Rapid detection method for surface opening characteristic of porous microcarrier
Through optical microscope combined with swelling and dehydration treatment technology, the cost and accuracy of the equipment for detecting the surface opening characteristics of porous microcarriers in the prior art is solved, and the equipment has low threshold, fast and efficient detection is achieved, which can truly reflect the porous microcarriers. Information on surface opening structure in liquid environments and distinguish between open and closed structures.
Patent Information
- Application Number
- CN202410843411.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art methods for detecting the surface opening characteristics of porous microcarriers are expensive, complex in operation and low in accuracy, and cannot meet the needs of production and application, especially in liquid environments where pore size information is biased.
The surface opening structure of porous microcarriers is marked and quantitatively analyzed by image analysis software to achieve rapid and accurate detection.
It lowers the equipment threshold, improves detection efficiency and accuracy, can truly reflect the surface opening structure information of the porous microcarrier in a liquid environment, and distinguishes the opening and closed structures by adjusting the degree of dehydration.
Smart Images

Figure CN118961694A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of detection technology, and in particular to a method for quickly detecting surface opening characteristics of a porous microcarrier. Background Art
[0002] Porous microcarriers for cell culture are an innovation in the field of biotechnology. As a three-dimensional scaffold, they provide a biomimetic growth environment for cells with a high degree of porosity and a specific pore size design to optimize cell adhesion, proliferation and differentiation. These porous microcarriers are usually made of biocompatible materials and not only support basic biological research, but also play an important role in drug screening, tissue engineering, regenerative medicine and cell agriculture, representing an important direction for the development of biomedical engineering towards efficient and precise cell culture technology.
[0003] Since porous microcarriers have an open surface pore structure, they can provide an ideal environment for cell proliferation and differentiation, and promote the process of large-scale cell culture and tissue regeneration. Therefore, porous microcarriers are increasingly used in 3D cell culture, tissue engineering, cell cultured meat and other fields.
[0004] The surface opening characteristics of porous microcarriers directly affect their culture effect as carriers, so it is necessary to detect their surface opening characteristics. At present, the surface opening characteristics of porous microcarriers are usually detected with the help of scanning electron microscopes, transmission electron microscopes and ultra-high resolution microscopes. However, the above detection methods have a series of defects: first, the equipment used in the above methods is relatively expensive and has a high threshold. At the same time, there are also problems such as long testing time and complicated operation, which cannot meet the actual needs of production and application; secondly, scanning electron microscopes and transmission electron microscopes can only detect porous microcarriers in dry powder form; but the working environment of porous microcarriers is a liquid environment, and their pore structure will swell in a liquid environment. Therefore, the pore size information obtained when the porous microcarrier is in dry powder form will deviate from that in its working environment, and the accuracy is low.
[0005] In summary, there is an urgent need to provide a detection method that has low equipment requirements and is efficient, accurate and fast to detect the surface opening characteristics of porous microcarriers. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for rapid detection of surface opening characteristics of porous microcarriers. The present invention uses a relatively conventional optical microscope to detect the surface opening characteristics of porous microcarriers, which has a low equipment threshold, is fast and efficient, and is more conducive to promotion. In addition, the method of the present invention can detect the surface opening characteristics of porous microcarriers in a swollen state, and the obtained data information can more truly and accurately reflect the surface opening structure information of the porous microcarriers in a working state.
[0007] The specific technical solution of the present invention is: a method for rapid detection of surface opening characteristics of porous microcarriers, comprising the following steps: 1) The porous microcarrier to be tested is immersed in water for swelling treatment.
[0008] 2) The swollen porous microcarrier is taken out and immersed in a dehydration solvent, so that the dehydration solvent replaces part of the water in the porous microcarrier.
[0009] 3) The porous microcarrier is taken out, the dehydration solvent is evaporated, and the surface opening structure of the porous microcarrier is photographed using an optical microscope to obtain a picture.
[0010] 4) The pore sizes of the surface opening structures of the porous microcarriers in the image are marked and quantitatively analyzed using image analysis software to obtain surface opening characteristic information.
[0011] Compared with the existing methods that require the use of high-end equipment such as scanning microscopes, transmission electron microscopes or ultra-high resolution microscopes to detect the surface opening characteristics of porous microcarriers, the present invention can complete the detection with only a relatively conventional optical microscope, which has a low equipment threshold and is more conducive to promotion. In addition, the method of the present invention also has the characteristics of high detection accuracy, rapidity and high efficiency.
[0012] In the present invention, the porous microcarrier is first subjected to a swelling treatment, and the pore size in the porous microcarrier becomes larger after swelling, so the detection data in this state can more truly and accurately reflect the surface opening structure information of the porous microcarrier in the working state (liquid environment). However, the present invention finds that since the porous microcarrier contains both surface opening structures and internal closed structures, and the porous microcarrier is swollen, its light transmittance is enhanced, which makes it difficult to effectively distinguish the above-mentioned open structure and closed structure. For this reason, the present invention dehydrates the porous microcarrier and finds that under an appropriate degree of dehydration, the light transmittance to the porous microcarrier can be significantly reduced without substantially affecting the pore size of the porous microcarrier, thereby being able to distinguish the open structure and the closed structure.
[0013] Preferably, in 1), the ratio of the porous microcarrier to water is 1-100 mg:10 mL. The swelling treatment is performed under room temperature oscillation for 1-10 h.
[0014] Under the above material ratio and swelling time, it can be ensured that the porous microcarrier is fully swollen and reaches a balanced state, at which time the pore structure in the porous microcarrier is opened after absorbing water, and is highly consistent with the state in its working environment.
[0015] Preferably, in 2), the dehydration solvent is anhydrous ethanol.
[0016] Anhydrous ethanol can replace the water in the swollen porous microcarriers, and due to the volatility of anhydrous ethanol, it can dehydrate the porous microcarriers, thereby adjusting the light transmittance of the porous microcarriers.
[0017] Preferably, in 2), the volume ratio of the swollen porous microcarrier to the dehydration solvent is 1:50-200; and after being immersed in the dehydration solvent, an oscillation treatment is performed for 5-60 minutes.
[0018] The present invention finds that the degree of dehydration has a great influence on the light transmittance and pore size of the porous microcarrier after swelling. Under the above material ratio and immersion time, the proportion of water replaced by anhydrous ethanol can be adjusted, which is conducive to distinguishing the open structure and the closed structure without affecting the pore size of the porous microcarrier.
[0019] Preferably, in 3), after the porous microcarrier is taken out, it is placed on a glass slide, left to stand for 1-10 minutes under an optical microscope, and then photographed.
[0020] When anhydrous ethanol replaces a certain proportion of water in the porous microcarriers, the anhydrous ethanol is allowed to evaporate by standing still, thereby adjusting the light transmittance of the porous microcarriers, and ultimately being able to effectively distinguish between open structures and closed structures.
[0021] Preferably, in 4), the image analysis software is at least one of imageJ, Imlab and image-pro.
[0022] Preferably, 4) specifically includes: inputting the image into image analysis software, calibrating the spatial standard of the image, and marking and measuring the pore size of the surface opening structure of the porous microcarrier.
[0023] Preferably, the marking measurement is to mark the long end aperture and the short end aperture of the surface opening structure with straight line segments respectively.
[0024] Compared with the prior art, the beneficial effects of the present invention are: (1) The present invention can detect the surface opening characteristics of porous microcarriers only by using a relatively conventional optical microscope. The equipment threshold is low, and the method is fast and efficient, which is more conducive to promotion.
[0025] (2) The present invention can detect the surface opening characteristics of the porous microcarrier in the swollen state, and the obtained data information can more realistically and accurately reflect the surface opening structure information of the porous microcarrier in the working state (liquid environment).
[0026] (3) The present invention adjusts the light transmittance of the porous microcarriers by controlling the degree of dehydration of the porous microcarriers after swelling, thereby significantly reducing the light transmittance of the porous microcarriers without substantially affecting the pore size of the porous microcarriers, thereby achieving the distinction between open structures and closed structures under an optical microscope. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a picture of the porous microcarrier powder in Example 1 taken through an optical microscope without any treatment.
[0028] Figure 2 This is a picture of the porous microcarrier powder in Example 1 taken through an optical microscope after swelling and before dehydration.
[0029] Figure 3 This is the picture after manual marking and measurement in Example 1.
[0030] Figure 4 This is the original scanning electron microscope image of the porous microcarrier powder in Comparative Example 1.
[0031] Figure 5 This is the picture after manual marking and measurement in Comparative Example 1.
[0032] Figure 6 This is a comparison chart of the average pore size data of the porous microcarrier surface opening structure finally obtained in Example 1 and Comparative Example 1.
[0033] Figure 7 This is a picture of the porous microcarrier powder in Comparative Example 2 taken through an optical microscope.
[0034] Figure 8 This is a picture of the porous microcarrier powder in Comparative Example 3 taken through an optical microscope. DETAILED DESCRIPTION
[0035] The present invention is further described below in conjunction with the examples. Unless otherwise specified, the materials, reagents, etc. used in the following examples can be obtained from commercial sources.
[0036] Overall embodiment A method for rapidly detecting the surface opening characteristics of a porous microcarrier comprises the following steps: 1) The porous microcarrier to be tested is immersed in water for swelling treatment.
[0037] In some specific implementation cases, the porous microcarrier is a commercially available or homemade porous microcarrier powder. In some more specific implementation cases, the commercially available porous microcarrier powder is selected from microcarriers for cell culture such as Cytopore, Cytodex, Cytoline, 3D TableTrix ®etc.; the particle size of the porous microcarrier powder can be 1nm~999um.
[0038] In some specific implementation cases, the ratio of the porous microcarrier to water is 1-100 mg:10 mL.
[0039] In some specific implementation cases, the swelling treatment is performed under room temperature oscillation for 1-10 hours.
[0040] 2) The swollen porous microcarrier is taken out and immersed in a dehydration solvent, so that the dehydration solvent replaces part of the water in the porous microcarrier.
[0041] In some specific implementation cases, the dehydration solvent is anhydrous ethanol.
[0042] In some specific implementation cases, the volume ratio of the swollen porous microcarrier to the dehydration solvent is 1:50-200.
[0043] In some specific implementation cases, the immersion in the dehydration solvent is followed by an oscillation treatment for 5-60 minutes.
[0044] 3) The porous microcarrier is taken out, the dehydration solvent is evaporated, and the surface opening structure of the porous microcarrier is photographed using an optical microscope to obtain a picture.
[0045] In some specific implementation cases, the porous microcarrier is taken out, placed on a glass slide, left to stand for 1-10 minutes under an optical microscope, and then photographed.
[0046] 4) The pore sizes of the surface opening structures of the porous microcarriers in the image are marked and quantitatively analyzed using image analysis software to obtain surface opening characteristic information.
[0047] In some specific implementation cases, the image analysis software is at least one of imageJ, Imlab and image-pro.
[0048] In some specific implementation cases, the image is input into the image analysis software, the spatial standard of the image is calibrated, and the pore size of the surface opening structure of the porous microcarrier is marked and measured.
[0049] In some specific implementation cases, the marking measurement is to mark the long end aperture and the short end aperture of the surface opening structure with straight line segments respectively.
[0050] Specific Examples and Comparative Examples Example 1 10 mg of 3D TableTrix purchased from Huakan Biotechnology ®The porous microcarrier powder was dissolved in a 10 mL centrifuge tube filled with deionized water. After dissolution, it was balanced at room temperature for 3 hours under shaking conditions to completely swell. After the swollen porous microcarriers were allowed to settle to the bottom of the centrifuge tube, the swollen porous microcarriers at the bottom of the centrifuge tube were sucked out with a rubber-tipped dropper and transferred to another centrifuge tube. Anhydrous ethanol was added to this centrifuge tube, and the ratio of swollen porous microcarriers to anhydrous ethanol was 1mL:50mL. The porous microcarriers after adding anhydrous ethanol were rapidly shaken for 10 minutes, at which time part of the water in the porous microcarriers was replaced by anhydrous ethanol. Take some of the porous microcarriers and place them on a glass slide, let it stand for 5 minutes, the anhydrous ethanol gradually evaporated, the light transmittance of the porous microcarriers decreased, and then the porous microcarriers were directly observed through an optical microscope. After confirming that the surface opening structure in the porous microcarriers can be distinguished, take pictures to obtain pictures.
[0051] The images captured above were input into the image-pro software, and then the spatial standard of the images was calibrated (the scale length used for spatial calibration can be obtained from the microscope manufacturer). After calibration, the pores on the surface of the porous microcarrier were manually marked and measured (the diameter of the surface opening structure was marked with a straight line segment, and the long end and the short end of the pore were measured separately).
[0052] The above measured data were collated and analyzed, and finally the surface opening characteristic information of the porous microcarrier sample in the working state was obtained (average pore size, average size of a single open channel = (channel long end diameter + channel long end diameter) / 2).
[0053] Figure 1 3D TableTrix purchased from Huakan Biotechnology in this example ® The porous microcarrier powder is taken under an optical microscope without any treatment (scale 100μm); Figure 1 It can be seen that in this state, the surface opening structure of the porous microcarrier powder cannot be clearly observed through an optical microscope.
[0054] Figure 2 The above porous microcarrier powder is photographed by optical microscope after swelling and before dehydration (scale 100 μm). Figure 2 It can be found that the light transmittance of the porous microcarrier is enhanced after swelling, which makes it difficult to effectively distinguish the surface open structure and the internal closed structure.
[0055] Figure 3 This is a manually marked measurement picture in this example (scale 100 μm). Figure 3 It can be seen that in this state, its surface opening structure can basically be identified through an optical microscope.
[0056] Comparative Example 1: Detection of the surface opening structure characteristics of porous microcarrier powder using scanning electron microscopy First, a 10mm×20mm conductive glue is attached to the center of the stage, and then the porous microcarrier powder (same as in Example 1) is evenly and non-pressurized to cover the conductive glue layer, and the excess porous microcarrier powder is removed by an ear-cleaning ball to keep it in a single layer. The stage and the porous microcarrier powder are pre-treated with gold spraying and observed. The scanning electron microscope image of the porous microcarrier powder under a fixed magnification field of view can be quickly obtained through the scanning electron microscope image. The captured image is input into the image pro software, and then the spatial standard of the image is calibrated (the scale length used for spatial calibration can be obtained from the scanning electron microscope manufacturer). After calibration, the surface opening structure pores of the porous microcarrier powder are manually marked and measured (the diameter of the surface opening pores is marked with a straight line segment, and the long end and the short end of the pore are measured respectively).
[0057] Figure 4 This is a scanning electron microscope image of the porous microcarrier powder obtained in this comparative example; Figure 5 Shown is a graph of the results of a manually labeled measurement.
[0058] Figure 6 The surface opening characteristic data (average pore size) of the porous microcarriers finally measured in Example 1 and Comparative Example 1. By comparison, it can be seen that the average pore size measured in Example 1 is significantly larger than that in Comparative Example 1. The reason is that the test sample in Comparative Example 1 is in a dry powder state, which is inconsistent with the pore size of the swollen state under a liquid working environment. Therefore, the data measured by the method of the present invention can more truly and accurately reflect the working state of the porous microcarrier and is more valuable.
[0059] Comparative Example 2 10 mg of 3D TableTrix purchased from Huakan Biotechnology ®The porous microcarrier powder was dissolved in a 10 mL centrifuge tube filled with deionized water. After dissolution, it was balanced at room temperature for 3 hours under shaking conditions to completely swell. After the swollen porous microcarriers were allowed to settle to the bottom of the centrifuge tube, the swollen porous microcarriers at the bottom of the centrifuge tube were sucked out with a rubber-tipped dropper and transferred to another centrifuge tube. Anhydrous ethanol was added to this centrifuge tube, and the ratio of swollen porous microcarriers to anhydrous ethanol was 1mL:30mL. The porous microcarriers after adding anhydrous ethanol were quickly shaken for 3 minutes, at which time part of the water in the porous microcarriers was replaced by anhydrous ethanol. Take some of the porous microcarriers and place them on a glass slide, let it stand for 5 minutes, the anhydrous ethanol gradually evaporated, and then the porous microcarriers were directly observed under an optical microscope. The results show that due to the small amount of anhydrous ethanol used in this comparative example and the short time for rapid oscillation to replace the water in the porous microcarrier, the dehydration degree of the porous microcarrier is weak, which leads to a limited reduction in the light transmittance of the porous microcarrier. In this state, it is still impossible to clearly distinguish the surface open structure and the closed structure of the porous microcarrier (such as Figure 7 as shown).
[0060] Comparative Example 3 10 mg of 3D TableTrix purchased from Huakan Biotechnology ® The porous microcarrier powder was dissolved in a 10 mL centrifuge tube filled with deionized water. After dissolution, it was balanced at room temperature for 3 hours under shaking conditions to completely swell. After the swollen porous microcarriers were allowed to settle to the bottom of the centrifuge tube, a rubber-tipped dropper was used to suck out the swollen porous microcarriers at the bottom of the centrifuge tube and transferred to another centrifuge tube. Anhydrous ethanol was added to this centrifuge tube, and the ratio of swollen porous microcarriers to anhydrous ethanol was 1mL:250mL. The porous microcarriers after adding anhydrous ethanol were rapidly shaken for 10 minutes, at which time most of the water in the porous microcarriers was replaced by anhydrous ethanol. Take some of the porous microcarriers and place them on a glass slide, let it stand for 10 minutes, the anhydrous ethanol gradually evaporated, and then the porous microcarriers were directly observed under an optical microscope. It was found that due to the large amount of anhydrous ethanol used in this comparative example, the dehydration degree of the porous microcarriers was too strong, resulting in too low light transmittance in the porous microcarriers. In this state, the surface opening structure and the closed structure of the content (such as) in the porous microcarriers could not be clearly and effectively observed under an optical microscope. Figure 8 In this state, the pore size in the porous microcarriers will also be reduced.
[0061] Example 2 5 mg of Cytopore porous microcarrier powder was dissolved in a 10 mL centrifuge tube filled with deionized water. After dissolution, it was balanced at room temperature for 5 hours under shaking conditions to completely swell. After the swollen porous microcarrier was allowed to settle at the bottom of the centrifuge tube, the swollen porous microcarrier at the bottom of the centrifuge tube was sucked out with a rubber-tipped dropper and transferred to another centrifuge tube. Anhydrous ethanol was added to this centrifuge tube, and the ratio of swollen porous microcarrier to anhydrous ethanol was 1 mL:100 mL. The porous microcarrier after adding anhydrous ethanol was rapidly shaken for 10 minutes, at which time part of the water in the porous microcarrier was replaced by anhydrous ethanol. Take part of the porous microcarrier and place it on a glass slide, let it stand for 10 minutes, the anhydrous ethanol gradually evaporated, the light transmittance of the porous microcarrier decreased, and then the porous microcarrier was directly observed through an optical microscope. After confirming that the surface opening structure in the porous microcarrier can be distinguished, take a picture to obtain a picture.
[0062] The images captured above were input into the image-pro software, and then the spatial standard of the images was calibrated (the scale length used for spatial calibration can be obtained from the microscope manufacturer). After calibration, the pores on the surface of the porous microcarrier were manually marked and measured (the diameter of the surface opening structure was marked with a straight line segment, and the long end and the short end of the pore were measured separately).
[0063] The above measured data were collated and analyzed, and finally the surface opening characteristic information of the porous microcarrier sample in the working state was obtained (average pore size, average size of a single open channel = (channel long end diameter + channel long end diameter) / 2).
[0064] Example 3 20 mg of Cytodex porous microcarrier powder was dissolved in a 10 mL centrifuge tube filled with deionized water. After dissolution, it was balanced at room temperature for 8 hours under shaking conditions to completely swell. After the swollen porous microcarriers were allowed to settle at the bottom of the centrifuge tube, the swollen porous microcarriers at the bottom of the centrifuge tube were sucked out with a rubber-tipped dropper and transferred to another centrifuge tube. Anhydrous ethanol was added to this centrifuge tube, and the ratio of swollen porous microcarriers to anhydrous ethanol was 1 mL:150 mL. The porous microcarriers after adding anhydrous ethanol were quickly shaken for 8 minutes, at which time part of the water in the porous microcarriers was replaced by anhydrous ethanol. Take part of the porous microcarriers and place them on a glass slide, let it stand for 8 minutes, the anhydrous ethanol gradually evaporated, the light transmittance of the porous microcarriers decreased, and then the porous microcarriers were directly observed through an optical microscope. After confirming that the surface opening structure in the porous microcarrier can be distinguished, take a picture to obtain a picture.
[0065] The images captured above were input into the image J software, and then the spatial standard of the images was calibrated (the scale length used for spatial calibration can be obtained from the microscope manufacturer). After calibration, the pores on the surface of the porous microcarrier were manually marked and measured (the diameter of the surface opening structure was marked with a straight line segment, and the long end and the short end of the pore were measured separately).
[0066] The above measured data were collated and analyzed, and finally the surface opening characteristic information of the porous microcarrier sample in the working state was obtained (average pore size, average size of a single open channel = (channel long end diameter + channel long end diameter) / 2).
[0067] Example 4 10 mg of 3D TableTrix purchased from Huakan Biotechnology ® The porous microcarrier powder was dissolved in a 10 mL centrifuge tube filled with deionized water. After dissolution, it was balanced at room temperature for 3 hours under shaking conditions to completely swell. After the swollen porous microcarriers were allowed to settle to the bottom of the centrifuge tube, the swollen porous microcarriers at the bottom of the centrifuge tube were sucked out with a rubber-tipped dropper and transferred to another centrifuge tube. Anhydrous ethanol was added to this centrifuge tube, and the ratio of swollen porous microcarriers to anhydrous ethanol was 1mL:50 mL. The porous microcarriers after adding anhydrous ethanol were rapidly shaken for 10 minutes, at which time part of the water in the porous microcarriers was replaced by anhydrous ethanol. Take part of the porous microcarriers and place them on a glass slide, let it stand for 5 minutes, the anhydrous ethanol gradually evaporated, the light transmittance of the porous microcarriers decreased, and then the porous microcarriers were directly observed through an optical microscope. After confirming that the surface opening structure in the porous microcarriers can be distinguished, take pictures to obtain pictures.
[0068] The images captured above were input into the Imlab software, and then the spatial standard of the images was calibrated (the scale length used for spatial calibration can be obtained from the microscope manufacturer). After calibration, the pores on the surface of the porous microcarrier were manually marked and measured (the diameter of the surface opening structure was marked with a straight line segment, and the long end and the short end of the pore were measured separately).
[0069] The above measured data were collated and analyzed, and finally the surface opening characteristic information of the porous microcarrier sample in the working state was obtained (average pore size, average size of a single open channel = (channel long end diameter + channel long end diameter) / 2).
[0070] Example 5 15 mg of 3D TableTrix purchased from Huakan Biotechnology ®The porous microcarrier powder was dissolved in a 10 mL centrifuge tube filled with deionized water. After dissolution, it was balanced at room temperature for 3 hours under shaking conditions to completely swell. After the swollen porous microcarriers were allowed to settle to the bottom of the centrifuge tube, the swollen porous microcarriers at the bottom of the centrifuge tube were sucked out with a rubber-tipped dropper and transferred to another centrifuge tube. Anhydrous ethanol was added to this centrifuge tube, and the ratio of swollen porous microcarriers to anhydrous ethanol was 1mL:70 mL. The porous microcarriers after adding anhydrous ethanol were rapidly shaken for 6 minutes, at which time part of the water in the porous microcarriers was replaced by anhydrous ethanol. Take part of the porous microcarriers and place them on a glass slide, let it stand for 5 minutes, the anhydrous ethanol gradually evaporated, the light transmittance of the porous microcarriers decreased, and then the porous microcarriers were directly observed through an optical microscope. After confirming that the surface opening structure in the porous microcarriers can be distinguished, take pictures to obtain pictures.
[0071] The images captured above were input into the image-pro software, and then the spatial standard of the images was calibrated (the scale length used for spatial calibration can be obtained from the microscope manufacturer). After calibration, the pores on the surface of the porous microcarrier were manually marked and measured (the diameter of the surface opening structure was marked with a straight line segment, and the long end and the short end of the pore were measured separately).
[0072] The above measured data were collated and analyzed, and finally the surface opening characteristic information of the porous microcarrier sample in the working state was obtained (average pore size, average size of a single open channel = (channel long end diameter + channel long end diameter) / 2).
[0073] Example 6 10 mg of 3D TableTrix purchased from Huakan Biotechnology ® The porous microcarrier powder was dissolved in a 10 mL centrifuge tube filled with deionized water. After dissolution, it was balanced at room temperature for 3 hours under shaking conditions to completely swell. After the swollen porous microcarriers were allowed to settle to the bottom of the centrifuge tube, the swollen porous microcarriers at the bottom of the centrifuge tube were sucked out with a rubber-tipped dropper and transferred to another centrifuge tube. Anhydrous ethanol was added to this centrifuge tube for immersion, and the ratio of swollen porous microcarriers to anhydrous ethanol was 1mL:100mL. The porous microcarriers after adding anhydrous ethanol were rapidly shaken for 10 minutes, at which time part of the water in the porous microcarriers was replaced by anhydrous ethanol. Take part of the porous microcarriers and place them on a glass slide, let it stand for 10 minutes, the anhydrous ethanol gradually evaporated, the light transmittance of the porous microcarriers decreased, and then the porous microcarriers were directly observed through an optical microscope. After confirming that the surface opening structure in the porous microcarriers can be distinguished, take pictures to obtain pictures.
[0074] The images captured above were input into the image-pro software, and then the spatial standard of the images was calibrated (the scale length used for spatial calibration can be obtained from the microscope manufacturer). After calibration, the pores on the surface of the porous microcarrier were manually marked and measured (the diameter of the surface opening structure was marked with a straight line segment, and the long end and the short end of the pore were measured separately).
[0075] The above measured data were collated and analyzed, and finally the surface opening characteristic information of the porous microcarrier sample in the working state was obtained (average pore size, average size of a single open channel = (channel long end diameter + channel long end diameter) / 2).
[0076] In summary, compared with the prior art, the method of the present invention has the following advantages: (1) The present invention can detect the surface opening characteristics of porous microcarriers only by using a relatively conventional optical microscope. The equipment threshold is low, and the method is fast and efficient, which is more conducive to promotion.
[0077] (2) The present invention can detect the surface opening characteristics of the porous microcarrier in the swollen state, and the obtained data information can more realistically and accurately reflect the surface opening structure information of the porous microcarrier in the working state (liquid environment).
[0078] (3) The present invention adjusts the light transmittance of the porous microcarriers by controlling the degree of dehydration of the porous microcarriers after swelling, thereby significantly reducing the light transmittance of the porous microcarriers without substantially affecting the pore size of the porous microcarriers, thereby achieving the distinction between open structures and closed structures under an optical microscope.
[0079] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0080] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for rapid detection of surface opening characteristics of porous microcarriers, characterized in that include: 1) Immerse the porous microcarrier in water for swelling treatment; 2) taking out the swollen porous microcarrier and immersing it in a dehydrating solvent, so that the dehydrating solvent replaces part of the water in the porous microcarrier; 3) The porous microcarrier is taken out, the dehydration solvent is evaporated, and the surface opening structure of the porous microcarrier is photographed using an optical microscope to obtain a picture; 4) The pore size of the surface opening structure of the porous microcarrier in the image is marked and quantitatively analyzed by image analysis software to obtain surface opening characteristic information.
2. The method according to claim 1, characterized in that: 1), the ratio of the porous microcarrier to water is 1-100 mg:10 mL.
3. The method according to claim 1 or 2, characterized in that: 1), the swelling treatment is carried out under room temperature shaking for 1-10 hours.
4. The method according to claim 1, characterized in that: 2), the dehydration solvent is anhydrous ethanol.
5. The method according to claim 1 or 4, characterized in that: 2), the volume ratio of the swollen porous microcarrier to the dehydration solvent is 1:50-200.
6. The method according to claim 1 or 4, characterized in that: 2) After immersing in a dehydrating solvent, the sample is shaken for 5-60 minutes.
7. The method according to claim 1, characterized in that: 3), after taking out the porous microcarrier, place it on a glass slide, let it stand for 1-10 minutes under an optical microscope, and then take a picture.
8. The method according to claim 1, characterized in that: 4), the image analysis software is at least one of imageJ, Imlab and image-pro.
9. The method according to claim 1 or 8, characterized in that: 4) Specifically including: inputting the image into the image analysis software, calibrating the spatial standard of the image, and marking and measuring the pore size of the surface opening structure of the porous microcarrier.
10. The method according to claim 9, characterized in that: The marking measurement is to mark the long end aperture and the short end aperture of the surface opening structure with straight line segments respectively.