Preparation method and application of compound sodium lithium boron sulfate

The lithium sodium boron sulfate material prepared by solid phase synthesis, high temperature melting method or hydrothermal method solves the problem of insufficient transmittance of existing birefringent materials in the deep ultraviolet band, and achieves a high birefringence in this band and transmittance, expanding its application scope.

CN118957758APending Publication Date: 2024-11-15XINJIANG TECH INST OF PHYSICS & CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411012504.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The limited transmittance of existing birefringent materials in the deep ultraviolet band limits their applications in polarization science, optical spectroscopy and laser industries, and most materials have insufficient birefringent index in the deep ultraviolet band.

Method used

The compound lithium boron sulfate (Li2NaB3S2O12) is prepared by solid phase synthesis method, high temperature melting method or hydrothermal method. This material has a monoclinic crystal structure, the space group is P21/c, the cutoff absorption edge is 184nm, and the experimental birefringence is It reached 0.057 at 1064nm, which matched the theoretical calculated value, and the calculated birefringence at 200nm reached 0.121.

Benefits of technology

The preparation of lithium boron sulfate material with a high birefringence and transmittance in the deep ultraviolet band has been achieved, and the application range of birefringence materials has been expanded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957758A_ABST
    Figure CN118957758A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a compound sodium lithium borosulfate, the chemical formula of the compound is Li2NaB3S2O12, the molecular weight is 325.43, the compound belongs to a monoclinic system, the space group is P21 / c, the cell parameters are as follows: a is equal to 11.6720, b is equal to 8.2574, c is equal to 9.6126, alpha is equal to beta is equal to 90 degrees, gamma is equal to 97.940 degrees, the unit cell volume is 917.583, and the compound is prepared by adopting a solid-phase synthesis method, a high-temperature melt method or a hydrothermal method. The sodium lithium boron sulfate does not deliquesce in air and is stable at the temperature of 463 DEG C or below, the cut-off absorption edge is 184 nm, the experimental birefringence at the position of 1064 nm reaches 0.057 and is basically matched with the theoretical calculation value of 0.052, the calculated birefringence at the position of 200 nm reaches 0.121, and therefore the sodium lithium boron sulfate is expected to serve as a deep ultraviolet birefringence crystal material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a compound sodium lithium borosulfate, belonging to the field of new materials. Background Art

[0002] Since birefringent materials can control the polarization of light, they are widely used in various fields such as polarization science, optical spectroscopy and laser industry. According to current research findings, the research and exploration of birefringent materials are mainly focused on π-conjugated groups with large polarizability anisotropy, such as [BO 3 ],[CO 3 ], [NO 3 ], which makes the crystal materials with π conjugated groups have relatively large birefringence, but at the same time, these materials are also constrained by the π conjugation effect, which limits their transmittance in the deep ultraviolet band. 2 , BaB 2 O 4 Most birefringent materials only reach the ultraviolet band, but not the deep ultraviolet band, which limits the wider application of birefringent materials. Therefore, it is urgent to discover new birefringent materials, which have both π-conjugated groups with large polarizability anisotropy to obtain a larger birefringence and non-π-conjugated groups to enable the material to obtain a certain transmittance in the deep ultraviolet band. Summary of the invention

[0003] The present invention aims to provide a preparation method and use of a compound sodium lithium borosulfate, the chemical formula of which is Li 2 NaB 3 S 2 O 12 , molecular weight is 325.43, belongs to monoclinic system, space group is P2 1 / c, the unit cell parameters are α=β=90°,γ=97.940°,the unit cell volume is The sodium lithium borosulfate obtained by the method of the present invention does not deliquesce in the air, is stable below 463°C, has a cut-off absorption edge of 184nm, and an experimental birefringence of 0.057 at 1064nm, which is basically consistent with the theoretical calculated value of 0.052, and the calculated birefringence at 200nm is 0.121, so it is expected to be used as a deep ultraviolet birefringent crystal material.

[0004] The present invention provides a method for preparing a compound sodium lithium borosulfate, wherein the chemical formula of the compound is Li 2 NaB 3 S 2 O 12, molecular weight is 325.43, belongs to monoclinic system, space group is P2 1 / c, the unit cell parameters are α=β=90°,γ=97.940°,the unit cell volume is It is made by solid phase synthesis method, high temperature melt method or hydrothermal method;

[0005] The solid phase synthesis method is used to prepare the compound sodium lithium borosulfate, and the specific operation is carried out according to the following steps:

[0006] The molar ratio of Li:Na:B:S=3-5:1.5-2.5:5-10:3-7.5 is to mix the Li-containing compound, the Na-containing compound, the B-containing compound and the S-containing compound uniformly, put them into a ceramic crucible, and then put them into a muffle furnace, heat them to 370-430°C, and keep the temperature constant for 30-60 hours to obtain the compound Li 2 NaB 3 S 2 O 12 ; The Li-containing compound is LiBO 2 , Li 2 CO 3 , Li 2 SO 4 、LiHCO 3 or LiOH; containing Na as compound NaBO 2 、Na 2 CO 3 、Na 2 SO 4 、NaHCO 3 or NaOH; Compound B is H 3 BO 3 , B 2 O 3 or HBO 2 ; The S-containing compound is Li 2 SO 4 、Na 2 SO 4 , Li 2 SO 3 、Na 2 SO 3 、LiHSO 4 or NaHSO 4 ;

[0007] The high temperature melt method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0008] a. The molar ratio of Li:Na:B:S=3-5:1.5-2.5:5-10:3-7.5 is to mix the Li-containing compound, the Na-containing compound and the B-containing compound evenly, put them into a ceramic crucible, and then put them into a muffle furnace, heat them to 370-430°C, and keep the temperature constant for 30-60 hours to obtain the compound Li 2 NaB 3 S 2 O 12 polycrystalline powder; the Li-containing compound is LiBO 2 , Li 2 CO 3 , Li 2 SO 4 、LiHCO 3 or LiOH; containing Na as compound NaBO 2 、Na 2 CO 3 、Na 2 SO 4 、NaHCO 3 or NaOH; Compound B is H 3 BO 3 , B 2 O 3 or HBO 2 ; The S-containing compound is Li 2 SO 4 、Na 2 SO 4 , Li 2 SO 3 、Na 2 SO 3 、LiHSO 4 or NaHSO 4 ;

[0009] b. Compound Li obtained in step a 2 NaB 3 S 2 O 12 The polycrystalline powder and flux are mixed evenly in a molar ratio of 1:0.1-0.5, and then put into a clean platinum crucible, and the temperature is raised to 500-550°C at a rate of 40-50°C / h, and the temperature is kept constant for 30-45 hours to obtain a mixed melt; the flux is H 3 BO 3 , B 2 O 3 , HBO 2 , PbO or PbF 2 ;

[0010] c. Place the mixed melt obtained in step b in a single crystal furnace, then cool it down to 450-480°C at a cooling rate of 0.1-0.5°C / h, cool it down to 350-400°C at a cooling rate of 0.2-0.6°C / h, and then cool it down to 30°C at a cooling rate of 3-10°C / h to obtain compound Li 2 NaB 3 S 2 O 12 ;

[0011] The hydrothermal method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0012] a. Mix the Li-containing compound, the Na-containing compound and the B-containing compound in a molar ratio of Li:Na:B:S=3-5:1.5-2.5:5-10:3-7.5, put them into a ceramic crucible, and then put them into a muffle furnace, heat them to 370-430°C, and keep the temperature constant for 30-60 hours to obtain the compound Li 2 NaB 3 S 2 O 12 polycrystalline powder; the Li-containing compound is LiBO 2 , Li 2 CO 3 , Li 2 SO 4 、LiHCO 3 or LiOH; containing Na as compound NaBO 2 、Na 2 CO 3 、Na 2 SO 4 、NaHCO 3 or NaOH; Compound B is H 3 BO 3 , B 2 O 3 or HBO 2 ; The S-containing compound is Li 2 SO 4 、Na 2 SO 4 , Li 2 SO 3 、Na 2 SO 3 、LiHSO 4 or NaHSO 4 ;

[0013] b. Compound Li obtained in step a 2 NaB 3 S 2 O 12The polycrystalline powder is placed in 5-30 mL of deionized water to dissolve, and the incompletely dissolved mixture is subjected to ultrasonic treatment at a temperature of 20-50° C. for 15-30 minutes to fully mix and dissolve;

[0014] c. Transfer the mixed solution obtained in step b into the liner of a clean, pollution-free autoclave with a volume of 100 mL, and tighten and seal the autoclave;

[0015] d. Place the autoclave in a thermostat, raise the temperature to 180-350°C at a rate of 10-30°C / h, keep the temperature constant for 4-7 days, and then cool it down to room temperature at a rate of 5-30°C / day to obtain compound Li 2 NaB 3 S 2 O 12 .

[0016] The compound sodium lithium borosulfate obtained by the method is used in preparing deep ultraviolet birefringent materials.

[0017] The preparation method of the compound sodium borosulfate lithium of the present invention comprises a platinum crucible, a ceramic crucible, a quartz tube, a conical flask, a beaker, and a hydrothermal kettle lined with polytetrafluoroethylene or a stainless steel liner equipped with a platinum sleeve. When the container is a quartz tube, it needs to be evacuated before sealing to avoid the quartz tube from bursting due to excessive volatilization pressure of the raw materials during the reaction. When the container is a conical flask or a beaker, the container must be cleaned with acid first, then rinsed with deionized water, and dried.

[0018] In the preparation method of the compound sodium lithium borosulfate of the present invention, the resistance furnace used in the preparation process is a muffle furnace or a drying box. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is the compound Li of the present invention 2 NaB 3 S 2 O 12 The structural diagram shows that the anionic group is composed of a planar boron-sulfur-oxygen structure;

[0020] Figure 2 is the compound Li of the present invention 2 NaB 3 S 2 O 12 The powder XRD spectrum of is consistent with the theoretical XRD spectrum;

[0021] Figure 3 is the compound Li of the present invention 2 NaB 3 S 2 O 12The EDS spectrum shows that the element types in the experiment and theory are consistent;

[0022] Figure 4 is the compound Li of the present invention 2 NaB 3 S 2 O 12 UV-Vis-NIR diffuse reflectance spectrum. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with examples. It should be noted that the present invention is not limited to the examples listed, and any improvements made on the basis of the present invention do not violate the spirit of the present invention. The raw materials or equipment used in the present invention, unless otherwise specified, are all commercially available.

[0024] Example 1

[0025] According to the reaction 2Li 2 SO 4 +Na 2 SO 4 +3B 2 O 3 →Li 2 NaB 3 S 2 O 12 , the compound Li was prepared by solid phase synthesis 2 NaB 3 S 2 O 12 :

[0026] According to the molar ratio of 1.5:0.75:2.5, Li 2 SO 4 ,Na 2 SO 4 and B 2 O 3 Mix well, put into a clean, pollution-free platinum crucible with a volume of 28 mL, heat to 370 ° C, keep constant temperature for 60 hours, and then cool naturally to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0027] Take some sample powder for powder XRD test, the test results are as follows Figure 2 shown.

[0028] Example 2

[0029] According to the reaction LiBO 2 +2NaBO 2 +3B 2 O3 +2Li 2 SO 3 →Li 2 NaB 3 S 2 O 12 , the compound Li was prepared by solid phase synthesis 2 NaB 3 S 2 O 12 :

[0030] LiBO was added in a molar ratio of 1:2:3:2 2 ,NaBO 2 ,B 2 O 3 and Li 2 SO 3 Mix well, put into a clean, pollution-free platinum crucible with a volume of 28 mL, heat to 390 ° C, keep constant temperature for 40 hours, and then cool to room temperature at a rate of 5 ° C / h to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0031] Example 3

[0032] According to the reaction 2LiBO 2 +NaBO 2 +4B 2 O 3 +2Na 2 SO 3 →Li 2 NaB 3 S 2 O 12 The solid phase synthesis method was used to prepare the synthetic compound Li 2 NaB 3 S 2 O 12 :

[0033] LiBO was added in a molar ratio of 2:1:4:2 2 ,NaBO 2 ,B 2 O 3 and Na 2 SO 3 Mix well, put into a clean, pollution-free platinum crucible with a volume of 28 mL, heat to 430 ° C, keep constant temperature for 60 hours, and then cool naturally to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0034] Take some sample powder for EDS test, the test results are as follows Figure 3 shown.

[0035] Example 4

[0036] According to the reaction Li 2 CO 3 +Na 2 CO 3 +3B 2 O 3 +2LiHSO 4 →Li 2 NaB 3 S 2 O 12 , the compound Li was prepared by solid phase synthesis 2 NaB 3 S 2 O 12 :

[0037] Li in a molar ratio of 1:1:3:2 2 CO 3 ,Na 2 CO 3 ,B 2 O 3 and Li 2 SO 4 Mix well, put into a clean, pollution-free platinum crucible with a volume of 28 mL, heat to 400 ° C, keep constant temperature for 40 hours, and then cool to room temperature at a rate of 5 ° C / h to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0038] Example 5

[0039] According to the reaction 4LiHCO 3 +NaHCO 3 +3B 2 O 3 +NaHSO 4 →Li 2 NaB 3 S 2 O 12 , the compound Li was prepared by solid phase synthesis 2 NaB 3 S 2 O 12 :

[0040] LiHCO was added in a molar ratio of 4:1:3:1 3 ,NaHCO 3 ,B 2 O3 and NaHSO 4 Mix well, put into a clean, pollution-free platinum crucible with a volume of 28 mL, heat to 420 ° C, keep constant temperature for 50 hours, and then cool to room temperature at a rate of 4 ° C / h to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0041] Example 6

[0042] According to the reaction 4LiOH+NaOH+2B 2 O 3 +NaHSO 4 →Li 2 NaB 3 S 2 O 12 , the compound Li was prepared by solid phase synthesis 2 NaB 3 S 2 O 12 :

[0043] LiOH, NaOH, HBO were mixed in a molar ratio of 4:1:4:1. 2 and NaHSO 4 Mix well, put into a clean, pollution-free platinum crucible with a volume of 28 mL, heat to 410 ° C, keep constant temperature for 50 hours, and then cool to room temperature at a rate of 4 ° C / h to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0044] Example 7

[0045] The high temperature melt method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0046] The compound Li obtained in Example 2 2 NaB 3 S 2 O 12 Polycrystalline powder and flux B in a molar ratio of 1:0.5 2 O 3 Mix well, put into a clean platinum crucible, heat to 530°C at a rate of 40°C / h, keep constant temperature for 45 hours, and obtain a mixed melt;

[0047] The mixed melt was placed in a single crystal furnace, and then cooled to 450°C at a rate of 0.4°C / h, then cooled to 380°C at a rate of 0.4°C / h, and then cooled to 20°C at a rate of 3°C / h to obtain compound Li 2 NaB3 S 2 O 12 .

[0048] Take some sample powder for UV-Vis-NIR diffuse reflectance spectroscopy test. The test results are as follows: Figure 4 shown.

[0049] Example 8

[0050] The high temperature melt method is used to prepare the compound sodium lithium borosulfate. The specific operation is carried out according to the following steps:

[0051] The compound Li obtained according to Example 1 2 NaB 3 S 2 O 12 The polycrystalline powder was mixed with flux HBO in a molar ratio of 1:0.1 2 Mix well, then put into a clean platinum crucible, first heat to 550℃ at a rate of 45℃ / h, keep constant temperature for 35 hours to obtain a mixed melt;

[0052] The mixed melt was placed in a single crystal furnace, and then cooled to 450°C at a rate of 0.2°C / h, cooled to 400°C at a rate of 0.3°C / h, and then cooled to 30°C at a rate of 7°C / h to obtain compound Li 2 NaB 3 S 2 O 12 .

[0053] Example 9

[0054] The high temperature melt method is used to prepare the compound sodium lithium borosulfate. The specific operation is carried out according to the following steps:

[0055] The compound Li obtained according to Example 3 2 NaB 3 S 2 O 12 The polycrystalline powder is mixed evenly with flux PbO at a molar ratio of 1:0.4, and then put into a clean platinum crucible, and the temperature is raised to 500°C at a rate of 42°C / h and kept at this temperature for 45 hours to obtain a mixed melt;

[0056] The mixed melt was placed in a single crystal furnace, and then cooled to 450°C at a rate of 0.4°C / h, cooled to 400°C at a rate of 0.6°C / h, and then cooled to 30°C at a rate of 3°C / h to obtain compound Li 2 NaB 3 S 2 O 12 .

[0057] Example 10

[0058] The high temperature melt method is used to prepare the compound sodium lithium borosulfate. The specific operation is carried out according to the following steps:

[0059] The compound Li obtained according to Example 4 2 NaB 3 S 2 O 12 The polycrystalline powder is mixed with flux PbF in a molar ratio of 1:0.5 2 Mix well, put into a clean platinum crucible, heat to 530°C at a rate of 40°C / h, keep constant temperature for 45 hours, and obtain a mixed melt;

[0060] The mixed melt was placed in a single crystal furnace, and then cooled to 430°C at a rate of 0.4°C / h, then cooled to 350°C at a rate of 0.4°C / h, and then cooled to 30°C at a rate of 10°C / h to obtain compound Li 2 NaB 3 S 2 O 12 .

[0061] Embodiment 11

[0062] The high temperature melt method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0063] The compound Li obtained according to Example 5 2 NaB 3 S 2 O 12 The polycrystalline powder was mixed with flux HBO in a molar ratio of 1:0.1 2 Mix well, put into a clean platinum crucible, heat to 550°C at a rate of 45°C / h, keep constant temperature for 35 hours, and obtain a mixed melt;

[0064] The mixed melt was placed in a single crystal furnace, and then cooled to 450°C at a rate of 0.2°C / h, cooled to 400°C at a rate of 0.3°C / h, and then cooled to room temperature at a rate of 7°C / h to obtain compound Li 2 NaB 3 S 2 O 12 ;

[0065] Example 12

[0066] The high temperature melt method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0067] The compound Li obtained according to Example 6 2 NaB 3 S 2 O 12 The polycrystalline powder is mixed with flux PbF in a molar ratio of 1:0.52 Mix well, put into a clean platinum crucible, heat to 550°C at a rate of 45°C / h, keep constant temperature for 30 hours, and obtain a mixed melt;

[0068] The mixed melt was placed in a single crystal furnace, and then cooled to 450°C at a rate of 0.5°C / h, cooled to 350°C at a rate of 0.6°C / h, and then cooled to 30°C at a rate of 10°C / h to obtain compound Li 2 NaB 3 S 2 O 12 .

[0069] Embodiment 13

[0070] The hydrothermal method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0071] The compound Li obtained in Example 1 2 NaB 3 S 2 O 12 The polycrystalline powder was placed in 5 mL of deionized water for dissolution, and the incompletely dissolved mixture was subjected to ultrasonic treatment at 20°C for 30 minutes to fully mix and dissolve;

[0072] The obtained mixed solution was transferred into the liner of a clean, non-polluting autoclave with a volume of 100 mL, and the autoclave was tightened and sealed;

[0073] The autoclave was placed in a thermostat, heated to 350°C at a rate of 10°C / h, kept at this temperature for 5 days, and then cooled to room temperature at a rate of 5°C / day to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0074] Embodiment 14

[0075] The hydrothermal method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0076] The compound Li obtained in Example 2 2 NaB 3 S 2 O 12 The polycrystalline powder was placed in 10 mL of deionized water and dissolved, and the incompletely dissolved mixture was subjected to ultrasonic treatment at 30°C for 20 minutes to fully mix and dissolve;

[0077] The obtained mixed solution was transferred into the liner of a clean, non-polluting autoclave with a volume of 100 mL, and the autoclave was tightened and sealed;

[0078] The autoclave was placed in a thermostat, heated to 300°C at a rate of 20°C / h, kept at this temperature for 6 days, and then cooled to room temperature at a rate of 10°C / day to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0079] Embodiment 15

[0080] The hydrothermal method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0081] The compound Li obtained in Example 3 2 NaB 3 S 2 O 12 The polycrystalline powder was placed in 15 mL of deionized water and dissolved, and the incompletely dissolved mixture was subjected to ultrasonic treatment at 25°C for 25 minutes to fully mix and dissolve;

[0082] The obtained mixed solution was transferred into the liner of a clean, non-polluting autoclave with a volume of 100 mL, and the autoclave was tightened and sealed;

[0083] The autoclave was placed in a thermostat, heated to 180°C at a rate of 25°C / h, kept at this temperature for 7 days, and then cooled to room temperature at a rate of 25°C / day to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0084] Example 16

[0085] The hydrothermal method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0086] The compound Li obtained in Example 4 2 NaB 3 S 2 O 12 The polycrystalline powder was placed in 30 mL of deionized water for dissolution, and the incompletely dissolved mixture was subjected to ultrasonic treatment at 50°C for 15 minutes to fully mix and dissolve;

[0087] The obtained mixed solution was transferred into the liner of a clean, non-polluting autoclave with a volume of 100 mL, and the autoclave was tightened and sealed;

[0088] The autoclave was placed in a thermostat, heated to 180°C at a rate of 30°C / h, kept at this temperature for 4 days, and then cooled to room temperature at a rate of 30°C / day to obtain the compound Li 2 NaB3 S 2 O 12 .

[0089] Embodiment 17

[0090] The hydrothermal method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0091] The compound Li obtained in Example 5 2 NaB 3 S 2 O 12 The polycrystalline powder was placed in 12 mL of deionized water for dissolution, and the incompletely dissolved mixture was subjected to ultrasonic treatment at 45°C for 15 minutes to fully mix and dissolve;

[0092] The obtained mixed solution was transferred into the liner of a clean, non-polluting autoclave with a volume of 100 mL, and the autoclave was tightened and sealed;

[0093] The autoclave was placed in a thermostat, heated to 200°C at a rate of 20°C / h, kept at this temperature for 6 days, and then cooled to room temperature at a rate of 25°C / day to obtain the compound Li 2 NaB 3 S 2 O 12 .

[0094] Embodiment 18

[0095] The hydrothermal method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps:

[0096] The compound Li obtained in Example 6 2 NaB 3 S 2 O 12 The polycrystalline powder was placed in 20 mL of deionized water and dissolved, and the incompletely dissolved mixture was subjected to ultrasonic treatment at 20°C for 15 minutes to fully mix and dissolve;

[0097] The obtained mixed solution was transferred into the liner of a clean, non-polluting autoclave with a volume of 100 mL, and the autoclave was tightened and sealed;

[0098] The autoclave was placed in a thermostat, heated to 350°C at a rate of 10°C / h, kept at this temperature for 5 days, and then cooled to room temperature at a rate of 15°C / day to obtain the compound Li 2 NaB 3 S 2 O 12 .

Claims

1. A method for preparing a compound of sodium lithium borosulfate, Features The chemical formula of the compound in this method is Li 2 NaB 3 S 2 O 12 , molecular weight is 325.43, belongs to monoclinic system, space group is P2 1 / c , the unit cell parameters are a=11.6720Å, b=8.2574Å, c=9.6126Å, α=β=90°, γ=97.940°, and the unit cell volume is 917.58Å 3 , made by solid phase synthesis, high temperature melt method or hydrothermal method; The solid phase synthesis method is used to prepare the compound sodium lithium borosulfate, and the specific operation is carried out according to the following steps: The Li-containing compound, the Na-containing compound, the B-containing compound and the S-containing compound are mixed uniformly in a molar ratio of Li:Na:B:S=3-5:1.5-2.5:5-10:3-7.5, and then placed in a ceramic crucible, and then placed in a muffle furnace, and the temperature is raised to 370-430°C and kept at a constant temperature for 30-60 hours to obtain the compound Li 2 NaB 3 S 2 O 12 ; The Li-containing compound is LiBO 2 , Li 2 CO 3 , Li 2 SO 4 、LiHCO 3 or LiOH; containing Na as compound NaBO 2 、Na 2 CO 3 、Na 2 SO 4 、NaHCO 3 or NaOH; Compound B is H 3 BO 3 , B 2 O 3 or HBO 2 ; The S-containing compound is Li 2 SO 4 、Na 2 SO 4 , Li 2 SO 3 、Na 2 SO 3 、LiHSO 4 or NaHSO 4 ; The high temperature melt method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps: a. Molar ratio of Li:Na:B:S=3-5:1.5-2.5:5-10: 3-7.5: Mix the Li-containing compound, the Na-containing compound and the B-containing compound evenly, put them into a ceramic crucible, and then put them into a muffle furnace, heat them to 370-430°C, and keep the temperature constant for 30-60 hours to obtain the compound Li 2 NaB 3 S 2 O 12 polycrystalline powder; the Li-containing compound is LiBO 2 , Li 2 CO 3 , Li 2 SO 4 、LiHCO 3 or LiOH; containing Na as compound NaBO 2 、Na 2 CO 3 、Na 2 SO 4 、NaHCO 3 or NaOH; Compound B is H 3 BO 3 , B 2 O 3 or HBO 2 ; The S-containing compound is Li 2 SO 4 、Na 2 SO 4 , Li 2 SO 3 、Na 2 SO 3 、LiHSO 4 or NaHSO 4 ; b. Compound Li obtained in step a 2 NaB 3 S 2 O 12 The polycrystalline powder and flux are mixed evenly in a molar ratio of 1:0.1-0.5, and then put into a clean platinum crucible, and the temperature is raised to 500-550°C at a rate of 40-50°C / h, and the temperature is kept constant for 30-45 hours to obtain a mixed melt; the flux is H 3 BO 3 , B 2 O 3 , HBO 2 , PbO or PbF 2 ; c. Place the mixed melt obtained in step b in a single crystal furnace, then cool it down to 450-480°C at a cooling rate of 0.1-0.5°C / h, cool it down to 350-400°C at a cooling rate of 0.2-0.6°C / h, and then cool it down to 30°C at a cooling rate of 3-10°C / h to obtain compound Li 2 NaB 3 S 2 O 12 ; The hydrothermal method for preparing the compound sodium lithium borosulfate is specifically carried out in the following steps: a. Mix the Li-containing compound, the Na-containing compound and the B-containing compound in a molar ratio of Li:Na:B:S=3-5:1.5-2.5:5-10:3-7.5, put them into a ceramic crucible, and then put them into a muffle furnace, heat them to 370-430°C, and keep the temperature constant for 30-60 hours to obtain the compound Li 2 NaB 3 S 2 O 12 polycrystalline powder; the Li-containing compound is LiBO 2 , Li 2 CO 3 , Li 2 SO 4 、LiHCO 3 or LiOH; containing Na as compound NaBO 2 、Na 2 CO 3 、Na 2 SO 4 、NaHCO 3 or NaOH; Compound B is H 3 BO 3 , B 2 O 3 or HBO 2 ; The S-containing compound is Li 2 SO 4 、Na 2 SO 4 , Li 2 SO 3 、Na 2 SO 3 、LiHSO 4 or NaHSO 4 ; b. Compound Li obtained in step a 2 NaB 3 S 2 O 12 The polycrystalline powder is placed in 5-30 mL of deionized water to dissolve, and the incompletely dissolved mixture is subjected to ultrasonic treatment at a temperature of 20-50° C. for 15-30 minutes to fully mix and dissolve; c. Transfer the mixed solution obtained in step b into the liner of a clean, pollution-free autoclave with a volume of 100 mL, and tighten and seal the autoclave; d. Place the autoclave in a thermostat, raise the temperature to 180-350°C at a rate of 10-30°C / h, keep the temperature constant for 4-7 days, and then cool it down to room temperature at a rate of 5-30°C / day to obtain compound Li 2 NaB 3 S 2 O 12 .

2. Use of the compound sodium lithium borosulfate obtained by the method of claim 1 in the preparation of deep ultraviolet birefringent materials.