Controllable construction method and application of heterostructure catalyst

The construction of metal-semiconductor heterostructure electrocatalysts through template cation exchange and reduction pyrolysis methods solves the problem of insufficient catalyst preparation complexity and controllability, significantly improves the catalytic performance of the redox reaction, and is suitable for a variety of energy applications.

CN118957664APending Publication Date: 2024-11-15UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411056798.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the preparation method of heterostructured catalysts is complex and insufficient controllability, and the interface distribution is uneven, making it difficult to effectively improve the catalytic performance of redox reaction (OER).

Method used

Using template-based cation exchange and reduction pyrolysis methods, metal-semiconductor heterostructure is constructed by placing metal organic frame materials in transition metal salt solution for cation exchange and pyrolysis under suitable reduction atmosphere and temperature. Electrocatalysts achieve significant improvement in catalytic activity.

Benefits of technology

This method simplifies the catalyst preparation process, realizes uniform dispersion of catalytic active sites and significant optimization of catalytic performance, overcomes the complexity and unevenness of interface construction of traditional methods, improves the catalytic performance of OER, and is suitable for water electrolysis, 金属空气电池和燃料电池等能源转化与储存技术。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957664A_ABST
    Figure CN118957664A_ABST
Patent Text Reader

Abstract

The invention discloses a controllable construction method and application of a heterostructure catalyst, and belongs to the field of materials science. The preparation method of the heterostructure catalyst comprises the following steps: putting a metal organic framework material containing coordination unsaturated metal sites into coordination ion exchange liquid, and carrying out cation exchange reaction to obtain a precursor; and carrying out pyrolysis on the precursor to obtain the heterostructure catalyst. According to the invention, the controllable construction of a metal-semiconductor heterostructure interface is realized by adopting cation exchange based on a template and assisted by a reduction pyrolysis method, so that the OER catalytic performance is optimized. The method is simple in technological process, mild in condition, convenient to operate, low in cost, green and efficient, no too strict experimental conditions exist in the synthesis process, and active sites of the prepared catalyst are evenly dispersed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of materials science, and in particular to a controllable construction method of a heterogeneous structure catalyst and application thereof. Background Art

[0002] At present, the development and application of clean and renewable energy have brought new opportunities to solve the growing energy demand and severe environmental problems. However, given its intermittent and volatile characteristics, it is generally difficult to achieve efficient and stable energy conversion. Therefore, the development of clean, low-carbon, safe and efficient renewable energy storage devices has become a global trend. The oxygen evolution reaction (OER) plays a key role in a series of clean energy storage and conversion processes (such as water electrolysis and metal-air batteries). However, this four-electron oxidation reaction requires continuous intermediate valence state change steps, which makes the kinetics of the catalytic cycle very complicated and exhibits slow overall catalytic kinetics. In order to solve the above problems, the development of low-cost and efficient catalyst materials is a research and development direction.

[0003] The strategy of interfacial optimization of non-precious metal catalysts is an important and widely used modification technology. By designing heterostructure electrocatalysts with high bonding strength, the coupling interactions produced can cause strong interfacial effects, thereby improving the performance of non-precious metal-based electrocatalysts. First, the introduction of heterogeneous interfaces can adjust the electronic structure of active sites, thereby optimizing the adsorption state and reaction activation energy barrier of specific reactants in catalytic reactions and enhancing reaction kinetics; secondly, the introduction of interfaces can bring about synergistic effects between different catalytic sites, which can promote different elementary reaction steps in the reaction process. A more evenly dispersed heterogeneous interface can increase the contact area between the two components in the catalyst, prevent the agglomeration of metal catalysts, and form as many key catalytic centers as possible, thereby improving the catalytic activity of the catalyst.

[0004] It can be seen that constructing heterogeneous interfaces for electrocatalysts can achieve quantum-scale electronic effects, atomic-scale synergistic effects, optimize molecular-scale catalytic processes, and improve nanoscale stability. It has been fully studied and proven that it can improve the catalytic performance of oxygen electrodes at multiple scales. However, the preparation methods of similar products in this field are still relatively complex and lack controllability, and the uniformity of interface distribution needs to be further improved. Summary of the invention

[0005] The object of the present invention is to provide a controllable construction method of a heterostructure catalyst and its application to solve the above-mentioned problems in the background technology. The present invention adopts a template-based cation exchange method assisted by reduction pyrolysis to achieve a controllable structure of the metal-semiconductor heterostructure interface to optimize the OER catalytic performance. The process of the present invention is simple and the conditions are mild, the operation is convenient, the cost is low, and it is green and efficient. There are no overly harsh experimental conditions during the synthesis process, and the active sites of the prepared catalyst are uniformly dispersed.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention is to provide a method for preparing a heterogeneous structure catalyst, comprising the following steps:

[0008] The metal organic framework material (MOFs) containing coordinated unsaturated metal sites (CUS) is placed in a coordinated ion exchange solution to undergo a cation exchange reaction to obtain a precursor;

[0009] The precursor is pyrolyzed to obtain the heterogeneous structure catalyst.

[0010] Preferably, the metal organic framework material containing coordinated unsaturated metal sites is a MILs series material.

[0011] Preferably, the metal organic framework material containing coordinated unsaturated metal sites is Mn-MIL-100.

[0012] Preferably, the acid anion species in the coordination ion exchange liquid is one or more of nitrate, acetate and sulfate, and the solvent is methanol, ethanol, N-N dimethylformamide (DMF) or N-N dimethylacetamide (DEF).

[0013] Preferably, the coordinating ion species in the coordinating ion exchange solution is Ni 2+ 、Co 2+ and Fe 2+ One or more of .

[0014] Preferably, the concentration of the coordinating ions in the coordinating ion exchange solution is 10-100 mM.

[0015] Preferably, the temperature of the cation exchange reaction is 20-80°C and the time is 2-24h.

[0016] Preferably, the Mn-MIL-100 is prepared by a solvothermal method.

[0017] Preferably, the pyrolysis atmosphere is a reducing atmosphere.

[0018] Preferably, the reducing atmosphere contains hydrogen.

[0019] Preferably, the pyrolysis atmosphere is a reducing atmosphere; the reducing atmosphere contains 3-10 vol% hydrogen.

[0020] Preferably, the pyrolysis temperature is 300-600° C. and the time is 1-5 h.

[0021] The second technical solution of the present invention is to provide a heterogeneous structure catalyst obtained according to the above preparation method.

[0022] The third technical solution of the present invention is to provide an application of the above-mentioned heterogeneous structure catalyst in catalytic oxygen evolution reaction.

[0023] The technical principles of the present invention are as follows:

[0024] The present invention places a self-supporting manganese-based metal organic framework material in a transition metal (iron, cobalt, nickel) salt solution for cation exchange, and achieves controllable exchange of cations by regulating the solution concentration and temperature. It then performs a pyrolysis treatment in a suitable reducing atmosphere and temperature, and utilizes the difference in standard electrode potential between metals to ultimately construct a transition metal / manganese oxide heterostructure electrocatalyst.

[0025] During the pyrolysis process, the coordinating ions added in the scheme are reduced to the corresponding metal elements, and the manganese ions are pyrolyzed to obtain manganese oxide, thereby forming a metal-semiconductor interface and realizing the construction of a heterostructure catalyst.

[0026] The beneficial technical effects of the present invention are as follows:

[0027] The present invention adopts a method based on template cation exchange and supplemented by reduction pyrolysis to achieve controllable construction of metal-semiconductor heterostructure interface to optimize OER catalytic performance. In the alkaline solution of electrolyte, the controllable regulation of heterostructure interface achieves a significant improvement in catalytic activity. This method overcomes the limitations of non-precious metal interface construction and interface unevenness in traditional methods such as liquid phase method and phase separation method. By regulating the ion concentration and temperature of cation exchange, the introduction and reduction of metal ions can be accurately controlled, thereby achieving accurate regulation of metal-semiconductor interface structure and significant optimization of catalytic performance. Compared with the traditional composite catalyst preparation method, the process flow of the cation exchange combined with pyrolysis of the present invention is simple and mild, easy to operate, low cost, green and efficient, there are no overly harsh experimental conditions in the synthesis process, and the active sites of the prepared catalyst are uniformly dispersed. In addition, the method of the present invention has a high degree of flexibility and scalability, and the type and number of active sites can be adjusted and optimized. The present invention exhibits efficient catalytic performance in the oxygen evolution reaction (OER) and can be widely used in energy conversion and storage technologies such as water electrolysis to produce hydrogen, metal-air batteries and fuel cells, significantly improving energy utilization efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 The scanning electron microscope photographs of the product of Example 1. (a) and (b) are scanning electron microscope photographs of different positions.

[0030] Figure 2 This is the X-ray diffraction spectrum of the product of Example 1.

[0031] Figure 3 This is a transmission electron microscope photograph of the product of Example 1.

[0032] Figure 4 (a) is the X-ray photoelectron spectrum of the 3s orbital of Mn in the products of Example 1 and Comparative Example 1, and (b) is the X-ray photoelectron spectrum of the 2p orbital of Ni in the product of Example 1.

[0033] Figure 5 This is the EDS diagram of the product in Example 1.

[0034] Figure 6 The linear sweep voltammetric characteristic curves of the products with different nickel ion concentrations in Example 2.

[0035] Figure 7 The linear sweep voltammetric characteristic curves of the products at different cation exchange temperatures in Example 2.

[0036] Figure 8 The Tafel plots and electrochemical impedance spectra of different products in Example 2 are shown in Figure 2. (a) is the Tafel plot, and (b) is the electrochemical impedance spectra.

[0037] Fig. 9 This is the linear sweep voltammetric characteristic curve of the product in Example 3. DETAILED DESCRIPTION

[0038] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0039] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0040] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0041] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.

[0042] Unless otherwise specified, the "room temperature" in the present invention is 20°C.

[0043] All raw materials used in the following examples and comparative examples of the present invention are commercially available products.

[0044] Example 1

[0045] Preparation of heterogeneous catalysts:

[0046] (1) 1 g of manganese nitrate and 1.65 g of trimesic acid were dissolved in 50 mL of methanol, mixed by magnetic stirring for 0.5 h, and then ultrasonicated for 0.5 h to obtain a dispersion; the obtained dispersion was transferred to a 50 mL Teflon-lined stainless steel autoclave, and then two pieces of carbon cloth were immersed in the solution respectively, reacted at 125 ° C for 1 h, and then naturally cooled to room temperature. After that, the sample was taken out, rinsed with ethanol, and then dried in a vacuum oven at 60 ° C to obtain a carbon cloth loaded with Mn-MIL-100 material.

[0047] (2) 0.4 mmol nickel acetate and 1 g urea were dissolved in 40 mL methanol, magnetically stirred for 0.5 h, and then ultrasonicated for 0.5 h to obtain a coordination ion exchange solution (wherein the nickel ion concentration was 10 mM); the prepared carbon cloth loaded with Mn-MIL-100 material was immersed in the coordination ion exchange solution, reacted at 20°C for 2 h, then washed with ethanol 5 times, and placed in a vacuum oven at 60°C for 12 h to obtain a precursor.

[0048] (3) The precursor was placed in a tube furnace under a H2 / Ar2 mixed atmosphere (H2 accounted for 5 vol%), heated to 550°C at a heating rate of 1°C / min, and pyrolyzed for 2 h to obtain a heterogeneous structure catalyst (denoted as MnO-Ni / CC).

[0049] Comparative Example 1

[0050] The only difference from Example 1 is that step (2) is omitted, and the carbon cloth loaded with Mn-MIL-100 material obtained in step (1) is directly placed in the tubular furnace of step (3) for pyrolysis under the same conditions, and the obtained product is recorded as MnO / CC.

[0051] Figure 1 The scanning electron microscope photographs of the product of Example 1. (a) and (b) are scanning electron microscope photographs of different positions.

[0052] like Figure 1 As shown, the product of Example 1 presents a good porous two-dimensional nanobelt structure, which maintains the basic ribbon shape of Mn-MIL-100.

[0053] Figure 2 This is the X-ray diffraction spectrum of the product of Example 1.

[0054] Depend on Figure 2 It can be seen that the diffraction peaks at 34.91°, 40.55°, 58.72°, and 70.188° correspond exactly to the (111), (200), (220), and (311) crystal planes of MnO (PDF#00-007-0230), while the diffraction peaks at 44.51° and 51.85° correspond to the (111) and (200) crystal planes of Ni (PDF#00-004-0850).

[0055] Figure 3 This is a transmission electron microscope photograph of the product of Example 1.

[0056] Depend on Figure 3 It can be found that the material as a whole has an obvious heterogeneous structure, that is, the Ni(111) and MnO(111) crystal planes are closely distributed inside the material.

[0057] Figure 4 (a) is the X-ray photoelectron spectrum of the 3s orbital of Mn in the products of Example 1 and Comparative Example 1, and (b) is the X-ray photoelectron spectrum of the 2p orbital of Ni in the product of Example 1.

[0058] X-ray photoelectron spectroscopy was performed on the Mn 3s orbital and the Ni 2p orbital. Figure 4 In (a), by comparing the products of Example 1 and Comparative Example 1, it can be seen that MnO-Ni / CC has an energy level difference of 6.2eV at 84.14eV and 90.34eV, which is 0.09eV more than 6.11eV of MnO / CC, proving that while Mn maintains a +2 valence state, part of the electrons on the Ni side flow to MnO on the semiconductor side. Figure 4As shown in (b), the product of Example 1 has obvious peaks of metallic nickel and planetary peaks at 853 eV, and no Ni with higher valence states exists. Combined with the above results, the construction of the manganese oxide-nickel material with a heterojunction structure (MnO-Ni / CC) in Example 1 is confirmed.

[0059] Figure 5 This is the EDS diagram of the product in Example 1.

[0060] Figure 5 It shows that the elements Mn, O, and Ni are evenly distributed, achieving a uniform distribution of catalytic active sites.

[0061] Example 2

[0062] Preparation of heterogeneous catalysts:

[0063] By adjusting only the amount of nickel acetate added in Example 1 to make the nickel ion concentration in the coordination ion exchange solution 10, 20, 40, 60, and 100 mM, and adjusting the cation exchange temperature to 20, 40, 60, and 80°C, heterogeneous structure catalysts with different loadings (denoted as MnO-Ni-x / CC-y, wherein x represents the nickel ion concentration and y represents the cation exchange temperature; and when the cation exchange temperature is 20°C, it is denoted as MnO-Ni-x / CC) are finally obtained.

[0064] Effect Example 1

[0065] The product of Comparative Example 1 and the heterogeneous structure catalysts with different loadings obtained in Example 2 were used to test the electrochemical performance of oxygen evolution in a three-electrode system. In the electrolytic cell, a platinum sheet was used as a counter electrode, Hg / HgO was used as a reference electrode, and the products of Comparative Example 1 and Example 2 were directly used as working electrodes without treatment, and the electrolyte was a 1 mol / L KOH solution.

[0066] The test results of the inductively coupled plasma test (ICP test) are shown in Table 1.

[0067] Table 1 Inductively coupled plasma test under different nickel ion concentration conditions

[0068] ICP Test Ni / Mn (atomic ratio) Ni(wt%) Mn (wt%) MnO / CC 0.0001 0.0004% 4.518% MnO-Ni-20 / CC 0.0864 0.4385% 4.5324% MnO-Ni-40 / CC 0.1396 0.7689% 4.9180% MnO-Ni-60 / CC 0.1817 0.9929% 4.8799% MnO-Ni-60 / CC-60 0.3371 1.7237% 4.5656%

[0069] As shown in Table 1, in the MnO / CC system with a manganese content of 4.5-4.92wt%, as the nickel ion concentration increases, the cation exchange is carried out under the conditions of 20mM, 40mM, and 60mM nickel ion concentrations, and the nickel content reaches 0.4385%, 0.7689%, and 0.9929%, respectively. Under the condition of a nickel ion concentration of 60mM, when the cation exchange temperature is further increased to 60°C, the nickel content in the system is further increased to 1.7237%, and the final nickel-manganese atomic ratio of the system can be quantitatively determined to be 0.3371:1.

[0070] Figure 6 The linear sweep voltammetric characteristic curves of the products with different nickel ion concentrations in Example 2.

[0071] Figure 7 The linear sweep voltammetric characteristic curves of the products at different cation exchange temperatures in Example 2.

[0072] Depend on Figure 6 It can be seen that compared with the unexchanged MnO / CC at 10 mA / cm 2 The corresponding overpotential is 523mV under 10mA / cm 2 However, as the nickel ion concentration increased to 100mM, MnO-Ni-100 / CC showed a significant attenuation, with an overpotential of 350mV at 10mA / cm 2 The overpotential corresponds to 400 mV. It is proved that 60 mM nickel ion concentration is the optimal exchange concentration for constructing MnO-Ni heterojunction.

[0073] from Figure 7 It can be seen that under 60℃, MnO-Ni-60 / CC-60 has a 2 The optimal overpotential was 320 mV.

[0074] Figure 8 The Tafel plots and electrochemical impedance spectra of different products in Example 2 are shown in Figure 2. (a) is the Tafel plot, and (b) is the electrochemical impedance spectra.

[0075] from Figure 8 As can be seen from (a), the Tafel slope of MnO-Ni-60 / CC-60 reaches the lowest 158mV·dec -1 , which proves that it has obvious improvement in kinetics (the Tafel slope of MnO-Ni-10 / CC is 239.45 mV·dec -1 ).

[0076] Figure 8As can be seen in (b), MnO-Ni-60 / CC-60 also exhibits the lowest interface impedance (Rs=1.7Ω), indicating that the improved heterogeneous interface has good conductivity and material transfer efficiency.

[0077] Example 3

[0078] Preparation of heterogeneous catalysts:

[0079] The only difference from Example 1 is that the addition of nickel acetate is omitted and 2.4 mmol of cobalt acetate or ferrous sulfate is supplemented, and the cation exchange temperature is adjusted to 60°C to obtain the final products (respectively recorded as MnO-Co-60 / CC-60 and MnO-Fe-60 / CC-60).

[0080] Effect Example 2

[0081] The product of Example 3 was used in a three-electrode system to test the electrochemical performance of oxygen evolution. In the electrolytic cell, a platinum sheet was used as a counter electrode, Hg / HgO was used as a reference electrode, and the product of Example 3 was directly used as a working electrode without treatment, and the electrolyte was a 1 mol / L KOH solution.

[0082] Fig. 9 This is the linear sweep voltammetric characteristic curve of the product in Example 3.

[0083] Depend on Fig. 9 It can be seen that compared with the manganese oxide-nickel heterojunction catalyst in Example 2, MnO-Co-60 / CC-60 and MnO-Fe-60 / CC-60 are respectively 2 It also exhibits low overpotentials of 310 mV and 280 mV, proving that the metal-semiconductor heterointerface structure under controllable conditions can greatly improve the electrocatalytic performance of MOF-based derivative materials.

[0084] In summary, the present invention adopts a method based on template cation exchange and assisted by reduction pyrolysis to achieve a controllable structure of the metal-semiconductor heterostructure interface to optimize the OER catalytic performance. In alkaline solution, the controllable regulation of the heterostructure interface achieves a significant improvement in catalytic activity. This method overcomes the uncertainty and complexity of interface construction in traditional methods. By regulating the ion concentration and temperature of cation exchange, the introduction and reduction of metal ions can be accurately controlled, thereby achieving precise regulation of the metal-semiconductor interface structure and significant optimization of catalytic performance, and the prepared catalyst active sites are uniformly dispersed. Compared with the traditional composite catalyst preparation method, the process flow of the cation exchange combined with pyrolysis of the present invention is simple and mild, easy to operate, low cost, green and efficient, and there are no overly harsh experimental conditions during the synthesis process, which is in line with the concept of green chemistry. In addition, the method of the present invention has a high degree of flexibility and scalability, and can be adjusted and optimized according to specific catalytic needs. The present invention exhibits efficient catalytic performance in oxygen evolution reaction (OER), and can be widely used in energy conversion and storage technologies such as water electrolysis for hydrogen production, metal-air batteries and fuel cells, significantly improving energy utilization efficiency.

[0085] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a heterogeneous structure catalyst, characterized in that: The following steps are involved: placing a metal organic framework material containing coordinated unsaturated metal sites in a coordinated ion exchange solution to undergo a cation exchange reaction to obtain a precursor; The precursor is pyrolyzed to obtain the heterogeneous structure catalyst.

2. The preparation method according to claim 1, characterized in that: The metal organic framework material containing coordinated unsaturated metal sites is a MILs series material.

3. The preparation method according to claim 2, characterized in that: The metal organic framework material containing coordinated unsaturated metal sites is Mn-MIL-100.

4. The preparation method according to claim 1, characterized in that: The type of coordination ion in the coordination ion exchange liquid is Ni 2+ 、Co 2+ and Fe 2+ One or more of .

5. The preparation method according to claim 3, characterized in that: The coordination ion concentration in the coordination ion exchange solution is 10-100 mM.

6. The preparation method according to claim 1, characterized in that: The temperature of the cation exchange reaction is 20-80°C and the time is 2-24h.

7. The preparation method according to claim 1, characterized in that: The pyrolysis atmosphere is a reducing atmosphere; the reducing atmosphere contains 3-10 vol% hydrogen.

8. The preparation method according to claim 1, characterized in that: The pyrolysis temperature is 300-600° C. and the time is 1-5 hours.

9. A heterogeneous structure catalyst obtained according to the preparation method according to any one of claims 1 to 8.