Surface acoustic wave temperature sensor and preparation method thereof

By introducing thermal stress compensation layer and strain isolation structure into the surface acoustic wave temperature sensor, the problems of low sensor sensitivity and inaccurate measurement are solved, and higher temperature measurement accuracy and sensitivity are achieved.

CN118960988APending Publication Date: 2024-11-15NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410969554.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing surface acoustic wave temperature sensors have low sensitivity, inaccurate measurement, difficult preparation of highly sensitive units, and problems of dispersed strain transmission of piezoelectric substrates.

Method used

The surface acoustic wave temperature sensor design is adopted, including a conductive layer, a piezoelectric layer and a thermal stress compensation layer. The thermal expansion coefficient of the thermal stress compensation layer is greater than that of the piezoelectric layer. The thermal strain transmission is concentrated through the strain isolation structure to improve measurement accuracy and sensitivity.

Benefits of technology

Through the combination of the thermal stress compensation layer and the strain isolation structure, more accurate temperature measurement is achieved, the sensitivity and measurement accuracy of the surface acoustic wave temperature sensor are improved, and the problem of insufficient accuracy of traditional sensors in high temperature harsh environments is solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118960988A_ABST
    Figure CN118960988A_ABST
Patent Text Reader

Abstract

The invention discloses a surface acoustic wave temperature sensor and a preparation method, and solves the problems that an existing surface acoustic wave sensor is low in sensitivity and inaccurate in measurement, a high-sensitivity unit is difficult to prepare, and strain transmission of a piezoelectric substrate is dispersed. The surface acoustic wave temperature sensor comprises a protective layer, a conductive layer, a piezoelectric layer and a thermal stress compensation layer, the conductive layer is provided with a grounding end bonding pad, a signal end bonding pad and an interdigital electrode; the piezoelectric layer is provided with a first strain isolation beam, a second strain isolation beam, a third strain isolation beam and a fourth strain isolation beam; the four strain isolation beams form a strain isolation structure; the thermal stress compensation layer is set to be a thermal stress compensation layer with a relatively large thermal expansion coefficient for thermal stress compensation of the piezoelectric layer when the temperature changes; and the strain isolation structure and the thermal stress compensation layer enable the waveguide to be sensitive to temperature change, so that more accurate measurement of the temperature of the single chip is realized, and the measurement accuracy and sensitivity are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sensors and mainly relates to a surface acoustic wave temperature sensor. Background Art

[0002] In recent years, with the continuous development of the new generation of Internet and intelligent integrated devices, the demand for new sensors has become more and more urgent, especially in the fields of aerospace, energy and nuclear power, which are in urgent need of sensors that can withstand harsh environments such as high temperature, high pressure and high rotation. Therefore, accurate measurement of high temperature is particularly urgent. The traditional high temperature measurement method has problems such as difficult wiring, complex installation structure and wired active, which makes it difficult to meet the actual needs of accurate measurement. The surface acoustic wave temperature sensor has the characteristics of small size, long communication distance, simple structure and wireless passive, making it easy to integrate into mobile devices. Its unique wireless passive characteristics are more potential than traditional sensors in high temperature and harsh environments. However, the waveguide excited by the temperature sensitive unit of the existing surface acoustic wave temperature sensor has low temperature sensitivity, which makes the surface acoustic wave sensor low in sensitivity and inaccurate measurement; at the same time, there are also problems such as difficulty in preparing high-sensitive units and dispersed strain transmission of piezoelectric substrates. CN115808260A proposes a strain isolation structure for the temperature sensitive unit to improve the accuracy of measurement, but ignores the impact of lateral strain transmission being greater than longitudinal strain transmission on the substrate. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art and solve the problems of low sensitivity and inaccurate measurement of the existing surface acoustic wave sensors, the present invention provides a surface acoustic wave temperature sensor and a preparation method thereof.

[0004] The technical solution adopted by the present invention to solve its technical problem is a surface acoustic wave temperature sensor, which includes a conductive layer, a piezoelectric layer and a thermal stress compensation layer; the piezoelectric layer and the conductive layer are arranged in sequence on the thermal stress compensation layer; the thermal expansion coefficient of the thermal stress compensation layer is greater than the thermal expansion coefficient of the piezoelectric layer.

[0005] Furthermore, the piezoelectric layer is a single crystal wafer that is temperature-sensitive in the tangential direction; the piezoelectric layer is provided with a strain isolation structure; the strain isolation structure includes a first through hole, a second through hole, a third through hole and a fourth through hole; the first through hole is connected to the second through hole through a first strain isolation beam; the third through hole is connected to the fourth through hole through a second strain isolation beam; the first through hole and the third through hole are connected through a third strain isolation beam; the second through hole and the fourth through hole are connected through a fourth strain isolation beam; the surfaces of the first strain isolation beam, the second strain isolation beam, the third strain isolation beam and the fourth strain isolation beam in contact with the thermal stress compensation layer are suspended, that is, they are not in contact with the thermal stress compensation layer.

[0006] Furthermore, the conductive layer includes a ground terminal pad, a signal terminal pad and a temperature sensitive unit; the temperature sensitive unit includes a forked electrode and a Bragg reflector; the Bragg reflector is located on both sides of the forked electrode; the ground terminal pad is connected to the Bragg reflector; the forked electrode includes a ground terminal forked electrode, a forked sensitive synapse and a signal terminal forked electrode; the ground terminal pad is connected to the ground terminal forked electrode; the signal terminal pad is connected to the signal terminal forked electrode; the signal terminal pad is connected to the first strain isolation beam; the signal terminal pad is connected to the signal terminal forked electrode; the ground terminal pad is connected to the second strain isolation beam; the ground terminal pad is connected to the ground terminal forked electrode; the third strain isolation beam is perpendicular to the direction in which the forked electrode is set; the fourth strain isolation beam is perpendicular to the direction in which the forked electrode is set.

[0007] Furthermore, the base material of the thermal stress compensation layer is one or more of sapphire, silicon carbide, diamond, nickel-titanium alloy, and aluminum foil.

[0008] Furthermore, a protective layer is arranged on the conductive layer.

[0009] Furthermore, the base material of the protective layer is one or more of aluminum oxide, silicon oxide and zirconium oxide ceramic films; the protective layer is located directly above the temperature sensitive unit to protect the interdigital electrodes from being oxidized and agglomerated and failed.

[0010] Furthermore, a method for calculating the temperature sensitivity of a surface acoustic wave temperature sensor is:

[0011] k(f,T)=k(f0,T0)[1+α(f-f0)]

[0012] Wherein, k(f0,T0) is the sensitivity of the resonant frequency of the piezoelectric layer, f0 is the resonant frequency of the piezoelectric layer; T0 is the temperature of the piezoelectric layer; α is the frequency-temperature coefficient of thermal stress compensation, k(f,T) is the sensitivity of the surface acoustic wave temperature sensor, f is the resonant frequency of the surface acoustic wave temperature sensor, and T is the temperature of the surface acoustic wave temperature sensor; when the substrate material of the thermal stress compensation layer is sapphire and the material of the piezoelectric layer is single crystal quartz, the range of α is (-50,50).

[0013] Furthermore, the present invention also provides a method for preparing a surface acoustic wave microsensor, comprising the following steps:

[0014] Step S1: preparing a piezoelectric layer;

[0015] The piezoelectric layer is etched layer by layer using picosecond ultraviolet laser etching to form a first through hole, a second through hole, a third through hole and a fourth through hole; the first strain isolation beam, the second strain isolation beam, the third strain isolation beam and the fourth strain isolation beam are then etched layer by layer using picosecond ultraviolet laser etching, and the strain isolation structure is suspended by picosecond ultraviolet laser etching to complete the preparation of the piezoelectric layer;

[0016] The picosecond ultraviolet laser has a wavelength of 355nm, a scanning speed of 500mm / s, and a power of 10W;

[0017] Step S2: bonding the thermal stress compensation layer and the piezoelectric layer;

[0018] After the etching of the piezoelectric layer is completed, a layer of gold film is sputtered on the lower surface of the piezoelectric layer and the upper surface of the thermal stress compensation layer; the thickness of the gold film is 150-200 nm;

[0019] Align and contact the thermal stress compensation layer, the piezoelectric layer and the suspended side of the stress isolation beam, and press and hold the thermal stress compensation layer and the piezoelectric layer. The bonding pressure during pressing is 1800-2000 mBar.

[0020] The pressed thermal stress compensation layer and the piezoelectric layer are kept at 450-480°C for 30-45 minutes and then cooled to form a new substrate and complete bonding;

[0021] Step S3: preparation of a conductive layer;

[0022] After bonding is completed, a conductive layer is prepared on the piezoelectric layer by direct current magnetron sputtering, and vacuum heat treatment is performed; after the vacuum heat treatment of the piezoelectric layer, a photoresist mask is prepared on the surface of the piezoelectric layer, the photoresist mask is patterned, the metal electrode is ion-beam-etched, the pattern is transferred to the metal electrode, the photoresist mask is removed, and the preparation of the conductive layer is completed;

[0023] Step S4: preparation of a protective layer;

[0024] After the conductive layer is prepared, a polyimide mask is made on the metal electrode, and then an oxide ceramic thin film protective layer is prepared by AC magnetron sputtering, and the polyimide mask is removed to complete the preparation of the protective layer.

[0025] The beneficial effects of the present invention are as follows: the thermal expansion coefficient of the thermal stress compensation layer is greater than the thermal expansion coefficient of the piezoelectric layer. During the temperature change process, the piezoelectric layer is thermally stressed, and the thermal strain generated by the temperature change is transmitted to the piezoelectric layer. The strain isolation structure provided in the piezoelectric layer concentrates the conducted thermal strain, making the waveguide more sensitive to temperature changes. By detecting the change in the central resonant frequency, a more accurate measurement of the temperature of a single chip is achieved, thereby improving the measurement accuracy and sensitivity; the strain isolation structure provided in the piezoelectric layer concentrates the strain directly below the temperature-sensitive unit structure, isolating the strain influence brought by the non-temperature-sensitive unit structure area of ​​the piezoelectric layer, while improving the accuracy of temperature measurement. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a structural schematic diagram of a surface acoustic wave temperature sensor;

[0027] Figure 2 is a schematic diagram of a piezoelectric layer structure;

[0028] Figure 3 is a cross-sectional view of a piezoelectric layer structure along the AA direction;

[0029] Figure 4 is a cross-sectional view of a piezoelectric layer structure along the BB direction;

[0030] Figure 5 is a schematic diagram of a conductive layer of a piezoelectric layer structure;

[0031] Figure 6 The present invention is a flow chart of a method for preparing a surface acoustic wave temperature sensor;

[0032] In the figure, 1 is a thermal stress compensation layer; 2 is a piezoelectric layer, 21 is a first through hole, 22 is a second through hole, 23 is a third through hole, 24 is a fourth through hole, 25 is a first strain isolation beam, 26 is a second strain isolation beam, 27 is a third strain isolation beam, 28 is a fourth strain isolation beam, and 29 is a strain isolation structure; 3 is a conductive layer, 31 is a signal end pad, 32 is a ground end pad, 33 is a Bragg reflection grating, 34 is an interdigital electrode, 341 is a signal end interdigital electrode, 342 is an interdigital sensitive synapse, 343 is a ground end interdigital electrode, and 35 is a temperature sensitive unit; 4 is a protective layer. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0034] The technical solution adopted by the present invention to solve the technical problem is a surface acoustic wave temperature sensor, comprising a protective layer, a conductive layer, a piezoelectric layer and a thermal stress compensation layer; the piezoelectric layer, the conductive layer and the protective layer are sequentially arranged on the thermal stress compensation layer; the thermal expansion coefficient of the thermal stress compensation layer is greater than the thermal expansion coefficient of the piezoelectric layer;

[0035] The thermal expansion coefficient of the thermal stress compensation layer is greater than that of the piezoelectric layer, and the thermal stress of the piezoelectric layer is compensated during the temperature change. The thermal stress compensation structure transfers the thermal strain generated by the temperature change to the piezoelectric layer, and the strain isolation structure provided on the piezoelectric layer concentrates the conducted thermal strain, making the waveguide more sensitive to temperature changes.

[0036] The piezoelectric layer is a single crystal wafer that is tangentially sensitive to temperature; the piezoelectric layer is provided with a strain isolation structure; the strain isolation structure comprises a first through hole, a second through hole, a third through hole and a fourth through hole; the first through hole is connected to the second through hole through a first strain isolation beam; the third through hole is connected to the fourth through hole through a second strain isolation beam; the first through hole is connected to the third through hole through a third strain isolation beam; the second through hole and the fourth through hole are connected through a fourth strain isolation beam; the surfaces of the first strain isolation beam, the second strain isolation beam, the third strain isolation beam and the fourth strain isolation beam that are in contact with the thermal stress compensation layer are suspended, that is, they are not in contact with the thermal stress compensation layer;

[0037] The conductive layer includes a ground terminal pad, a signal terminal pad and a temperature sensitive unit; the temperature sensitive unit includes a forked electrode and a Bragg reflector; the Bragg reflector is located on both sides of the forked electrode; the ground terminal pad is connected to the Bragg reflector; the forked electrode includes a ground terminal forked electrode, a forked sensitive synapse and a signal terminal forked electrode; the ground terminal pad is connected to the ground terminal forked electrode; the signal terminal pad is connected to the signal terminal forked electrode; the signal terminal pad is connected to the first strain isolation beam; the signal terminal pad is connected to the signal terminal forked electrode; the ground terminal pad is connected to the second strain isolation beam; the ground terminal pad is connected to the ground terminal forked electrode; the third strain isolation beam is perpendicular to the direction in which the forked electrode is set; the fourth strain isolation beam is perpendicular to the direction in which the forked electrode is set;

[0038] The third strain isolation beam and the fourth strain isolation beam are arranged in the direction of surface acoustic wave transmission, that is, the third strain isolation beam is perpendicular to the direction in which the interdigital electrodes are arranged and the fourth strain isolation beam is perpendicular to the direction in which the interdigital electrodes are arranged. When the temperature changes, the transverse strain generated by the thermal stress compensation layer and the temperature field is greater than the longitudinal strain; the third strain isolation beam and the fourth strain isolation beam provide more transverse strain transmission to improve the accuracy of measurement;

[0039] The base material of the protective layer is one or more of aluminum oxide, silicon oxide and zirconium oxide ceramic films; the protective layer is located directly above the temperature sensitive unit to protect the interdigital electrodes from being oxidized and agglomerated and failed;

[0040] The base material of the thermal stress compensation layer is one or more of sapphire, silicon carbide, diamond, nickel-titanium alloy, and aluminum foil;

[0041] A method for calculating the temperature sensitivity of a surface acoustic wave temperature sensor is:

[0042] k(f,T)=k(f0,T0)[1+α(f-f0)]

[0043] Wherein, k(f0,T0) is the sensitivity of the resonant frequency of the piezoelectric layer, f0 is the resonant frequency of the piezoelectric layer; T0 is the temperature of the piezoelectric layer; α is the frequency-temperature coefficient of thermal stress compensation, k(f,T) is the sensitivity of the surface acoustic wave temperature sensor, f is the resonant frequency of the surface acoustic wave temperature sensor, and T is the temperature of the surface acoustic wave temperature sensor; when the substrate material of the thermal stress compensation layer is sapphire and the material of the piezoelectric layer is single crystal quartz, the range of α is (-50,50);

[0044] The substrate in which the thermal stress compensation layer is combined with the piezoelectric layer provides additional stress compensation, and at the same temperature, the resonant frequency changes more, thereby improving the sensitivity of the surface acoustic wave temperature sensor;

[0045] Based on a surface acoustic wave temperature sensor, the present invention also provides a method for preparing the surface acoustic wave temperature sensor, comprising the following steps:

[0046] Step S1: preparing a piezoelectric layer;

[0047] The piezoelectric layer is etched layer by layer using picosecond ultraviolet laser etching to form a first through hole, a second through hole, a third through hole and a fourth through hole; the first strain isolation beam, the second strain isolation beam, the third strain isolation beam and the fourth strain isolation beam are then etched layer by layer using picosecond ultraviolet laser etching, and the strain isolation structure is suspended by picosecond ultraviolet laser etching to complete the preparation of the piezoelectric layer;

[0048] The picosecond ultraviolet laser has a wavelength of 355nm, a scanning speed of 500mm / s, and a power of 10W;

[0049] Step S2: bonding the thermal stress compensation layer and the piezoelectric layer;

[0050] After the etching of the piezoelectric layer is completed, a layer of gold film is sputtered on the lower surface of the piezoelectric layer and the upper surface of the thermal stress compensation layer; the thickness of the gold film is 150-200 nm;

[0051] Align and contact the thermal stress compensation layer, the piezoelectric layer and the suspended side of the stress isolation beam, and press and hold the thermal stress compensation layer and the piezoelectric layer. The bonding pressure during pressing is 1800-2000 mBar.

[0052] The pressed thermal stress compensation layer and piezoelectric layer are kept at 450-480°C for 30-45 minutes and then cooled to form a new substrate and complete bonding;

[0053] Step S3: preparation of a conductive layer;

[0054] After bonding is completed, a conductive layer is prepared on the piezoelectric layer by direct current magnetron sputtering, and vacuum heat treatment is performed; after the vacuum heat treatment of the piezoelectric layer, a photoresist mask is prepared on the surface of the piezoelectric layer, the photoresist mask is patterned, the metal electrode is ion-beam-etched, the pattern is transferred to the metal electrode, the photoresist mask is removed, and the preparation of the conductive layer is completed;

[0055] Step S4: preparation of a protective layer;

[0056] After the conductive layer is prepared, a polyimide mask is made on the metal electrode, and then an oxide ceramic thin film protective layer is prepared by AC magnetron sputtering, and the polyimide mask is removed to complete the preparation of the protective layer.

[0057] The key process parameters in the embodiment are as follows:

[0058] Key Parameters Parameter range unit Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Gold film thickness 150~200 nm 150 160 170 180 190 200 Bonding pressure 1800~2000 mBar 1800 1840 1880 1920 1960 2000 Bonding holding temperature 450~480 ℃ 450 456 462 468 474 480 Bonding duration 30~45 min 30 33 36 39 42 45

[0059] When the ambient temperature of the piezoelectric layer 2 changes, the stiffness, density of the piezoelectric layer 2 and the wavelength of the surface acoustic wave generated by the temperature sensitive unit 35 change, causing the resonant frequency of the surface acoustic wave to shift; the resonant frequency of the surface acoustic wave output by the temperature sensitive unit 35 decreases linearly with increasing temperature; when the ambient temperature changes, the thermal expansion coefficient of the thermal stress compensation layer 1 is different from that of the piezoelectric layer 2, and the thermal stress compensation layer 1 generates thermal strain to compensate the piezoelectric layer 2; when the ambient temperature changes, the strain isolation structure concentrates the strain generated by the temperature sensitive unit in the area directly below the temperature sensitive unit, isolates the strain interference generated in the non-temperature sensitive unit area of ​​the piezoelectric layer 2, and improves the accuracy of surface acoustic wave temperature sensing.

[0060] The strain isolation structure provided on the piezoelectric layer makes the waveguide sensitive to temperature; the strain isolation structure provided on the piezoelectric layer concentrates the strain just below the temperature sensitive unit structure, avoids strain interference in the non-temperature sensitive unit area, and improves the accuracy of temperature measurement.

[0061] The conductive layer converts the AC signal into a periodic electromagnetic field, and loads the periodic electromagnetic field into the piezoelectric layer;

[0062] The interdigitated sensitive synapse 342 can avoid the generation of microcavities during the patterning process, and can also suppress the lateral mode resonance, reduce the energy loss of the surface acoustic wave, and improve the intensity and peak value of the surface acoustic wave excitation signal.

[0063] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0064] like Figure 1As shown, it is a schematic diagram of the structure of a surface acoustic wave temperature sensor provided by an example of the present invention, and the sensor includes: a thermal stress compensation layer 1, which is a thermal stress compensation substrate; a piezoelectric layer 2, which is a temperature sensitive substrate and is provided with a first through hole 21, a second through hole 22, a third through hole 23 and a fourth through hole 24, and a first strain isolation beam 25, a second strain isolation beam 26, a third strain isolation beam 27, a fourth strain isolation beam 28 and a strain isolation structure surrounded by the first through hole 21, a second through hole 22, a third through hole 23 and a fourth through hole 24; a conductive layer 3, which is provided with a ground terminal pad 31, a signal terminal pad 32 and a cross-finger sensitive layer 31 ... The interdigital electrodes 34 of the sensing synapse 342, the signal end pad 32 is configured to convert the AC signal into a periodic electromagnetic field and load it into the piezoelectric layer, and together with the ground end pad 31 and the interdigital electrodes 34 constitute a surface acoustic wave excitation unit; the protective layer 4, the protective layer is configured to protect the interdigital electrodes from being oxidized and agglomerated and failed, and the protective layer is located directly above the temperature sensitive unit 35; when the temperature of the waveguide obtained from the surface acoustic wave excitation unit changes, the thermal stress compensation substrate and the strain isolation structure make the waveguide sensitive to temperature changes, thereby achieving more accurate measurement of the single-chip temperature and improving the measurement accuracy and sensitivity.

[0065] Specifically, in this embodiment, Figure 2-4 As shown, Figure 2 A schematic structural diagram of a piezoelectric layer 2 provided in an embodiment of the present invention. Figure 3 for Figure 2 The cross-section along the AA direction, Figure 4 for Figure 2 The cross-sectional view along the BB direction in the figure. The piezoelectric layer 2 is a piezoelectric single crystal material with a relatively high temperature coefficient. The piezoelectric layer 2 is provided with a first through hole 21, a second through hole 22, a third through hole 23 and a fourth through hole 24, and a strain isolation structure formed by a first strain isolation beam 25 connecting the first through hole 21 and the second through hole 22, a second strain isolation beam 26 connecting the third through hole and the fourth through hole, a third strain isolation beam 27 connecting the first through hole 21 and the third through hole 23, and a fourth strain isolation beam 28 connecting the second through hole 22 and the fourth through hole 24. The strain isolation structure is suspended and does not contact the thermal stress compensation layer 1. The third strain isolation beam and the fourth strain isolation beam are arranged in the transmission direction of the surface acoustic wave. When the temperature changes, the transverse strain generated by the thermal stress compensation layer and the temperature field is greater than the longitudinal strain. The third strain isolation beam and the fourth strain isolation beam provide more transverse strain transmission, thereby improving the accuracy of the measurement.

[0066] The strain isolation structure is located directly below the interdigital electrode 34 and the Bragg reflector 33 provided on the conductive layer 3, the ground terminal pad 31 provided on the conductive layer completely covers the first strain isolation beam 25 and extends, and the signal terminal pad 32 provided on the conductive layer 3 completely covers the second strain isolation beam 26 and extends. Figure 5As shown, it is a schematic diagram of the structure of a conductive layer 3 provided by an example of the present invention, wherein the conductive layer 3 includes: a ground terminal pad 31, a signal terminal pad 32, and a Bragg reflector 33, wherein the ground terminal pad 31 is connected to the Bragg reflector 33; interdigitated electrodes 34, wherein the interdigitated electrodes 34 include a ground terminal interdigitated electrode 341, an interdigitated sensitive synapse 342, and a signal terminal interdigitated electrode 343, wherein the ground terminal pad 31 is connected to the ground terminal interdigitated electrode 341, and the signal terminal pad 32 is connected to the signal terminal interdigitated electrode 34, and the Bragg reflector 33 is located on both sides of the interdigitated electrode 34; and the interdigitated sensitive synapse 342 is located at the end of one interdigit and in the gap between the side interdigits.

[0067] Furthermore, when the ambient temperature of the piezoelectric layer 2 changes, the stiffness, density and wavelength of the surface acoustic wave generated by the temperature sensitive unit 35 of the piezoelectric layer 2 change, causing the surface acoustic wave resonance frequency to shift. At a certain temperature, the surface acoustic wave resonance frequency output by the temperature sensitive unit 35 decreases linearly with the increase of temperature. When the ambient temperature changes, the thermal expansion coefficient of the thermal stress compensation layer 1 is different from that of the piezoelectric layer 2, and the thermal stress compensation layer 1 generates thermal strain to compensate the piezoelectric layer 2; when the ambient temperature changes, the strain isolation structure concentrates the strain generated by the temperature sensitive unit (not shown in the figure) in the area directly below the temperature sensitive unit (not shown in the figure), isolates the strain interference generated by the non-temperature sensitive unit area of ​​the piezoelectric layer 2, and realizes the improvement of the accuracy of surface acoustic wave temperature sensing.

[0068] Furthermore, in the method for controlling the sensitive characteristics of surface acoustic wave temperature sensing, when measuring temperature, an alternating current signal is input into the conductive layer 3, and the conductive layer 3 converts the received alternating current signal into a periodic electromagnetic field, and loads the converted periodic electromagnetic field onto the piezoelectric layer 2. After being excited by the electromagnetic field, the piezoelectric layer 2 generates a surface acoustic wave, and the Bragg reflector 33 can reflect the generated surface acoustic wave, and the interdigital electrode 34 can convert the reflected surface acoustic wave back into an electrical signal for transmission, thereby obtaining a resonant frequency signal; in particular, the interdigital sensitive synapse 342 reduces the difficulty of preparation during the preparation of the interdigital electrode 34, and avoids the generation of microcavities during the patterning process. The interdigital sensitive synapse 342 suppresses the transverse mode resonance, reduces the energy loss of the surface acoustic wave, and improves the intensity and peak value of the surface acoustic wave excitation signal. Surface acoustic waves are very sensitive to disturbances on the waveguide surface, and changes in elastic modulus, density, and strain will cause the frequency, amplitude, and phase of the acoustic wave to shift. Compared with capacitance and inductance sensors, surface acoustic wave sensors have the advantages of high quality factor, long communication distance, and small size.

[0069] Specifically, in this embodiment, the thermal stress compensation layer 1 is a sapphire wafer with a diameter of 4 inches and a thickness of 450 μm; the piezoelectric layer 2 is a single crystal quartz with a diameter of 4 inches and a thickness of 200 μm, and the Euler angle is (0°, 160°, 37°)

[0070] Furthermore, the protective layer is one or more of aluminum oxide, silicon oxide and zirconium oxide ceramic films; the protective layer is located directly above the temperature sensitive unit; and the conductive layer is one or more of gold, aluminum, platinum, platinum-rhodium alloy and platinum-iridium alloy films.

[0071] Specifically, the method for improving the temperature sensitivity of the surface acoustic wave temperature sensor includes:

[0072] The sensitivity of the surface acoustic wave temperature sensor is related to the resonant frequency f and temperature T, and the formula is:

[0073] k(f,T)=k(f0,T0)[1+α(f-f0)]

[0074] Wherein, k(f0,T0) is the sensitivity of the resonant frequency when there is only a piezoelectric layer, α is the frequency-temperature coefficient of thermal stress compensation, and k(f,T) is the sensitivity of the surface acoustic wave temperature sensor.

[0075] The new substrate in which the thermal stress compensation layer is combined with the piezoelectric layer provides additional stress compensation. At the same temperature, the resonant frequency changes more greatly, thereby improving the sensitivity of the surface acoustic wave temperature sensor.

[0076] like Figure 6 FIG. 1 is a flow chart of a method for preparing a surface acoustic wave temperature sensor provided by an embodiment of the present invention, wherein the method comprises:

[0077] Step S1: etching the piezoelectric layer using a picosecond ultraviolet laser with a wavelength of 355 nm, a scanning speed of 500 mm / s, and a power of 10 W to etch the first through hole, the second through hole, the third through hole, and the fourth through hole layer by layer through the laser; then reducing the thickness of the stress isolation structure layer by layer through laser etching to make it smaller than the thickness of the piezoelectric layer, thereby completing the preparation of the piezoelectric layer;

[0078] Step S2: After the piezoelectric layer is prepared, a layer of gold film is sputtered on the lower surface of the piezoelectric layer and the upper surface of the thermal stress compensation layer, and the film thickness is 200nm. Align the suspended sides of the stress isolation beam of the thermal stress compensation layer and the piezoelectric layer, and press the thermal stress compensation layer and the piezoelectric layer with a bonding pressure of 2000mBar; after the pressing reaches the preset time threshold, keep the pressed thermal stress compensation layer and the piezoelectric layer at a set temperature of 480℃ for a preset time of 30 minutes and then cool to form a new substrate, completing the bonding;

[0079] Step S3: after bonding is completed, a conductive layer is prepared on the piezoelectric layer by direct current magnetron sputtering, and vacuum heat treatment is performed; a photoresist mask is prepared on the surface obtained by the heat treatment, and the photoresist mask is patterned; the metal electrode is ion-beam-etched to transfer the pattern to the metal electrode, and the photoresist mask is removed to complete the preparation of the conductive layer;

[0080] Step S4: after the conductive layer is prepared, a polyimide mask is made on the metal electrode, and then an oxide ceramic thin film protective layer is prepared by AC magnetron sputtering, and the polyimide mask is removed to complete the preparation of the protective layer.

Claims

1. A surface acoustic wave temperature sensor, characterized in that: It comprises a conductive layer, a piezoelectric layer and a thermal stress compensation layer; the piezoelectric layer and the conductive layer are sequentially arranged on the thermal stress compensation layer; and the thermal expansion coefficient of the thermal stress compensation layer is greater than the thermal expansion coefficient of the piezoelectric layer.

2. A surface acoustic wave temperature sensor according to claim 1, characterized in that: The piezoelectric layer is a single crystal wafer that is temperature-sensitive in the tangential direction; the piezoelectric layer is provided with a strain isolation structure; the strain isolation structure includes a first through hole, a second through hole, a third through hole and a fourth through hole; the first through hole is connected to the second through hole through a first strain isolation beam; the third through hole is connected to the fourth through hole through a second strain isolation beam; the first through hole and the third through hole are connected through a third strain isolation beam; the second through hole and the fourth through hole are connected through a fourth strain isolation beam; the surfaces of the first strain isolation beam, the second strain isolation beam, the third strain isolation beam and the fourth strain isolation beam that are in contact with the thermal stress compensation layer are suspended, that is, they are not in contact with the thermal stress compensation layer.

3. A surface acoustic wave temperature sensor according to claim 2, characterized in that: The conductive layer includes a ground terminal pad, a signal terminal pad and a temperature sensitive unit; the temperature sensitive unit includes a forked electrode and a Bragg reflector; the Bragg reflector is located on both sides of the forked electrode; the ground terminal pad is connected to the Bragg reflector; the forked electrode includes a ground terminal forked electrode, a forked sensitive synapse and a signal terminal forked electrode; the ground terminal pad is connected to the ground terminal forked electrode; the signal terminal pad is connected to the signal terminal forked electrode; the signal terminal pad is connected to the first strain isolation beam; the signal terminal pad is connected to the signal terminal forked electrode; the ground terminal pad is connected to the second strain isolation beam; the ground terminal pad is connected to the ground terminal forked electrode; the third strain isolation beam is perpendicular to the direction in which the forked electrode is set; the fourth strain isolation beam is perpendicular to the direction in which the forked electrode is set.

4. A surface acoustic wave temperature sensor according to claim 1, characterized in that: The base material of the thermal stress compensation layer is one or more of sapphire, silicon carbide, diamond, nickel-titanium alloy and aluminum foil.

5. A surface acoustic wave temperature sensor according to claim 1, characterized in that: A protective layer is arranged on the conductive layer.

6. A surface acoustic wave temperature sensor according to claim 1, characterized in that: The base material of the protective layer is one or more of aluminum oxide, silicon oxide and zirconium oxide ceramic films; the protective layer is located directly above the temperature sensitive unit to protect the interdigital electrodes from being oxidized and agglomerated and ineffective.

7. A surface acoustic wave temperature sensor according to claim 1, characterized in that: A method for calculating the temperature sensitivity of a surface acoustic wave temperature sensor is: k(f,T)=k(f0,T0)[1+α(f-f0)] Wherein, k(f0,T0) is the sensitivity of the resonant frequency of the piezoelectric layer, f0 is the resonant frequency of the piezoelectric layer; T0 is the temperature of the piezoelectric layer; α is the frequency-temperature coefficient of thermal stress compensation, k(f,T) is the sensitivity of the surface acoustic wave temperature sensor, f is the resonant frequency of the surface acoustic wave temperature sensor, and T is the temperature of the surface acoustic wave temperature sensor; when the substrate material of the thermal stress compensation layer is sapphire and the material of the piezoelectric layer is single crystal quartz, the range of α is (-50,50).

8. A surface acoustic wave temperature sensor according to claim 5, characterized in that: A method for preparing a surface acoustic wave microsensor comprises the following steps: Step S1: preparing a piezoelectric layer; The piezoelectric layer is etched layer by layer using picosecond ultraviolet laser etching to form a first through hole, a second through hole, a third through hole and a fourth through hole; the first strain isolation beam, the second strain isolation beam, the third strain isolation beam and the fourth strain isolation beam are then etched layer by layer using picosecond ultraviolet laser etching, and the strain isolation structure is suspended by picosecond ultraviolet laser etching to complete the preparation of the piezoelectric layer; The picosecond ultraviolet laser has a wavelength of 355nm, a scanning speed of 500mm / s, and a power of 10W; Step S2: bonding the thermal stress compensation layer and the piezoelectric layer; After the etching of the piezoelectric layer is completed, a layer of gold film is sputtered on the lower surface of the piezoelectric layer and the upper surface of the thermal stress compensation layer; the thickness of the gold film is 150-200 nm; Align and contact the thermal stress compensation layer, the piezoelectric layer and the suspended side of the stress isolation beam, and press and hold the thermal stress compensation layer and the piezoelectric layer. The bonding pressure during pressing is 1800-2000 mBar. The pressed thermal stress compensation layer and the piezoelectric layer are kept at 450-480°C for 30-45 minutes and then cooled to form a new substrate and complete bonding; Step S3: preparation of a conductive layer; After bonding is completed, a conductive layer is prepared on the piezoelectric layer by direct current magnetron sputtering, and vacuum heat treatment is performed; after the vacuum heat treatment of the piezoelectric layer, a photoresist mask is prepared on the surface of the piezoelectric layer, the photoresist mask is patterned, the metal electrode is ion-beam-etched, the pattern is transferred to the metal electrode, the photoresist mask is removed, and the preparation of the conductive layer is completed; Step S4: preparation of a protective layer; After the conductive layer is prepared, a polyimide mask is made on the metal electrode, and then an oxide ceramic thin film protective layer is prepared by AC magnetron sputtering, and the polyimide mask is removed to complete the preparation of the protective layer.

Citation Information

Cited By

  • Wide-temperature-range high-linearity wireless temperature sensor based on thermal stress collaborative suppression and design method

    CN121829805A