETAILED DESCRIPTION

[0046] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0047] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0048] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0049] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0050] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0051] All raw materials used in the examples of the present invention are commercially available.

[0052] The technical solution of the present invention is further illustrated by the following embodiments.

[0053] Example 1

[0054] Stainless steel pretreatment: Cut the 316 stainless steel mesh (1400 mesh) into a size of 1cm×2.5cm, then polish its surface with sandpaper, and place the polished stainless steel mesh in a 3mol·L -1 Immerse it in a beaker of hydrochloric acid, then put the beaker into an ultrasonic machine and start ultrasonication for 30 minutes. Pour out the hydrochloric acid and rinse with clean water. Then pour it into a beaker in turn and ultrasonicate with acetone, anhydrous ethanol, and deionized water for 10 minutes respectively. Finally, dry it in a vacuum drying oven for use.

[0055] The outer surface of the stainless steel substrate was electrodeposited by constant current cyclic voltammetry using a three-electrode system. The pretreated stainless steel mesh was used as the working electrode, the platinum sheet was used as the counter electrode, and the silver-silver chloride electrode was used as the reference electrode. 2.3264g (8mmol) of nickel nitrate hexahydrate, 0.2171g (5mmol) of cerium nitrate hexahydrate and 0.5844g (10mmol) of sodium chloride were dissolved in 100mL of water, and the stainless steel mesh was electrodeposited by cyclic voltammetry, scanning 28CV between -1.2V and -0.6V. After washing with deionized water, it was placed in an oven for drying.

[0056] Taking dithiooxamide as the non-metallic sulfur source, the weighed 0.05328 g (0.4 mmol) of dithiooxamide and the stainless steel mesh after electrodeposition were placed in a porcelain boat respectively. Then, the porcelain boat containing dithiooxamide was placed above the air inlet. Finally, pistons were placed at both ends of the tube (i.e., both ends of the tubular furnace). After passing argon for 15 minutes, the argon was adjusted to a rate of one bubble per minute, and then the tubular furnace was opened. The temperature was set to 350°C and calcined for 2 hours to obtain a loaded nickel and cerium bimetallic sulfide catalyst, recorded as Ni-Ce-S-28CV (Ni-Ce-S-2h, Ni-Ce-S-350°C).

[0057] Example 2

[0058] Same as Example 1, except that the voltage is scanned between -1.2V and -0.6V for 14CV, which is recorded as Ni-Ce-S-14CV.

[0059] Example 3

[0060] Same as Example 1, except that the voltage is scanned between -1.2V and -0.6V for 35CV, which is recorded as Ni-Ce-S-35CV.

[0061] Example 4

[0062] Same as Example 1, except that 42CV is scanned between -1.2V and -0.6V, which is recorded as Ni-Ce-S-42CV.

[0063] Example 5

[0064] Same as Example 1, except that the calcination temperature is set at 250°C for 2h, and is recorded as Ni-Ce-S-250°C.

[0065] Example 6

[0066] Same as Example 1, except that the calcination temperature is set at 450°C for 2h, which is recorded as Ni-Ce-S-450°C.

[0067] Example 7

[0068] Same as Example 1, except that the calcination temperature is set at 550°C for 2h, and is recorded as Ni-Ce-S-550°C.

[0069] Example 8

[0070] The same as Example 1, except that the calcination temperature is set at 350° C. for 1 h, which is recorded as Ni—Ce—S-1 h.

[0071] Example 9

[0072] Same as Example 1, except that the calcination temperature is set at 350° C. for 3 h, recorded as Ni—Ce—S-3h.

[0073] Example 10

[0074] Same as Example 1, except that the calcination temperature is set at 350° C. for 4 h, which is recorded as Ni—Ce—S-4h.

[0075] The SEM image of the nickel and cerium bimetallic sulfide catalyst in Example 1 is shown in Figure 1 , SEM spectrum is shown in Figure 2 , it can be seen that the stainless steel mesh surface has been successfully loaded with three elements: nickel, cerium, and sulfur. The catalyst surface forms small balls with rough surfaces and different shapes, which are evenly distributed, and the small balls are tightly gathered together. The small particles gathered together increase the electrochemical active surface area in the stainless steel, so that more new active sites will appear. When the number of active sites increases, the reaction will occur faster, which enhances the activity of the catalyst and improves the catalytic activity of the stainless steel material. Moreover, from the SEM energy spectrum, it can be seen that the stainless steel sample contains three elements: Ni, Ce, and S, and the ratio is 6:13:1.

[0076] The XRD pattern of the nickel and cerium bimetallic sulfide catalyst in Example 1 is shown in Figure 3, blue is the PDF standard card 78-0638 of CeS, and green is the PDF standard card 89-2729 of NiS. In the XRD spectrum of stainless steel, there are diffraction peaks at 35.2°, 45.6°, and 53.4°, which just correspond to the Ni standard spectrum. There are diffraction peaks at 30.03° and 34.50°, and their values ​​just correspond to the Ce standard spectrum. This shows that the surface of stainless steel contains Ni and S, and the content of nickel is higher than that of cerium.

[0077] The full XPS spectrum of the nickel and cerium bimetallic sulfide catalyst in Example 1 is shown in Figure 4 It can be directly observed that there are four elements, Ni, Ge, S, and C, on the surface of the stainless steel sample, indicating that the stainless steel base has been successfully loaded with these elements through constant current cyclic voltammetry electrodeposition, sintering and other steps.

[0078] The high resolution spectra of (a) C1s, (b) Ni2p, (c) Ce3d, and (d) S2p of the nickel and cerium bimetallic sulfide catalyst in Example 1 are shown in Figure 5 , Figure 5 The a in the figure shows the high-resolution spectrum of C1s. It can be seen that there are peaks at 284.8eV and 288.4eV, indicating that the stainless steel sample contains carbon and carbon oxides. The peak energy is higher than the XPS standard peak position. The presence of carbon-oxygen bonds on the surface makes the energy higher. The peaks at 293.19eV and 295.90eV indicate that the sample contains carbonates. Figure 5 The figure b shows the high-resolution spectrum of Ni 2p. It can be seen that there are peaks at 861.10eV, 873.55eV, and 881.60eV, indicating that the stainless steel sample contains Ni 2p. 3 / 2 and Ni 2p 1 / 2 The peak at 853.25 eV indicates that the sample contains Ni 2+ It can also be seen that there is a peak at 855.81eV, which represents the multiple splitting peaks of divalent nickel oxide. Figure 5 The figure c shows the high-resolution spectrum of Ce 3d. It can be seen that there are peaks at 881.95eV, 873.35eV, and 904.34eV. By comparing with the XPS standard peak position diagram of Ce, it can be seen that the stainless steel sample contains Ce element and exists in the form of titanium oxide. The peaks at 881.95eV, 873.35eV, and 904.34eV represent the presence of Ce. 3+ , the peak at 904.34eV indicates that it is Ce 4+ . Figure 5The figure d in the figure shows the high-resolution spectrum of S2p. It can be seen that there are peaks at 164.95eV, 168.80eV, and 162.50eV, indicating that the stainless steel sample contains S element. The peak at 164.95eV indicates the presence of S element. When the peak at 162.5eV appears, it means that metal sulfide may appear. The peak at 168.8eV indicates that it is S +5 , and its binding energy will move upward as the number of atoms increases.

[0079] From the characterization results of SEM, XRD, XPS and other figures, it can be seen that the stainless steel samples have been successfully loaded with elements such as nickel, cerium, sulfur, carbon and their compound states, and the introduction of non-metallic elements has caused the characteristic peaks of Ni and Ce metal atoms to be higher than the standard peaks, indicating that the introduction of sulfur reduces the electron cloud density around the metal atoms, so the electron cloud density around sulfur itself increases, thereby enhancing the adsorption capacity of hydrogen atoms and further improving the catalytic performance.

[0080] The prepared nickel and cerium bimetallic sulfide catalyst in Example 1 was heated to 1 mol·L -1 The potassium hydroxide was tested using an electrochemical workstation, and different numbers of cycles gave the samples different characteristics.

[0081] Figure 6 a means that the -1 The LSV curve of the electrode polarization of the supported nickel and cerium bimetallic sulfide catalyst measured at a scan rate of 10 mA cm -2 In the case of 14 cycles, the overpotential is 124.6 mV, the overpotential is 77.6 mV for 28 cycles, the overpotential is 160.6 mV for 35 cycles, and the overpotential is 129.6 mV for 42 cycles, with 25% Pt / C (purchased from Adamas reagent) as a comparison. The lower the overpotential, the better the catalytic activity. Figure 6 The corresponding Tafel slope is plotted based on the hydrogen evolution LSV curve to judge the catalytic activity. The Tafel of the stainless steel sample at 14, 28, 35, and 42 cycles is 70.9 mV·dec. -1 、53.8mV·dec -1 、175.4mV·dec -1 、72.3mV·dec -1 .

[0082] Figure 7 This is the active area of ​​the nickel-cerium bimetallic sulfide catalyst sample at 1cm×1cm under different numbers of cycles (14, 28, 35, and 42 cycles respectively). The larger the active area, the more active sites it can provide, and the faster the catalytic reaction rate.

[0083] Double layer capacitance C of bimetallic sulfide catalysts loaded with nickel and cerium at different CV cycles dl See Ac Figure 8 Double layer capacitance is a commonly used measurement method to calculate ECSA, which can determine the surface area activity of the electrode. dl is based on Figure 7 The slope of the active area. Its value is proportional to ECSA, C dl The larger the value, the greater the activity and the better the catalytic effect. The values ​​are 62.8mF·cm -2 、67.5mF·cm -2 、52.3mF·cm -2 、59.7mF·cm -2 . Figure 8 In the middle, b represents the impedance measured by setting the open circuit voltage as a parameter. It can be seen that the impedance of the stainless steel sample is the smallest when it is 28 turns. The smaller the impedance, the higher the efficiency of electron movement in electrolyzed water.

[0084] Double layer capacitance C at different cycle numbers dl The overpotential, Tafel slope and impedance are 28﹤14﹤42<35. The best one has the minimum overpotential of 77.6mV at 28 cycles, which is 30mV different from the overpotential of the platinum carbon electrode.

[0085] LSV (a) and Tafel (b) of the supported nickel and cerium bimetallic sulfide catalysts with different sintering times are shown in Fig. 9 It can be seen that when the current density is 10 mA·cm -2 Under the condition of different sintering time in the tube furnace, the overpotential is affected differently. The overpotential is 125.6mV at 1h, 77.6mV at 2h, 224.6mV at 3h, and 228.6mV at 4h. It can be seen that the overpotential is the smallest at 2h. Combined with the Tafel diagram, it is 73.9mV·dec at 1h. -1 , 46mV·dec- at 2h 1 , 178mV·dec at 3h -1 , 190mV·dec at 4h -1 The order of its values ​​is consistent with the order of overpotentials, and Tafel is the smallest at 2h.

[0086] The samples prepared with different sintering times (1, 2, 3, and 4 hours) were scanned at a rate of 10 to 50 mV·s. -1 The active area is plotted as Fig.10 , Double layer capacitance C of Ni / Ce bimetallic sulfide catalysts loaded with different sintering times dl (a) and Ac(b) see Fig.11 It can be seen that the slope is 41.1mF·cm at 1h -2 , slope 67.5mF·cm at 2h -2 , slope 30.9mF·cm at 3h -2 , slope 20mF·cm at 4h -2 , which shows that the holding time of tube furnace sintering is 2h C dl is the largest, which means that its active area is the largest, and combined with Fig.11 The impedance diagram in b shows that the impedance is the smallest at 2h.

[0087] For overpotential, Tafel, double layer capacitance C dl Sort by size 2h﹤1h﹤3h<4h, and then calculate the double layer capacitance C dl The order is 2h>1h>3h>4h. From the order, it can be seen that the smaller the overpotential, the smaller the Tafel impedance and the larger the active area, indicating that its catalytic performance is better. Its minimum overpotential at 2 hours is 77.6mV, which is 30mV different from the overpotential of the platinum carbon electrode.

[0088] LSV (a) and Tafel (b) of the supported Ni and Ce bimetallic sulfide catalysts at different sintering temperatures are shown in Fig.12 It can be seen that when the current density is 10 mA·cm -2 Under the condition of different heating temperatures of tube furnace sintering, the overpotential is affected differently. The overpotential is 124mV at 250℃, 77mV at 350℃, 160mV at 450℃, and 129mV at 550℃. It can be seen that the overpotential is the smallest at 350℃. Combined with the Tafel diagram, the overpotential of the sample at 250℃ is 216mV·dec -1 , 350℃: 46mV·dec -1 , 450℃: 155mV·dec -1 、550℃: 99mV·dec -1 The order of its values ​​is consistent with the order of overpotentials, and Tafel is the smallest at 350℃.

[0089] The modified Ni-Ce bimetallic sulfide catalysts loaded with different sintering temperatures (250℃, 350℃, 450℃, 550℃) showed a scanning rate of 10-50mV·s -1 The active area is shown in Fig.13 , Double layer capacitance C of Ni / Ce bimetallic sulfide catalysts loaded with different sintering temperatures dl (a) and Ac(b) see Fig.14 It can be seen that the slope of the sample is 11.4mF·cm at 250℃ -2, slope 67.5mF·cm at 350℃ -2 , slope 14.5mF·cm at 450℃ -2 , slope 29.4mF·cm at 550℃ -2 , which shows that when the tube furnace sintering temperature is 350℃ dl It is the largest, which means that its active area is the largest. Combined with the impedance diagram, it can be seen that the impedance is the smallest at 350°C, and the order of impedance size is consistent with the order of overpotential size.

[0090] For overpotential, Tafel, double layer capacitance C dl Sort by size 350℃﹤550℃﹤450℃<250℃, and then sort the double layer capacitance C dl The order is 350℃>550℃>450℃>250℃. From the order, we can see that the smaller the overpotential, the smaller the Tafel impedance and the larger the active area, indicating that the catalytic performance is better. At 350℃, the minimum overpotential is 77.6mV, which is 30mV different from the overpotential of the platinum carbon electrode.

[0091] In order to test the stability, we first configured 1moL·L -1 The potassium hydroxide solution was used as the measuring solution, the platinum sheet was used as the counter electrode, and the mercuric chloride was used as the reference electrolysis. The nickel and cerium bimetallic sulfide catalysts loaded in Example 1 were used as the working electrodes to form a standard three-electrode system. The relationship between the current and time was measured by the it curve test with a fixed voltage. The voltage was set to 0.2V and the time was 24 hours. The final measurement result - the constant current stability test curve of the electrode is shown in Fig.15 It can be seen that the current initially drops from 0.1 to 0.05 and then remains stable. Therefore, it can be judged that the nickel and cerium bimetallic sulfide catalyst prepared by using the stainless steel mesh as the substrate of the present invention has good stability.

[0092] In summary, the present invention characterized the sample of the compound loaded with nickel and cerium bimetallic sulfur obtained by the electrodeposition method and the tube furnace sintering method. The final result showed that the sample successfully loaded the three elements of nickel, cerium and sulfur, and was in the form of small spheres and evenly distributed. Through electrochemical measurement, it was found that when the number of cycles was 14, 28, 35, and 42, the overpotential was 124.6mV, 77.6mV, 160.6mV, and 129.6mV; the Tafel slope was 70.9mV·dec -1 、53.8mV·dec -1 、175.4mV·dec -1 、72.3mV·dec -1 ; Double layer capacitance C dl 62.8mF·cm-2, 67.5mF·cm -2 、52.3mF·cm-2 、59.7mF·cm -2 .

[0093] When the tube furnace sintering temperature is 250℃, 350℃, 450℃, and 550℃, the overpotential is 284.6mV, 77.6mV, 147.6mV, and 98.6mV; the Tafel slope is 216mV·dec -1 、46mV·dec -1 、155mV·dec -1 、99mV·dec -1 ; Double layer capacitance C dl 11.4mF·cm -2 、67.5mF·cm -2 、14.5mF·cm -2 、29.4mF·cm -2 .

[0094] When the sintering time is 1h, 2h, 3h, and 4h, the overpotential is 125.6mV, 77.6mV, 224.6mV, and 228.6mV; the Tafel slope is 73.9mV·dec -1 、42.6mV·dec -1 、178mV·dec -1 、190mV·dec -1 ; Double layer capacitance C dl 41.1mF·cm -2 、67.5mF·cm -2 、30.9mF·cm -2 、20mF·cm -2 It is concluded that the overpotential is 77.6mV and the Tafel slope is 46mV·dec at 28cv, 350℃ and 2h. -1 , double layer capacitance C dl 67.5mF cm -2 The impedance is minimal and stable. Under this condition, the bimetallic sulfide catalyst loaded with nickel and cerium has the highest efficiency and the best catalytic effect.

[0095] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a nickel-cerium bimetallic sulfide catalyst, It is characterized in that Using a stainless steel mesh as a substrate, firstly using an electrodeposition method to load nickel and cerium bimetallics, and then performing a sulfidation treatment to prepare the loaded nickel and cerium bimetallic sulfide catalyst; The electrodeposition solution in the electrodeposition process is nickel nitrate hexahydrate, cerium nitrate hexahydrate, sodium chloride and water; The sulfur source in the sulfurization treatment is dithiooxamide.

2. The method for preparing the supported nickel and cerium bimetallic sulfide catalyst according to claim 1, It is characterized in that The stainless steel mesh was pretreated before electrodeposition: the stainless steel mesh was cut into 1 cm×2.5 cm, and its surface was polished with sandpaper. The polished stainless steel mesh was placed in hydrochloric acid and ultrasonicated for 30 minutes. The hydrochloric acid was poured out and washed with water. Then, acetone, anhydrous ethanol and water were ultrasonicated for 10 minutes respectively, and finally dried.

3. The method for preparing the supported nickel and cerium bimetallic sulfide catalyst according to claim 1, It is characterized in that The molar ratio of nickel nitrate hexahydrate, cerium nitrate hexahydrate and sodium chloride in the electrodeposition solution is 8:5:

10.

4. The method for preparing the supported nickel and cerium bimetallic sulfide catalyst according to claim 3, It is characterized in that The process of the electrodeposition method is: using a three-electrode system, immersing three electrodes in an electrodeposition solution, and performing electrodeposition on the stainless steel mesh using cyclic voltammetry.

5. The method for preparing the supported nickel and cerium bimetallic sulfide catalyst according to claim 4, It is characterized in that The number of turns of the electrodeposition is 14 to 42.

6. The method for preparing the supported nickel and cerium bimetallic sulfide catalyst according to claim 1, It is characterized in that The process of the sulfurization treatment is: using a sulfur source to perform a sulfurization treatment on the stainless steel mesh after electrodeposition under the condition of high-temperature calcination.

7. The method for preparing the supported nickel and cerium bimetallic sulfide catalyst according to claim 6, It is characterized in that The high temperature calcination temperature is 250-550° C. and the time is 1-4 hours.

8. A supported nickel and cerium bimetallic sulfide catalyst, It is characterized in that Prepared according to the method according to any one of claims 1 to 7.

9. Use of the supported nickel and cerium bimetallic sulfide catalyst according to claim 8 in hydrogen production by electrohydrolysis.

Citation Information

Cited By

  • Composite electrode material and preparation method and application thereof

    CN120400887A

  • Method for synthesizing Mn0. 43Cd0. 57S / Cu2MoS4 photocatalyst by adopting solvothermal method

    CN120550825A

  • A method for synthesizing Mn 0.43 Cd 0.57 A method for synthesizing a S / Cu2MoS4 photocatalyst