Sandy soil anti-liquefaction reinforcement method based on plant urease induced calcium carbonate deposition (EICP) technology
Through the plant urease-induced calcium carbonate deposition technology, a constitutive model was established in combination with sand and urease and cementitious liquid, a sand liquefaction problem was solved, efficient, environmentally friendly and economical sand solidification was achieved, and the operation process was simplified and costs were reduced. Provides effective technical support for soil reinforcement.
Patent Information
- Application Number
- CN202411032188.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing sand and soil are prone to liquefaction under the action of earthquake loads, resulting in sand blasting, water gushing and sinking of surface buildings. The traditional reinforcement methods have problems such as high pollution and large workload, and it is impossible to effectively analyze the stress and strain curve of the sand and soil.
Using plant urease-induced calcium carbonate deposition (EICP) technology, standard sand soil is combined with urease and cementitious liquid in a certain proportion, and through compaction layering and stand-alone treatment, a constitutive model is established to improve the liquefaction resistance of sand soil. Use Sigmoid function to fit the best fit result.
It has achieved efficient, environmentally friendly and economical solidification of sand and soil, significantly improved liquefaction resistance, simplified operating procedures, reduced costs, and provided theoretical support and practical guidance, providing effective solutions for the field of soil reinforcement.
Smart Images

Figure CN118962066A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of civil engineering and construction, and in particular relates to a sand anti-liquefaction reinforcement method based on plant urease-induced calcium carbonate deposition (EICP) technology. Background Art
[0002] Under the action of seismic load, the pore water pressure of saturated sand will increase rapidly, resulting in a significant decrease in the shear strength of the soil, which will cause liquefaction phenomena such as sandblasting, water gushing and sinking of surface buildings, causing serious harm to the surrounding environment and infrastructure. The more mature liquefied foundation treatment methods currently include dynamic compaction, soil replacement, and gravel piles, but they have limitations such as high pollution and large workload. Against this background, EICP foundation reinforcement technology came into being. Its basic principle is to use urease as a catalyst. Under suitable environmental conditions, urease catalyzes the hydrolysis of urea, and the reaction products react with the cementing fluid to form calcium carbonate precipitation. By filling the gaps between sand particles, the compactness and compressive strength are increased, thereby improving the anti-liquefaction performance of sand. EICP technology for strengthening foundations has the advantages of sustainability, environmental protection, and low cost. At present, research on the dynamic characteristics of EICP solidified sand is still in its infancy. Therefore, it is necessary for us to systematically carry out research on the dynamic and liquefaction characteristics of EICP solidified sand.
[0003] The patent application document with publication number CN 115032365 A discloses a soil reinforcement research method and application based on improved EICP technology. By extracting urease and formulating the optimal mineralization solution, porosity experiments and mechanical property experiments are carried out on the sample sand column to obtain the optimal reinforcement plan of the sand column. However, due to the limitations of the mechanical properties of sand, it is impossible to analyze the stress-strain curve of the mechanical properties of the reinforced sand. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a sand anti-liquefaction reinforcement method based on plant urease induced calcium carbonate deposition (EICP) technology. By combining sand with urease and binder in a certain proportion, a constitutive model is established to achieve the improvement and application of sand solidification. The present invention can enhance the anti-liquefaction ability of solidified sand, effectively solve the liquefaction problems such as water spraying, sand bubbling and subsidence, and has the technical effects of high efficiency, environmental protection, significant economic benefits and good durability.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] A method for strengthening sandy soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology comprises the following steps:
[0007] Step 1: Select standard sand with a particle size of 0.072-4.8 mm, and bake the standard sand for 24-28 hours at a temperature of 90-110°C;
[0008] Step 2: According to the dry density of 1.46-1.54g / cm 3 Weigh a certain mass of the standard sand sample prepared in step 1;
[0009] Step 3, prepare urease solution and cementing solution, and pour the urease solution and cementing solution into the standard sand sample prepared in step 2 in sequence, according to the mass ratio, urease solution: cementing solution = 1:1 or 1:2 or 2:1 or 3:2 or 2:3;
[0010] Step 4, compacting and stratifying the sand obtained in step 2, the number of layers is 4-5, injecting the urease solution obtained in step 3, and then standing for 30-50 minutes; then injecting the cementing solution obtained in step 3, and standing for 24-32 hours after completion, to obtain a standard sand sample; according to the mass ratio, sand: urease solution: cementing solution = 143.26:1:1 or 145.22:1:2 or 147.19:2:1 or 149.15:2:3 or 151.11:3:2;
[0011] Step 5: Test the standard sand sample obtained in step 4, establish a constitutive model, and use the Sigmoid function to fit it to obtain the best fitting result.
[0012] The preparation method of the urease solution in step 3 is:
[0013] Step 3.1, select soybeans with a size of 0.5cm-0.9cm;
[0014] Step 3.2, crushing the soybeans selected in step 3.1, and screening the soybean powder with 100-140 mesh;
[0015] Step 3.3, mixing the soybean powder screened in step 3.2 with deionized water, according to the mass ratio, soybean powder: deionized water = 1:1 or 1:2 or 2:1 or 2:3 or 3:2, stirring with a magnetic stirrer for 1-1.8 hours, and standing at a low temperature environment of 4°C-12°C for 24-28 hours to obtain a mixture supernatant;
[0016] Step 3.4, pouring the supernatant of the mixture obtained in step 3.3 into a centrifuge tube, and centrifuging at a speed of 3000 r / min-4000 r / min and a temperature of 4° C.-12° C. for 15-23 minutes to obtain a urease solution;
[0017] The preparation method of the cementing liquid is:
[0018] Anhydrous calcium chloride solution and urea solution are mixed to obtain a cementing solution; calculated by mass ratio, anhydrous calcium chloride solution: urea solution = 1:1 or 1:2 or 2:1 or 2:3 or 3:2.
[0019] The specific method of step 5 is:
[0020] Step 5.1, based on the standard sand sample obtained in step 4, establish a constitutive model, and preliminarily fit the constitutive model using the following Sigmoid function:
[0021] Where: d ——axial dynamic stress; L——maximum stress value; k——slope factor; ε0——inflection point position; ε d ——axial dynamic strain;
[0022] Step 5.2, fit the constitutive model according to the Sigmoid function of step 5.1, adjust the values of parameters L, k and ε0 to approximate the shape of the model, and control the curvature and fitting degree of the constitutive model to obtain the Sigmoid function that meets all working conditions:
[0023] Where: d ——dynamic load (in kPa); σ3——confining pressure (in kPa); CSR——cyclic stress ratio; ρ d ——Dry density of sand; P c ——EICP bonding number; f——vibration frequency; k1, k2, k3, k4——fitting coefficients.
[0024] Compared with the prior art, the advantages of the present invention are:
[0025] (1) The traditional sand solidification uses lime, cement and other materials which are expensive, and the solidified soil has poor strength, is prone to cracking, temperature shrinkage, cracking, softening and poor anti-seepage ability. Compared with the traditional sand solidification method, the soybean, anhydrous calcium chloride and urea selected in the present invention are widely available, easy to obtain, low in cost, more durable in solidification effect, and not easily affected by environmental factors. The present invention does not require large-scale equipment and complex process flow. It only needs to mix soybean, anhydrous calcium chloride and urea green materials in a certain proportion and evenly spread them on the surface of the sand to be reinforced, and then through simple irrigation or rainwater leaching, the sand can be quickly solidified. The selected solidification material is green and environmentally friendly, and embodies significant green environmental protection characteristics. The material does not contain any harmful chemicals, has excellent degradation performance, effectively prevents the risk of soil and groundwater pollution, and significantly reduces the generation of toxic compounds in the ecosystem, which has positive significance for protecting the environment and maintaining ecological balance; the method of reinforcing sand based on plant urease induction of the present invention has the effects of high efficiency, environmental protection, significant economic benefits and good durability.
[0026] (2) Compared with the application of traditional solidification methods, the application prospect of the plant urease-induced calcium carbonate deposition (EICP) technology adopted in the present invention is increasingly broad, involving the fields of geotechnical engineering, structure and water conservancy. In geotechnical engineering, methods such as cast-in-place piles and compaction piles are commonly used to solidify sand; in structural engineering, methods such as water solidification, formwork solidification and wet covering are commonly used to solidify concrete; in water conservancy engineering, reinforcement methods such as polymer solidification, cement solidification and lime solidification are commonly used to solidify dams; the present invention uses plant urease-induced calcium carbonate deposition (EICP) technology to generate calcium carbonate, which can be used for geotechnical engineering sand solidification to improve the shear strength of sand; it can be used to repair cracks in concrete in structural engineering to fill the cracks and solidify them, thereby enhancing the strength and stability of concrete; it can be used to solidify dams in water conservancy engineering to effectively prevent water infiltration and erosion, and improve the durability and safety of the dam.
[0027] (3) Compared with MICP solidification sandy soil technology, the plant urease-induced calcium carbonate deposition (EICP) technology of the present invention has a simpler and more cost-effective operation process. Soybean is used as the main source of plant urease, which is widely planted and relatively cheap, making the entire reinforcement process more economical and efficient. Through comparative experiments, it was found that the sandy soil reinforced by plant urease was superior to the sandy soil reinforced by MICP in terms of density and strength, and the EICP technology does not require the cultivation of microorganisms, thus avoiding the influence of complex environment on the solidification of sandy soil. In addition, plant urease is also environmentally friendly, will not pollute the soil, and meets the requirements of sustainable development. In practical applications, the plant urease-induced sandy soil reinforcement method of the present invention has achieved remarkable results.
[0028] (4) Compared with the traditional consolidation test, the plant urease-induced calcium carbonate deposition (EICP) technology of the present invention analyzes the dynamic characteristics of sand during consolidation and accurately describes the solidification mode of sand under various factors. By simulating the constitutive model, the reinforcement effect of the EICP technology is predicted and verified, and the effectiveness of the EICP technology in sand reinforcement is verified. This provides strong theoretical support and practical guidance for the application of the EICP technology in the field of soil reinforcement in the future.
[0029] In summary, the technology of strengthening sandy soil by plant urease-induced calcium carbonate deposition (EICP) has significant advantages and broad application prospects. It is not only efficient, environmentally friendly and economical, but also easy to operate and low-cost. At the same time, this technology has also been fully supported by theory and verified in practice, providing strong technical support and solutions for the future field of soil reinforcement. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a flow chart of the preparation of standard sand soil samples of the present invention.
[0031] Figure 2 is the constitutive model diagram under confining pressure of the present invention, wherein, Figure 2 (a) is the stress-strain diagram at 25 kPa under the present invention, Figure 2 (b) is the 25 kPa effective stress diagram of the present invention, Figure 2 (c) is the 50 kPa stress-strain diagram of the present invention, Figure 2 (d) is the 50 kPa effective stress diagram of the present invention, Figure 2 (e) is the stress-strain diagram of the present invention at 100 kPa, Figure 2 (f) is the 100 kPa effective stress diagram of the present invention.
[0032] Figure 3 is the constitutive model diagram under the cementation number of the present invention, where: Figure 3 (a) is the present invention P c = Secondary stress-strain diagram, Figure 3 (b) is the present invention P c =2nd effective stress diagram, Figure 3 (c) is the present invention P c = 4th order stress-strain diagram, Figure 3 (d) is the present invention P c = 4th effective stress diagram, Figure 3 (e) is the present invention P c =6th stress-strain diagram, Figure 3 (f) is the present invention P c =6th effective stress diagram.
[0033] Figure 4 is the constitutive model diagram under the cyclic stress ratio of the present invention, wherein, Figure 4 (a) is the stress-strain diagram of CSR=0.25 of the present invention, Figure 4 (b) is the effective stress diagram of CSR=0.25 of the present invention, Figure 4 (c) is the stress-strain diagram of CSR=0.30 of the present invention, Figure 4 (d) is the effective stress diagram of CSR=0.30 of the present invention, Figure 4 (e) is the stress-strain diagram of CSR=0.35 of the present invention, Figure 4 (f) is the effective stress diagram of CSR=0.35 of the present invention.
[0034] Figure 5 is the constitutive model diagram of the present invention under dry density, wherein, Figure 5 (a) is the present invention d =1.6g / cm 3 Stress-strain diagram, Figure 5 (b) is the present invention d =1.6g / cm 3 Effective stress diagram, Figure 5 (c) is the present invention d =1.7g / cm 3 Stress-strain diagram, Figure 5 (d) is the present invention d =1.7g / cm 3 Effective stress diagram.
[0035] Figure 6 is the constitutive model diagram at the frequency of the present invention, where Figure 6 (a) is the stress-strain diagram of the present invention at f = 1 Hz, Figure 6 (b) is the effective stress diagram of the present invention at f = 1 Hz, Figure 6 (c) is the stress-strain diagram of the present invention at f = 3 Hz, Figure 6 (d) is the effective stress diagram of the present invention at f=3 Hz.
[0036] Figure 7 is a simulation diagram of the constitutive model of the present invention, wherein, Figure 7 (a) Constitutive model simulation diagram under 500 vibrations. Figure 7 (b) Constitutive model simulation diagram under 1000 vibration times. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with the embodiments of the present invention.
[0038] The sand anti-liquefaction mechanism of the plant urease induced calcium carbonate deposition (EICP) technology of the present invention is: the urease of the present invention can assist calcium carbonate mineralization, urease and urea in the cementing solution are hydrolyzed to produce ammonium ions, which will be degraded into a second ammonium molecule and carbonic acid as the reaction proceeds, and continue to be hydrolyzed in water to generate carbonate ions, hydrogen ions, ammonium ions and hydroxide ions. The hydroxide ions produced by the reaction are acidic and will cause the pH to increase, and carbonate ions will be generated, wherein the hydroxide ions react with calcium ions under dissolution, and the increase in acidity creates conditions for the reaction between ions to generate calcium carbonate precipitation. The presence of urease can accelerate the urea hydrolysis reaction, so that the concentrations of ammonia ions and carbonate ions in the solution increase rapidly, thereby accelerating the consolidation of the soil body. This consolidation method does not produce harmful gases, and the strength of the solidified soil body is high, and it has the effects of high efficiency, environmental protection, significant economic benefits, and good durability, thereby improving the anti-liquefaction performance of the sand.
[0039] Example 1
[0040] A method for strengthening sandy soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology comprises the following steps:
[0041] Step 1: Select standard sand with a particle size of 0.072-4.8 mm and bake the standard sand for 24 hours at a temperature of 90°C;
[0042] Step 2: According to the dry density of 1.46g / cm 3 Weigh a certain mass of the standard sand sample prepared in step 1;
[0043] Step 3, prepare urease solution and cementing liquid, and pour the urease solution and cementing liquid into the standard sand sample prepared in step 2 in sequence, according to the mass ratio, urease solution: cementing liquid = 1:1;
[0044] The preparation method of the urease solution is:
[0045] Step 3.1, select soybeans with a size of 0.5 cm;
[0046] Step 3.2, crushing the soybeans selected in step 3.1, and screening the soybean powder with 100 mesh;
[0047] Step 3.3, mixing the soybean powder screened in step 3.2 with deionized water, according to the mass ratio of soybean powder: deionized water = 1:1, stirring with a magnetic stirrer for 1 hour, and standing at 4°C for 24 hours to obtain a mixture supernatant;
[0048] Step 3.4, pouring the supernatant of the mixture obtained in step 3.3 into a centrifuge tube, and centrifuging at a speed of 3000 r / min and a temperature of 4° C. for 15 minutes to obtain a urease solution;
[0049] The preparation method of the cementing liquid is:
[0050] Anhydrous calcium chloride solution and urea solution are mixed to obtain a cementing solution; according to the mass ratio, anhydrous calcium chloride solution: urea solution = 1:1.
[0051] Step 4: compact and layer the sand obtained in step 2 into 4 layers, inject the urease solution obtained in step 3, and then let it stand for 30 minutes; then inject the cementing solution obtained in step 3, and let it stand for 24 hours after completion to obtain a standard sand sample; according to the mass ratio, sand: urease solution: cementing solution = 143.26:1:1;
[0052] Step 5: Test the standard sand sample obtained in step 4, establish a constitutive model, and use the Sigmoid function to fit it to obtain the best fitting result.
[0053] According to the fitting results, the plant urease-induced calcium carbonate deposition (EICP) technology reduced the gaps between sand specimens, increased the viscosity between sand specimens and the shear strength of sand, and achieved the solidification and anti-liquefaction of sand specimens.
[0054] The specific method of step 5 is:
[0055] Step 5.1, based on the standard sand sample obtained in step 4, establish a constitutive model, and preliminarily fit the constitutive model using the following Sigmoid function:
[0056] Where: d ——axial dynamic stress; L——maximum stress value; k——slope factor; ε0——inflection point position; ε d ——axial dynamic strain;
[0057] Step 5.2, fit the constitutive model according to the Sigmoid function of step 5.1, adjust the values of parameters L, k and ε0 to approximate the shape of the model, and control the curvature and fitting degree of the constitutive model to obtain the Sigmoid function that meets all working conditions:
[0058] Where: d ——dynamic load (in kPa); σ3——confining pressure (in kPa); CSR——cyclic stress ratio; ρ d ——Dry density of sand; P c ——EICP bonding number; f——vibration frequency; k1, k2, k3, k4——fitting coefficients.
[0059] Example 2
[0060] A method for strengthening sandy soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology comprises the following steps:
[0061] Step 1: Select standard sand with a particle size of 0.072-4.8 mm, and bake the standard sand for 25 hours at a temperature of 95°C;
[0062] Step 2: According to the dry density of 1.48g / cm 3 Weigh a certain mass of the standard sand sample prepared in step 1;
[0063] Step 3, prepare urease solution and cementing liquid, and pour the urease solution and cementing liquid into the standard sand sample prepared in step 2 in sequence, according to the mass ratio, urease solution: cementing liquid = 1:2;
[0064] The preparation method of the urease solution is:
[0065] Step 3.1, select soybeans with a size of 0.6 cm;
[0066] Step 3.2, crushing the soybeans selected in step 3.1, and screening the soybean powder with 110 mesh;
[0067] Step 3.3, mixing the soybean powder screened in step 3.2 with deionized water, according to the mass ratio of soybean powder: deionized water = 1:2, stirring with a magnetic stirrer for 1.2 hours, and standing at a low temperature environment of 6°C for 25 hours to obtain a mixture supernatant;
[0068] Step 3.4, pouring the supernatant of the mixture obtained in step 3.3 into a centrifuge tube, and centrifuging at a speed of 3200 r / min and a temperature of 6° C. for 17 minutes to obtain a urease solution;
[0069] The preparation method of the cementing liquid is:
[0070] Anhydrous calcium chloride solution and urea solution are mixed to obtain a cementing solution; according to the mass ratio, anhydrous calcium chloride solution: urea solution = 1:2.
[0071] Step 4: compact and layer the sand obtained in step 3 into 4 layers, inject the urease solution obtained in step 3, and then let it stand for 35 minutes; then inject the cementing solution obtained in step 3, and let it stand for 26 hours after completion to obtain a standard sand sample; according to the mass ratio, sand: urease solution: cementing solution = 145.22:1:2;
[0072] Step 5: Test the standard sand sample obtained in step 4, establish a constitutive model, and use the Sigmoid function to fit it to obtain the best fitting result.
[0073] According to the fitting results, the plant urease-induced calcium carbonate deposition (EICP) technology reduced the gaps between sand specimens, increased the viscosity between sand specimens and the shear strength of sand, and achieved the solidification and anti-liquefaction of sand specimens.
[0074] The specific method of step 5 is:
[0075] Step 5.1, based on the standard sand sample obtained in step 4, establish a constitutive model, and preliminarily fit the constitutive model using the following Sigmoid function:
[0076] Where: d ——axial dynamic stress; L——maximum stress value; k——slope factor; ε0——inflection point position; ε d ——axial dynamic strain;
[0077] Step 5.2, fit the constitutive model according to the Sigmoid function of step 5.1, adjust the values of parameters L, k and ε0 to approximate the shape of the model, and control the curvature and fitting degree of the constitutive model to obtain the Sigmoid function that meets all working conditions:
[0078] Where: d ——dynamic load (in kPa); σ3——confining pressure (in kPa); CSR——cyclic stress ratio; ρ d ——Dry density of sand; P c ——EICP bonding number; f——vibration frequency; k1, k2, k3, k4——fitting coefficients.
[0079] Example 3
[0080] A method for strengthening sandy soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology comprises the following steps:
[0081] Step 1: Select standard sand with a particle size of 0.072-4.8 mm, and bake the standard sand for 26 hours at a temperature of 100°C;
[0082] Step 2: According to the dry density of 1.50g / cm 3 Weigh a certain mass of the standard sand sample prepared in step 1;
[0083] Step 3, prepare urease solution and cementing liquid, and pour the urease solution and cementing liquid into the standard sand sample prepared in step 2 in sequence, according to the mass ratio, urease solution: cementing liquid = 2:1;
[0084] The preparation method of the urease solution is:
[0085] Step 3.1, select soybeans with a size of 0.7 cm;
[0086] Step 3.2, crushing the soybeans selected in step 3.1, and screening the soybean powder with 120 mesh;
[0087] Step 3.3, mixing the soybean powder screened in step 3.2 with deionized water, according to the mass ratio of soybean powder: deionized water = 2:1, stirring with a magnetic stirrer for 1.4 hours, and standing at a low temperature environment of 8°C for 26 hours to obtain a mixture supernatant;
[0088] Step 3.4, pouring the supernatant of the mixture obtained in step 3.3 into a centrifuge tube, and centrifuging at a speed of 3600 r / min and a temperature of 8° C. for 19 minutes to obtain a urease solution;
[0089] The preparation method of the cementing liquid is:
[0090] Anhydrous calcium chloride solution and urea solution are mixed to obtain a cementing solution; according to the mass ratio, anhydrous calcium chloride solution: urea solution = 2:1.
[0091] Step 4: compact and layer the sand obtained in step 3 into 4 layers, inject the urease solution obtained in step 3, and then let it stand for 40 minutes; then inject the cementing solution obtained in step 3, and let it stand for 28 hours after completion to obtain a standard sand sample; according to the mass ratio, sand: urease solution: cementing solution = 147.19:2:1;
[0092] Step 5: Test the standard sand sample obtained in step 4, establish a constitutive model, and use the Sigmoid function to fit it to obtain the best fitting result.
[0093] According to the fitting results, the plant urease-induced calcium carbonate deposition (EICP) technology reduced the gaps between sand specimens, increased the viscosity between sand specimens and the shear strength of sand, and achieved the solidification and anti-liquefaction of sand specimens.
[0094] The specific method of step 5 is:
[0095] Step 5.1, based on the standard sand sample obtained in step 4, establish a constitutive model, and preliminarily fit the constitutive model using the following Sigmoid function:
[0096] Where: d ——axial dynamic stress; L——maximum stress value; k——slope factor; ε0——inflection point position; ε d ——axial dynamic strain;
[0097] Step 5.2, fit the constitutive model according to the Sigmoid function of step 5.1, adjust the values of parameters L, k and ε0 to approximate the shape of the model, and control the curvature and fitting degree of the constitutive model to obtain the Sigmoid function that meets all working conditions:
[0098] Where: d ——dynamic load (in kPa); σ3——confining pressure (in kPa); CSR——cyclic stress ratio; ρ d ——Dry density of sand; P c ——EICP bonding number; f——vibration frequency; k1, k2, k3, k4——fitting coefficients.
[0099] Example 4
[0100] A method for strengthening sandy soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology comprises the following steps:
[0101] Step 1: Select standard sand with a particle size of 0.072-4.8 mm, and bake the standard sand for 27 hours at a temperature of 105°C;
[0102] Step 2: According to the dry density of 1.52g / cm 3 Weigh a certain mass of the standard sand sample prepared in step 1;
[0103] Step 3, prepare urease solution and cementing liquid, and pour the urease solution and cementing liquid into the standard sand sample prepared in step 2 in sequence, according to the mass ratio, urease solution: cementing liquid = 2:3;
[0104] The preparation method of the urease solution is:
[0105] Step 3.1, select soybeans with a size of 0.8 cm;
[0106] Step 3.2, crushing the soybeans selected in step 3.1, and screening the soybean powder with 130 mesh;
[0107] Step 3.3, mixing the soybean powder screened in step 3.2 with deionized water, according to the mass ratio of soybean powder: deionized water = 2:3, stirring with a magnetic stirrer for 1.6 hours, and standing at a low temperature environment of 10°C for 27 hours to obtain a mixture supernatant;
[0108] Step 3.4, pouring the supernatant of the mixture obtained in step 3.3 into a centrifuge tube, and centrifuging at a speed of 3800 r / min and a temperature of 10° C. for 21 minutes to obtain a urease solution;
[0109] The preparation method of the cementing liquid is:
[0110] Anhydrous calcium chloride solution and urea solution are mixed to obtain a cementing solution; according to the mass ratio, anhydrous calcium chloride solution: urea solution = 2:3.
[0111] Step 4: compact and layer the sand obtained in step 3 into 5 layers, inject the urease solution obtained in step 3, and then let it stand for 45 minutes; then inject the cementing solution obtained in step 3, and let it stand for 30 hours after completion to obtain a standard sand sample; according to the mass ratio, sand: urease solution: cementing solution = 149.15:2:3;
[0112] Step 5: Test the standard sand sample obtained in step 4, establish a constitutive model, and use the Sigmoid function to fit it to obtain the best fitting result.
[0113] According to the fitting results, the plant urease-induced calcium carbonate deposition (EICP) technology reduced the gaps between sand specimens, increased the viscosity between sand specimens and the shear strength of sand, and achieved the solidification and anti-liquefaction of sand specimens.
[0114] The specific method of step 5 is:
[0115] Step 5.1, based on the standard sand sample obtained in step 4, establish a constitutive model, and preliminarily fit the constitutive model using the following Sigmoid function:
[0116] Where: d ——axial dynamic stress; L——maximum stress value; k——slope factor; ε0——inflection point position; ε d ——axial dynamic strain;
[0117] Step 5.2, fit the constitutive model according to the Sigmoid function of step 5.1, adjust the values of parameters L, k and ε0 to approximate the shape of the model, and control the curvature and fitting degree of the constitutive model to obtain the Sigmoid function that meets all working conditions:
[0118] Where: d ——dynamic load (in kPa); σ3——confining pressure (in kPa); CSR——cyclic stress ratio; ρ d ——Dry density of sand; P c ——EICP bonding number; f——vibration frequency; k1, k2, k3, k4——fitting coefficients.
[0119] Example 5
[0120] A method for strengthening sandy soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology comprises the following steps:
[0121] Step 1: Select standard sand with a particle size of 0.072-4.8 mm, and bake the standard sand for 28 hours at a temperature of 110°C;
[0122] Step 2: According to the dry density of 1.54g / cm 3 Weigh a certain mass of the standard sand sample prepared in step 1;
[0123] Step 3, prepare urease solution and cementing liquid, and pour the urease solution and cementing liquid into the standard sand sample prepared in step 2 in sequence, according to the mass ratio, urease solution: cementing liquid = 3:2;
[0124] The preparation method of the urease solution is:
[0125] Step 3.1, select soybeans with a size of 0.9 cm;
[0126] Step 3.2, crushing the soybeans selected in step 3.1, and screening the soybean powder with 140 mesh;
[0127] Step 3.3, mixing the soybean powder screened in step 3.2 with deionized water, according to the mass ratio of soybean powder: deionized water = 3:2, stirring with a magnetic stirrer for 1.8 hours, and standing at a low temperature environment of 12°C for 28 hours to obtain a mixture supernatant;
[0128] Step 3.4, pouring the supernatant of the mixture obtained in step 3.3 into a centrifuge tube, and centrifuging at a speed of 4000 r / min and a temperature of 12° C. for 23 minutes to obtain a urease solution;
[0129] The preparation method of the cementing liquid is:
[0130] Anhydrous calcium chloride solution and urea solution are mixed to obtain a cementing solution; according to the mass ratio, anhydrous calcium chloride solution: urea solution = 3:2.
[0131] Step 4: compact and layer the sand obtained in step 3 into 5 layers, inject the urease solution obtained in step 3, and then let it stand for 50 minutes; then inject the cementing solution obtained in step 3, and let it stand for 32 hours after completion to obtain a standard sand sample; according to the mass ratio, sand: urease solution: cementing solution = 151.11:3:2;
[0132] Step 5: Test the standard sand sample obtained in step 4, establish a constitutive model, and use the Sigmoid function to fit it to obtain the best fitting result.
[0133] According to the fitting results, the plant urease-induced calcium carbonate deposition (EICP) technology reduced the gaps between sand specimens, increased the viscosity between sand specimens and the shear strength of sand, and achieved the solidification and anti-liquefaction of sand specimens.
[0134] The specific method of step 5 is:
[0135] Step 5.1, based on the standard sand sample obtained in step 4, establish a constitutive model, and preliminarily fit the constitutive model using the following Sigmoid function:
[0136] Where: d ——axial dynamic stress; L——maximum stress value; k——slope factor; ε0——inflection point position; ε d ——axial dynamic strain;
[0137] Step 5.2, fit the constitutive model according to the Sigmoid function of step 5.1, adjust the values of parameters L, k and ε0 to approximate the shape of the model, and control the curvature and fitting degree of the constitutive model to obtain the Sigmoid function that meets all working conditions:
[0138] Where: d ——dynamic load (in kPa); σ3——confining pressure (in kPa); CSR——cyclic stress ratio; ρ d ——Dry density of sand; P c ——EICP bonding number; f——vibration frequency; k1, k2, k3, k4——fitting coefficients.
[0139] Test verification
[0140] An orthogonal experimental scheme was designed for key influencing factors of EICP-solidified sand.
[0141] The orthogonal test scheme of key influencing factors of EICP solidified sand formulated by the present invention is as follows: by considering different soybean urease concentrations (20 g·L -1 , 40g·L -1 、60g·L -1 、80g·L -1 、100g·L -1 ), cementing fluid concentration (0.8Mol·L -1 , 1.0Mol·L -1 , 1.2Mol·L -1 , 1.4Mol·L -1 、1.6Mol·L -1), pH value (6, 7, 8, 9, 10) and static curing time (1h, 2h, 3h, 4h, 5h) were used to analyze the effects of urease activity and calcium carbonate production in the EICP reaction. A test tube orthogonal experiment was used, and a total of 25 groups of experiments were carried out. The experimental scheme is shown in Table 1.
[0142] Table 1 Orthogonal test scheme for key factors affecting EICP curing
[0143]
[0144]
[0145] Preferably, the effects of the above five factors on urease activity and calcium carbonate production in the EICP reaction are analyzed, and an orthogonal test of key influencing factors of EICP solidification of standard sand is carried out: According to the test scheme requirements in Table 1, the urease and binder prepared in step 3 are used to carry out an orthogonal test. According to the results of the chart analysis, the degree of influence of each factor on urease activity and calcium carbonate production is arranged in the following order: urease concentration> binder concentration> pH value> incubation time. That is, the effects of urease concentration and binder concentration on urease activity and calcium carbonate production are significant, while the effects of pH value and incubation time are relatively slight. In summary, based on the results of the orthogonal test, the present invention ultimately determines the priority order of each factor on urease activity and calcium carbonate production and the recommended level of each factor, specifically urease concentration 100g·L -1 , cementing fluid concentration 1.4 mol·L -1 , pH value is 8, and the culture time is 5 days.
[0146] Design a constitutive model test for EICP-stabilized sand.
[0147] Table 2 Constitutive model test scheme
[0148]
[0149]
[0150] Analysis of the dynamic characteristics of EICP-solidified standard sand: According to the requirements of the test scheme in Table 2, the constitutive model was developed. According to the geotechnical test method standard (GB / T50123-2019), the test adopted a stress-controlled loading method, axially applied a sinusoidal oscillating load, set the cycle to 10,000 times, recorded 20 data points in each cycle, and stopped the test when the pore pressure reached the confining pressure. A total of 108 groups of tests were carried out in the embodiment of the present invention. During the test, 3 repeated tests were set for each group of samples, and the average of the parallel samples was taken as the data result, so as to determine the accuracy and reliability of the constitutive model data.
[0151] Design the constitutive model of EICP-solidified sand.
[0152] Table 3 Fitting values of empirical parameters of constitutive model
[0153]
[0154]
[0155] Based on the constitutive model, we can try to use the Sigmoid function in step 5 to fit the stress-strain curve: Sigmoid function: Where: d ——axial dynamic stress; L——maximum stress value; k——slope factor; ε0——inflection point position; ε d ——Axial dynamic strain. After using the preliminary Sigmoid function, by adjusting the values of parameters L, k and ε0, the Sigmoid function that meets all working conditions is obtained: Where: d ——dynamic load (in kPa); σ3——confining pressure (in kPa); CSR——cyclic stress ratio; ρ d ——Dry density of sand; P c ——EICP bonding times; f——vibration frequency; k1, k2, k3, k4——fitting coefficients. The hysteresis curve parameters L, k and ε0 and R corresponding to each sample group under different confining pressure, bonding times, dry density and vibration frequency are calculated by the least squares method. 2 Through this calculation, our goal is to minimize the sum of squares of the difference between the fitting value and the measured value, so as to obtain the best fitting result to meet the hysteresis curve fitting requirements under all working conditions. The data obtained are shown in Table 3. Finally, the hysteresis curve model for EICP solidified standard sand is obtained:
[0156]
[0157] Where:
[0158] σ d ——dynamic load (in kPa);
[0159] σ3——confining pressure (in kPa);
[0160] CSR – Cyclic Stress Ratio;
[0161] ρ d ——Dry density of sand;
[0162] P c ——EICP bonding times;
[0163] f——vibration frequency.
[0164] Figure 1It is a flow chart of the preparation of standard sand soil samples of the present invention.
[0165] Figure 2 is the constitutive model diagram under confining pressure of the present invention, wherein, Figure 2 (a) is the stress-strain diagram at 25 kPa under the present invention, Figure 2 (b) is the 25 kPa effective stress diagram of the present invention, Figure 2 (c) is the 50 kPa stress-strain diagram of the present invention, Figure 2 (d) is the 50 kPa effective stress diagram of the present invention, Figure 2 (e) is the stress-strain diagram of the present invention at 100 kPa, Figure 2 (f) is the 100 kPa effective stress diagram of the present invention. It can be seen from the figure that under the same test conditions, as the confining pressure increases, the liquefaction resistance decreases, the effective stress path moves faster to the left, the axial strain growth rate increases, and the hysteresis curve area increases. The main reason for the above phenomenon is that increasing the confining pressure will lead to an increase in the dynamic stress in the soil, thereby strengthening the friction and bonding between the particles in the soil, and then improving the shear strength of the soil.
[0166] Figure 3 is the constitutive model diagram under the cementation number of the present invention, where: Figure 3 (a) is the present invention P c = Secondary stress-strain diagram, Figure 3 (b) is the present invention P c =2nd effective stress diagram, Figure 3 (c) is the present invention P c = 4th order stress-strain diagram, Figure 3 (d) is the present invention P c = 4th effective stress diagram, Figure 3 (e) is the present invention P c =6th stress-strain diagram, Figure 3 (f) is the present invention P c =6 times effective stress diagram. It can be seen from the figure that under the same test conditions, with the increase of cementation times, the liquefaction resistance increases, the rate of effective stress path moving to the left decreases, the rate of axial strain growth slows down, and the area of hysteresis curve decreases. The main reason for the above phenomenon is that during the cementation process, more bonding and friction forces will be formed between the particles in the soil, which strengthens the interaction between the particles, and these bonding and friction forces are very critical to the contribution of shear strength.
[0167] Figure 4 is the constitutive model diagram under the cyclic stress ratio of the present invention, wherein, Figure 4 (a) is the stress-strain diagram of CSR=0.25 of the present invention, Figure 4 (b) is the effective stress diagram of CSR=0.25 of the present invention, Figure 4(c) is the stress-strain diagram of CSR=0.30 of the present invention, Figure 4 (d) is the effective stress diagram of CSR=0.30 of the present invention, Figure 4 (e) is the stress-strain diagram of CSR=0.35 of the present invention, Figure 4 (f) is the effective stress diagram of CSR=0.35 of the present invention. It can be seen from the figure that under the same test conditions, as the cyclic stress ratio increases, the liquefaction resistance decreases, the effective stress path moves faster to the left, the axial strain growth rate increases, and the hysteresis curve area increases. The main reason for the above phenomenon is that the increase in the cyclic stress ratio causes the dynamic stress in the soil to increase, which in turn causes the particle rearrangement phenomenon, thereby reducing the particle contact points and causing the shear strength to decrease; at the same time, the interaction potential between the particles will lead to the crushing and wear of the particles, thereby weakening the bonding force and friction between the particles.
[0168] Figure 5 is the constitutive model diagram of the present invention under dry density, wherein, Figure 5 (a) is the present invention d =1.6g / cm 3 Stress-strain diagram, Figure 5 (b) is the present invention d =1.6g / cm 3 Effective stress diagram, Figure 5 (c) is the present invention d =1.7g / cm 3 Stress-strain diagram, Figure 5 (d) is the present invention d =1.7g / cm 3 Effective stress diagram. As can be seen from the figure, under the same test conditions, with the increase of dry density, the liquefaction resistance increases, the effective stress path moves to the left at a slower rate, the axial strain growth rate decreases, and the hysteresis curve area decreases. The main reason for the above phenomenon is that with the increase of dry density, the particles inside the soil are arranged more closely and the pores and voids are reduced. Such changes will significantly improve the shear strength of the soil;
[0169] Figure 6 is the constitutive model diagram at the frequency of the present invention, where Figure 6 (a) is the stress-strain diagram of the present invention at f = 1 Hz, Figure 6 (b) is the effective stress diagram of the present invention at f = 1 Hz, Figure 6 (c) is the stress-strain diagram of the present invention at f = 3 Hz, Figure 6(d) is the effective stress diagram of the present invention at f = 3Hz. It can be seen from the figure that under the same test conditions, as the frequency increases, the liquefaction resistance increases, the rate of effective stress path moving to the left decreases, the rate of axial strain growth slows down, and the area of the hysteresis curve decreases. The main reason for the above phenomenon is that the increase in frequency will cause the soil to be subjected to more frequent and rapid loading and unloading processes, limiting the rearrangement of particles in the soil and the interaction between particles. Therefore, the increase in frequency is conducive to improving the shear strength of the soil and enhancing the liquefaction resistance.
[0170] Figure 7 is a simulation diagram of the constitutive model of the present invention, wherein, Figure 7 (a) Constitutive model simulation diagram under 500 vibrations. Figure 7 (b) Constitutive model simulation diagram under 1000 vibrations. It can be seen from the figure that by adopting the hysteresis curve model proposed in this paper, the fitting curve obtained shows a good fit with the hysteresis curve obtained in the experiment. Based on this fact, it can be concluded that the hysteresis curve model proposed in this paper can accurately simulate the development law of the hysteresis curve of EICP-solidified standard sand under different conditions. In other words, the model has good utility and adaptability in describing the evolution of the hysteresis curve of EICP-solidified standard sand.
[0171] The present invention provides a method for strengthening sand soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology, which aims to solve the key problem faced when implementing EICP using the in-situ perfusion method in the current technology, namely, it is difficult to accurately evaluate the impact of external factors on the EICP reinforcement effect, and then it is difficult to accurately judge the specific impact of external factors on the EICP reinforcement effect. Through the implementation of the present invention, it is expected to provide a more scientific, accurate and effective technical method for the field of sand soil against liquefaction reinforcement.
Claims
1. A method for strengthening sandy soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology, characterized in that: The following steps are involved: Step 1: Select standard sand with a particle size of 0.072-4.8 mm, and bake the standard sand for 24-28 hours at a temperature of 90-110°C; Step 2: According to the dry density of 1.46-1.54g / cm 3 Weigh a certain mass of the standard sand sample prepared in step 1; Step 3, prepare urease solution and cementing solution, and pour the urease solution and cementing solution into the standard sand sample prepared in step 2 in sequence, according to the mass ratio, urease solution: cementing solution = 1:1 or 1:2 or 2:1 or 3:2 or 2:3; Step 4, compacting and stratifying the sand obtained in step 2, the number of layers is 4-5, injecting the urease solution obtained in step 3, and then standing for 30-50 minutes; then injecting the cementing solution obtained in step 3, and standing for 24-32 hours after completion, to obtain a standard sand sample; according to the mass ratio, sand: urease solution: cementing solution = 143.26:1:1 or 145.22:1:2 or 147.19:2:1 or 149.15:2:3 or 151.11:3:2; Step 5: Test the standard sand sample obtained in step 4, establish a constitutive model, and use the Sigmoid function to fit it to obtain the best fitting result.
2. The method for strengthening sandy soil against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology according to claim 1, characterized in that: The preparation method of the urease solution in step 3 is: Step 3.1, select soybeans with a size of 0.5cm-0.9cm; Step 3.2, crushing the soybeans selected in step 3.1, and screening the soybean powder with 100-140 mesh; Step 3.3, mixing the soybean powder screened in step 3.2 with deionized water, according to the mass ratio, soybean powder: deionized water = 1:1 or 1:2 or 2:1 or 2:3 or 3:2, stirring with a magnetic stirrer for 1-1.8 hours, and standing at a low temperature environment of 4°C-12°C for 24-28 hours to obtain a mixture supernatant; Step 3.4, pouring the supernatant of the mixture obtained in step 3.3 into a centrifuge tube, and centrifuging at a speed of 3000 r / min-4000 r / min and a temperature of 4° C.-12° C. for 15-23 minutes to obtain a urease solution; The preparation method of the cementing liquid is: Anhydrous calcium chloride solution and urea solution are mixed to obtain a cementing solution; calculated by mass ratio, anhydrous calcium chloride solution: urea solution = 1:1 or 1:2 or 2:1 or 2:3 or 3:
2.
3. The method for strengthening sand against liquefaction based on plant urease-induced calcium carbonate deposition (EICP) technology according to claim 1, characterized in that: The specific method of step 5 is: Step 5.1, based on the standard sand sample obtained in step 4, establish a constitutive model, and preliminarily fit the constitutive model using the following Sigmoid function: Where: d ——axial dynamic stress; L——maximum stress value; k——slope factor; ε0——inflection point position; ε d ——axial dynamic strain; Step 5.2, fit the constitutive model according to the Sigmoid function of step 5.1, adjust the values of parameters L, k and ε0 to approximate the shape of the model, and control the curvature and fitting degree of the constitutive model to obtain the Sigmoid function that meets all working conditions: Where: d ——dynamic load (in kPa); σ3——confining pressure (in kPa); CSR——cyclic stress ratio; ρ d ——sand dry density; P c ——EICP bonding number; f——vibration frequency; k1, k2, k3, k4——fitting coefficients.
Citation Information
Cited By
Design method for soil solidification by inducing calcium carbonate precipitation through urease
CN122548851A