Bonding method applied to electronic component with ultra-narrow pitch micro convex points
Through the low-temperature solid-state diffusion bonding and high-temperature fast reflux methods, the problems of tin extrusion and flux residue in ultra-narrow pitch micro-bulge interconnects are solved, and a high-reliability and efficient bonding effect is achieved, suitable for 20 micrometers and below micro bump interconnections.
Patent Information
- Application Number
- CN202411057325.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
In the prior art, when achieving ultra-narrow pitch micro-bulge interconnection, the thermal conductivity of the non-conductive film is insufficient, resulting in high time costs, tin extrusion and solder joint short circuit problems, and flux residue affects reliability, especially at 20 microns and It is difficult to clean and control at the following pitches.
The micro bumps are pre-bonded by low-temperature solid-state diffusion bonding method. By adjusting the bonding pressure, the degree of tin extrusion is controlled, and the solder is fully melted and connected during the rapid reflow of high temperatures is avoided, and the use of flux is improved. The reliability and efficiency of interconnection.
High reliability and high efficiency bonding of ultra-narrow pitch micro-bulge points is achieved, avoiding tin extrusion and solder joint short circuit problems, reducing flux residues, and improving production efficiency and density.
Smart Images

Figure CN118969649A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a bonding method for electronic components applied to ultra-narrow pitch micro-bumps. Background Art
[0002] With the rapid development of microelectronic integration technology, the performance of processors is getting higher and higher, and the interconnection size between chips is shrinking. There is an urgent need to develop a higher density chip-to-chip interconnection method. In the related technology, ultra-narrow pitch micro-bump interconnection is applied in high bandwidth memory (HBM) products, mainly through the process based on thermal compression bonding and non-conductive film (TC-NCF) or mass reflow with molded underfill (MR-MUF) process to achieve ultra-narrow pitch micro-bump interconnection. Among them, the TC-NCF process wraps the micro-bumps in a non-conductive film, and can simultaneously realize the interconnection of micro-bumps and non-conductive films between chips by applying high temperature and high pressure. However, the thermal conductivity of the non-conductive film is poor, and the time cost of stacking multiple chips is high. Tin (Sn) is obviously squeezed out under pressure. The extruded Sn will contact the surrounding micro-bumps to cause solder joint short circuits, and may also cause copper (Cu) column sidewall corrosion, causing a series of reliability problems; the MR-MUF process is assisted by flux. Multiple chips are first attached to the circuit, and then batch reflow is performed at about 260°C. Multiple chips can be interconnected at one time, but because flux is needed, the flux cleaning step needs to be added. As the micro-bump interconnection pitch reaches 20 microns (μm) and below, the flux cleaning becomes very difficult. The residual flux will cause porous micro-bumps for micro-bumps, which seriously affects the interconnection reliability. Summary of the invention
[0003] One object of the present invention is to provide a bonding method for electronic components applied to ultra-narrow pitch micro-bumps, firstly pre-bonding the micro-bumps by low-temperature solid-state diffusion bonding, and accurately controlling the degree of Sn extrusion by adjusting the bonding pressure during the pre-bonding process; and then high-temperature rapid reflow is used to enable the electronic components to achieve high-reliability and high-efficiency bonding for ultra-narrow pitch micro-bump interconnection. Another object of the present invention is to provide a bonding device for electronic components applied to ultra-narrow pitch micro-bumps. Another object of the present invention is to provide a computer-readable medium. Still another object of the present invention is to provide a computer device.
[0004] In order to achieve the above objectives, the present invention discloses, on one hand, a bonding method for electronic components applied to ultra-narrow pitch micro-bumps, comprising:
[0005] obtaining electronic components to be bonded;
[0006] Pre-bonding the micro-bumps of the electronic components to be bonded by solid-state diffusion bonding to obtain a pre-bonded sample;
[0007] The pre-bonded sample is heated to reflux to generate a bonded sample.
[0008] Preferably, before pre-bonding the micro-bumps of the electronic components to be bonded by solid-state diffusion bonding to obtain the pre-bonded sample, the method further comprises:
[0009] The surfaces of the electronic components to be bonded are ultrasonically cleaned by the cleaning material to generate cleaned electronic components to be bonded.
[0010] Preferably, the micro-bumps of the electronic components to be bonded are pre-bonded by solid-state diffusion bonding to obtain a pre-bonded sample, comprising:
[0011] During the pre-bonding process, protective gas is continuously injected, and hot-press bonding is performed on the micro-bumps of the electronic components to be bonded according to the preset pre-bonding temperature, pre-bonding time and pre-bonding pressure to generate a pre-bonding sample, and the pre-bonding temperature is lower than the melting point of the solder.
[0012] Preferably, the pre-bonding temperature is 200 degrees Celsius, the pre-bonding time is 3 minutes, and the pre-bonding pressure is 0.8 MPa.
[0013] Preferably, the protective gas is continuously injected during the pre-bonding process, including
[0014] In the beginning of the bonding process, an inert gas is injected, and a determination is made at a preset time interval whether the current temperature reaches a preset temperature threshold;
[0015] If so, start injecting formic acid gas;
[0016] If not, continue to execute the step of determining whether the current temperature reaches the preset temperature threshold according to the preset time interval until the current temperature reaches the preset temperature threshold.
[0017] Preferably, the pre-bonded sample is heated and refluxed to generate a bonded sample, comprising:
[0018] The pre-bonded sample is heated by the hot plate of the bonding equipment according to the preset reflow temperature and reflow time so that the solder of the upper and lower micro-bumps melts to complete the connection and generate a bonding sample.
[0019] Preferably, the reflux temperature is 260 degrees Celsius and the reflux time is 1 minute.
[0020] Preferably, after heating the pre-bonded sample to reflux to generate a bonded sample, the method further comprises:
[0021] The micro bumps of the bonding sample are bottom filled with the preset filling material to complete the filling protection of the bonding sample.
[0022] Preferably, the electronic components to be bonded include chips and / or wafers, and the bonding samples include chip-to-chip bonding samples, chip-to-wafer bonding samples or wafer-to-wafer bonding samples.
[0023] Preferably, the diameter of the micro-bump is less than or equal to 30 microns, the pitch of the micro-bump is less than or equal to 40 microns, the height of the micro-bump is less than or equal to 20 microns, and the thickness of the solder is less than or equal to 8 microns.
[0024] Preferably, the method further comprises:
[0025] The shear strength of the bonded sample is tested according to the preset shear pressure, and the shear strength is generated based on the shear pressure and the diameter of the micro-bump.
[0026] The present invention also discloses a computer-readable medium on which a computer program is stored. When the program is executed by a processor, the method described above is implemented.
[0027] The present invention also discloses a computer device, including a memory and a processor, wherein the memory is used to store information including program instructions, the processor is used to control the execution of program instructions, and the processor implements the above method when executing the program.
[0028] The present invention also discloses a computer program product, including a computer program / instruction, and the method described above is implemented when the computer program / instruction is executed by a processor.
[0029] The present invention obtains an electronic component to be bonded; pre-bonds micro-bumps of the electronic component to be bonded by solid-state diffusion bonding to obtain a pre-bonded sample; heats and refluxes the pre-bonded sample to generate a bonding sample, first pre-bonds the micro-bumps by low-temperature solid-state diffusion bonding, and accurately controls the extrusion degree of Sn by adjusting the bonding pressure during the pre-bonding process; and then achieves high-reliability and high-efficiency bonding of the electronic component for ultra-narrow pitch micro-bump interconnection by high-temperature rapid reflux. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1A flow chart of a bonding method for electronic components with ultra-narrow pitch micro-bumps provided in an embodiment of the present invention;
[0032] Figure 2 A flow chart of another bonding method for electronic components with ultra-narrow pitch micro-bumps provided in an embodiment of the present invention;
[0033] Figure 3 A schematic diagram of a bonding point under pre-bonding temperature and pre-bonding pressure conditions provided by an embodiment of the present invention;
[0034] Figure 4 A schematic diagram of a bonding point under another pre-bonding temperature and pre-bonding pressure condition provided by an embodiment of the present invention;
[0035] Figure 5 A schematic diagram of a bonding point under another pre-bonding temperature and pre-bonding pressure condition provided by an embodiment of the present invention;
[0036] Figure 6 A schematic diagram of a bonding point under another pre-bonding temperature and pre-bonding pressure condition provided by an embodiment of the present invention;
[0037] Figure 7 A schematic diagram of a bonding sample after reflow and 500 times magnification provided by an embodiment of the present invention;
[0038] Figure 8 A schematic diagram of a bonding sample after reflow and magnification 1500 times provided in an embodiment of the present invention;
[0039] Fig. 9 A comparative schematic diagram of shear strength tests under different bonding methods provided by an embodiment of the present invention;
[0040] Fig.10 A schematic diagram of a bonding sample after SSD-R bonding of an electronic component A provided by an embodiment of the present invention;
[0041] Fig.11 A schematic diagram of a bonding sample after SSD-R bonding of an electronic component B provided by an embodiment of the present invention;
[0042] Fig.12 A schematic diagram of a bonding sample after SSD-R bonding of an electronic component C provided by an embodiment of the present invention;
[0043] Fig.13 A schematic diagram of a bonding sample after SSD-R bonding of an electronic component D provided by an embodiment of the present invention;
[0044] Fig.14 A schematic diagram of the structure of a computer device provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0045] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] In order to facilitate the understanding of the technical solution provided by the present application, the relevant contents of the technical solution of the present application are first described below. The present application belongs to high-density micro-bump bonding, and the technologies involved include but are not limited to advanced semiconductor packaging, metal low-temperature solid-state bonding, and high-temperature rapid reflow. At present, the two mainstream high-density interconnection methods in the industry include: copper-copper / silicon dioxide-silicon dioxide (Cu-Cu / SiO2-SiO2) hybrid bonding (Hybrid Bonding) and narrow pitch Cu column micro-bump bonding (Fine Pitch Microbump). Cu-Cu / SiO2-SiO2 hybrid bonding (Hybrid Bonding) uses hydrogen bonds between SiO2 to achieve pre-bonding at room temperature, and then uses the difference in thermal expansion coefficients of copper and silicon dioxide to achieve bonding interconnection between copper and copper through high-temperature annealing at 250℃ to 300℃. Narrow pitch micro-bump (Fine Pitch Microbump) technology is a mature inter-chip interconnection technology. The micro-bump structure is generally a copper column + solder cap, which is realized by wafer-level electroplating process. Micro-bumps are interconnected by melting the solder and then cooling and solidifying it through a high-temperature thermal compression bonding (TCB) or flux reflow process at about 260°C. At present, the industry's mass-produced micro-bump indicators are about 20μm in diameter and 40μm in pitch. It is expected that the next generation of mass-produced micro-bump indicators will need to reach a diameter of 10μm and a pitch of 20μm. Compared with hybrid bonding, narrow-pitch micro-bumps have the characteristics of mature technology development, high interconnection density, controllable process costs, and compatibility between equipment and manufacturers. However, in the application of micro-bumps with a pitch below 40μm, the melt extrusion of Sn at high temperature has become a problem that seriously affects the process yield. Because under high temperature conditions, the yield strength of Sn is reduced, and the applied small pressure can cause a large amount of deformation and extrusion. The extruded Sn will contact the surrounding micro-bumps to cause a short circuit in the solder joints, and may also cause erosion of the sidewalls of the Cu column, causing a series of reliability problems.
[0047] The present application is to realize pre-bonding of micro-bumps by low-temperature solid-state diffusion bonding (SSD); remove the surface oxide layer of micro-bumps by inert gas (N2) protection and formic acid gas reduction during the bonding process; accurately control the extrusion degree of Sn by adjusting the SSD bonding pressure during the pre-bonding process; achieve high reliability and high efficiency bonding of the chip by high-temperature rapid reflow; and completely protect the micro-bumps by molding bottom filler. For the convenience of description, this invention is referred to as SSD-R bonding method.
[0048] Figure 1 A flow chart of a bonding method for electronic components with ultra-narrow pitch micro-bumps provided in an embodiment of the present invention, such as Figure 1 As shown, the method includes:
[0049] Step 101: Obtain electronic components to be bonded.
[0050] Step 102: pre-bonding the micro-bumps of the electronic components to be bonded by solid-state diffusion bonding to obtain a pre-bonded sample.
[0051] Step 103: heat the pre-bonded sample for reflux to generate a bonded sample.
[0052] In the technical solution provided by the embodiment of the present invention, an electronic component to be bonded is obtained; the micro-bumps of the electronic component to be bonded are pre-bonded by solid-state diffusion bonding to obtain a pre-bonded sample; the pre-bonded sample is heated and refluxed to generate a bonding sample, and the micro-bumps are first pre-bonded by low-temperature solid-state diffusion bonding, and the extrusion degree of Sn is accurately controlled by adjusting the bonding pressure during the pre-bonding process; and then high-temperature rapid reflux is performed to enable the electronic components to achieve high-reliability and high-efficiency bonding for ultra-narrow pitch micro-bump interconnection.
[0053] Figure 2 A flowchart of another bonding method for electronic components with ultra-narrow pitch micro-bumps provided in an embodiment of the present invention is shown in FIG. Figure 2 As shown, the method includes:
[0054] Step 201: Obtain electronic components to be bonded.
[0055] In an embodiment of the present invention, the electronic components to be bonded include chips and / or wafers. Specifically, if applied to chip-to-chip (Die-to-Die, referred to as: D2D) bonding, the chip to be bonded is selected as the electronic component to be bonded; if applied to chip-to-wafer (Die-to-Wafer, referred to as: D2W) bonding, the chip and wafer to be bonded are selected as the electronic components to be bonded; if applied to wafer-to-wafer (Wafer-to-Wafer, referred to as: W2W) bonding, the wafer to be bonded is selected as the electronic component to be bonded.
[0056] Step 202: ultrasonically clean the surface of the electronic component to be bonded by using a cleaning material to generate a cleaned electronic component to be bonded.
[0057] In the embodiment of the present invention, the cleaning material includes but is not limited to acetone, alcohol, and deionized water. Specifically, a single chip on a wafer is selected, and the surface of the chip / wafer is ultrasonically cleaned using acetone, alcohol, and deionized water in sequence to remove organic matter and residues that may remain on the surface, so that the surface reaches a high degree of cleanliness, and a cleaned electronic component to be bonded is generated.
[0058] It is worth noting that if applied to W2W bonding, the step of selecting the chip is omitted.
[0059] It is worth noting that the cleaning method includes but is not limited to the above-mentioned ultrasonic cleaning method, and cleaning methods such as plasma cleaning, acid cleaning and isopropyl alcohol cleaning can also be used.
[0060] It is worth noting that the micro-bump Cu column (in a broad sense) on the chip is a copper / nickel / copper (Cu / Ni / Cu) structure, the micro-bump diameter is 30μm, the solder cap material is a tin-silver alloy (Sn1.8Ag), and the solder cap thickness is 8μm. Other generalized Cu column structures (such as Cu, Cu / Ni, Cu / Ni / Cu / Ni, Ni, etc.), solder materials (such as Sn, SnPb, SnAgCu, SnBi, etc.), micro-bump diameter designs, and micro-bump height designs of each layer should all be regarded as similar embodiments. This application will not be repeated one by one.
[0061] In the embodiment of the present invention, it is applied to ultra-narrow pitch micro-bumps, the diameter of the micro-bumps is less than or equal to 30 μm, the micro-bump pitch is less than or equal to 40 μm, the micro-bump height is less than or equal to 20 μm, and the solder thickness is less than or equal to 8 μm.
[0062] Step 203: During the pre-bonding process, the protective gas is continuously injected, and the micro-bumps of the electronic components to be bonded are hot-pressed and bonded according to the preset pre-bonding temperature, pre-bonding time and pre-bonding pressure to generate a pre-bonding sample, wherein the pre-bonding temperature is less than the melting point of the solder.
[0063] In an embodiment of the present invention, the SSD pre-bonding process can be carried out by means of a thermocompression bonding device, which supports flip-chip, reflow, and thermocompression bonding processes, supports a protective atmosphere, has an alignment accuracy of up to ±3μm, a pre-bonding process temperature range of from room temperature to 450 degrees Celsius, and a maximum bonding pressure of 2000N.
[0064] It is worth noting that there are differences in the process parameters supported by different thermal compression bonding devices. Devices that support the above process parameters and functions can be applied to this application and are regarded as similar embodiments of this application.
[0065] It is worth noting that the pre-bonding temperature, pre-bonding time and pre-bonding pressure all have specified selection ranges, and the selection criteria are as follows: the pre-bonding temperature should be lower than the melting point of the selected solder; the pre-bonding time is based on successful pre-bonding; the pre-bonding pressure is based on successful pre-bonding and no Sn extrusion.
[0066] The hot-press bonding method using a temperature higher than the melting point of the solder is called solid-liquid diffusion bonding (Solid-Liquid Inter-Diffusion, abbreviated as: SLID). Figure 3 A schematic diagram of a bonding point under a pre-bonding temperature and pre-bonding pressure condition provided by an embodiment of the present invention, such as Figure 3 As shown in the figure, under the conditions of pre-bonding temperature of 260°C and pre-bonding pressure of 0.8 MPa, Sn extrusion is obvious at the bonding point. Figure 4 A schematic diagram of a bonding point under another pre-bonding temperature and pre-bonding pressure condition provided by an embodiment of the present invention, such as Figure 4 As shown in the figure, under the conditions of pre-bonding temperature of 200°C and pre-bonding pressure of 2.4 MPa, Sn extrusion is obvious at the bonding point. Figure 5 A schematic diagram of a bonding point under another pre-bonding temperature and pre-bonding pressure condition provided by an embodiment of the present invention, such as Figure 5 As shown, Sn is slightly squeezed out at the bonding point under the conditions of a pre-bonding temperature of 200°C and a pre-bonding pressure of 1.6 MPa. Figure 6 A schematic diagram of a bonding point under another pre-bonding temperature and pre-bonding pressure condition provided by an embodiment of the present invention, such as Figure 6 As shown in Figure 1, under the conditions of pre-bonding temperature of 200°C and pre-bonding pressure of 0.8 MPa, Sn did not squeeze out at the bonding point. Figure 3 As shown in Figure 1, once the temperature is raised above the melting point of the solder, Sn extrusion is very likely to occur at the solder joint. Different bonding pressures of SSD bonding will also affect the degree of Sn extrusion, such as Figures 4 to 6As shown, 0.8MPa pressure is the best for Sn extrusion control. As a preferred solution, the pre-bonding temperature is 200°C, the pre-bonding time is 3 minutes, and the pre-bonding pressure is 0.8MPa, which can achieve solid-state diffusion between solders, and the pre-bonding pressure is adjusted to control Sn from extrusion.
[0067] It is worth noting that no matter how high the pressure of SSD bonding is, since the temperature has not reached the melting point of solder, there is incomplete contact at the bonding interface, which is consistent with the characteristics of metal cold pressing. To achieve good mechanical strength, these incomplete contact areas need to be eliminated, and a subsequent fast reflow process needs to be introduced.
[0068] Furthermore, at the beginning of the bonding process, an inert gas is injected, and it is determined whether the current temperature reaches the preset temperature threshold at a preset time interval; if so, formic acid gas is injected; if not, the step of determining whether the current temperature reaches the preset temperature threshold at a preset time interval is continued until the current temperature reaches the preset temperature threshold.
[0069] It is worth noting that the preset temperature threshold can be set according to the temperature at which the formic acid gas has the best reducing performance, which is not limited in the embodiment of the present invention. As an optional solution, the temperature threshold is 150°C.
[0070] In the embodiment of the present invention, the inert gas is nitrogen (N2), and N2 atmosphere protection is introduced in the early stage of bonding. After heating, formic acid gas is continuously introduced to perform pre-bonding in the formic acid gas protection atmosphere to prevent oxidation, thereby ensuring the reliability of bonding.
[0071] Step 204, heating the pre-bonded sample by a hot plate of the bonding equipment according to a preset reflow temperature and reflow time so that the solder of the upper and lower micro-bumps melts to complete the connection and generate a bonding sample.
[0072] In the embodiment of the present invention, the bonding equipment is replaced by any equipment that can provide high temperature heating, and the reflow time should be adjusted according to the actual equipment temperature control capability and process requirements. The embodiment of the present invention is not limited to this. As an optional solution, in order to adapt to large-scale production of the process, the reflow time is 1 minute.
[0073] In the embodiment of the present invention, the reflux temperature can be adjusted according to the actual temperature control capability of the equipment and the process requirements, and the range of the reflux temperature is greater than or equal to 250° C.
[0074] In the embodiment of the present invention, the pre-bonded chip / wafer is subjected to high-temperature rapid reflow, so that the solder of the upper and lower micro-bumps melts and completes the connection under the action of its own gravity. At this time, the bonding interface is in complete contact, and the mechanical strength is significantly improved.
[0075] As a preferred solution, the reflux temperature is 260° C. and the reflux time is 1 minute. Figure 7 A schematic diagram of a bonding sample after reflow and 500 times magnification provided by an embodiment of the present invention, such as Figure 7 As shown, the bonding interfaces at the connection points of each upper and lower micro-bump are in complete contact.
[0076] Figure 8 A schematic diagram of a bonding sample after reflow and 1500 times magnification provided by an embodiment of the present invention, such as Figure 8 As shown in the figure, the bonding interface at the connection between the upper and lower micro-bumps is completely in contact, and there is basically no Sn extrusion. The total height after bonding is measured to be 39.78μm, which meets the design value.
[0077] In the embodiment of the present invention, the bonding sample includes a chip-to-chip bonding sample, a chip-to-wafer bonding sample or a wafer-to-wafer bonding sample.
[0078] Step 205: Use a preset filling material to fill the bottom of the micro-bumps of the bonding sample to complete the filling protection of the bonding sample.
[0079] In the embodiment of the present invention, the filling material can be selected according to actual needs, and the embodiment of the present invention does not limit this. As an optional solution, the filling material is liquid epoxy molding compound (LMC for short).
[0080] It is worth mentioning that the filling material should have good fluidity, curing properties and mechanical properties.
[0081] Specifically, through the filling process, the filling material is injected into the bottom gap of the bonded sample to form a stable protective layer, thereby completing the filling protection of the bonded sample.
[0082] It is worth noting that the SSD-R bonding method proposed in this application is not only applicable to the bonding of two-layer chips / wafers, but also to the vertical stacking bonding of multiple chips. The solid-state bonding method completely replaces the deoxidation and adhesion of the flux, which not only ensures that the Sn bumps are not squeezed out, but also avoids the problem of flux residue. It has potential in the micro-bump bonding scenario with a narrower pitch (≤20μm).
[0083] Furthermore, the SSD-R bonding method of the present application was compared with the TC-NCF process and the MR-MUF process in the traditional process by SLID method. The test results are shown in Table 1:
[0084] Table 1
[0085] TC-NCF MR-MUF SSD-R Production efficiency × √ √ Thermal conductivity × √ √ Sn extrusion control × √ √ Flux cleaning unnecessary need unnecessary
[0086] It can be seen that the SSD-R bonding method of the present application has excellent performance in production efficiency, thermal conductivity, Sn extrusion control, and flux cleaning.
[0087] Step 206: Perform a shear strength test on the bonded sample according to a preset shear pressure, and generate a shear strength based on the shear pressure and the diameter of the micro-bump.
[0088] In the embodiment of the present invention, the shear strength of the bonding point under different bonding modes is tested. Fig. 9 A comparative schematic diagram of shear strength tests under different bonding modes provided in an embodiment of the present invention, such as Fig. 9 As shown, the bonding methods include SSD method, SSD-R method and SLID method, among which the SSD method is represented by a triangle, the SSD-R method is represented by a five-pointed star, and the SLID method is represented by a pentagon; the horizontal axis of the comparison diagram is shear pressure (Bonding Strength), the unit is MPa; the vertical axis is shear strength (Shear Strength), the unit is MPa.
[0089] In the embodiment of the present invention, the value of the shear strength is a nominal value, and the shear strength is generated by calculating the shear pressure and the diameter of the micro-bump. Specifically, the circular cross-sectional area of the micro-bump is calculated according to the diameter of the micro-bump; the shear pressure is divided by the circular cross-sectional area to obtain the shear strength. As an optional solution, the diameter of the micro-bump is 30 μm.
[0090] In the embodiment of the present invention, the nominal shear strength of the SLID bonded sample and the 2.4MPa SSD-R bonded sample is higher than the actual value because the force bearing area increases due to Sn extrusion. Fig. 9 It can be seen that the SSD pre-bonded samples have a certain shear strength, which can support the transportation of pre-bonded chips / wafers between different equipment. The shear strength of the SSD-R bonded samples is significantly improved. For example, the shear strength of the 0.8MPa SSD-R bonded sample can reach 22.21MPa, which meets the shear strength standard of micro-bumps. So in summary, the SSD-R bonding method can achieve good bonding strength while controlling Sn extrusion.
[0091] The above embodiment first selected a sample with a micro-bump diameter of 30 μm, because its Sn thickness can be made very thick (8 μm in the embodiment of the present invention), and the control of Sn extrusion is more difficult. Solving the Sn extrusion problem of this sample, the bonding of other narrower pitch micro-bumps can be solved in theory. Furthermore, the SSD-R bonding method is used to bond electronic components of different sizes to further verify the reliability of the SSD-R bonding method. The electronic components of various sizes are shown in Table 2:
[0092] Table 2
[0093] No. Micro bump diameter Micro bump pitch Micro bump height Solder thickness A 30μm 60μm 20μm 8μm B 30μm 60μm 17μm 6μm C 20μm 40μm 16μm 4μm D 10μm 20μm 10μm 4μm
[0094] Among them, the micro-bump diameter of electronic component A is 30μm, the micro-bump pitch is 60μm, the micro-bump height is 20μm, and the solder thickness is 8μm; the micro-bump diameter of electronic component B is 30μm, the micro-bump pitch is 60μm, the micro-bump height is 17μm, and the solder thickness is 6μm; the micro-bump diameter of electronic component C is 20μm, the micro-bump pitch is 40μm, the micro-bump height is 16μm, and the solder thickness is 4μm; the micro-bump diameter of electronic component D is 10μm, the micro-bump pitch is 20μm, the micro-bump height is 10μm, and the solder thickness is 4μm.
[0095] Fig.10 A schematic diagram of a bonding sample after SSD-R bonding of an electronic component A provided by an embodiment of the present invention is shown as follows: Fig.10 As shown, the left picture is a bonding sample after reflow at a magnification of 500 times, and the bonding interfaces at the connection of each upper and lower micro-bump are in complete contact; the right picture is a bonding sample after reflow at a magnification of 1500 times, and the bonding interfaces at the connection of the upper and lower micro-bumps are in complete contact, the bonding effect is good, and there is no Sn extrusion.
[0096] Fig.11 A schematic diagram of a bonding sample after SSD-R bonding of an electronic component B provided by an embodiment of the present invention is shown as follows: Fig.11 As shown, the left picture is a bonding sample after reflow at a magnification of 500 times, and the bonding interfaces at the connection of each upper and lower micro-bump are in complete contact; the right picture is a bonding sample after reflow at a magnification of 1500 times, and the bonding interfaces at the connection of the upper and lower micro-bumps are in complete contact, the bonding effect is good, and there is no Sn extrusion.
[0097] Fig.12 A schematic diagram of a bonding sample after SSD-R bonding of an electronic component C provided by an embodiment of the present invention, such as Fig.12 As shown, the left picture is a bonding sample after reflow at a magnification of 500 times, and the bonding interfaces at the connection of each upper and lower micro-bump are in complete contact; the right picture is a bonding sample after reflow at a magnification of 1500 times, and the bonding interfaces at the connection of the upper and lower micro-bumps are in complete contact, the bonding effect is good, and there is no Sn extrusion.
[0098] Fig.13 A schematic diagram of a bonding sample after SSD-R bonding of an electronic component D provided by an embodiment of the present invention is shown as follows: Fig.13As shown, the left picture is a bonding sample after reflow at a magnification of 500 times, and the bonding interfaces at the connection of each upper and lower micro-bump are in complete contact; the right picture is a bonding sample after reflow at a magnification of 1500 times, and the bonding interfaces at the connection of the upper and lower micro-bumps are in complete contact, the bonding effect is good, and there is basically no Sn extrusion.
[0099] The SSD-R bonding method of the present application can realize ultra-narrow pitch micro-bump interconnection with a pitch of less than 40 μm, can control the Sn extrusion problem during the bonding process, and avoid the bonding process involving flux-assisted processes. It has good application prospects in the next generation of ultra-narrow pitch micro-bump bonding applications in the industry.
[0100] It is worth noting that the acquisition, storage, use, and processing of data in the technical solution of this application are in compliance with the relevant provisions of laws and regulations. The user information in the embodiments of this application is obtained through legal and compliant channels, and the acquisition, storage, use, and processing of user information are authorized and agreed by the customer.
[0101] In the technical solution of the bonding method for electronic components applied to ultra-narrow pitch micro-bumps provided in the embodiment of the present invention, an electronic component to be bonded is obtained; the micro-bumps of the electronic component to be bonded are pre-bonded by solid-state diffusion bonding to obtain a pre-bonded sample; the pre-bonded sample is heated and refluxed to generate a bonding sample, and the micro-bumps are first pre-bonded by low-temperature solid-state diffusion bonding, and the extrusion degree of Sn is accurately controlled by adjusting the bonding pressure during the pre-bonding process; and then the electronic component is subjected to high-temperature rapid reflux to achieve high-reliability and high-efficiency bonding for ultra-narrow pitch micro-bump interconnection.
[0102] The systems, devices, modules or units described in the above embodiments may be implemented by computer chips or entities, or by products with certain functions. A typical implementation device is a computer device, and specifically, the computer device may be, for example, a personal computer, a laptop computer, a cellular phone, a camera phone, a smart phone, a personal digital assistant, a media player, a navigation device, an email device, a game console, a tablet computer, a wearable device, or a combination of any of these devices.
[0103] An embodiment of the present invention provides a computer device, including a memory and a processor, the memory is used to store information including program instructions, the processor is used to control the execution of the program instructions, and the program instructions, when loaded and executed by the processor, implement the steps of the above-mentioned embodiment of the bonding method for electronic components with ultra-narrow pitch micro-bumps. For a specific description, please refer to the above-mentioned embodiment of the bonding method for electronic components with ultra-narrow pitch micro-bumps.
[0104] Reference below Fig.14, which shows a schematic diagram of the structure of a computer device 600 suitable for implementing an embodiment of the present application.
[0105] like Fig.14 As shown, the computer device 600 includes a central processing unit (CPU) 601, which can perform various appropriate operations and processes according to a program stored in a read-only memory (ROM) 602 or a program loaded from a storage part 608 into a random access memory (RAM) 603. In the RAM 603, various programs and data required for the operation of the computer device 600 are also stored. The CPU 601, the ROM 602, and the RAM 603 are connected to each other via a bus 604. An input / output (I / O) interface 605 is also connected to the bus 604.
[0106] The following components are connected to the I / O interface 605: an input section 606 including a keyboard, a mouse, etc.; an output section 607 including a cathode ray tube (CRT), a liquid crystal feedback device (LCD), etc., and a speaker, etc.; a storage section 608 including a hard disk, etc.; and a communication section 609 including a network interface card such as a LAN card, a modem, etc. The communication section 609 performs communication processing via a network such as the Internet. A drive 610 is also connected to the I / O interface 605 as needed. A removable medium 611, such as a magnetic disk, an optical disk, a magneto-optical disk, a semiconductor memory, etc., is installed on the drive 610 as needed, so that a computer program read therefrom is installed as needed as the storage section 608.
[0107] In particular, according to an embodiment of the present invention, the process described above with reference to the flowchart can be implemented as a computer software program. For example, an embodiment of the present invention includes a computer program product, which includes a computer program tangibly contained on a machine-readable medium, and the computer program includes program code for executing the method shown in the flowchart. In such an embodiment, the computer program can be downloaded and installed from a network through the communication part 609, and / or installed from the removable medium 611.
[0108] Computer readable media include permanent and non-permanent, removable and non-removable media that can be implemented by any method or technology to store information. Information can be computer readable instructions, data structures, program modules or other data. Examples of computer storage media include, but are not limited to, phase change memory (PRAM), static random access memory (SRAM), dynamic random access memory (DRAM), other types of random access memory (RAM), read-only memory (ROM), electrically erasable programmable read-only memory (EEPROM), flash memory or other memory technology, compact disk read-only memory (CD-ROM), digital versatile disk (DVD) or other optical storage, magnetic cassettes, magnetic tape disk storage or other magnetic storage devices or any other non-transmission media that can be used to store information that can be accessed by a computing device. As defined herein, computer readable media does not include temporary computer readable media (transitory media), such as modulated data signals and carrier waves.
[0109] For the convenience of description, the above device is described in various units according to their functions. Of course, when implementing the present application, the functions of each unit can be implemented in the same or multiple software and / or hardware.
[0110] The present invention is described with reference to flowcharts and / or block diagrams of methods, devices (systems), and computer program products according to embodiments of the present invention. It should be understood that each process and / or block in the flowchart and / or block diagram, as well as the combination of processes and / or blocks in the flowchart and / or block diagram, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor, or other programmable data processing device to produce a machine, so that the instructions executed by the processor of the computer or other programmable data processing device generate instructions for implementing the processes in the flowchart and / or block diagram. Figure 1 A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.
[0111] These computer program instructions may also be stored in a computer-readable memory capable of directing a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer-readable memory produce an article of manufacture comprising an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1 A function specified in one or more boxes.
[0112] These computer program instructions can also be loaded onto a computer or other programmable data processing device so that a series of operating steps are executed on the computer or other programmable device to produce a computer-implemented process, thereby providing instructions for implementing the process. Figure 1 A process or multiple processes and / or boxes Figure 1 A step that specifies a function in one or more boxes.
[0113] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the process, method, commodity or device including the elements.
[0114] The acquisition, storage, use, and processing of data in the technical solution of this application comply with the relevant provisions of national laws and regulations.
[0115] Those skilled in the art will appreciate that the embodiments of the present application may be provided as methods, systems or computer program products. Therefore, the present application may adopt the form of a complete hardware embodiment, a complete software embodiment or an embodiment in combination with software and hardware. Moreover, the present application may adopt the form of a computer program product implemented on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) that contain computer-usable program code.
[0116] The present application may be described in the general context of computer-executable instructions executed by a computer, such as program modules. Generally, program modules include routines, programs, objects, components, data structures, etc. that perform specific tasks or implement specific abstract data types. The present application may also be practiced in distributed computing environments where tasks are performed by remote processing devices connected through a communication network. In a distributed computing environment, program modules may be located in local and remote computer storage media, including storage devices.
[0117] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0118] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A bonding method for electronic components with ultra-narrow pitch micro-bumps, It is characterized in that The method comprises: obtaining electronic components to be bonded; Pre-bonding the micro-bumps of the electronic component to be bonded by solid-state diffusion bonding to obtain a pre-bonded sample; The pre-bonded sample is heated to reflux to generate a bonded sample.
2. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 1, It is characterized in that Before pre-bonding the micro-bumps of the electronic components to be bonded by solid-state diffusion bonding to obtain the pre-bonded samples, the method further includes: The surface of the electronic component to be bonded is ultrasonically cleaned by the cleaning material to generate the cleaned electronic component to be bonded.
3. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 1, It is characterized in that The method of pre-bonding the micro-bumps of the electronic components to be bonded by solid-state diffusion bonding to obtain a pre-bonded sample comprises: During the pre-bonding process, protective gas is continuously injected, and the micro-bumps of the electronic components to be bonded are subjected to hot-press bonding according to the preset pre-bonding temperature, pre-bonding time and pre-bonding pressure to generate the pre-bonding sample, wherein the pre-bonding temperature is lower than the melting point of the solder.
4. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 3, It is characterized in that The pre-bonding temperature is 200 degrees Celsius, the pre-bonding time is 3 minutes, and the pre-bonding pressure is 0.8 MPa.
5. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 3, It is characterized in that The continuous injection of protective gas during the pre-bonding process includes: In the beginning of the bonding process, an inert gas is injected, and a determination is made at a preset time interval whether the current temperature reaches a preset temperature threshold; If so, start injecting formic acid gas; If not, continue to execute the step of determining whether the current temperature reaches the preset temperature threshold according to the preset time interval until the current temperature reaches the preset temperature threshold.
6. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 1, It is characterized in that The step of heating and refluxing the pre-bonded sample to generate a bonded sample comprises: The pre-bonded sample is heated by a hot plate of a bonding device according to a preset reflow temperature and reflow time so that the solder of the upper and lower micro-bumps melts to complete the connection, thereby generating the bonded sample.
7. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 6, It is characterized in that The reflux temperature is 260 degrees Celsius, and the reflux time is 1 minute.
8. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 1, It is characterized in that After the pre-bonded sample is heated and refluxed to generate a bonded sample, the method further includes: The micro-bumps of the bonding sample are bottom-filled using a preset filling material to complete the filling protection of the bonding sample.
9. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 1, It is characterized in that The electronic components to be bonded include chips and / or wafers, and the bonding samples include chip-to-chip bonding samples, chip-to-wafer bonding samples or wafer-to-wafer bonding samples.
10. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 1, It is characterized in that The diameter of the micro-bump is less than or equal to 30 microns, the pitch of the micro-bump is less than or equal to 40 microns, the height of the micro-bump is less than or equal to 20 microns, and the thickness of the solder is less than or equal to 8 microns.
11. The bonding method for electronic components applied to ultra-narrow pitch micro-bumps according to claim 1, It is characterized in that The method further comprises: The bonding sample is subjected to a shear strength test according to a preset shear pressure, and the shear strength is generated according to the shear pressure and the diameter of the micro-bumps.
Citation Information
Patent Citations
Multi-layer mixed synchronization bonding structure and method for three-dimensional packaging
CN102169845A
Method for realizing silicon carbide bonding by virtue of material diffusion and mutual dissolution
CN104876180A
Chip and substrate bonding method, display panel with chip and substrate bonding method and electronic equipment with chip and substrate bonding method
CN116072772A
Preparation process and application of high-density copper pillar micro-bumps for realizing ultra-narrow pitch interconnection
CN116137232A
Nano laminated Cu-Sn low-temperature solid diffusion bonding process method
CN117877996A