Low-pressure corrosion foil as well as preparation method and application thereof
By adjusting the corrosion liquid components and the power-up current waveform, and using the superposition waveform of square wave and triangular wave, the problem of uneven distribution of the aperture diameter of the low-voltage anode foil was solved, and high-specific capacitance, high-intensity, low-voltage corrosion suitable for the 50-100Vf voltage segment was prepared. Foil, suitable for automotive grade aluminum electrolytic capacitors.
Patent Information
- Application Number
- CN202411193003.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
AI Technical Summary
The existing technology of low-voltage anode foils in the voltage range of 50-100Vf have problems such as uneven pore size distribution and inapplicable etching hole size, resulting in increased production costs and poor product performance.
By adjusting the corrosion liquid components, current waveform, current density and power-up time, the superposition waveform of square wave and triangle wave is used to control the aperture size and distribution uniformity, and a high specific capacity and high intensity low-pressure corrosion foil is prepared.
It realizes low-voltage corrosion foil with moderate pore size, uniform pore size distribution, suitable for 50-100Vf voltage segment applications, sandwich thickness reaches more than 37μm and tensile force reaches more than 27N/cm, and is suitable for the preparation of automotive grade aluminum electrolytic capacitors.
Smart Images

Figure CN118957725A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum foil, and more specifically, to a low-pressure corrosion foil and a preparation method and application thereof. Background Art
[0002] Automotive grade capacitors are a very important component in automotive circuits, and their function is to stabilize the voltage of the entire automotive circuit system. In the automotive circuit system, the presence of high-power load devices such as engines and gearboxes will cause voltage fluctuations and noise interference. If not handled, it will have a serious impact on the normal operation of automotive electronic equipment, and even cause some failures and damage. Therefore, the application of automotive grade capacitors is particularly necessary. Since the environment in which cars are stored and driven is mostly harsh, and the internal space of the car is limited, the requirements for automotive grade capacitors in terms of high capacitance, low ESR, low leakage current, high temperature stability, etc. are relatively high. This requires the anode foil to have high specific capacitance, high strength, and the size of the pits is suitable for the applied voltage and evenly distributed, and the pit structure is stable.
[0003] There are two main processes for existing low-voltage products. One of them uses a sine wave or square wave AC waveform. The aperture of the anode foil is relatively large and the strength is relatively low, which is more suitable for large-width aluminum electrolytic capacitors above 100Vf. The other AC waveform is a triangular wave. The aperture of the anode foil is smaller, which is more suitable for products below 50Vf. For products in the formation voltage range of 50-100Vf, it does not require a large aperture. If the anode foil prepared by sine wave or square wave is suitable for products above 100Vf due to its large aperture, and the specific capacitance of the anode foil in this voltage range is low, thicker light foil is required, which increases the preparation cost; if the anode foil prepared by triangular wave is suitable for products below 50Vf due to its small aperture, a large number of small holes will be completely blocked by aluminum oxide during formation. For low-voltage foils in the range of 50-100Vf, it is still necessary to explore waveforms with better performance.
[0004] CN 105006367 A discloses a step non-sinusoidal frequency conversion corrosion method for increasing the specific capacitance of low-voltage anode foil for aluminum electrolytic capacitors and reducing contact resistance and discrete rate by adjusting power waveform, power frequency, etching solution composition, current density, etching time and temperature. The method adopts a combined waveform and combines a specific multi-stage etching solution to achieve low-temperature corrosion, less weight loss of aluminum foil and good contact resistance. When the formation voltage is 20Vf, the specific capacitance is 85-95μF / cm 2 However, the prior art does not pay attention to the problem that the pore size distribution of the etched foil is uneven within the voltage range of 50-100 Vf, and the size of the etched holes is not suitable for the voltage within this range. Summary of the invention
[0005] In order to overcome the above problems existing in the prior art, the purpose of the present invention is to provide a method for preparing a low-voltage etching foil, by adjusting the content of the etching solution components, the waveform of the alternating current, the current density, and the power-on time to obtain a low-voltage foil with high specific capacity, high strength, and a uniform distribution of etching holes suitable for 50-100Vf.
[0006] Another object of the present invention is to provide a low-pressure corrosion foil.
[0007] Another object of the present invention is to provide a vehicle-grade capacitor.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing a low-pressure corrosion foil, characterized in that it comprises the following steps:
[0010] S1. Pretreatment: pre-treating the electronic light foil in a treatment solution;
[0011] S2. One-stage corrosion: the aluminum foil is electrically corroded in the corrosion solution;
[0012] S3. Medium treatment: passivating the aluminum foil in a medium treatment solution;
[0013] S4. Hole growth corrosion: The treated aluminum foil is electro-etched in the etching solution;
[0014] S5. Repeat steps S3 to S4 8 to 10 times;
[0015] S6. Post-treatment: The aluminum foil after electrochemical corrosion is immersed in a sulfuric acid solution and a polyol solution, respectively, and then subjected to heat treatment to obtain a low-voltage corrosion electrode foil;
[0016] In step S2, the etching solution is an aqueous solution of 0.5-2 wt.% sulfuric acid, 5-25 wt.% hydrogen chloride and 2-10 wt.% aluminum chloride, the temperature of the etching solution is 40°C-55°C, and the current density of the electro-etching is 0.45-0.54 A / cm 2 , the current frequency is 25-35Hz, and the power-on time is 25-65s;
[0017] In step S4, the etching solution is an aqueous solution of 0.5-2 wt.% sulfuric acid, 5-20 wt.% hydrogen chloride and 6-15 wt.% aluminum chloride, the temperature of the etching solution is 35°C-50°C, and the current density of the electro-etching is 0.35-0.41 A / cm 2 , the current frequency is 20-30Hz, and the power-on time is 90-130s;
[0018] In step S5, the temperature of the treatment solution and the etching solution is 15-35°C, and the current density of the electro-etching is 0.15-0.3A / cm 2 , the current frequency is 15 to 25 Hz, and as the number of repeated steps increases, at least one of the temperature, current density or current frequency decreases;
[0019] In step S2 and step S4, the current waveform of the energized corrosion is a superimposed waveform of a square wave and a triangular wave. The width of the square wave in the energized corrosion current waveform is 2% to 8% of the superimposed waveform period, the amplitude of the square wave is 20% to 35% of the superimposed waveform amplitude, and the number of square waves in one period is 12 to 16.
[0020] The invention mainly prepares a low-pressure etching foil with moderate pore size, uniform pore size distribution, high strength and high specific volume by adjusting the content of etching solution components in a first-stage etching and pore growth corrosion stage and the current waveform of the electrified corrosion.
[0021] Traditional corrosion current waveforms are mostly square waves, triangular waves, and sine waves. Because the current of the square wave rises to a very large level in an instant, the active point area begins to form holes, and there are more holes. The current size remains unchanged for a long time, resulting in parallel holes. Therefore, the hole diameter of the corrosion foil using the square wave is too large, and it is more suitable for products above 100Vf. As the hole diameter increases, the increase in weight loss is greater, which can easily cause problems such as foil brittleness. For triangular waves and sine waves, the current is always in the process of changing, and fewer parallel holes are formed. Except for the small current change at the peak current of the sine wave, the current change rate of the rest is different. The triangular wave is different. The current change rate remains constant for a period of time, which can ensure that the corrosion pit has the opportunity to develop vertically. At the same time, the constant current size can trigger the initiation of new pitting. The triangular wave has small holes, large density, and deep holes, while the sine wave has large and shallow holes, which are not suitable for the application range of 50-100Vf. The waveform of the present invention is a square wave superimposed on a triangular wave, which increases the pore density and hole depth and appropriately enlarges the pore diameter, thereby being more suitable for application in the voltage range of 50-100Vf.
[0022] The width of the square wave in the superimposed waveform mainly affects the size of the aperture. The larger the width of the square wave, the larger the aperture. The amplitude of the square wave mainly affects the depth of the hole. The larger the amplitude, the deeper the hole. The number of square waves mainly affects the size of the aperture. The more square waves, the larger the aperture. Therefore, it is necessary to control the width, amplitude and number of square waves in the superimposed waveform within a suitable range so that the prepared etched foil is suitable for application in the voltage range of 50-100Vf.
[0023] The temperature of the liquid medicine will increase the activity of chloride ions. At a higher activity, it is conducive to multiple pores. If the pores need to be deeper, the pores should be suppressed and the temperature should be lowered. By adjusting the temperature of the liquid medicine, the activity of chloride ions is affected, and the growth of pores is regulated.
[0024] The current density and power-on time of the electrified corrosion affect the electrostatic capacity of the aluminum foil. If the current density is too small, the hole growth will be insufficient, and if it is too large, the corrosion layer of the aluminum foil will fall off due to the violent reaction. If the power-on time is too short, the pits cannot grow fully, and if the time is too long, the thickness of the aluminum foil will become thinner.
[0025] The current frequency needs to be controlled within a suitable range for the initial pore formation and the later hole growth corrosion. In the initial stage, the pore formation is mainly carried out by a slightly higher current frequency. The higher the frequency, the greater the pore density, and the aluminum ions are kept at a higher state to balance the pore formation conditions under high frequency and prevent uneven pores caused by over-corrosion. The later hole deepening requires a slightly lower current frequency to reduce the number of pores, and the current focuses more on expanding and deepening the pores, so as not to cause the pores formed in the previous stage to merge and the pores can develop to a deeper level.
[0026] Preferably, in step S2, the etching solution is an aqueous solution of 0.5-2 wt.% sulfuric acid, 10-20 wt.% hydrogen chloride and 2-6 wt.% aluminum chloride, the temperature of the etching solution is 48°C-52°C, and the current density of the electrocorrosion is 0.4-0.45 A / cm 2 The current frequency is 28-33Hz and the power-on time is 55-60s.
[0027] Preferably, in step S4, the etching solution is an aqueous solution of 0.5-2 wt.% sulfuric acid, 5-15 wt.% hydrogen chloride and 6-9 wt.% aluminum chloride, the temperature of the etching solution is 42°C-48°C, and the current density of the electrocorrosion is 0.37-0.4 A / cm 2 The current frequency is 25-30Hz and the power-on time is 110-120s.
[0028] Preferably, in step S5, the temperature of the intermediate treatment solution and the etching solution is 18-28°C, and the current density of the electrocorrosion is 0.19-0.25 A / cm 2 , the current frequency is 18 to 24 Hz, and as the number of repeated steps increases, at least one of the temperature, current density or current frequency decreases.
[0029] Preferably, in step S3, the intermediate treatment liquid is a dihydrogen phosphate aqueous solution with a concentration of 2 to 5 wt.%, the passivation temperature is 80 to 95° C., and the passivation time is 45 to 75 s.
[0030] The aluminum foil is immersed in a solution containing phosphate, and a primary aluminum phosphate film is formed on the surface of the aluminum foil through a chemical reaction with metallic aluminum. This phosphating layer has good corrosion resistance and can protect the foil. In the next step of corrosion, the surface of the foil will not produce invalid dissolution such as surface erosion.
[0031] Preferably, the dihydrogen phosphate may be at least one of potassium dihydrogen phosphate, sodium dihydrogen phosphate, and calcium dihydrogen phosphate.
[0032] Preferably, in step S6, the concentration of the sulfuric acid solution is 15-25wt.%, the immersion temperature is 55-65°C, and the immersion time is 50-90s; the concentration of the polyhydroxy compound solution is 1-3wt.%, the immersion temperature is 55-65°C, and the immersion time is 50-90s.
[0033] The polyol may be triethanolamine.
[0034] The function of the polyhydroxy compound in the present invention is to utilize its hydroxyl group to form a hydrate film with aluminum, thereby promoting the formation of a crystalline aluminum oxide film on the surface of the foil and providing a better basis for subsequent chemical formation.
[0035] Preferably, in step S6, the heat treatment is performed at a temperature of 450 to 500° C. and for a time of 20 to 40 seconds.
[0036] The role of heat treatment is to transform the alumina crystal form, so that the amorphous β-alumina on the surface of the aluminum foil and inside the pores is transformed into the crystalline γ-alumina. It also removes the bound water in the hydrated film and also has the function of drying the corroded foil. If the heat treatment temperature is too high, over-crystallization may occur, causing the aluminum oxide film to be brittle and cracked; if the heat treatment temperature is too low, an effective specific crystal aluminum oxide film cannot be formed on the surface of the aluminum foil, and the pressure resistance is poor.
[0037] Preferably, after step S1, step S2 and step S3, water washing treatment is also included respectively.
[0038] Preferably, in step S1, the treatment liquid is a 1-3 wt. % phosphoric acid solution, the temperature of the treatment liquid is 60-80° C., and the treatment time is 30-60 s.
[0039] The purpose of water washing is to clean away waste acid and other substances remaining on the surface of the foil.
[0040] The present invention also protects the low-pressure etching foil prepared by the method for preparing the low-pressure etching foil.
[0041] The present invention also protects a low-pressure corrosion foil, wherein the specific capacitance of the low-pressure corrosion foil 64Vf is 28-30 μF / cm 2 The sandwich thickness is 37-40 μm, the average pore size is 160-200 nm, and the tensile force is 27-29 N / cm.
[0042] Under the applied voltage of 50-100Vf, since theoretically each volt of voltage requires an aluminum oxide thickness of about 1.4-1.5nm, the maximum thickness of aluminum oxide required for this range of applied voltage is 150nm. In order to ensure that the aluminum oxide grown during formation does not completely block the holes, the average pore size needs to be controlled at 160-200nm, and most pore sizes are controlled at around 180nm.
[0043] The present invention also protects a vehicle-standard capacitor, including an aluminum electrolytic capacitor, and the aluminum electrolytic capacitor includes the low-voltage corrosion foil described above.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The invention prepares a low-pressure etching foil with moderate pore size, uniform pore size distribution, high strength and high specific volume by adjusting the content of etching solution components in the first stage of etching and the pore growth corrosion stage, the current waveform of the electrified corrosion, the current density, the electrification time and other parameters.
[0046] The present invention prepares low-voltage corrosion foil, and the pore size is controlled between 160 and 200 nm, which is more suitable for a formation voltage of 50-100 Vf. The core thickness can reach more than 37 μm, and the tension can reach more than 27 N / cm, which is more suitable for cutting products with small widths and is suitable for preparing automotive-grade aluminum electrolytic capacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 The current waveforms of the electrocorrosion in Examples 1 to 3 are shown.
[0048] Figure 2 This is the current waveform of the electric corrosion in Example 4.
[0049] Figure 3 This is the current waveform of the electrical corrosion in Example 5.
[0050] Figure 4 This is the current waveform of the electric corrosion in Example 6.
[0051] Figure 5 This is the current waveform of the electric corrosion in comparative example 1.
[0052] Figure 6 This is the current waveform of the electric corrosion in comparative example 2.
[0053] Figure 7 This is the current waveform of the electric corrosion in comparative example 3.
[0054] Figure 8 The pore size distribution diagram of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0055] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0056] In all the current waveforms of the electrocorrosion in Examples 1 to 3, the width of the square wave is 4% of the period of the superimposed waveform, the amplitude of the square wave is 25% of the amplitude of the superimposed waveform, and the number of square waves in one period is 12. Figure 1 shown.
[0057] Example 1
[0058] A method for preparing a low-pressure corrosion foil comprises the following steps:
[0059] S1. Pretreatment: The electronic light foil is placed in a 2wt.% phosphoric acid treatment solution at a temperature of 75°C for 50s;
[0060] S2. One-stage corrosion: The pretreated aluminum foil was placed in an aqueous solution of 1wt.% sulfuric acid, 15wt.% hydrogen chloride and 4wt.% aluminum chloride at a temperature of 50°C, and a current density of 0.5A / cm 2 , a corrosion test was conducted under an alternating current with a frequency of 30 Hz and the power-on time was 60 s;
[0061] S3. Medium treatment: immerse a section of the corroded foil in a 3wt.% dihydrogen phosphate solution at a temperature of 85°C for 60 seconds;
[0062] S4. Hole Growth Corrosion: The treated aluminum foil was placed in a solution of 1wt.% sulfuric acid, 10wt.% hydrogen chloride and 7.5wt.% aluminum chloride at a temperature of 45°C, and a current density of 0.4A / cm 2 , deep corrosion was carried out under AC with a frequency of 27 Hz and the power-on time was 120 s;
[0063] S5.1 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 28°C, and the current density is 0.25A / cm 2 , the current frequency is 24Hz;
[0064] S5.2 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 23°C, and the current density is 0.25A / cm 2 , the current frequency is 22Hz;
[0065] S5.3 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 20°C, and the current density is 0.25A / cm 2 , the current frequency is 20Hz;
[0066] S5.4 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 18°C, and the current density is 0.25A / cm 2 , the current frequency is 18Hz;
[0067] S6. Post-treatment: The AC-corroded foil was placed in a 20wt.% sulfuric acid solution at a temperature of 60°C for 60 seconds, and then the foil was immersed in a 2wt.% triethanolamine solution at a temperature of 60°C for 60 seconds;
[0068] Heat treatment: The post-treated foil was heat treated at 480°C for 35 seconds.
[0069] Example 2
[0070] A method for preparing a low-pressure corrosion foil comprises the following steps:
[0071] S1. Pretreatment: The electronic light foil is placed in a 2wt.% phosphoric acid treatment solution at a temperature of 75°C for 50s;
[0072] S2. One-stage corrosion: The pretreated aluminum foil was placed in an aqueous solution of 1wt.% sulfuric acid, 15wt.% hydrogen chloride and 6wt.% aluminum chloride at a temperature of 50°C, and a current density of 0.5A / cm 2 , a corrosion test was conducted under an alternating current with a frequency of 30 Hz and a power-on time of 55 s;
[0073] S3. Medium treatment: a section of the corroded foil is immersed in a 3wt.% dihydrogen phosphate solution at a temperature of 85°C for 55s;
[0074] S4. Hole growth corrosion: The treated aluminum foil was placed in a solution of 1wt.% sulfuric acid, 10wt.% hydrogen chloride and 7.5wt.% aluminum chloride at a temperature of 45°C, and a current density of 0.4A / cm 2 , deep corrosion was carried out under AC with a frequency of 27 Hz and the power-on time was 110 s;
[0075] S5.1 Repeat steps (3) and (4) 3 times, except that the temperature of the treatment solution and the etching solution is 28°C, and the current density is 0.25A / cm 2 , the current frequency is 24Hz;
[0076] S5.2 Repeat steps (3) and (4) 3 times, except that the temperature of the treatment solution and the etching solution is 22°C, and the current density is 0.25A / cm 2 , the current frequency is 20Hz;
[0077] S5.3 Repeat steps (3) and (4) 3 times, except that the temperature of the treatment solution and the etching solution is 18°C, and the current density is 0.25A / cm 2 , the current frequency is 18Hz;
[0078] S6. Post-treatment: The AC-corroded foil was placed in a 20wt.% sulfuric acid solution at a temperature of 60°C for 60 seconds, and then the foil was immersed in a 2wt.% triethanolamine solution at a temperature of 60°C for 60 seconds;
[0079] Heat treatment: The post-treated foil is heat treated at 480°C for 35 seconds.
[0080] Example 3
[0081] A method for preparing a low-pressure corrosion foil comprises the following steps:
[0082] S1. Pretreatment: The electronic light foil is placed in a 2wt.% phosphoric acid treatment solution at a temperature of 75°C for 50s;
[0083] S2. One-stage corrosion: The pretreated aluminum foil was placed in an aqueous solution of 1wt.% sulfuric acid, 15wt.% hydrogen chloride and 4wt.% aluminum chloride at a temperature of 50°C, and a current density of 0.48A / cm 2 , a corrosion test was conducted under an alternating current with a frequency of 31 Hz and a power-on time of 55 s;
[0084] S3. Medium treatment: a section of the corroded foil is immersed in a 3wt.% dihydrogen phosphate solution at a temperature of 85°C for 55s;
[0085] S4. Hole growth corrosion: The treated aluminum foil was placed in a solution of 1wt.% sulfuric acid, 10wt.% hydrogen chloride and 7.5wt.% aluminum chloride at a temperature of 45°C, and a current density of 0.37A / cm 2 , deep corrosion was carried out under AC with a frequency of 28 Hz and the power-on time was 110 s;
[0086] S5.1 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 27°C, and the current density is 0.23A / cm 2 , the current frequency is 24Hz;
[0087] S5.2 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 23°C, and the current density is 0.22A / cm 2 , the current frequency is 22Hz;
[0088] S5.3 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 21°C, and the current density is 0.21A / cm 2 , the current frequency is 20Hz;
[0089] S5.4 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 19°C, and the current density is 0.20A / cm 2 , the current frequency is 19Hz;
[0090] S5.5 Repeat steps (3) and (4) twice, except that the temperature of the treatment solution and the etching solution is 17°C, and the current density is 0.19 A / cm 2 , the current frequency is 18Hz;
[0091] S6. Post-treatment: The AC-corroded foil was placed in a 20wt.% sulfuric acid solution at a temperature of 60°C for 60 seconds, and then the foil was immersed in a 2wt.% triethanolamine solution at a temperature of 60°C for 60 seconds;
[0092] Heat treatment: The post-treated foil is heat treated at 480°C for 35 seconds.
[0093] Example 4
[0094] A method for preparing a low-voltage corrosion foil, which differs from Example 1 in that in step S2 and step S4, the width of the square wave in the current waveform of the electrified corrosion is 6% of the period of the superimposed waveform, the amplitude of the square wave is 25% of the amplitude of the superimposed waveform, and the number of square waves in one period is 12. The current waveform is as follows Figure 2 shown.
[0095] Example 5
[0096] A method for preparing a low-voltage corrosion foil, which differs from Example 1 in that in step S2 and step S4, the width of the square wave in the corrosion current waveform is 4% of the superimposed waveform period, the amplitude of the square wave is 30% of the superimposed waveform amplitude, and the number of square waves in one period is 12. The current waveform is as follows Figure 3 shown.
[0097] Example 6
[0098] A method for preparing a low-voltage corrosion foil, which differs from Example 1 in that in step S2 and step S4, the width of the square wave in the corrosion current waveform is 4% of the superimposed waveform period, the amplitude of the square wave is 25% of the superimposed waveform amplitude, and the number of square waves in one period is 16. The current waveform is as follows Figure 4 shown.
[0099] Comparative Example 1
[0100] A method for preparing a low-voltage corrosion foil, which differs from Example 1 in that in step S2 and step S4, the waveform of the corrosion current is a traditional triangular wave. The current waveform is as follows Figure 5 shown.
[0101] Comparative Example 2
[0102] A method for preparing a low-voltage corrosion foil, which differs from Example 1 in that in step S2 and step S4, the waveform of the corrosion current is a sine wave. The current waveform is as follows Figure 6 shown.
[0103] Comparative Example 3
[0104] A method for preparing a low-voltage corrosion foil, which differs from Example 1 in that in step S2 and step S4, the waveform of the corrosion current is a traditional square wave. Figure 7 shown.
[0105] Comparative Example 4
[0106] A method for preparing a low-voltage corrosion foil, which differs from Example 1 in that the current density in step S2 and step S4 is increased by 20%.
[0107] Comparative Example 5
[0108] A method for preparing a low-voltage corrosion foil is different from Example 1 in that the power-on time in step S2 and step S4 is increased by 20%.
[0109] Results
[0110] Tensile test method: Use a tensile tester (WZL-100B horizontal computer tensile tester) to test the tensile force of the corroded foil. The test tensile speed is 10±1mm / min, and the tensile force at the break is measured. Measure five test pieces, and take the average tensile force as the tensile strength of the foil, in N / cm. When reading the data, keep one decimal place and round it off.
[0111] The specific volume, tensile force, sandwich thickness, average pore size and corrosion foil thickness of the low-pressure corrosion foils of the above embodiments and comparative examples were tested respectively.
[0112] The specific test results of each embodiment are shown in Table 1 below:
[0113] Table 1
[0114]
[0115] The test results of each comparative example are shown in Table 2 below:
[0116] Table 2
[0117]
[0118] It can be seen from the above data that the pore size of the low-voltage corrosion foil of the present invention is controlled between 160-200nm, which is more suitable for 50-100Vf, and the core thickness can reach more than 37μm, and the tensile force can reach more than 27N / cm, which is more suitable for cutting small-width products and is suitable for preparing automotive-grade aluminum electrolytic capacitors.
[0119] It can be seen from Comparative Example 1 that in step S2 and step S4, the waveform of the corrosion current is a traditional triangular waveform, and the aperture of the low-voltage corrosion foil is too small. When applied to this voltage range, a large number of tiny holes will be completely blocked by aluminum oxide, and because aluminum oxide is very brittle, thicker plain foil is required to support it, resulting in increased costs.
[0120] It can be seen from Comparative Example 2 that in step S2 and step S4, the waveform of the corrosion current is a sine wave, which will cause the aperture of the low-voltage corrosion foil to be too large.
[0121] It can be seen from Comparative Example 3 that in step S2 and step S4, the waveform of the corrosion current is a traditional square wave waveform, and pore formation is likely to occur during the corrosion process, resulting in the pore size of the low-voltage corrosion foil being too large, and the output current is always large, resulting in increased weight loss. The increase in specific volume cannot increase in the same proportion as the increase in weight loss, causing the foil to be brittle and easy to break.
[0122] It can be seen from Comparative Example 4 that in step S2 and step S4, the current density of the corrosion current is increased, thereby increasing the corrosion amount, slightly increasing the pore density, and reducing the pore size, which is not suitable for a formation voltage above 50 Vf.
[0123] It can be seen from Comparative Example 5 that in step S2 and step S4, the corrosion time is simply increased. As the corrosion time increases, the damage increases and the corrosion layer becomes deeper, but the increase in specific volume is limited. As the amount of corrosion increases, the sandwich thickness becomes thinner and the strength becomes lower, which is not suitable for a formation voltage above 50Vf.
[0124] Figure 8 The pore size distribution diagram of Example 1 and Comparative Example 1 shows that when the cumulative pore capacity is greater than 0.0012 mL / g, the pore size of the corrosion foil of Example 1 is mainly concentrated between 160-200 nm, and the pore size distribution is uniform; while the pore size of the corrosion foil of Comparative Example 1 is mainly distributed between 100-170 nm, the pore size distribution span is large, the pore size distribution is uneven, the pore size is small, and it is not suitable for a formation voltage above 50 Vf.
[0125] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a low-pressure corrosion foil, characterized in that: The steps include: S1. Pretreatment: pre-treating the electronic light foil in a treatment solution; S2. One-stage corrosion: the aluminum foil is electrically corroded in the corrosion solution; S3. Medium treatment: passivating the aluminum foil in a medium treatment solution; S4. Hole growth corrosion: The treated aluminum foil is electro-etched in the etching solution; S5. Repeat steps S3 to S4 8 to 10 times; S6. Post-treatment: The aluminum foil after electrochemical corrosion is immersed in a sulfuric acid solution and a polyol solution, respectively, and then subjected to heat treatment to obtain a low-voltage corrosion electrode foil; In step S2, the etching solution is an aqueous solution of 0.5-2 wt.% sulfuric acid, 5-25 wt.% hydrogen chloride and 2-10 wt.% aluminum chloride, the temperature of the etching solution is 40°C-55°C, and the current density of the electro-etching is 0.45-0.54 A / cm 2 , the current frequency is 25-35Hz, and the power-on time is 25-65s; In step S4, the etching solution is an aqueous solution of 0.5-2 wt.% sulfuric acid, 5-20 wt.% hydrogen chloride and 6-15 wt.% aluminum chloride, the temperature of the etching solution is 35°C-50°C, and the current density of the electro-etching is 0.35-0.42 A / cm 2 , the current frequency is 20-30Hz, and the power-on time is 90-130s; In step S5, the temperature of the treatment solution and the etching solution is 15-35°C, and the current density of the electro-etching is 0.15-0.3A / cm 2 , the current frequency is 15 to 25 Hz, and as the number of repeated steps increases, at least one of the temperature, current density or current frequency decreases; In step S2 and step S4, the current waveform of the energized corrosion is a superimposed waveform of a square wave and a triangular wave. The width of the square wave in the energized corrosion current waveform is 2% to 8% of the superimposed waveform period, the amplitude of the square wave is 20% to 35% of the superimposed waveform amplitude, and the number of square waves in one period is 12 to 16.
2. The method for preparing the low-pressure corrosion foil according to claim 1, characterized in that: In step S2, the etching solution is an aqueous solution of 0.5-2 wt.% sulfuric acid, 10-20 wt.% hydrogen chloride and 2-6 wt.% aluminum chloride, the temperature of the etching solution is 48°C-52°C, and the current density of the electro-etching is 0.4-0.45 A / cm 2 The current frequency is 28-33Hz and the power-on time is 55-60s.
3. The method for preparing the low-pressure etching foil according to claim 1, characterized in that: In step S4, the etching solution is an aqueous solution of 0.5-2 wt.% sulfuric acid, 5-15 wt.% hydrogen chloride and 6-9 wt.% aluminum chloride, the temperature of the etching solution is 42°C-48°C, and the current density of the electro-etching is 0.37-0.4 A / cm 2 The current frequency is 25-30Hz and the power-on time is 110-120s.
4. The method for preparing the low-pressure etching foil according to claim 1, characterized in that: In step S5, the temperature of the intermediate treatment solution and the etching solution is 18-28°C, and the current density of the electro-etching is 0.19-0.25A / cm 2 , the current frequency is 18 to 24 Hz, and as the number of repeated steps increases, at least one of the temperature, current density or current frequency decreases.
5. The method for preparing the low-pressure etching foil according to claim 1, characterized in that: In step S3, the intermediate treatment liquid is a dihydrogen phosphate aqueous solution with a concentration of 2 to 5 wt.%, the passivation temperature is 80 to 95° C., and the passivation time is 45 to 75 seconds.
6. The method for preparing the low-pressure etching foil according to claim 1, characterized in that: In step S6, the concentration of the sulfuric acid solution is 15-25wt.%, the immersion temperature is 55-65°C, and the immersion time is 50-90s; the concentration of the polyhydroxy compound solution is 1-3wt.%, the immersion temperature is 55-65°C, and the immersion time is 50-90s.
7. The method for preparing the low-pressure etching foil according to claim 1, characterized in that: In step S6, the heat treatment is performed at a temperature of 450 to 500°C and for a time of 20 to 40 seconds.
8. The low-pressure etching foil prepared by the method for preparing the low-pressure etching foil according to any one of claims 1 to 7.
9. The low-pressure corrosion foil according to claim 8, characterized in that: The specific capacitance of the low-voltage corrosion foil 64Vf is 28-30 μF / cm 2 , thickness is 37-40μm, average pore size is 160-200nm, and tensile force is 27-29N / cm.
10. A vehicle-grade capacitor, characterized in that: An aluminum electrolytic capacitor is included, wherein the aluminum electrolytic capacitor includes the low voltage etching foil of claim 8.
Citation Information
Cited By
Composite pulse waveform hole forming technology for high-thickness aluminum foil and anode foil
CN119361327A
High-thickness aluminum foil anode foil composite pulse waveform hole-making technology
CN119361327B
Composite pulse waveform pore generation technology for high-thickness aluminium foil anode foil
WO2025251761A1