Preparation method of elastic comfortable antistatic clean clothes fabric

By using a combination technology of two-component elastic fiber yarn and conductive wire in clean clothing fabrics, combined with the use of conductive mica powder and composite sodium alginate microspheres, the antistatic, elastic recovery performance and resistance of clean clothing fabrics are solved. The problems in high temperature properties achieve soft, anti-wrinkle and efficient anti-static effects.

CN118958003APending Publication Date: 2024-11-15AGILETEX TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411038789.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing clean clothing fabrics are difficult to improve at the same time in terms of antistatic properties, elastic recovery performance, high temperature resistance and softness, and are prone to static electricity and wrinkles, affecting the wearing experience and corporate image.

Method used

Using a combination of two-component elastic fiber yarn and conductive wire, the uniform distribution of fibers and conductive wires is ensured through network composite and twisting technology, and conductive mica powder and composite sodium alginate microspheres are added to the dyeing and finishing process to form conductive Network to improve antistatic and hydrophobicity.

Benefits of technology

It achieves the improvement of permanent elasticity, wrinkle resistance, anti-static and softness of clean clothing fabrics, maintains the integrity of the conductive wire, and is suitable for high-temperature environments and ISO level 5 cleaning conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of an elastic comfortable antistatic clean clothes fabric, and belongs to the technical field of clean clothes fabrics, the preparation method comprises the steps of raw material selection, gray fabric weaving, dyeing and finishing process, calendaring process and coating process; the raw materials are selected, the yarns are made of polyester filaments, and the elastic yarns are made of bi-component elastic fibers; the warp yarns comprise first warp yarns and second warp yarns; the first warp yarns are polyester DTY (50-150) D / (24-288) F twisted yarns or bi-component elastic polyester filament twisted yarns, and the second warp yarns are stranded twisted yarns of the first warp yarns and (10-50) D / (3-6) F chinlon-based conductive filaments; the prepared fabric has certain barrier property and comfort, also has the characteristics of static electricity resistance, low dust generation, permanent elasticity and crease resistance, and is good in high temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cleanroom clothing fabrics, and in particular to a method for preparing elastic, comfortable and antistatic cleanroom clothing fabrics. Background Art

[0002] Today's cleanroom clothing fabrics are all woven from polyester filaments, and high-density weaving is required to achieve a protective effect. The material and weaving method make the surface of the cleanroom clothing fabric stiff, with a strong "plastic feel", poor moisture absorption, and a stuffy feeling after long-term wear. The elastic recovery performance is poor and the wrinkle resistance is poor. Workers wear cleanroom clothing to work in controlled environments, such as cleanrooms, and the wearing experience is extremely poor. At the same time, due to improper care, cleanroom clothing has obvious wrinkles, which affects the appearance and the image of the company. Conventional elastic fabrics are mainly achieved by adding a certain component of spandex. This kind of fabric will cause elastic aging after high temperature or mechanical stretching. The cleanroom clothing of some pharmaceutical factories has to face high-temperature sterilization, so this problem will be more serious.

[0003] Moreover, cleanroom clothing fabrics have poor moisture absorption properties and are more likely to generate static electricity, causing static adsorption, which can lead to failure of precision parts in the electronics industry. Therefore, cleanroom clothing needs to have certain anti-static properties. However, when conductive threads are added to elastic fabrics, the two fiber materials have different shrinkage properties. When stretched, the conductive threads will break or the fabric surface will be uneven. Therefore, elastic fabrics rarely appear at the same time as conductive threads.

[0004] In order to solve the above problems, the most commonly used method is to twist the conductive thread with the yarn, but the conductive thread is easy to break, which will cause the conductive thread to break during long-term wearing and taking off, and the antistatic property will decrease. The addition of conductive thread will also cause the softness of the fabric to decrease.

[0005] Therefore, the most common problem currently encountered with cleanroom clothing fabrics is that it is difficult to simultaneously improve elastic recovery and wrinkle resistance as well as high temperature resistance, antistatic properties, and long-lasting antistatic properties and softness. Summary of the invention

[0006] In view of the above problems, the present invention provides a method for preparing an elastic, comfortable and antistatic cleanroom clothing fabric. The prepared fabric has certain barrier properties and comfort, and also has the characteristics of antistatic, low dust generation, permanent elasticity and wrinkle resistance, good high temperature resistance and long-lasting antistatic properties, and high softness.

[0007] In order to achieve the above purpose, the present invention provides the following technical solutions: A method for preparing elastic, comfortable and antistatic cleanroom clothing fabric, comprising: selection of raw materials, grey fabric weaving, dyeing and finishing processes; The raw materials are selected such that the yarns are made of polyester filaments and the stretch yarns are made of bicomponent stretch fibers; The yarn is composed of warp yarn and weft yarn; The warp yarns include first warp yarns and second warp yarns; The first warp yarn is polyester DTY (50-150) D / (24-288) F twisted yarn or bicomponent stretch polyester filament twisted yarn, and the second warp yarn is the first warp yarn and (10-50) D / (3-6) F polyester-based conductive yarn ply twisted yarn; The ratio of the first warp yarn to the second warp yarn is 20-50:1; The weft yarns include a first weft yarn and a second weft yarn; The first weft yarn is a polyester filament + bicomponent elastic polyester filament twisted yarn network composite yarn; The polyester filament + bicomponent elastic polyester filament network composite yarn is combined by a direct meshing method, the polyester filament is matte or semi-gloss DTY (50-100) D / (24-144) F, and the ratio of the polyester filament to the bicomponent elastic polyester filament is 0-1:1-2; When preparing the first weft yarn, polyester filament and bicomponent stretch polyester filament are network processed on a winding machine, and the nozzle air pressure is 0.2-0.8MPa; The second weft yarn is a ply-twisted yarn of the first weft yarn and (10-50)D / (3-6)F polyester-based conductive yarn; The ratio of the first weft yarn to the second weft yarn is 10-50:0-1; The two-component elastic twisted yarns in the warp yarn and the weft yarn are all dull polyester DTY (30-200) D / (24-72) F or semi-dull polyester DTY (30-200) D / (24-72) F, and the yarn type is T400 or SPH; The twisted yarns in the warp and weft are twisted at a ratio of 1:1, with a twist of 600-800 twists / m, using S twist; The grey fabric weaving comprises warping the yarn on a warping device, controlling the warp density to be 100-300 yarns / inch, the weft density to be 100-200 yarns / inch, and the grey fabric width to be 63-97 inches; the grey fabric weaving method is woven (woven), and the organization structure is 1 / 1 plain weave or 2 / 3 twill; The dyeing and finishing process includes: pre-treatment (cold stacking, washing), dyeing in the vat, opening width, and shaping; The pre-treatment is divided into cold stacking and water washing; The cold stacking time is 10-30h, the cold stacking temperature is room temperature, the concentration of sodium hydroxide is 10-60g / L, the concentration of hydrogen peroxide is 10-80g / L, the concentration of the chelating dispersant is 1-10g / L, and the concentration of the added hydrogen peroxide is 27.5%; The manufacturer of the chelating dispersant is Jiangsu Fumiao Technology Co., Ltd., and the model is Delecolor DC-40S; The water washing temperature is gradually reduced to room temperature, first washing at 100°C, then washing at 70°C and 40°C in sequence; In the pre-treatment, the width of the grey cloth after leaving the machine shrinks uniformly by 10-30%; The dyeing process is high-temperature overflow dyeing, the dyeing temperature is 110-150°C, the dyeing time is 1-3h, and the dye used is disperse dye; The dyeing process is carried out by slowly increasing the temperature in a gradient manner, firstly increasing the temperature to 25-30°C within 20-40 minutes, then increasing the temperature to 120-130°C within 30-60 minutes, increasing the temperature to 130-135°C within 60-120 minutes, and keeping the temperature at 130-135°C for 60-70 minutes; The function of the opening is to flatten the rope-shaped fabric coming out of the dye vat without winding it, so as to facilitate drying and shaping; The setting temperature of the setting is 160-190°C, the speed is 20-60m / min, and the overfeeding control is 10-20%; The calendering process is to calender the fabric at a calendering temperature of 110-120° C. and a speed of 20-40 m / min; The coating process is to coat the fabric surface with a coating agent, the coating temperature is 130-140°C, the air volume is 75-80%, and the coating agent dosage is 35-38g / m 2 ; The preparation method of the coating agent comprises the following steps: mixing conductive mica powder, polyvinyl pyrrolidone and tridecafluorooctyl trimethoxysilane, grinding the mixture at a speed of 800-1000 rpm for 50-70 min, and then mixing the mixture with acrylate emulsion and composite sodium alginate microspheres, stirring the mixture at a speed of 300-400 rpm for 80-100 min to obtain the coating agent; The mass ratio of conductive mica powder, polyvinyl pyrrolidone, tridecafluorooctyl trimethoxysilane, acrylic emulsion, and composite sodium alginate microspheres is 3-4:0.5-0.6:0.9-1:85-90:10-12; The particle size of the conductive mica powder is 0.5 μm; The solid content of the acrylic emulsion is 30%; The preparation method of the composite sodium alginate microspheres comprises the following steps: uniformly mixing sodium alginate, water-soluble polystyrene sulfonic acid doped with polyaniline and water to obtain a mixed sodium alginate aqueous solution; uniformly mixing calcium chloride and water to obtain a calcium chloride aqueous solution; while stirring the calcium chloride aqueous solution at a stirring speed of 500-600 rpm, dripping the mixed sodium alginate aqueous solution, controlling the dripping time to be 140-160 min, continuing to stir for 5-6 h after the dripping is completed, filtering, washing the filter residue with deionized water for 4-6 times, and drying at 70-80° C. to obtain the composite sodium alginate microspheres; The mass ratio of sodium alginate, water-soluble polystyrene sulfonic acid doped polyaniline, and water is 1.2-1.5:0.8-1:100-110; The mass ratio of calcium chloride to water is 1.3-1.5:100-110; The mass ratio of the calcium chloride aqueous solution to the mixed sodium alginate aqueous solution is 1:2-3.

[0008] Compared with the prior art, the present invention has the following beneficial effects: (1) The preparation method of the elastic, comfortable and antistatic clean clothing fabric of the present invention comprises the following steps: the warp yarn is polyester filament, the weft yarn is a combination of polyester filament and bicomponent elastic polyester filament network composite yarn, and the conductive yarn is woven in the warp direction or in both the warp direction and the weft direction, so that the elasticity of the fabric is achieved while ensuring that the conductive yarn and the elastic fiber shrink in unison and are not broken; (2) The preparation method of the elastic, comfortable and antistatic cleanroom clothing fabric of the present invention comprises a coating process after the dyeing and finishing process and the shaping process. The coating raw materials in the coating process are conductive mica powder, polyvinyl pyrrolidone, tridecafluorooctyl trimethoxysilane, acrylic emulsion and composite sodium alginate microspheres. The conductive mica powder has excellent conductive properties and can further improve the antistatic property of the cleanroom clothing fabric. The polyvinyl pyrrolidone can improve the dispersibility of the conductive mica powder. The tridecafluorooctyl trimethoxysilane can improve the hydrophobicity of the cleanroom clothing fabric. The composite sodium alginate microspheres are sodium alginate microspheres adsorbed with water-soluble polystyrene sulfonic acid doped with polyaniline. The presence of water-soluble polystyrene sulfonic acid doped with polyaniline can form a conductive network with the conductive mica powder, further improving the antistatic property of the cleanroom clothing fabric. The presence of the sodium alginate microspheres can also improve the moisture permeability and softness, and protect the conductive filaments in the cleanroom clothing fabric, further preventing the conductive filaments from breaking during the folding process. (3) The preparation method of the elastic, comfortable and antistatic cleanroom clothing fabric of the present invention, the finished product weight of the prepared cleanroom clothing fabric is 135-170gsm, the shrinkage rate of washing at 60°C is -0.4% to -0.8% / -0.9% to -1.0%, and the shrinkage rate of high-temperature sterilization at 121°C is -0.5% to -1.0% / -2.1% to -2.4%; the weft elastic elongation is 55-70%, and the weft elastic recovery rate is 70-90%. After washing and sterilizing 100 times, the weft elastic elongation is 45-65%, and the weft elastic recovery rate is 87-88%. The surface resistivity is 3.0*10^6-2.6*10^7Ω / □. When washed in an ISO 5 environment, the dust generation rate is 257-452 pieces / min / piece, and the moisture permeability is 8567-8942g / m 2 *d. Overall fabric style: The fabric surface is 0.4cm stripe style or 0.4cm*0.4cm grid style, weft direction, or four-sided elastic, with an overall soft, smooth and drapey feel. DETAILED DESCRIPTION

[0009] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0010] Example 1 A method for preparing an elastic, comfortable, antistatic cleanroom clothing fabric, specifically comprising: 1. Selection of raw materials: The yarn used is made of polyester filament, and the elastic yarn used is bicomponent elastic fiber; The polyester filament yarn has a smooth surface, less hairiness, and dust is not easy to adhere to; the elastic yarn is a two-component elastic yarn, and the two-component yarn has permanent elasticity after dyeing. At the same time, the dumbbell-shaped cross-section has a larger specific surface area than ordinary polyester filaments, so the moisture absorption and perspiration performance is enhanced; The yarn is composed of warp yarn and weft yarn, the warp yarn includes a first warp yarn and a second warp yarn, the first warp yarn is a polyester 75D / 48FDTY twisted yarn, and the second warp yarn is a polyester 75D / 48FDTY and 20D / 3F polyester-based conductive yarn ply twisted yarn; The twisted yarns are twisted at a ratio of 1:1, with a twist of 600 twists / m and an S twist. The ratio of the first warp yarn to the second warp yarn is 34:1; The weft yarn is a two-component elastic polyester filament twisted yarn network composite yarn, and the two-component elastic polyester filament is SPH polyester matte 80D / 24F; The twisted yarns are twisted at a ratio of 1:1, with a twist of 600 twists / m and an S twist. 2. Grey fabric weaving: warp the yarn on the warping equipment, control the warp density to 228 yarns / inch, the weft density to 120 yarns / inch, and the grey fabric width to 82 inches; the grey fabric weaving method is woven (woven), and the organization structure is 1 / 1 plain weave; 3. Dyeing and finishing process, including: pre-treatment (cold pile, washing), dyeing in the vat, opening width, and shaping; The pretreatment is divided into cold stacking and water washing. The cold stacking time is 24 hours, the cold stacking temperature is room temperature, the concentration of sodium hydroxide is 20g / L, the concentration of hydrogen peroxide is 10g / L, the concentration of chelating dispersant is 2g / L, and the concentration of hydrogen peroxide added is 27.5%. After the cold stacking, the fabric is washed with water, and the washing temperature is gradually reduced to room temperature, specifically, first washed at 100°C, then washed at 70°C and 40°C in sequence, and the width of the grey cloth after leaving the machine is uniformly shrunk by 20%; The manufacturer of the chelating dispersant is Jiangsu Fumiao Technology Co., Ltd., and the model is Delecolor DC-40S; The in-tank dyeing is high-temperature overflow dyeing, the dyeing temperature is 130° C., the dyeing time is 3 hours, and the dye used is a disperse dye; during the in-tank dyeing, a gradient slow temperature increase method is adopted during the dyeing process, specifically, the temperature is first increased to 25° C. within 30 minutes, then increased to 125° C. within 40 minutes, and then increased to 130° C. within 80 minutes, and kept at 130° C. for 60 minutes; The function of the opening width is to flatten the rope-shaped fabric coming out of the dye vat without winding it, so as to facilitate drying and shaping; The setting temperature of the setting is 180°C, the speed is 30m / min, and the overfeed control is 13%; 4. Calendering process: Calender the fabric at a calendering temperature of 110°C and a speed of 20m / min; 5. Coating process: Coating the fabric surface with coating agent, the coating temperature is 130℃, the air volume is 75%, and the coating agent dosage is 35g / m 2 ; The preparation method of the coating agent is as follows: conductive mica powder, polyvinyl pyrrolidone and tridecafluorooctyl trimethoxysilane are mixed, and then ground at a speed of 800 rpm for 50 minutes, and then mixed with acrylic emulsion and composite sodium alginate microspheres, and stirred at a speed of 300-400 rpm for 80 minutes to obtain the coating agent; The mass ratio of conductive mica powder, polyvinyl pyrrolidone, tridecafluorooctyl trimethoxysilane, acrylic emulsion, and composite sodium alginate microspheres is 3:0.5:0.9:85:10; The particle size of the conductive mica powder is 0.5 μm; The solid content of the acrylic emulsion is 30%; The preparation method of the composite sodium alginate microspheres is as follows: sodium alginate, water-soluble polystyrene sulfonic acid doped with polyaniline and water are uniformly mixed to obtain a mixed sodium alginate aqueous solution; calcium chloride and water are uniformly mixed to obtain a calcium chloride aqueous solution; while stirring the calcium chloride aqueous solution at a stirring speed of 500 rpm, the mixed sodium alginate aqueous solution is added dropwise, the dropping time is controlled to be 140 minutes, and after the dropping is completed, the stirring is continued for 5 hours, and the filter residue is filtered, and after the filter residue is washed with deionized water for 4 times, it is dried at 70° C. to obtain the composite sodium alginate microspheres; The mass ratio of sodium alginate, water-soluble polystyrene sulfonic acid doped polyaniline, and water is 1.2:0.8:100; The mass ratio of calcium chloride to water is 1.3:100; The mass ratio of the calcium chloride aqueous solution to the mixed sodium alginate aqueous solution is 1:2.

[0011] The fabric obtained in this embodiment has a gram weight of 135gsm, a shrinkage rate of -0.4% / -0.9% after washing at 60°C, and a shrinkage rate of -1.0% / -2.1% after high-temperature sterilization at 121°C; a weft elastic elongation of 55%, a weft elastic recovery rate of 90%, a weft elastic elongation of 50% after 100 times of washing and sterilization, and a weft elastic recovery rate of 87%, a surface resistivity of 2.6*10^7Ω / □, and a surface resistivity of 3.3*10^7Ω / □ after folding tests for 100 times. The dust generation rate is 257 pieces / min / piece when washed under an ISO 5 environment, and the moisture permeability is 8942g / m 2 *d, Overall fabric style: The fabric has a 0.4cm striped style, is elastic in the weft direction, has a transverse softness of 53.15mN, and a longitudinal softness of 48.89mN. It is soft, smooth, and has a drapey feel overall.

[0012] Example 2 A method for preparing an elastic, comfortable, antistatic cleanroom clothing fabric, specifically comprising: 1. Selection of raw materials: The yarn used is made of polyester filament, and the elastic yarn used is bicomponent elastic fiber; The polyester filament yarn has a smooth surface, less hairiness, and dust is not easy to adhere to; the elastic yarn is a two-component elastic yarn, and the two-component yarn has permanent elasticity after dyeing. At the same time, the dumbbell-shaped cross-section has a larger specific surface area than ordinary polyester filaments, so the moisture absorption and perspiration performance is enhanced; The yarn is composed of warp yarn and weft yarn, the warp yarn includes a first warp yarn and a second warp yarn, the first warp yarn is a polyester 75D / 48FDTY twisted yarn, and the second warp yarn is a first warp yarn and a 20D / 3F polyester-based conductive yarn twisted yarn; When twisting the twisted yarn, both yarns are twisted at a ratio of 1:1, with a twist of 800 twists / m and an S twist; The ratio of the first warp yarn to the second warp yarn is 34:1; The weft yarn includes a first weft yarn and a second weft yarn, the first weft yarn is a polyester filament + a bicomponent elastic polyester filament twisted yarn network composite yarn, the two are combined by a direct meshing method, the polyester filament is a matte 75D / 48F, and the bicomponent elastic polyester filament is a T400 matte polyester 75D / 36F; the ratio of the polyester filament to the bicomponent elastic polyester filament twisted yarn in the first weft yarn is 1:1; the second weft yarn is a twisted yarn of the first weft yarn and a 20D / 3F polyester-based conductive yarn; The twisted yarns are twisted at a ratio of 1:1, with a twist of 600 twists / m and an S twist. The ratio of the first weft yarn to the second weft yarn is 17:1; When preparing the first weft yarn, the polyester filament and the two-component stretch polyester filament are network-processed on a winding machine, and the nozzle air pressure is 0.6 MPa; when preparing the second weft yarn, the conductive yarn and the first weft yarn are twisted, and the twist is 800 twists / m; 2. Grey fabric weaving: warp the yarn on the warping equipment, control the warp density to 240 strands / inch, the weft density to 125 strands / inch, and the grey fabric width to 82 inches; the grey fabric weaving method is woven (woven), and the structure is 2 / 3 twill; 3. Dyeing and finishing process, including: pre-treatment (cold pile, washing), dyeing in the vat, opening width, and shaping; The pretreatment is divided into cold stacking and water washing. The cold stacking time is 24 hours, the cold stacking temperature is room temperature, the concentration of sodium hydroxide is 10g / L, the concentration of hydrogen peroxide is 15g / L, the concentration of chelating dispersant is 8g / L, and the concentration of hydrogen peroxide added is 27.5%; the water washing temperature is gradually reduced to room temperature, specifically, first washing at 100°C, then washing at 70°C and 40°C in sequence, and the width of the grey cloth after leaving the machine shrinks uniformly by 20%; The manufacturer of the chelating dispersant is Jiangsu Fumiao Technology Co., Ltd., and the model is Delecolor DC-40S; The dyeing process is high-temperature overflow dyeing, the dyeing temperature is 130℃, the dyeing time is 3h, and the dye used is disperse dye; the dyeing process is carried out by slowly increasing the temperature in a gradient, specifically, firstly increasing the temperature to 25℃ within 30min, then increasing the temperature to 125℃ within 40min, increasing the temperature to 130℃ within 80min, and keeping the temperature at 130℃ for 60min; The function of the opening is to flatten the rope-shaped fabric coming out of the dye vat without winding it, so as to facilitate drying and shaping; The setting temperature of the setting is 180°C, the speed is 30m / min, and the overfeed control is 13%; 4. Calendering process: Calender the fabric at a calendering temperature of 115°C and a speed of 30m / min; 5. Coating process: The fabric surface is coated with a coating agent, the coating temperature is 135°C, the air volume is 80%, and the coating agent dosage is 36g / m 2 ; The coating agent is prepared by mixing conductive mica powder, polyvinyl pyrrolidone and tridecafluorooctyl trimethoxysilane, grinding the mixture at a speed of 900 rpm for 60 minutes, and then mixing the mixture with acrylic emulsion and composite sodium alginate microspheres, stirring the mixture at a speed of 400 rpm for 90 minutes to obtain the coating agent. The mass ratio of conductive mica powder, polyvinyl pyrrolidone, tridecafluorooctyl trimethoxysilane, acrylic emulsion, and composite sodium alginate microspheres is 3.5:0.5:0.9:88:11; The particle size of the conductive mica powder is 0.5 μm; The solid content of the acrylic emulsion is 30%; The preparation method of the composite sodium alginate microspheres is as follows: sodium alginate, water-soluble polystyrene sulfonic acid doped with polyaniline, and water are uniformly mixed to obtain a mixed sodium alginate aqueous solution; calcium chloride and water are uniformly mixed to obtain a calcium chloride aqueous solution; while stirring the calcium chloride aqueous solution at a stirring speed of 550 rpm, the mixed sodium alginate aqueous solution is added dropwise, the dropping time is controlled to be 150 min, and after the dropping is completed, the stirring is continued for 5.5 h, and the mixture is filtered, and the filter residue is washed with deionized water for 5 times, and then dried at 75° C. to obtain the composite sodium alginate microspheres; The mass ratio of sodium alginate, water-soluble polystyrene sulfonic acid doped polyaniline, and water is 1.4:0.9:105; The mass ratio of calcium chloride to water is 1.4:105; The mass ratio of the calcium chloride aqueous solution to the mixed sodium alginate aqueous solution is 1:2.5.

[0013] The fabric obtained in this embodiment has a gram weight of 160gsm, a shrinkage rate of -0.8% / -1.0% after washing at 60°C, and a shrinkage rate of -0.5% / -2.4% after high-temperature sterilization at 121°C; a weft elastic elongation of 70%, a weft elastic recovery rate of 90%, a weft elastic elongation of 50% after 100 times of washing and sterilization, and a weft elastic recovery rate of 88%, a surface resistivity of 3.0*10^6Ω / □, and a surface resistivity of 4.1*10^6Ω / □ after folding tests for 100 times. The dust generation rate is 452 pieces / min / piece when washed under an ISO 5 environment, and the moisture permeability is 8672g / m 2*d, Overall fabric style: The fabric surface is 0.4cm*0.4cm grid style, with weft elasticity, lateral softness of 49.52mN, and longitudinal softness of 45.07mN. It is soft, smooth and has a drapey feel overall.

[0014] Example 3 A method for preparing a stretch cleanroom clothing fabric, specifically comprising: 1. Selection of raw materials: The yarn used is made of polyester filament, and the elastic yarn used is bicomponent elastic fiber; The polyester filament yarn has a smooth surface, less hairiness, and dust is not easy to adhere to; the elastic yarn is a two-component elastic yarn, and the two-component yarn has permanent elasticity after dyeing. At the same time, the dumbbell-shaped cross-section has a larger specific surface area than ordinary polyester filaments, so the moisture absorption and perspiration performance is enhanced; The yarn is composed of warp yarn and weft yarn, the warp yarn includes a first warp yarn and a second warp yarn, the first warp yarn is an 80D / 24F SPH two-component elastic twisted yarn; the second warp yarn is a twisted yarn of the first warp yarn and a 20D / 3F polyester-based conductive yarn; The twisted yarns are twisted at a ratio of 1:1, with a twist of 800 twists / m and an S twist. The ratio of the first warp yarn to the second warp yarn is 34:1; The weft yarn includes a first weft yarn and a second weft yarn, the first weft yarn is a two-component elastic polyester filament twisted yarn; the two-component elastic polyester filament is SPH matte polyester 80D / 36F; The second weft yarn is a ply-twisted yarn of the first weft yarn and 20D / 3F polyester-based conductive yarn; The twisted yarns are twisted at a ratio of 1:1, with a twist of 800 twists / m and an S twist. The ratio of the first weft yarn to the second weft yarn is 17:1; 2. Grey fabric weaving: warp the yarn on the warping equipment, control the warp density to 232 yarns / inch, the weft density to 124 yarns / inch, and the grey fabric width to 82 inches; the grey fabric weaving method is woven (woven), and the structure is 2 / 3 twill; 3. Dyeing and finishing process, including: pre-treatment (cold pile, washing), dyeing in the vat, opening width, and shaping; The pretreatment is divided into cold stacking and water washing. The cold stacking time is 24 hours, the cold stacking temperature is room temperature, the concentration of sodium hydroxide is 10g / L, the concentration of hydrogen peroxide is 15g / L, the concentration of chelating dispersant is 8g / L, and the concentration of hydrogen peroxide added is 27.5%; the water washing temperature is gradually reduced to room temperature, specifically, first washing at 100°C, then washing at 70°C and 40°C in sequence, and the width of the grey cloth after leaving the machine shrinks uniformly by 20%; The manufacturer of the chelating dispersant is Jiangsu Fumiao Technology Co., Ltd., and the model is Delecolor DC-40S; The dyeing process is high-temperature overflow dyeing, the dyeing temperature is 130℃, the dyeing time is 3h, and the dye used is disperse dye; the dyeing process is carried out by slowly increasing the temperature in a gradient, specifically, firstly increasing the temperature to 25℃ within 30min, then increasing the temperature to 125℃ within 40min, increasing the temperature to 130℃ within 80min, and keeping the temperature at 130℃ for 60min; The function of the opening is to flatten the rope-shaped fabric coming out of the dye vat without winding it, so as to facilitate drying and shaping; The setting temperature of the setting is 180°C, the speed is 30m / min, and the overfeed control is 13%; 4. Calendering process: Calender the fabric at a calendering temperature of 120°C and a speed of 40m / min; 5. Coating process: The fabric surface is coated with a coating agent, the coating temperature is 140°C, the air volume is 80%, and the coating agent dosage is 38g / m 2 ; The preparation method of the coating agent is as follows: conductive mica powder, polyvinyl pyrrolidone and tridecafluorooctyl trimethoxysilane are mixed, and then ground at a grinding speed of 1000 rpm for 70 minutes, and then mixed with acrylic emulsion and composite sodium alginate microspheres, and stirred at a stirring speed of 400 rpm for 100 minutes to obtain the coating agent; The mass ratio of conductive mica powder, polyvinyl pyrrolidone, tridecafluorooctyl trimethoxysilane, acrylic emulsion, and composite sodium alginate microspheres is 4:0.6:1:90:12; The particle size of the conductive mica powder is 0.5 μm; The solid content of the acrylic emulsion is 30%; The preparation method of the composite sodium alginate microspheres is as follows: sodium alginate, water-soluble polystyrene sulfonic acid doped with polyaniline and water are mixed evenly to obtain a mixed sodium alginate aqueous solution; calcium chloride and water are mixed evenly to obtain a calcium chloride aqueous solution; while stirring the calcium chloride aqueous solution at a stirring speed of 600 rpm, the mixed sodium alginate aqueous solution is added dropwise, the dropping time is controlled to be 160 minutes, and after the dropping is completed, the stirring is continued for 6 hours, and the filter residue is filtered, and after the filter residue is washed with deionized water for 6 times, it is dried at 80° C. to obtain the composite sodium alginate microspheres; The mass ratio of sodium alginate, water-soluble polystyrene sulfonic acid doped polyaniline, and water is 1.5:1:110; The mass ratio of calcium chloride to water is 1.5:110; The mass ratio of the calcium chloride aqueous solution to the mixed sodium alginate aqueous solution is 1:3.

[0015] The fabric obtained in this embodiment has a gram weight of 170gsm, a shrinkage rate of -0.8% / -1.0% after washing at 60°C, a shrinkage rate of -0.5% / -2.4% after high-temperature sterilization at 121°C, a weft elastic elongation of 70%, a weft elastic recovery rate of 90%, a weft elastic elongation of 50% after 100 times of washing and sterilization, a weft elastic recovery rate of 88%, a surface resistivity of 3.0*10^6Ω / □, a surface resistivity of 4.8*10^6Ω / □ after folding test 100 times, a dust generation rate of 452 pieces / min / piece when washed under ISO 5 environment, and a moisture permeability of 8567g / m 2 *d, Overall fabric style: The fabric surface is 0.4cm*0.4cm grid style, elastic on all four sides, with a lateral softness of 55.27mN and a longitudinal softness of 51.34mN. It is soft, smooth and has a drapey feel overall.

[0016] Comparative Example This comparative example is based on Example 2, except that the calendering process in step 4 and the coating process in step 5 are omitted; the remaining operations are the same as those in Example 2; The fabric obtained in this comparative example has a gram weight of 148gsm, a shrinkage rate of -0.9% / -1.2% after washing at 60°C, and a shrinkage rate of -0.7% / -2.7% after high-temperature sterilization at 121°C; a weft elastic elongation of 67%, a weft elastic recovery rate of 86%, a weft elastic elongation of 55% after 100 times of washing and sterilization, and a weft elastic recovery rate of 86%, a surface resistivity of 2.5*10^7Ω / □, and a surface resistivity of 5.8*10^8Ω / □ after folding tests for 100 times. The dust generation rate is 520 pieces / min / piece when washed under an ISO 5 environment, and the moisture permeability is 7721g / m 2 *d, Overall fabric style: The fabric surface is 0.4cm*0.4cm grid style, with weft elasticity, lateral softness of 62.1mN, and longitudinal softness of 57.4mN. It is soft, smooth and has a drapey feel overall.

[0017] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an elastic, comfortable, antistatic cleanroom clothing fabric, characterized in that: Including the selection of raw materials, grey fabric weaving, dyeing and finishing, calendering and coating processes; The raw materials are selected such that the yarns are all made of polyester filaments, and the elastic yarns are made of bicomponent elastic fibers.

2. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 1, characterized in that: The yarn is composed of warp yarn and weft yarn; The warp yarns include first warp yarns and second warp yarns; The first warp yarn is polyester DTY (50-150) D / (24-288) F twisted yarn or bicomponent stretch polyester filament twisted yarn, and the second warp yarn is the first warp yarn and (10-50) D / (3-6) F nylon-based conductive yarn twisted yarn; The ratio of the first warp yarn to the second warp yarn is 20-50:1; The weft yarns include a first weft yarn and a second weft yarn; The first weft yarn is a polyester filament + bicomponent elastic polyester filament twisted yarn network composite yarn; The polyester filament + bicomponent elastic polyester filament network composite yarn is combined by a direct meshing method, the polyester filament is matte or semi-gloss DTY (50-100) D / (24-144) F, and the ratio of the polyester filament to the bicomponent elastic polyester filament is 0-1:1-2; When preparing the first weft yarn, polyester filament and bicomponent stretch polyester filament are network processed on a winding machine, and the nozzle air pressure is 0.2-0.8MPa; The second weft yarn is a ply-twisted yarn of the first weft yarn and (10-50)D / (3-6)F polyester-based conductive yarn; The ratio of the first weft yarn to the second weft yarn is 10-50:0-1.

3. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 1, characterized in that: The two-component elastic twisted yarns in the warp yarn and the weft yarn are all dull polyester DTY (30-200) D / (24-72) F or semi-dull polyester DTY (30-200) D / (24-72) F, and the yarn type is T400 or SPH; The twisted yarns in the warp and weft are twisted at a ratio of 1:1, with a twist of 600-800 twists / m, and adopt an S twist.

4. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 1, characterized in that: The grey cloth is weaved by warping the yarn on a warping device, controlling the warp density to be 100-300 yarns / inch, the weft density to be 100-200 yarns / inch, and the grey cloth width to be 63-97 inches; the grey cloth is woven by machine, and the organization structure is 1 / 1 plain weave or 2 / 3 twill.

5. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 1, characterized in that: The dyeing and finishing process includes pre-treatment, dyeing in the vat, opening the width, and shaping; The pre-treatment is divided into cold stacking and water washing; The cold stacking time is 10-30h, the cold stacking temperature is room temperature, the concentration of sodium hydroxide is 10-60g / L, the concentration of hydrogen peroxide is 10-80g / L, the concentration of the chelating dispersant is 1-10g / L, and the concentration of the added hydrogen peroxide is 27.5%; The manufacturer of the chelating dispersant is Jiangsu Fumiao Technology Co., Ltd., and the model is Delecolor DC-40S; The water washing temperature is gradually reduced to room temperature, first washing at 100°C, then washing at 70°C and 40°C in sequence; In the pre-treatment, the width of the grey cloth after leaving the machine shrinks uniformly by 10-30%.

6. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 5, characterized in that: The dyeing process is high-temperature overflow dyeing, the dyeing temperature is 110-150°C, the dyeing time is 1-3h, and the dye used is disperse dye; The dyeing process is carried out by slowly increasing the temperature in a gradient manner, firstly increasing the temperature to 25-30°C within 20-40 minutes, then increasing the temperature to 120-130°C within 30-60 minutes, increasing the temperature to 130-135°C within 60-120 minutes, and keeping the temperature at 130-135°C for 60-70 minutes; The setting temperature of the setting is 160-190° C., the vehicle speed is 20-60 m / min, and the overfeeding is controlled at 10-20%.

7. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 1, characterized in that: The calendering process calenders the fabric at a calendering temperature of 110-120° C. and a speed of 20-40 m / min.

8. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 1, characterized in that: The coating process is to coat the fabric surface with a coating agent, the coating temperature is 130-140°C, the air volume is 75-80%, and the coating agent dosage is 35-38g / m 2 .

9. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 1, characterized in that: The coating agent is prepared by mixing conductive mica powder, polyvinyl pyrrolidone and tridecafluorooctyl trimethoxysilane, grinding the mixture, and then mixing the mixture with acrylate emulsion and composite sodium alginate microspheres, stirring the mixture, and obtaining the coating agent. The mass ratio of conductive mica powder, polyvinyl pyrrolidone, tridecafluorooctyl trimethoxysilane, acrylic emulsion, and composite sodium alginate microspheres is 3-4:0.5-0.6:0.9-1:85-90:10-12; The particle size of the conductive mica powder is 0.5 μm; The solid content of the acrylic ester emulsion is 30%.

10. The method for preparing the elastic, comfortable, antistatic cleanroom clothing fabric according to claim 1, characterized in that: The preparation method of the composite sodium alginate microspheres comprises the following steps: uniformly mixing sodium alginate, water-soluble polystyrene sulfonic acid doped with polyaniline and water to obtain a mixed sodium alginate aqueous solution; uniformly mixing calcium chloride and water to obtain a calcium chloride aqueous solution; while stirring the calcium chloride aqueous solution, dropwise adding the mixed sodium alginate aqueous solution, continuing stirring after the dropwise addition is completed, filtering, washing and drying the filter residue to obtain the composite sodium alginate microspheres; The mass ratio of sodium alginate, water-soluble polystyrene sulfonic acid doped polyaniline, and water is 1.2-1.5:0.8-1:100-110; The mass ratio of calcium chloride to water is 1.3-1.5:100-110; The mass ratio of the calcium chloride aqueous solution to the mixed sodium alginate aqueous solution is 1:2-3; The dropwise addition time of the mixed sodium alginate aqueous solution is 140-160 min.

Citation Information