Nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water as well as preparation method and application of nickel-copper hydroxide carbon cloth sensitive electrode
By loading new sensitive electrodes with nickel-copper hydroxide on carbon cloth, combined with hydrothermal method and electrochemical method, the problems of expensive, low sensitivity and slow response of ammonia nitrogen detection equipment in the prior art are solved, and high sensitivity is achieved. Fast and economical ammonia nitrogen detection effect.
Patent Information
- Application Number
- CN202411018640.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing electrochemical sensing technology has problems such as expensive equipment, toxic reagents, complex operation, low sensitivity and slow response speed when detecting ammonia nitrogen in water. Traditional ion-selective electrodes are easily disturbed, and precious metal catalytic electrodes are costly and responsive. slow.
Using a new sensitive electrode with nickel-copper hydroxide loaded on a carbon cloth, nickel-copper hydroxide is synthesized by hydrothermal method, combined with cyclic voltammetry and timing current method for detection, avoiding the use of precious metals and complex preparation processes, and enhancing the Catalytic performance and anti-interference ability.
It realizes sensitive, accurate and fast ammonia nitrogen detection, with low detection limit, wide linear range, high sensitivity, excellent stability and economy, faster response speed, suitable for real-time monitoring.
Smart Images

Figure CN118961836A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical sensing, and in particular relates to a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water, a preparation method and an application thereof. Background Art
[0002] Ammonia nitrogen is a common pollutant in water with certain physiological toxicity. Excessive ammonia nitrogen can cause poisoning of aquatic organisms or eutrophication pollution, produce nitrates, consume dissolved oxygen, and seriously affect the ecosystem and human health. In recent years, low-toxic chloramines have been used more and more widely in the disinfection process, but if they are not handled properly, tap water may also contain a large amount of ammonia nitrogen. Efficient, rapid and accurate detection and monitoring of the concentration of ammonia nitrogen in water bodies has important application value. At present, a variety of analytical techniques have been developed for the detection of ammonia nitrogen, such as chemiluminescence, spectrophotometry, mass spectrometry, capillary electrophoresis, chromatography, etc. However, these technologies have problems such as expensive equipment, use of toxic reagents, and complex operation. Electrochemical detection technology has the advantages of simple operation, miniaturization, fast response speed, and suitability for on-site detection, and has been widely studied.
[0003] The performance of ammonia nitrogen electrochemical sensors is mainly determined by the sensitive electrodes used. Traditional ion-selective electrode and other potential-type electrochemical methods are susceptible to interference from various anions and cations, and require additional circuit compensation, resulting in higher prices. Secondly, its low sensitivity makes it difficult for the sensor to detect low concentrations of ammonia nitrogen. At present, there are many electrochemical sensors based on voltammetry, which detect ammonia nitrogen through catalytic current, have strong anti-interference ability and high sensitivity, but often require the use of precious metals, which makes them more expensive, and the voltammetry method requires a long period of stirring, standing and scanning, and the response is slow.
[0004] Carbon cloth (CC) has good conductivity, three-dimensional porous structure and excellent acid and alkali resistance. It is usually selected as the base material for preparing self-supporting electrodes, avoiding the increase in impedance caused by the use of additional conductive additives. Nickel (Ni) is a magnetic metal element that is often used to form alloys or catalysis. Copper (Cu) is an element widely present on the surface of the earth's crust, with abundant reserves and economical prices. Nickel and copper elements have good catalytic ability, and some of their compounds can even exceed commercial platinum carbon. Compared with precious metals, they have excellent economic benefits. Studies have shown that the main active substances for the catalytic oxidation of ammonia nitrogen by nickel and copper metals are their hydroxides. The catalytic potential of copper is low, but the catalytic ability is correspondingly weak; the catalytic ability of nickel is strong, but its catalytic potential is high, and the background current is high, which is not conducive to detection. By doping nickel hydroxide with copper, its ammonia nitrogen catalytic oxidation barrier can be greatly reduced, its catalytic ability can be enhanced, and it is helpful for electrochemical detection. Summary of the invention
[0005] The purpose of the present invention is to provide a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water, a preparation method and its application. The present invention uses carbon cloth as a substrate and loads nickel-copper hydroxide on its surface to construct a new type of ammonia nitrogen sensitive electrode. The sensitive electrode has good sensitivity to ammonia nitrogen in water within a certain concentration range and can achieve sensitive, accurate and rapid detection.
[0006] The first aspect of the present invention is to provide a method for preparing a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water, the steps of which are as follows:
[0007] (1) Soak the carbon cloth in the pretreatment solution for a certain period of time, take it out, and clean it with ultrasonic cleaning of deionized water;
[0008] (2) dissolving a copper source, a nickel source and urea in deionized water and stirring to obtain a hydrothermal deposition solution;
[0009] (3) adding the carbon cloth treated in step (1) and the hydrothermal deposition liquid obtained in step (2) into a hydrothermal kettle for hydrothermal reaction, taking out the carbon cloth after the hydrothermal reaction, washing and drying it to obtain the nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water.
[0010] Preferably, in step (1), the pretreatment solution is prepared by concentrated nitric acid (mass fraction of 65% to 68%) and concentrated sulfuric acid (mass fraction of 95% to 98%) in a volume ratio of 2 to 3:1, and the carbon cloth is immersed in the pretreatment solution for 60 to 72 hours;
[0011] Preferably, in step (2), the copper source is copper nitrate, and the nickel source is nickel nitrate; the sum of the concentrations of metal ions nickel and copper in deionized water is 30-100 mmol / L, nickel accounts for 10%-90% of the total molar number of nickel and copper, and the molar ratio of urea to the sum of metal ions nickel and copper is 1.5-2.5:1;
[0012] Preferably, in step (3), the hydrothermal reaction temperature is 110-130° C., and the hydrothermal reaction time is 2-8 h.
[0013] The second aspect of the present invention is to provide a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water, which is prepared by the above preparation method.
[0014] The third aspect of the present invention is to provide the use of the nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water in electrochemical detection of ammonia nitrogen in water, and the detection steps are as follows:
[0015] (1) Using the nickel-copper hydroxide carbon cloth sensitive electrode prepared by the present invention as the working electrode, the platinum sheet as the counter electrode, and mercury / mercuric oxide as the reference electrode, a supporting electrolyte is prepared for electrochemical testing;
[0016] (2) Activating the working electrode by cyclic voltammetry in a potassium hydroxide solution until the curve stabilizes;
[0017] (3) A certain concentration of ammonia nitrogen solution is added to the supporting electrolyte, and the ammonia nitrogen is detected by chronoamperometry to obtain an ammonia nitrogen response curve. The linear relationship between the current intensity and the ammonia nitrogen concentration is then fitted and used for the detection of unknown ammonia nitrogen concentration.
[0018] Preferably, in step (1), the supporting electrolyte is a 0.1-1 mol / L KOH aqueous solution.
[0019] The beneficial effects of the present invention are:
[0020] 1. Metallic copper and metallic nickel have good ammonia nitrogen catalytic ability, and their main active substances are their hydroxides. The catalytic potential of copper is low, but the catalytic ability is correspondingly weak; the catalytic ability of nickel is strong, but its catalytic potential is high, and the background current is high, which is not conducive to detection. Nickel-copper hydroxide is directly synthesized by a one-step hydrothermal method, avoiding the complicated steps of preparing alloys and oxidation; the combination of nickel and copper elements effectively improves the ammonia nitrogen catalytic performance and enhances its ammonia nitrogen sensitivity; the hydroxide form gives the material a strong local negative charge, which can effectively resist the interference and corrosion of anions such as chloride ions and fluoride ions.
[0021] 2. The novel sensitive electrode of the present invention exhibits excellent sensing capabilities when detecting ammonia nitrogen, including a lower detection limit, a wider linear range, a higher sensitivity, and excellent stability and repeatability. It is cheaper and more economical than precious metal electrodes. Compared with the commonly used cyclic voltammetry and differential pulse voltammetry, it eliminates the time-consuming stirring and standing process, has a faster response speed, and can be used for real-time monitoring. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The SEM photos of the prepared electrodes at different magnifications; in, Figure 1 (a) and Figure 1 (b) is a SEM photograph of the nickel-copper hydroxide carbon cloth sensitive electrode (NC-8@CC) prepared in Example 1 at different magnifications. Figure 1 (c) and Figure 1 (d) is the SEM photos of the pretreated carbon cloth sensitive electrode in Example 1 at different magnifications; pass Figure 1 (a) and Figure 1 (b) It can be found that the morphology of the prepared NC-8@CC is a loose porous structure composed of fine needle-like structures, which is conducive to material transport. Figure 1 (c) and Figure 1(d) The smooth surface of the carbon cloth proves that the nickel-copper hydroxide material was successfully grown on the carbon cloth.
[0023] Figure 2 The SEM photos of the prepared electrodes at different magnifications; in, Figure 2 (a) Figure 2 (b) Figure 2 (c) and Figure 2 (d) is the SEM photos of the nickel hydroxide carbon cloth (NC-10@CC) sensitive electrode prepared in Example 5 at different magnifications; pass Figure 2 It can be found that the morphology of the prepared nickel hydroxide carbon cloth sensitive electrode is a porous structure assembled by dense nanoneedles, which is significantly different from nickel copper hydroxide.
[0024] Figure 3 X-ray diffraction (XRD) patterns of pretreated carbon cloth (CC), sensitive electrodes (NC-10@CC, NC-8@CC and NC-0@CC) prepared in Example 5 and Example 1; pass Figure 3 As a result, the successful synthesis of nickel-copper hydroxide sensitive electrode was demonstrated. Figure 3 It can be found that the corresponding hydroxide diffraction peaks appear on the sensitive electrode, and the NC-8@CC sensitive electrode simultaneously shows the diffraction peaks of basic copper carbonate and basic nickel carbonate.
[0025] Figure 4 For the different electrode pairs prepared, 5 mM NH 4 CV test results of Cl; in, Figure 4 (a) Figure 4 (b) Figure 4 (c) and Figure 4 (d) CV test result curves of the pretreated carbon cloth, copper hydroxide carbon cloth sensitive electrode, nickel hydroxide carbon cloth sensitive electrode and nickel copper hydroxide carbon cloth sensitive electrode (NC-8@CC) prepared in Example 5 to 5 mM ammonia nitrogen, respectively, with the horizontal axis being the applied voltage and the vertical axis being the corresponding current density; pass Figure 4 It can be found that only nickel hydroxide carbon cloth and nickel copper hydroxide carbon cloth have a greater response to ammonia nitrogen, and nickel copper hydroxide is stronger.
[0026] Figure 5 The chronoamperometric test results of the nickel-copper hydroxide carbon cloth sensitive electrode prepared in Example 1 for ammonia nitrogen; Figure 5(a) is the chronoamperometric test curve of the nickel-copper hydroxide carbon cloth sensitive electrode prepared in Example 1 under different potentials for continuous injection of 500 μM ammonia nitrogen. Figure 5 (b) is the chronoamperometric test curve of the nickel-copper hydroxide carbon cloth sensitive electrode prepared in Example 1 at different ammonia nitrogen concentrations, and the electrolyte is 0.2M KOH; Figure 5 (d) Figure 5 (b) The enlarged image of the black circled part. The horizontal axis of these three figures is the timing time, and the vertical axis is the current density; Figure 5 (c) is the fitted linear relationship curve between ammonia nitrogen concentration and current density, with the horizontal axis being the added ammonia nitrogen concentration and the vertical axis being the current density. Figure 5 (a) It can be observed that the response at 0.60V and 0.65V is significantly greater than that at other potentials, so the optimal detection potential is around 0.60V~0.65V. Figure 5 (b) It can be found that with the continuous addition of ammonia nitrogen, the response current shows a step-like upward trend. Figure 5 (c) It can be found that in the range of ammonia nitrogen concentration of 1~100 μM, the linear relationship is y (mA cm -2 ) = 3.9×10 -3 x (μM) + 0.1336 (R 2 =0.999), sensitivity is 3.9 μA μM −1 cm −2 ; In the range of ammonia nitrogen concentration of 100~400 μM, the linear relationship is y(mA cm -2 ) = 3.13×10 -3 x (μM) + 0.2288 (R 2 =0.996), with a sensitivity of 3.13 μA μM −1 cm −2 .Depend on Figure 5 (d) It can be seen that at relatively low concentrations (1μM~5μM), this electrode still has a good response.
[0027] Figure 6 The test results of repeatability, stability and anti-interference of the nickel-copper hydroxide carbon cloth sensitive electrode prepared in Example 1; Figure 6 (a) is the anti-interference test result of the nickel-copper hydroxide carbon cloth sensitive electrode prepared in Example 1 under 0.60V it test for different interferents; the horizontal axis is the timing time, and the vertical axis is the current density. 4 Cl was 50 μM, and the interferents were 1 mM each. Figure 6 (b) Figure 6(a) The current density bar graph after adding various interferences shows that the interference is small, with an RSD of only 0.43%, which has good anti-interference performance. Figure 6 (c) The electrode was treated with 50 μM NH 4 The results of Cl detection had an RSD of 1.82%, which showed good repeatability. Figure 6 (d) The electrode repeatedly detected 50 μM NH 4 The results of Cl showed an RSD of 3.73%, which showed good stability. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the implementation methods of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1:
[0034] A method for preparing a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water, the steps of which are as follows:
[0035] 1. Mix concentrated nitric acid (mass fraction 68%) and concentrated sulfuric acid (mass fraction 98%) in a volume ratio of 3:1 to obtain a pretreatment solution, and soak the carbon cloth in the pretreatment solution for 72 hours. After the pretreatment, take out the carbon cloth and wash it with deionized water to obtain a pretreated carbon cloth (CC);
[0036] 2. Use deionized water to prepare a solution with a total metal ion concentration of 70mM (nickel-copper molar ratio of 8:2) and a urea concentration of 140mM, and stir for 30 minutes to form a uniform and stable hydrothermal deposition solution.
[0037] 3. Add the pretreated carbon cloth (CC) obtained in step (1) and 30 ml of the hydrothermal deposition liquid obtained in step (2) into a 50 ml hydrothermal kettle and react at 120° C. for 6 h. After the reaction is completed, take out the carbon cloth, wash it with deionized water under ultrasound, and dry it to obtain a nickel copper hydroxide carbon cloth sensitive electrode (NC-8@CC) for detecting ammonia nitrogen in water.
[0038] 4. Prepare a KOH solution with a concentration of 0.2M as the electrolyte for ammonia nitrogen detection. The nickel-copper hydroxide carbon cloth sensitive electrode prepared in step (3) is used as the working electrode, the platinum sheet is used as the counter electrode, and the mercury / mercury oxide electrode is used as the reference electrode. Use an electrochemical workstation (Chenhua CHI760D) to activate the electrode by cyclic voltammetry, with a potential window of 0.2-0.7V, a scan rate of 50mV / s, and 50 cycles. In addition, ammonia nitrogen was linearly tested by chronoamperometry, and different concentrations of NH 4 Cl solution, the ammonia nitrogen response curve was obtained, and the linear relationship between the current intensity and the ammonia nitrogen concentration was fitted. The results showed that with the continuous addition of ammonia nitrogen, the response current showed a step-like upward trend. In the range of ammonia nitrogen concentration of 1 to 100 μM, the linear relationship was y (mA cm -2 )=3.9×10 -3 x(μM)+0.1336(R 2 =0.999), sensitivity is 3.9μA μM -1 cm -2 The calculated detection limit is 0.62 μM. In the range of ammonia nitrogen concentration from 100 to 400 μM, the linear relationship is y (mA cm -2 )=3.13×10 -3 x(μM)+0.2288(R 2 =0.996), sensitivity is 3.13μA μM -1 cm -2 ; It fully shows that the nickel copper hydroxide carbon cloth sensitive electrode prepared by the present invention has good sensitivity in detecting ammonia nitrogen in water. Then, 500 μM NH 4 Cl solution, the baseline current density is 0.49 mA cm -2 , the response current density is 2.8 mA cm -2 The difference between the response current density and the baseline current density is proportional to its sensitivity, while the baseline current density is related to the error. When the sensitivity is the same, the lower the baseline current, the lower the detection limit.
[0039] Embodiment 2:
[0040] 1. The pretreatment process of the carbon cloth is the same as in Example 1;
[0041] 2. The preparation process of the hydrothermal deposition liquid is the same as in Example 1;
[0042] 3. The preparation process of nickel copper hydroxide carbon cloth sensitive electrode is as in Example 1;
[0043] 4. An IT test was conducted in a 1M KOH solution, and the other conditions were the same as those in Example 1. The results showed that the baseline current density of the prepared nickel-copper hydroxide carbon cloth sensitive electrode in the IT test was 0.64 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 3.31 mA cm -2 .
[0044] Embodiment 3:
[0045] 1. The pretreatment process of the carbon cloth is the same as in Example 1;
[0046] 2. The preparation process of the hydrothermal deposition liquid is the same as in Example 1;
[0047] 3. The preparation process of nickel copper hydroxide carbon cloth sensitive electrode is as in Example 1;
[0048] 4. The electrochemical test process was the same as in Example 2, except that the potential was 0.55 V. The results showed that the baseline current density of the prepared nickel-copper hydroxide carbon cloth sensitive electrode in the IT test was 0.80 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 2.92 mA cm -2 .
[0049] Embodiment 4:
[0050] 1. The pretreatment process of the carbon cloth is the same as in Example 1;
[0051] 2. The carbon cloth was directly used for electrochemical testing. The electrochemical testing process was the same as in Example 3. The results showed that the baseline current density of the pretreated carbon cloth electrode in the IT test was 0.31 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 0.38 mA cm -2 , which proves that the carbon cloth has a weak response to ammonia nitrogen.
[0052] Embodiment 5:
[0053] 1. The pretreatment process of the carbon cloth is the same as in Example 1;
[0054] 2. The preparation process of the hydrothermal deposition solution is the same as in Example 1, except that the molar ratios of nickel and copper are 10:0, 6:4, 4:6, 2:8 and 0:10 respectively;
[0055] 3. The preparation process of the sensitive electrode is the same as in Example 1, and nickel hydroxide carbon cloth sensitive electrode (NC-10@CC), nickel copper hydroxide carbon cloth sensitive electrode (NC-6@CC, NC-4@CC, NC-2@CC) and copper hydroxide carbon cloth sensitive electrode (NC-0@CC) are obtained respectively;
[0056] 4. The electrochemical test process is as in Example 3. The results show that in the IT test, when the molar ratio of nickel to copper is 10:0, the baseline current density of the prepared nickel-copper hydroxide carbon cloth sensitive electrode is 1.4 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 2.3 mA cm -2 When the molar ratio of nickel to copper is 6:4, the baseline current density is 0.48 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 1.4 mA cm -2 When the molar ratio of nickel to copper is 4:6, the baseline current density is 0.40 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 0.80 mA cm -2 When the molar ratio of nickel to copper is 2:8, the baseline current density is 0.39 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 0.78 mA cm -2 When the molar ratio of nickel to copper is 0:10, the baseline current density is 0.27 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 0.40 mA cm -2 Compared with Example 3, the sensitivity of these electrodes is lower, indicating that the optimal nickel-copper ratio is about 8:2, and the detection performance of nickel hydroxide and copper hydroxide alone is poor.
[0057] Embodiment 6:
[0058] 1. The pretreatment process of the carbon cloth is the same as in Example 1;
[0059] 2. The preparation process of the hydrothermal deposition liquid is the same as in Example 1;
[0060] 3. The preparation process of the nickel-copper hydroxide carbon cloth sensitive electrode is the same as that in Example 1, except that the hydrothermal reaction time is 2 h, 4 h, and 8 h, respectively.
[0061] 4. The electrochemical test process is the same as in Example 2. The results show that in the IT test, when the hydrothermal reaction time is 2 h, the baseline current density of the prepared nickel-copper hydroxide carbon cloth sensitive electrode is 0.40 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 2.2 mA cm -2 When the hydrothermal reaction time is 4 h, the baseline current density is 0.78 mA cm -2 After adding 500 μM ammonia nitrogen, the response current density was 2.4 mA cm -2 When the hydrothermal reaction time is 8 h, the baseline current density is 0.72 mA cm -2After adding 500 μM ammonia nitrogen, the response current density was 2.3 mA cm -2 Compared with Example 2, the sensitivity of these electrodes is lower, demonstrating that the optimal hydrothermal time is about 6 h.
[0062] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water, the steps of which are as follows: (1) Soak the carbon cloth in the pretreatment solution for a certain period of time, take it out, and clean it with ultrasonic cleaning of deionized water; (2) dissolving a copper source, a nickel source and urea in deionized water and stirring to obtain a hydrothermal deposition solution; (3) adding the carbon cloth treated in step (1) and the hydrothermal deposition liquid obtained in step (2) into a hydrothermal kettle for hydrothermal reaction, taking out the carbon cloth after the hydrothermal reaction, washing and drying it to obtain the nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water.
2. The method for preparing a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water according to claim 1, characterized in that: In step (1), the pretreatment solution is prepared by mixing concentrated nitric acid with a mass fraction of 65% to 68% and concentrated sulfuric acid with a mass fraction of 95% to 98% in a volume ratio of 2 to 3:1, and the carbon cloth is immersed in the pretreatment solution for 60 to 72 hours.
3. The method for preparing a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water according to claim 1, characterized in that: In step (2), the copper source is copper nitrate, and the nickel source is nickel nitrate; the sum of the concentrations of metal ions nickel and copper in deionized water is 30-100 mmol / L, nickel accounts for 10%-90% of the total molar number of nickel and copper, and the molar ratio of urea to the sum of metal ions nickel and copper is 1.5-2.5:
1.
4. The method for preparing a nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water according to claim 1, characterized in that: In step (3), the hydrothermal reaction temperature is 110 to 130° C., and the hydrothermal reaction time is 2 to 8 hours.
5. A nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water, characterized in that: The method is prepared by any one of claims 1 to 4.
6. Use of the nickel-copper hydroxide carbon cloth sensitive electrode for detecting ammonia nitrogen in water as described in claim 5 in electrochemical detection of ammonia nitrogen in water.
Citation Information
Patent Citations
Three-dimension carbon cloth / nickel iron layer shaped hydroxide nanosheet composite material and application thereof
CN108107101A
Sensitive electrode for direct electrochemical detection of ammonia nitrogen in water and preparation method of sensitive electrode
CN110514729A
Sensitive electrode material for direct electrochemical detection of ammonia nitrogen in water and preparation method thereof
CN112362713A
Silver nano dendritic crystal composite electrode, preparation method thereof and ammonia nitrogen detection method
CN112432978A