PP diffusion plate and manufacturing method thereof

By designing composite light diffuser and quantum dot layer in PP diffuser plates, combining the use of microspheres and nucleating agents, the problem of insufficient haze and transparency of the existing diffuser plates is solved, and a high-color gamut LED backlight display screen is realized Color performance improves.

CN118962876APending Publication Date: 2024-11-15CHANGZHOU AOZHI POLYMER GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411347574.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing diffusion plates lack haze and transparency, making it difficult to meet the color performance needs of high-color gamut LED backlit displays.

Method used

Using a PP diffusion plate including two upper and lower diffusion layers and an intermediate quantum dot layer, the diffusion layer consists of composite light diffusion agent and modified polypropylene. The quantum dot layer contains green light perovskite, which is manufactured by in-mold coextrusion and using Microspheres and nucleating agents improve haze and transparency.

Benefits of technology

It significantly improves the haze and transparency of the diffusion plate, enhances color expression capabilities, and is suitable for high-color gamut LED backlit displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a PP diffusion plate and a manufacturing method thereof, and relates to the technical field of diffusion plate materials. The PP diffusion plate comprises an upper diffusion layer, a lower diffusion layer and a middle quantum dot layer, the upper diffusion layer, the lower diffusion layer and the middle quantum dot layer are manufactured through in-mold three-layer co-extrusion molding, and the diffusion layers comprise composite light diffusant and modified polypropylene; the composite light diffusant comprises acrylic acid microspheres and polymethyl methacrylate microspheres; the acrylic acid microspheres are prepared by polymerizing styrene and methacrylic acid emulsion, and the polymethyl methacrylate microspheres are prepared by dispersing and polymerizing methyl methacrylate, so that the high haze of the diffusion layer is effectively improved; a nucleating agent capable of improving transparency is introduced into the diffusion layer, so that the transparency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a PP diffusion plate and a manufacturing method thereof, belonging to the technical field of chemical analysis. Background Art

[0002] The diffusion plate uses the continuous refraction, reflection and scattering of light between chemical particles and resin. While covering the light source and the dazzling light source, it can make the light source emit uniform, soft and beautiful light, achieving a comfortable effect of light transmission and opacity. Compared with the traditional CCFL backlight source, LED backlight has many advantages such as high color gamut, high brightness, long life, energy saving and environmental protection, and real-time color control. The high color gamut LED backlight makes the screens of electronic products such as TVs, mobile phones, and tablets that use it have more vivid colors and higher color reproduction. In order to make the display color more perfect, richer in color and closer to the color of the real world, R&D personnel have been committed to finding ways to increase the color gamut value of LED backlight display screens.

[0003] The invention patent with announcement number CN114895492A discloses a quantum dot diffusion plate, including a chain dot layer, an upper surface and a lower surface covered with a protective layer, which has a high brightness effect, thereby reducing the overall cost of the backlight module, but the haze and transparency of the diffusion plate still need to be improved. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a PP diffusion plate with high haze and high transparency and a manufacturing method thereof.

[0005] A technical solution proposed by the present invention to solve the above technical problems is: a PP diffuser plate, comprising two diffusion layers, an upper diffusion layer and a quantum dot layer in the middle; the diffusion layer comprises the following components in mass percentage: 6-12% of a composite light diffuser, and the rest is modified polypropylene; the quantum dot layer comprises the following components in mass percentage: 1-3% of a green light perovskite, 2-5% of a composite light diffuser, and the rest is polypropylene; the green perovskite is a green quantum dot with a particle size of 2-3 nm.

[0006] Preferably, the composite light diffuser comprises acrylic microspheres and polymethyl methacrylate microspheres; the mass ratio of the acrylic microspheres to the polymethyl methacrylate microspheres is 1-3:1.

[0007] Preferably, the modified polypropylene is prepared by mixing polypropylene, a nucleating agent and an antioxidant; and the antioxidant is antioxidant 1010.

[0008] Preferably, the thickness of the PP diffuser plate is 1.7-1.9 mm; the thickness of the diffusion layer is 5.5-7.5% of the thickness of the PP diffuser plate.

[0009] Preferably, the manufacturing method of the PP diffuser plate is as follows: the composite light diffuser and modified polypropylene in the diffusion layer, the green light perovskite, the composite light diffuser and polypropylene in the quantum dot layer are prepared according to mass percentage ratio, and a diffusion layer sheet layer, a quantum dot layer sheet layer and a diffusion layer sheet layer are formed by in-mold co-extrusion molding, which are sequentially stacked and composited together, and the extrusion speed is 2.6~3.6m / min to obtain a PP diffuser plate.

[0010] Preferably, the preparation method of the acrylic microspheres is: methacrylic acid, chloroform, ethylene glycol dimethacrylate, azobisisobutyl cyanide and styrene are mixed in a volume ratio of 0.8-0.9:10:2-4:0.1:1-2, and a 30-50% sodium dodecyl sulfate aqueous solution with a mass fraction of 30-50% and a mass fraction of 30-50% of methacrylic acid is added dropwise at a rate of 0.6-0.8 ml / min, and microwave irradiation is performed at 400-600 W for 1.5-2.5 h, and finally washed with methanol and deionized water for 3-5 times, and dried to obtain acrylic microspheres.

[0011] Preferably, the preparation method of the polymethyl methacrylate microspheres is as follows: under a nitrogen atmosphere, polyvinyl pyrrolidone, ethanol and deionized water are mixed in equal masses, methyl methacrylate (1.2 to 1.4 times the mass of polyvinyl pyrrolidone) and azobisisobutyronitrile (0.02 to 0.04 times the mass of polymethyl methacrylate) are added dropwise at a rate of 1 to 3 ml / min, and after microwave irradiation at 600 to 700 W for 1 to 3 min, the power is reduced to 300 to 400 W, and the irradiation is continued for 12 to 16 min, and finally irradiated at 120 to 140 W for 30 to 50 min, and after centrifugation, the mixture is washed with anhydrous ethanol and deionized water in sequence and dried to obtain polymethyl methacrylate microspheres.

[0012] Preferably, the preparation method of the modified polypropylene is: polypropylene, a nucleating agent and an antioxidant are mixed in a mass ratio of 100:1:0.1-0.2, and added into a twin-screw extruder for melt extrusion granulation, the extruder temperature is 220-240° C., and the rotation speed is 40-60 rpm.

[0013] Preferably, the preparation method of the nucleating agent is: glucose, allyl bromide, tin powder and 0.5 mol / L hydrobromic acid are mixed in a mass ratio of 3:2:2:30-50, stirred and reacted at room temperature and 200-400 rpm for 48 hours, neutralized with sodium hydroxide solution to a pH of 6.98-7.02, filtered and rotary evaporated to obtain allyl sorbitol; allyl sorbitol, aldehyde cyclodextrin, p-toluenesulfonic acid, cyclohexane and methanol are mixed in a mass ratio of 3.5-3.7:4:0.25:10:18-20, heated to 62-64°C, reacted until no water is generated, adjusted the pH to 8-9 with sodium hydroxide solution, distilled and washed with boiling water and boiling cyclohexane for 3-5 times, filtered and dried to obtain a nucleating agent.

[0014] Preferably, the preparation method of the aldehyde cyclodextrin is as follows: β-cyclodextrin and deionized water are mixed in a mass ratio of 1:20~30, the temperature is raised to 60~62°C, the temperature is lowered by 18~22°C after stirring and dissolving, 1.1~1.5 times the mass of β-cyclodextrin sodium periodate is added, the reaction is carried out in the dark for 1~2h, ethylene glycol is used to terminate the reaction, calcium chloride is added until no precipitate is generated, the precipitate is filtered and transferred to a dialysis bag with a molecular weight cutoff of 100D for dialysis for 4~6h, the water is changed twice, and finally freeze-dried at -40~-60°C to obtain aldehyde cyclodextrin.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The PP diffusion plate of the present invention comprises two diffusion layers, an upper diffusion layer and a quantum dot layer in the middle, which are manufactured by three-layer co-extrusion molding in a mold, and the diffusion layer comprises a composite light diffuser and modified polypropylene; The composite light diffuser includes acrylic microspheres and polymethyl methacrylate microspheres; acrylic microspheres are prepared by emulsion polymerization of styrene and methacrylic acid, and polymethyl methacrylate microspheres are prepared by dispersion polymerization of methyl methacrylate; when preparing acrylic microspheres and polymethyl methacrylate microspheres, microwave irradiation is performed to obtain acrylic microspheres and polymethyl methacrylate microspheres with different but relatively uniform particle sizes, which are added to modified polypropylene for scattering, thereby effectively improving the haze of the diffusion layer; The different particle sizes of the components of the composite light diffuser will have a certain impact on the transparency of the diffusion layer, so a nucleating agent that can improve the transparency is introduced into the diffusion layer; the nucleating agent is prepared by the reaction of allyl sorbitol and aldehyde cyclodextrin; the aldehyde cyclodextrin with two aldehyde groups is linked to allyl sorbitol to form a nucleating agent with a cross-linked structure with the hydroxyl group on the allyl sorbitol as the cross-linking point, and after being mixed with polypropylene, the nucleating agent and the antioxidant, it crystallizes as a heterogeneous core before the polypropylene melt, reducing the size of the spherulites formed by the crystallization of the polypropylene melt, thereby improving the transparency. DETAILED DESCRIPTION

[0016] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention. Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art.

[0017] The method for preparing the green perovskite (CH3NH3PbBr3 quantum dots) used in the present invention is prepared by referring to the method of Example 3 in application number CN104861958 A.

[0018] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the yellowing-resistant PS diffusion plates prepared in the examples and comparative examples as follows: Haze: The PP diffuser plates manufactured in the examples and comparative examples were tested for haze using NDH-5000.

[0019] Transparency: The PP diffuser plates manufactured in the examples and comparative examples were tested for light transmittance by WGT-S. Example 1

[0020] In this embodiment, the diffusion layer includes the following components in percentage by mass: 6% of the composite light diffuser and the rest of the modified polypropylene; In this embodiment, the quantum dot layer includes the following components in percentage by mass: 1% green light perovskite, 2% composite light diffuser, and the rest is polypropylene; the green perovskite is a green quantum dot with a particle size of 2 nm. The manufacturing method of the PP diffuser plate in this embodiment is as follows: S1. Methacrylic acid, chloroform, ethylene glycol dimethacrylate, azobisisobutyl cyanide and styrene were mixed in a volume ratio of 0.8:10:2:0.1:1, and a 30% sodium dodecyl sulfate aqueous solution with a mass fraction of 30 times the mass of methacrylic acid was added dropwise at a rate of 0.6 ml / min, and the mixture was irradiated with a 400 W microwave for 1.5 h. Finally, the mixture was washed with methanol and deionized water for 3 times, and dried to obtain acrylic microspheres; S2. Under a nitrogen atmosphere, polyvinyl pyrrolidone, ethanol and deionized water were mixed in equal mass, and methyl methacrylate (1.2 times the mass of polyvinyl pyrrolidone) and azobisisobutyronitrile (0.02 times the mass of polymethyl methacrylate) were added dropwise at a rate of 1 ml / min. After irradiation at 600 W for 1 min, the power was reduced to 300 W, and the irradiation was continued for 12 min. Finally, the irradiation was carried out at 120 W for 30 min. After centrifugation, the mixture was washed with anhydrous ethanol and deionized water in turn and dried to obtain polymethyl methacrylate microspheres. S3. The acrylic microspheres and polymethyl methacrylate microspheres were mixed in a mass ratio of 1:1 to prepare a composite light diffuser; S4. β-cyclodextrin and deionized water were mixed in a mass ratio of 1:20, heated to 60°C, stirred to dissolve, and then cooled by 18°C, and sodium periodate (1.1 times the mass of β-cyclodextrin) was added, and the mixture was reacted in the dark for 1 hour, and ethylene glycol was used to terminate the reaction. Calcium chloride was added until no precipitation was generated, and the mixture was filtered and transferred to a dialysis bag with a molecular weight cutoff of 100D for 4 hours, and the water was changed twice, and finally freeze-dried at -40°C to obtain aldehyde cyclodextrin; glucose, allyl bromide, tin powder and 0.5 mol / L hydrobromic acid were mixed in a mass ratio of 3:2:2:30, stirred at room temperature and 200 rpm for 48 hours, and the pH was neutralized to 6.98 with sodium hydroxide solution, and filtered and rotary evaporated to obtain allyl sorbitol; allyl sorbitol, aldehyde cyclodextrin, p-toluenesulfonic acid, cyclohexanesulfonic acid, Alkane and methanol are mixed in a mass ratio of 3.5:4:0.25:10:18, heated to 62°C, reacted until no water is generated, adjusted to pH 8 with sodium hydroxide solution, distilled and washed 3 times with boiling water and boiling cyclohexane, filtered and dried to obtain a nucleating agent; polypropylene, nucleating agent and antioxidant are mixed in a mass ratio of 100:1:0.1, added to a twin-screw extruder for melt extrusion granulation, the extruder temperature is 220°C, the speed is 40rpm S5. Prepare the composite light diffuser and modified polypropylene in the diffusion layer, the green light perovskite, the composite light diffuser and polypropylene in the quantum dot layer according to the mass percentage ratio, and form a diffusion layer sheet layer, a quantum dot layer sheet layer and a diffusion layer sheet layer which are laminated and compounded in sequence through in-mold co-extrusion molding. The extrusion speed is 2.6m / min to obtain a PP diffuser plate. Example 2

[0021] In this embodiment, the diffusion layer includes the following components in percentage by mass: 9% of the composite light diffuser and the rest of the modified polypropylene; In this embodiment, the quantum dot layer includes the following components in percentage by mass: 2% green light perovskite, 4% composite light diffuser, and the rest is polypropylene; the green perovskite is a green quantum dot with a particle size of 2 nm. The manufacturing method of the PP diffuser plate in this embodiment is as follows: S1. Methacrylic acid, chloroform, ethylene glycol dimethacrylate, azobisisobutyl cyanide and styrene were mixed in a volume ratio of 0.85:10:3:0.1:1.5, and a 40% sodium dodecyl sulfate aqueous solution with a mass fraction of 40 times the mass of methacrylic acid was added dropwise at a rate of 0.7 ml / min, and the mixture was irradiated with a 500 W microwave for 2 h. Finally, the mixture was washed with methanol and deionized water for 4 times, and dried to obtain acrylic microspheres; S2. In a nitrogen atmosphere, polyvinyl pyrrolidone, ethanol and deionized water were mixed in equal mass, and methyl methacrylate (1.3 times the mass of polyvinyl pyrrolidone) and azobisisobutyronitrile (0.03 times the mass of polymethyl methacrylate) were added dropwise at a rate of 2 ml / min. After irradiation at 650 W microwave for 2 min, the power was reduced to 350 W, and the irradiation was continued for 14 min, and finally irradiated at 130 W for 40 min. After centrifugation, the mixture was washed with anhydrous ethanol and deionized water in turn and dried to obtain polymethyl methacrylate microspheres; S3. The acrylic microspheres and polymethyl methacrylate microspheres were mixed in a mass ratio of 2:1 to prepare a composite light diffuser; S4. β-cyclodextrin and deionized water were mixed in a mass ratio of 1:25, heated to 61°C, stirred to dissolve, and then cooled by 20°C, and sodium periodate 1.3 times the mass of β-cyclodextrin was added, and the reaction was carried out in the dark for 1.5 hours. The reaction was terminated with ethylene glycol, and calcium chloride was added until no precipitation was generated. The mixture was filtered and transferred to a dialysis bag with a molecular weight cutoff of 100D for 5 hours. The water was changed twice, and finally freeze-dried at -50°C to obtain aldehyde cyclodextrin; glucose, allyl bromide, tin powder and 0.5 mol / L hydrobromic acid were mixed in a mass ratio of 3:2:2:40, stirred at room temperature and 300 rpm for 48 hours, neutralized with sodium hydroxide solution to pH 7.00, filtered and rotary evaporated to obtain allyl sorbitol; allyl sorbitol, aldehyde cyclodextrin, p-toluenesulfonic acid, cyclohexane and methanol in a mass ratio of 3.6:4:0.25:10:19, heated to 63°C, reacted until no water was generated, adjusted the pH to 8.5 with sodium hydroxide solution, distilled and washed 4 times with boiling water and boiling cyclohexane, filtered and dried to obtain a nucleating agent; polypropylene, nucleating agent and antioxidant were mixed in a mass ratio of 100:1:0.15, added to a twin-screw extruder for melt extrusion granulation, the extruder temperature was 230°C and the speed was 50rpm S5. Prepare the composite light diffuser and modified polypropylene in the diffusion layer, the green light perovskite, the composite light diffuser and polypropylene in the quantum dot layer according to the mass percentage ratio, and form a diffusion layer sheet layer, a quantum dot layer sheet layer and a diffusion layer sheet layer which are laminated and compounded together in sequence through in-mold co-extrusion molding. The extrusion speed is 3.1m / min to obtain a PP diffuser plate. Example 3

[0022] In this embodiment, the diffusion layer includes the following components in percentage by mass: 12% of the composite light diffuser and the rest of the modified polypropylene; In this embodiment, the quantum dot layer includes the following components in percentage by mass: 3% green light perovskite, 5% composite light diffuser, and the rest is polypropylene; the green perovskite is a green quantum dot with a particle size of 3 nm. The manufacturing method of the PP diffuser plate in this embodiment is as follows: S1. Methacrylic acid, chloroform, ethylene glycol dimethacrylate, azobisisobutyl cyanide and styrene were mixed in a volume ratio of 0.9:10:4:0.1:2, and a 50% sodium dodecyl sulfate aqueous solution with a mass fraction of 50 times the mass of methacrylic acid was added dropwise at a rate of 0.8 ml / min, and the mixture was irradiated at 600 W microwave for 2.5 h. Finally, the mixture was washed with methanol and deionized water for 5 times, and dried to obtain acrylic microspheres; S2. Under a nitrogen atmosphere, polyvinyl pyrrolidone, ethanol and deionized water were mixed in equal mass, and methyl methacrylate (1.4 times the mass of polyvinyl pyrrolidone) and azobisisobutyronitrile (0.04 times the mass of polymethyl methacrylate) were added dropwise at a rate of 3 ml / min. After irradiation at 700 W for 3 min, the power was reduced to 400 W, and the irradiation was continued for 16 min, and finally irradiated at 140 W for 50 min. After centrifugation, the mixture was washed with anhydrous ethanol and deionized water in turn and dried to obtain polymethyl methacrylate microspheres. S3. The acrylic microspheres and polymethyl methacrylate microspheres were mixed in a mass ratio of 3:1 to prepare a composite light diffuser; S4. β-cyclodextrin and deionized water were mixed in a mass ratio of 1:30, heated to 62°C, stirred to dissolve, and then cooled by 22°C, and sodium periodate (1.5 times the mass of β-cyclodextrin) was added, and the reaction was carried out in the dark for 2 hours. The reaction was terminated with ethylene glycol, and calcium chloride was added until no precipitation was generated. The mixture was filtered and transferred to a dialysis bag with a molecular weight cutoff of 100D for 6 hours. The water was changed twice, and finally freeze-dried at -60°C to obtain aldehyde cyclodextrin; glucose, allyl bromide, tin powder and 0.5 mol / L hydrobromic acid were mixed in a mass ratio of 3:2:2:50, stirred at room temperature and 400 rpm for 48 hours, neutralized with sodium hydroxide solution to pH 7.02, filtered and rotary evaporated to obtain allyl sorbitol; allyl sorbitol, aldehyde cyclodextrin, p-toluenesulfonic acid, cyclohexanesulfonic acid Alkane and methanol are mixed in a mass ratio of 3.7:4:0.25:10:20, heated to 64°C, reacted until no water is generated, adjusted to pH 9 with sodium hydroxide solution, distilled and washed 5 times with boiling water and boiling cyclohexane, filtered and dried to obtain a nucleating agent; polypropylene, nucleating agent and antioxidant are mixed in a mass ratio of 100:1:0.2, added to a twin-screw extruder for melt extrusion granulation, the extruder temperature is 240°C and the speed is 60rpm S5. Prepare the composite light diffuser and modified polypropylene in the diffusion layer, the green light perovskite, the composite light diffuser and polypropylene in the quantum dot layer according to the mass percentage ratio, and form the diffusion layer sheet layer, the quantum dot layer sheet layer and the diffusion layer sheet layer which are laminated and compounded together in sequence through in-mold co-extrusion molding. The extrusion speed is 3.6m / min to obtain a PP diffuser plate.

[0023] Comparative Example 1 The manufacturing method of comparative example 1 is the same as that of example 2. The difference between the PP diffuser plate and example 2 is that the composite light diffuser is only polymethyl methacrylate microspheres.

[0024] Comparative Example 2 The manufacturing method of Comparative Example 2 is the same as that of Example 2. The difference between the PP diffuser plate and Example 2 is that the composite light diffuser is only acrylic microspheres.

[0025] Comparative Example 3 The manufacturing method of Comparative Example 3 is the same as that of Example 2. The difference between the PP diffuser plate and Example 2 is that the nucleating agent is only allyl sorbitol.

[0026] Comparative Example 4 The manufacturing method of comparative example 4 is the same as that of example 2. The difference between the PP diffuser plate and example 2 is that the diffuser layer only includes the composite light diffuser and polypropylene.

[0027] Effect example Table 1 below shows the performance analysis results of the PP diffuser plates prepared using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4:

[0029] By comparing the experimental data of the examples and the comparative examples in Table 1, it can be clearly found that the PP diffuser plates prepared using Examples 1, 2, and 3 have excellent haze and transparency.

[0030] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, it can be found that a composite light diffuser is added to the diffusion layer, and the composite light diffuser includes acrylic microspheres and polymethyl methacrylate microspheres. When preparing the acrylic microspheres and polymethyl methacrylate microspheres, microwave irradiation is carried out to obtain acrylic microspheres and polymethyl methacrylate microspheres with different but relatively uniform particle sizes, which are added to modified polypropylene for scattering, thereby effectively improving the haze of the diffusion layer.

[0031] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 3, Comparative Example 4, it can be found that the different particle sizes of the composite light diffuser components will have a certain impact on the transparency of the diffusion layer. Therefore, a nucleating agent capable of improving the transparency is introduced into the diffusion layer, and the aldehyde cyclodextrin with two aldehyde groups is linked to allyl sorbitol to form a cross-linked structure with the hydroxyl group on allyl sorbitol as the cross-linking point. After being mixed with polypropylene, the nucleating agent and the antioxidant, the nucleating agent acts as a heterogeneous core and crystallizes before the polypropylene melt, thereby reducing the size of the spherulites formed by the crystallization of the polypropylene melt, thereby improving the transparency.

[0032] Obviously, the above embodiments are merely examples for clearly illustrating the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.

Claims

1. A PP diffuser plate, characterized in that: It includes two diffusion layers, an upper diffusion layer and a quantum dot layer in the middle; the diffusion layer includes the following components in mass percentage: 6-12% of a composite light diffuser and the rest is modified polypropylene; the quantum dot layer includes the following components in mass percentage: 1-3% of green light perovskite, 2-5% of a composite light diffuser and the rest is polypropylene; the green perovskite is a green quantum dot with a particle size of 2-3nm.

2. A PP diffuser plate according to claim 1, characterized in that: The composite light diffuser comprises acrylic microspheres and polymethyl methacrylate microspheres; the mass ratio of the acrylic microspheres to the polymethyl methacrylate microspheres is 1-3:

1.

3. A PP diffuser plate according to claim 1, characterized in that: The modified polypropylene is prepared by mixing polypropylene, a nucleating agent and an antioxidant; the antioxidant is antioxidant 1010.

4. A PP diffuser plate according to claim 1, characterized in that: The thickness of the PP diffusion plate is 1.7-1.9 mm; the thickness of the diffusion layer is 5.5-7.5% of the thickness of the PP diffusion plate.

5. A method for manufacturing a PP diffuser plate as claimed in claim 1, characterized in that: The following steps are involved: The composite light diffuser and modified polypropylene in the diffusion layer, the green light perovskite, the composite light diffuser and polypropylene in the quantum dot layer are prepared according to the mass percentage ratio, and the diffusion layer sheet layer, the quantum dot layer sheet layer and the diffusion layer sheet layer which are laminated and compounded together are formed by in-mold co-extrusion molding, and the extrusion speed is 2.6~3.6m / min to obtain a PP diffuser plate.

6. The method for manufacturing a PP diffuser plate according to claim 5, characterized in that: The preparation method of the acrylic microspheres comprises: mixing methacrylic acid, chloroform, ethylene glycol dimethacrylate, azobisisobutyl cyanide and styrene in a volume ratio of 0.8-0.9:10:2-4:0.1:1-2, adding dropwise a sodium dodecyl sulfate aqueous solution having a mass fraction of 30-50% and a mass fraction of 30-50% of the mass of methacrylic acid at a rate of 0.6-0.8 ml / min, irradiating with a microwave at 400-600 W for 1.5-2.5 h, and finally washing with methanol and deionized water for 3-5 times, and drying to obtain the acrylic microspheres.

7. The method for manufacturing a PP diffuser plate according to claim 5, characterized in that: The preparation method of the polymethyl methacrylate microspheres is as follows: in a nitrogen atmosphere, polyvinyl pyrrolidone, ethanol and deionized water are mixed in equal masses, methyl methacrylate in an amount of 1.2 to 1.4 times the mass of polyvinyl pyrrolidone and azobisisobutyronitrile in an amount of 0.02 to 0.04 times the mass of polymethyl methacrylate are added dropwise at a rate of 1 to 3 ml / min, microwave irradiation is performed at 600 to 700 W for 1 to 3 min, the power is reduced to 300 to 400 W, the irradiation is continued for 12 to 16 min, and finally the irradiation is performed at 120 to 140 W for 30 to 50 min, and after centrifugation, the mixture is washed with anhydrous ethanol and deionized water in sequence and dried to obtain the polymethyl methacrylate microspheres.

8. The method for manufacturing a PP diffuser plate according to claim 5, characterized in that: The preparation method of the modified polypropylene is as follows: polypropylene, a nucleating agent and an antioxidant are mixed in a mass ratio of 100:1:0.1-0.2, and added into a twin-screw extruder for melt extrusion granulation, wherein the extruder temperature is 220-240° C. and the rotation speed is 40-60 rpm.

9. The method for manufacturing a PP diffuser plate according to claim 8, characterized in that: The preparation method of the nucleating agent comprises the following steps: mixing glucose, allyl bromide, tin powder and 0.5 mol / L hydrobromic acid in a mass ratio of 3:2:2:30-50, stirring and reacting at room temperature and 200-400 rpm for 48 hours, neutralizing with sodium hydroxide solution to a pH of 6.98-7.02, filtering and rotary evaporating to obtain allyl sorbitol; mixing allyl sorbitol, aldehyde cyclodextrin, p-toluenesulfonic acid, cyclohexane and methanol in a mass ratio of 3.5-3.7:4:0.25:10:18-20, heating to 62-64°C, reacting until no water is generated, adjusting the pH to 8-9 with sodium hydroxide solution, distilling and washing with boiling water and boiling cyclohexane for 3-5 times, filtering and obtaining the nucleating agent.

10. The method for manufacturing a PP diffuser plate according to claim 9, characterized in that: The preparation method of the aldehyde cyclodextrin is as follows: β-cyclodextrin and deionized water are mixed at a mass ratio of 1:20-30, the temperature is raised to 60-62° C., the temperature is lowered by 18-22° C. after stirring and dissolving, sodium periodate is added in an amount of 1.1-1.5 times the mass of β-cyclodextrin, the reaction is carried out in a dark environment for 1-2 hours, ethylene glycol is used to terminate the reaction, calcium chloride is added until no precipitation is generated, the aldehyde cyclodextrin is filtered and transferred to a dialysis bag with a molecular weight cutoff of 100D for dialysis for 4-6 hours, the water is changed twice, and finally, the aldehyde cyclodextrin is freeze-dried at -40--60° C. to obtain the aldehyde cyclodextrin.