Preparation method of efficient deep ultraviolet light-emitting structure
By using beveled angle substrate, high-temperature thermal annealing and patterning processing technology in AlGaN-based deep ultraviolet light emitting diodes, macro-step AlN layer is formed, which solves the problems of low radiation recombination efficiency and morphological defects, and achieves efficient luminescence Structural preparation.
Patent Information
- Application Number
- CN202411022812.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The radiation recombination efficiency of AlGaN-based deep ultraviolet light-emitting diodes is low, resulting in limited industrial development and market applications. Existing improvement methods such as high-temperature thermal annealing, patterned AlN method and large-inclination substrate epitaxial method have surface cracking and morphological defects. .
An AlN layer is prepared on a substrate with a certain oblique angle to avoid the surface morphology of the macrostage, followed by high-temperature thermal annealing and patterning to form an AlN layer with a surface morphology of the macrostage, and finally quantums are formed in the AlGaN structural layer. Linear luminescent structures to enhance quantum confined domain effects.
The radiation recombination efficiency of the deep ultraviolet luminescent structure is significantly improved, the crystal quality is improved, the surface cracking and morphological defects are reduced, and the luminescence efficiency is improved.
Smart Images

Figure CN118969917A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a method for preparing a high-efficiency deep ultraviolet light-emitting structure. Background Art
[0002] AlGaN (aluminum gallium nitride) based deep ultraviolet light-emitting diodes (DUV LEDs) have many advantages such as no mercury pollution, low voltage, small size, and easy integration. They are widely used in public health, environmental protection, biochemical testing, medical treatment, national defense, etc. However, the current electro-optical conversion efficiency of AlGaN-based DUV LEDs is extremely low (usually <10%), which seriously restricts the industrial development and market application of AlGaN-based DUV-LEDs. The low radiation recombination efficiency in the active area is a key issue.
[0003] There are two main reasons for the low radiative recombination efficiency of AlGaN-based deep ultraviolet active regions: 1. Due to the lack of low-cost, large-size, high-quality AlN single crystal substrates, AlGaN-based deep ultraviolet light-emitting active regions are basically grown on AlN (aluminum nitride) / sapphire templates. Due to the serious lattice mismatch and thermal mismatch between AlN and sapphire substrates, and the weak surface migration ability of Al (aluminum) atoms, the dislocation density in AlN is very high and the residual strain is very strong. Dislocations and strains will be transmitted to the upper AlGaN active region, and dislocations are typical non-radiative recombination centers, which will reduce the radiative recombination efficiency of the active region. 2. In the AlGaN material required for the deep ultraviolet active region, the size of Al atoms and Ga (gallium) atoms is relatively close, and it is difficult to form the more significant phase separation in InGaN (indium gallium nitride) materials. Therefore, it is difficult to produce a quantum dot-like effect, and it is impossible to effectively shield the influence of defects such as dislocations on the recombination process, and it is impossible to significantly improve the radiative recombination efficiency.
[0004] At present, the commonly used methods to improve crystal quality mainly include high-temperature thermal annealing, patterned AlN and high-angle substrate epitaxy. However, the above three methods alone have obvious disadvantages and cannot maximize the radiation recombination efficiency: simply using the high-temperature thermal annealing method can improve the crystal quality, but there will be relatively serious compressive strain, which will cause the subsequent AlGaN growth to easily have serious hillocks morphology and cannot enhance the quantum confinement effect; simply using the patterned AlN method can improve the crystal quality, but tensile strain will be generated during the closing process, which is easy to cause surface cracking and cannot enhance the quantum confinement effect; simply using the high-angle substrate epitaxial technology can improve the crystal quality and enhance the quantum confinement effect by self-organizing to form quantum wires, but the existence of macro-steps will lead to continuous tensile strain, which is easy to cause surface cracking.
[0005] According to a UV optoelectronic device and a method for preparing the same disclosed in China with the announcement number CN112670383B, although the dislocation density of the material is reduced by depositing AlN material on a sapphire substrate with a large tilt angle to obtain a first wafer, and placing the first wafer in a high-temperature annealing furnace for high-temperature thermal annealing to obtain a second wafer with a serrated macro-step interface, the dislocations will eventually be bounded by the macro-steps, and there will be physical limitations after the dislocations interact to a certain extent. Dislocations bounded by different macro-steps cannot meet again to interact with each other, so it is impossible to further reduce the dislocation density and regulate the strain. The Chinese invention with announcement number CN108155090A discloses a high-quality AlN epitaxial film and its preparation method and application. Although it obtains a crack-free, atomically flat AlN epitaxial film with very low dislocation density by patterning a sapphire substrate or an AlN template and high-temperature annealing, it lacks the physical process of macro-step-induced dislocation tilting, and the probability of dislocation interaction is lower; and without the carrier confinement enhancement effect brought by the macro-step, it is impossible to shield the negative impact of residual dislocations on the light-emitting active area, and the improvement of luminous efficiency is limited. Therefore, it is of great significance to develop a preparation process that can simultaneously meet the requirements of significantly improving the radiation recombination efficiency of the deep ultraviolet light-emitting structure, improving the crystal quality, and reducing the morphological defects of the deep ultraviolet light-emitting structure, in order to improve the luminous efficiency of the deep ultraviolet light-emitting structure. Summary of the invention
[0006] In order to solve the problem that it is impossible to reduce the morphological defects of the deep ultraviolet light-emitting structure while significantly improving the radiation recombination efficiency and improving the crystal quality of the deep ultraviolet light-emitting structure, considering that high-temperature thermal annealing, patterned AlN and high-angle substrate epitaxy can all improve the crystal quality, the three methods of high-temperature thermal annealing, patterned AlN and high-angle substrate epitaxy are simply combined together. However, after the combination, it is found that the wafers prepared by the preparation process obtained by simply combining the three methods are always prone to cracking on the surface, resulting in the quality of the prepared wafers not meeting the requirements. Therefore, the inventors continued to conduct extensive research on the production process of deep ultraviolet light-emitting structures. During one research process, the inventors accidentally discovered that the main reason why the wafer is prone to cracking on the surface is that, in order to ensure that a macro-step morphology is formed on the upper surface of the AlGaN structural layer, it is necessary to ensure that the AlGaN structural layer is grown on an AlN layer with a macro-step surface. However, when the AlN layer directly grown on the substrate has a macro-step morphology, this macro-step morphology will introduce strong tensile strain into the prepared wafer, and surface cracks are likely to occur during annealing, which results in the final prepared wafer being prone to surface cracks. Based on this discovery, the inventors came up with the idea of first preparing an AlN layer without a macro-step surface on a substrate to avoid introducing strong tensile strain into the prepared wafer; then, subjecting the preliminarily prepared wafer to a high-temperature thermal annealing treatment to introduce compressive strain while reducing the dislocation density in the AlN layer, thereby greatly reducing the probability of wafer cracking during the preparation process; next, by patterning and epitaxially growing the AlN layer, the dislocation density in the AlN layer is further reduced, and an AlN surface layer with a macro-step surface morphology is formed, wherein the macro-step induces dislocation tilt while introducing tensile strain to compensate for the compressive strain introduced in the early stage; finally, an AlGaN structural layer including n-type AlGaN and AlGaN having a surface with a macro-step morphology is prepared on the upper surface of the AlN surface layer, so as to form a quantum wire light-emitting structure at the edge of the macro-step, while the macro-step terrace maintains a quantum well structure, thereby effectively enhancing the quantum confinement effect and improving the radiative recombination efficiency.
[0007] Therefore, according to one aspect of the present invention, a method for preparing a high-efficiency deep ultraviolet light-emitting structure is provided, characterized in that it comprises the following steps:
[0008] S10: preparing an AlN layer on a substrate having a certain bevel angle, and controlling the surface of the AlN layer not to form a macro-step surface morphology, so as to obtain a first wafer;
[0009] S20: performing high temperature thermal annealing on the first wafer to obtain an annealed wafer;
[0010] S30: performing a patterning process on the AlN layer on the annealed wafer to form a patterned AlN layer;
[0011] S40: performing epitaxial growth on the upper surface of the patterned AlN layer to prepare an AlN surface layer having a macro-step surface morphology;
[0012] S50: preparing an AlGaN structural layer on the upper surface of the AlN surface layer, and ensuring that the surface of the AlGaN structural layer has a macro-step morphology.
[0013] Since the present invention controls the surface of the AlN layer directly grown on the substrate to not form a macro-step surface morphology, the introduction of strong tensile strain in the prepared wafer is avoided; and by subjecting the preliminarily prepared wafer to a high-temperature thermal annealing treatment, compressive strain is introduced while reducing the dislocation density in the AlN layer, thereby greatly reducing the probability of cracking of the wafer during the preparation process; at the same time, by subjecting the AlN layer to a graphical treatment and epitaxial growth, the dislocation density in the AlN layer is further reduced, and an AlN surface layer with a macro-step surface morphology is formed, and while the macro-step induces dislocation tilt (strengthening the interaction of dislocations, reducing the number of dislocations penetrating into the light-emitting active region, and reducing the non-radiative recombination of the light-emitting active region), tensile strain is introduced to compensate for the compressive strain introduced in the early stage, and an AlGaN structural layer including n-type AlGaN and AlGaN with a macro-step morphology on the surface is prepared on the upper surface of the AlN surface layer, thereby forming a quantum wire light-emitting structure at the edge of the macro-step, and the macro-step terrace will maintain a quantum well structure, thereby effectively enhancing the quantum confinement effect, shielding the negative effects of non-radiative recombination centers formed by dislocations, and improving the radiative recombination efficiency.
[0014] In some embodiments, in step S10, the AlN layer is prepared on a substrate having a certain bevel angle by high temperature magnetron sputtering or MOCVD (Metal-organic Chemical Vapor Deposition) growth method. Since magnetron sputtering belongs to non-equilibrium deposition, the AlN layer directly grown on the substrate can be prevented from forming a macro-step surface morphology, and therefore, strong tensile strain will not be introduced into the obtained wafer.
[0015] In some embodiments, the thickness of the AlN layer ranges from 100nm to 600nm (nanometers); and / or the sputtering temperature range of the high-temperature magnetron sputtering method is 600℃ to 800℃ (degrees Celsius); the preparation temperature of the MOCVD growth method is 1000℃ to 1150℃, the N / Al molar ratio (molar ratio of nitrogen to aluminum) is 500 to 1500, and the preparation speed is 1μm / h to 5μm / h (millimeter per hour). The present invention can avoid the problem of poor crystal quality of the prepared AlN layer due to too low temperature by limiting the lower limit temperature of the high-temperature magnetron sputtering method; and the present invention can avoid the problem of insufficient hole depth of the subsequent patterned AlN due to too thin thickness, which leads to the hole being unable to effectively prevent the AlN nucleation growth inside the hole, resulting in the problem of disordered closure of the AlN layer and poor crystal quality by controlling the thickness range of the AlN layer; it can also avoid the problem of large thermal mismatch between the AlN layer and the substrate due to too thick thickness, which leads to very poor crystal quality of the AlN layer. When the MOCVD growth method is used to prepare the AlN layer, by avoiding growth conditions such as high temperature, low molar ratio, and slow growth rate, the film is deposited under conditions far from quasi-equilibrium growth, avoiding a long surface migration length of atoms, thereby preparing an AlN layer without macro-step morphology.
[0016] In some embodiments, in step S10, the substrate is a sapphire substrate or a SiC (silicon carbide) substrate.
[0017] In some embodiments, in step S10, the surface of the sapphire substrate or SiC substrate on which the AlN layer is grown has a c-plane (0001) with a bevel angle of α, wherein 0.2°<α≤1°, and the bevel direction is the c-axis deviating from the m-axis or the c-axis deviating from the a-axis. Thus, on the one hand, it can be avoided that the desired macro-step surface morphology is difficult to form during the growth of the AlN layer due to a too small inclination angle; on the other hand, it can be avoided that the subsequent patterned AlN layer is difficult to achieve surface closure due to a too large inclination angle; preferably, a sapphire substrate with a c-axis deviating from the m-axis bevel direction is selected to make the surface closure faster.
[0018] In some embodiments, in step S20, when the first wafer is subjected to high-temperature thermal annealing, the surfaces of the AlN layers of the two first wafers are bonded together, the annealing temperature is 1600°C to 1800°C, the annealing atmosphere is an inert gas or a nitrogen-containing gas, and the annealing time of the high-temperature section is 0h to 24h (hours). Thus, atomic rearrangement can be achieved through high-temperature thermal annealing, the dislocation density in the AlN layer can be reduced, and a high-quality base layer can be provided for subsequent patterned AlN; moreover, the high-temperature thermal annealing can introduce a strong compressive strain in the AlN layer during the cooling process, and the tensile strain generated in the subsequent patterned AlN closing process and the tensile strain generated by the large-angle substrate epitaxy can be compensated, so as to avoid surface cracking caused by excessive tensile strain and hillocks on the surface caused by excessive compressive strain; at the same time, the use of inert gas as the annealing atmosphere can protect the AlN layer from being oxidized during the high-temperature thermal annealing process, and the use of nitrogen-containing gas as the annealing atmosphere can inhibit the decomposition of the AlN layer during the high-temperature thermal annealing process. Preferably, in step S20, the inert gas is helium, or the nitrogen-containing gas is nitrogen.
[0019] In some embodiments, in step S30, the AlN layer on the annealed wafer is patterned to prepare a patterned AlN layer having a hexagonal hole structure. Since AlN has a hexagonal symmetric structure, the present invention prepares a patterned AlN layer having a hexagonal hole structure, which can ensure that the six faces of the hexagonal hole have the same closing speed during the closing process, and it is not easy to generate new dislocations, so that a flat surface is easily obtained.
[0020] In some embodiments, the hexagonal hole structure has a side spacing of 500nm to 1000nm, a patterning period of 800nm to 1500nm, a depth of the hexagonal hole structure greater than 100nm, and the six faces inside the hexagonal hole correspond to the six a-faces or six m-faces of AlN. The present invention controls the size of the hexagonal hole, thereby ensuring that AlN has a thinner closed thickness and can effectively reduce the dislocation density; moreover, the present invention ensures the selective growth of AlN by limiting the hole depth.
[0021] In some embodiments, in step S40, epitaxial growth is performed on the upper surface of the patterned AlN layer at 1150°C to 1350°C to prepare an AlN surface layer with a macro-step surface morphology. The present invention can control the temperature of epitaxial growth on the upper surface of the patterned AlN layer to avoid the AlN surface closing very slowly, increasing the closing thickness, and increasing the cost due to the weak surface migration ability of Al atoms caused by too low temperature; it can also avoid the AlN lateral closing speed being too fast due to too high temperature, resulting in new dislocations and surface unevenness at the closing boundary, so that the hexagonal holes can be evenly closed to obtain a surface morphology with macro-steps and no holes.
[0022] In some embodiments, the AlGaN structural layer is a composite structural layer of n-type AlGaN and AlGaN. The growth temperature is 1040°C to 1100°C, the edge of the macro-step is on the non-polar surface, and the rest of the macro-step terrace is a polar surface. Due to the different migration and incorporation behaviors of Al atoms and Ga atoms on polar and non-polar surfaces, AlGaN with a lower component will be formed at the edge of the macro-step, while AlGaN with a higher component will be formed on the macro-step terrace. If we use the conventional process for growing a quantum well structure, a quantum wire structure will be formed at the edge of the macro-step, while the macro-step terrace will maintain a quantum well structure. This can effectively enhance the quantum confinement effect and improve the efficiency of radiation recombination. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of a process for preparing a high-efficiency deep ultraviolet light-emitting structure according to an embodiment of the present invention;
[0024] Figure 2 The surface morphology images taken by atomic force microscope of AlN with the same thickness grown on substrates with different bevel angles and bevel directions under the same process conditions;
[0025] Figure 3 Schematic diagram of the comparison of photoluminescence spectra between a quantum structure without typical macro-step morphology and a quantum structure with typical macro-step morphology. DETAILED DESCRIPTION
[0026] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.
[0027] It should also be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include" and "comprise" include not only those elements, but also other elements that are not explicitly listed, or also include elements inherent to such processes, methods, articles or equipment. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the existence of other identical elements in the process, method, article or equipment that includes the elements. The terms used in this article are generally commonly used terms by those skilled in the art. If they are inconsistent with commonly used terms, the terms in this article shall prevail.
[0028] In this article, the term "macro-step" refers to a relatively large step structure artificially created on the surface of a semiconductor material or a wafer. These step structures can be used to improve the crystal quality of the material and the performance of the device.
[0029] In this article, the term "patterning" refers to the process of making specific patterns on the surface of the wafer, which will determine the size, shape and layout of the final semiconductor device. It usually includes the following main processes: photolithography, exposure, development, etching, (ion implantation), and removal of photoresist.
[0030] In this article, the term "hillocks" generally refers to small hillocks or hillock-like protrusions formed on the surface of thin film materials. These protrusions may be formed due to a variety of reasons, including thermal stress, uneven diffusion of materials, electromigration, etc.
[0031] In this article, the term "radiative recombination efficiency" refers to the proportion of energy released in the form of photons when electrons jump from the conduction band to the valence band in semiconductor materials. This is a very important parameter in light-emitting diodes (LEDs) and other optoelectronic devices because it is directly related to the luminous efficiency and performance of the device.
[0032] In this article, the term "quantum dot-like effect" refers to the behavior of quantum dots in a material due to size confinement or other factors. Quantum dots are nanoscale semiconductor materials that have size-dependent electronic and optical properties that are different from those of traditional bulk materials.
[0033] In this article, the term "quantum confinement effect" refers to the fact that when the size of a particle reaches the nanometer level, the electron energy level near the Fermi level splits from a continuous state into discrete energy levels.
[0034] In this article, the term "carrier confinement enhancement effect" refers to the phenomenon in semiconductor materials where carriers (electrons and holes) are confined in a specific spatial region by physical or chemical means, thereby enhancing their photoelectric properties. This effect is particularly significant in low-dimensional semiconductor materials, such as quantum wells, quantum wires, and quantum dots.
[0035] In this article, the term "carrier localization effect" refers to the fact that in semiconductor materials, electrons and holes are confined in a limited spatial region, causing their energy states to change from continuous energy bands to discrete energy levels. This effect is usually observed in low-dimensional semiconductor structures or semiconductor materials with a certain degree of disorder, such as amorphous semiconductors, polycrystalline semiconductors, or doped semiconductors.
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The following will be combined with the attached Figure 1 The preparation method of the high-efficiency deep ultraviolet light-emitting structure is described in detail.
[0038] According to one aspect of the present invention, a method for preparing a high-efficiency deep ultraviolet light-emitting structure is provided, characterized in that it comprises the following steps:
[0039] S10: preparing an AlN layer on a substrate having a certain bevel angle, and controlling the surface of the AlN layer not to form a macro-step surface morphology, so as to obtain a first wafer;
[0040] S20: performing high temperature thermal annealing on the first wafer to obtain an annealed wafer;
[0041] S30: performing a patterning process on the AlN layer on the annealed wafer to form a patterned AlN layer;
[0042] S40: performing epitaxial growth on the upper surface of the patterned AlN layer to prepare an AlN surface layer having a macro-step surface morphology;
[0043] S50: preparing an AlGaN structural layer on the upper surface of the AlN surface layer, and ensuring that the surface of the AlGaN structural layer has a macro-step morphology.
[0044] Since the present invention controls the surface of the AlN layer directly grown on the substrate to not form a macro-step surface morphology, the introduction of strong tensile strain in the prepared wafer is avoided; and by performing high-temperature thermal annealing treatment on the initially prepared wafer, the dislocation density in the AlN layer is reduced while introducing compressive strain, thereby greatly reducing the probability of cracking of the wafer during the preparation process; at the same time, by performing graphic processing and epitaxial growth on the AlN layer, the dislocation density in the AlN layer is further reduced, and an AlN surface layer with a macro-step surface morphology is formed, and an AlGaN structural layer including n-type AlGaN and AlGaN with a macro-step morphology on the surface is prepared on the upper surface of the AlN surface layer, so as to form a quantum wire structure on the edge of the macro-step, and the macro-step terrace will maintain a quantum well structure, thereby effectively enhancing the quantum confinement effect and improving the radiation recombination efficiency.
[0045] In some embodiments, in step S10, the AlN layer is prepared on a substrate having a certain bevel angle by a high-temperature magnetron sputtering method. Since magnetron sputtering belongs to non-equilibrium deposition, the AlN layer directly grown on the substrate can be prevented from forming a macro-step surface morphology, and therefore, a strong tensile strain will not be introduced into the prepared wafer. Preferably, the sputtering temperature range of the high-temperature magnetron sputtering method is 600°C to 800°C. The present invention can avoid the problem of poor crystal quality of the prepared AlN layer due to too low temperature by limiting the lower limit temperature of the high-temperature magnetron sputtering method.
[0046] In some embodiments, in step S10, the substrate is a sapphire substrate or a SiC substrate. Preferably, in step S10, the surface of the sapphire substrate or SiC substrate on which the AlN layer is grown has a c-plane (0001) with a bevel angle of α, wherein 0.2°<α≤1°, and the bevel direction is the c-axis deviating from the m-axis or the c-axis deviating from the a-axis. This is because when the bevel angle is too small, it is difficult for the AlN surface layer prepared on the patterned AlN layer to form the desired macro-step surface morphology. Figure 3 As shown in Figures (a) and (c), the larger the bevel angle, the more obvious the macrosteps. Even without considering the surface morphology, Figure 2 As shown in Figures (a) to (d), Figure 2 As shown in Figures (e) to (h) in Figure 1, the larger the bevel angle, the more obvious the macro step. Figure 2 As shown in Figure (c) (bevel angle of c-axis offset to m-axis 2°), Figure (d) (bevel angle of c-axis offset to m-axis 4°), Figure (g) (bevel angle of c-axis offset to a-axis 2°) and Figure (h) (bevel angle of c-axis offset to a-axis 4°), when the bevel angle is large (e.g., greater than 1°), as the bevel angle increases, the difficulty of closing the surface holes of the prepared AlN surface layer with macro-step surface morphology will increase. Preferably, a sapphire substrate with a bevel direction of c-axis offset to m-axis is selected to make the surface closing speed faster (e.g., Figure 2 Figure (b) and Figure 2 (as shown in Figure (f)).
[0047] In some embodiments, in step S10, the thickness of the AlN layer grown on the substrate is in the range of 100 to 600 nm. The present invention can control the thickness range of the AlN layer to avoid the problem that the hole depth of the subsequent patterned AlN is insufficient due to the thickness being too thin, and the hole cannot effectively prevent the AlN nucleation growth inside the hole, resulting in the AlN layer closing disorder and poor crystal quality; it can also avoid the problem that the AlN layer and the substrate have a large thermal mismatch due to the thickness being too thick, and the AlN layer has very poor crystal quality.
[0048] In other embodiments, in step S10, the difference from the previous embodiment is that the method for preparing the AlN layer is not a high-temperature magnetron sputtering method, but a MOCVD growth method. In order to ensure that the AlN layer without macro-step morphology can be prepared, the preparation temperature needs to be controlled at 1000°C to 1150°C, the molar ratio of nitrogen to aluminum needs to be controlled at 500 to 1500, and the preparation speed needs to be controlled at 1 μm / h to 5 μm / h.
[0049] In some embodiments, in step S20, when the first wafer is subjected to high-temperature thermal annealing, the surfaces of the AlN layers of the two first wafers are bonded together, the annealing temperature is 1600-1800°C, the annealing atmosphere is an inert gas or a nitrogen-containing gas, and the annealing time in the high-temperature section is 0-24 hours. Thus, atomic rearrangement can be achieved through high-temperature thermal annealing, the dislocation density in the AlN layer can be reduced, and a high-quality base layer can be provided for subsequent patterned AlN; moreover, the high-temperature thermal annealing can introduce a strong compressive strain in the AlN layer during the cooling process, which can compensate for the tensile strain generated during the subsequent patterned AlN closing process and the tensile strain generated by the large-angle substrate epitaxy, avoiding surface cracking due to excessive tensile strain and hillocks on the surface due to excessive compressive strain. Preferably, in step S20, the inert gas is helium, or the nitrogen-containing gas is nitrogen.
[0050] In some embodiments, in step S30, the AlN layer on the annealed wafer is patterned to prepare a patterned AlN layer having a hexagonal hole structure. Since AlN is a hexagonal symmetrical structure, the present invention prepares a patterned AlN layer having a hexagonal hole structure, which can ensure that the six faces of the hexagonal hole have the same closing speed during the closing process, and it is not easy to generate new dislocations, so that a flat surface is easily obtained. Preferably, the spacing between opposite sides of the hexagonal hole structure is 500 to 1000nm, the patterning period is 800 to 1500nm, the depth of the hexagonal hole structure is greater than 100nm, and the six faces inside the hexagonal hole correspond to the six a-faces or six m-faces of AlN respectively. The present invention controls the size of the hexagonal hole, which not only ensures that AlN has a thinner closing thickness, but also can effectively reduce the dislocation density; moreover, the present invention ensures the selective growth of AlN by limiting the hole depth.
[0051] In some embodiments, in step S40, epitaxial growth is performed on the upper surface of the patterned AlN layer at 1150-1350°C to prepare an AlN surface layer with a macro-step surface morphology. The present invention can avoid the weak surface migration ability of Al atoms due to too low temperature, the very slow closing of the AlN surface, the increased closing thickness, and the increased cost by controlling the temperature of epitaxial growth on the upper surface of the patterned AlN layer; it can also avoid the situation where the AlN lateral closing speed is too fast due to too high temperature, resulting in new dislocations and surface unevenness at the closing boundary, so that the hexagonal holes can be evenly closed to obtain a surface morphology with macro-steps and no holes. In some preferred embodiments, in order to ensure the rapid closing of the AlN layer and the stable maintenance of the macro-steps, the molar ratio of the N source to the Al source needs to be maintained between 250 and 1000. In some preferred embodiments, when the MOCVD method is used to prepare the AlN surface layer with a macro-step surface morphology, the N source is ammonia and the Al source is trimethylaluminum. In some preferred embodiments, in order to suppress the pre-reaction between the N source and the Al source, the growth pressure needs to be maintained at 30 mbar to 100 mbar.
[0052] In some embodiments, in step S50, the AlGaN structure layer prepared on the upper surface of the AlN surface layer is a composite structure layer of n-type AlGaN and AlGaN. The growth temperature is 1040-1100°C, the edge of the macro-step is on the non-polar surface, and the other positions of the macro-step terrace are polar surfaces. Due to the different migration and incorporation behaviors of Al atoms and Ga (gallium) atoms on polar and non-polar surfaces, AlGaN with a lower component will be formed on the edge of the macro-step, while AlGaN with a higher component will be formed on the macro-step terrace. If we use the conventional process for growing a quantum well structure, a quantum wire structure will be formed on the edge of the macro-step, while the macro-step terrace will maintain a quantum well structure. This can effectively enhance the quantum confinement effect and improve the radiation recombination efficiency. In some preferred embodiments, in order to ensure the stable maintenance of the macro-step on the AlGaN surface, the molar ratio of the N (nitrogen) source and the (Al+Ga) source needs to be maintained between 400 and 1500. In some preferred embodiments, when the AlGaN structure layer with a macro-step morphology on the surface is prepared by MOCVD, the Ga source is trimethylgallium, the N source is ammonia, and the Al source is trimethylaluminum. In some preferred embodiments, in order to suppress pre-reaction and high-pressure etching, the growth pressure is maintained between 70mbar and 200mbar. In some preferred embodiments, the difference in Al composition between the well and the barrier of the light-emitting layer in the AlGaN structure layer is greater than 10%, and the thickness of the well is 0.5nm to 1.5nm, which can significantly enhance the quantum confinement effect.
[0053] The method for preparing a high-efficiency deep ultraviolet light-emitting structure of the present invention will be exemplified below with reference to specific embodiments.
[0054] Embodiment 1
[0055] In the first step, c-plane (0001) sapphire is selected as the substrate, and the upper surface of the sapphire substrate is set to be inclined from the c-axis to the m-axis, and the inclination angle α is 1°.
[0056] The second step is to deposit an AlN layer on the upper surface of the sapphire substrate by using a high temperature magnetron technology, wherein the deposition thickness is controlled to be 100 nm and the sputtering temperature is controlled to be 650° C., so as to prepare an AlN layer without a macro-step surface morphology on the upper surface of the sapphire substrate, thereby forming a first wafer;
[0057] The third step is to place the first wafer into an annealing furnace for high-temperature thermal annealing. The surfaces of the AlN layers of every two first wafers are bonded together. The annealing temperature is 1600° C., the annealing atmosphere is helium, and the annealing time in the high-temperature section is 24 hours.
[0058] In the fourth step, a 200nm SiO2 (silicon dioxide) dielectric layer is deposited on the AlN layer, and then a layer of imprint glue is applied and dried; then, the pattern on the patterned template is transferred to the imprint glue; then, the imprint glue with the pattern is used as a mask, and the pattern is transferred to the SiO2 dielectric layer by RIE (Reactive Ion Etching) etching method; finally, the imprint glue is removed, and the SiO2 dielectric layer with the pattern is used as a new mask, and the AlN is etched into a pattern by RIE etching method, and the etching gas is oxygen ions and boron trichloride, so that the AlN layer forms a patterned AlN layer with a hexagonal hole structure, the opposite side spacing of the hexagonal hole structure is 500nm, the patterning period is 1500nm, the depth of the hexagonal hole structure is greater than 100nm, and the six faces inside the hexagonal hole correspond to the six a-faces of AlN respectively.
[0059] The fifth step is to place the sapphire substrate with the patterned AlN layer into the reaction chamber of the MOCVD equipment, and perform AlN epitaxy at a temperature of 1150°C, controlling the molar ratio of the N source to the Al source to be 250 and the growth pressure to be 30 mbar (millibars) to close the holes in the patterned AlN layer. Without considering the surface morphology, Figure 2 (b) shows the surface of AlN epitaxial growth obtained under the condition that the tilt angle of the sapphire substrate is 1.0°. Figure 2 Compared with the AlN epitaxial surface obtained under the condition of sapphire substrate tilt angle of 0.2° in Figure (a), it has obvious macro steps and no holes. Figure 3 As shown in Figure (c), when the c-axis is 4° off the m-axis, the internal quantum efficiency (IQE) of the deep ultraviolet light-emitting structure is as high as 68% (as shown in Figure 5). Figure 3 As shown in Figure (d), it is much higher than Figure 3 In (b), the internal quantum efficiency (IQE) of the deep ultraviolet light-emitting structure obtained when the tilt angle of the sapphire substrate is 0.2° is 45%. It can be seen that without considering the surface morphology, the larger the tilt angle, the more obvious the macro-steps, and the greater the luminous efficiency.
[0060] In the sixth step, the molar ratio of the N source and the (Al+Ga) source is controlled to be 400, the growth pressure is 70 mbar, and n-type AlGaN and AlGaN are prepared at a temperature of 1040°C to form an AlGaN structural layer. The Al composition difference of the well and barrier of the light-emitting layer in the AlGaN structural layer is controlled to be >10%, and the thickness of the well is 0.5 nm.
[0061] Embodiment 2
[0062] The difference from the first embodiment is that:
[0063] In the first step, c-plane (0001) SiC is selected as the substrate, and the upper surface of the SiC substrate is set to be inclined from the c-axis to the m-axis, and the inclination angle α is 0.8°.
[0064] In the fourth step, the dielectric layer is SiNx (silicon nitride).
[0065] The surface of the AlN epitaxial layer obtained by this embodiment has obvious macro-steps and no holes.
[0066] Embodiment 3
[0067] The difference between this embodiment and the first embodiment is that:
[0068] In the first step, c-plane (0001) sapphire is selected as the substrate, and the upper surface of the sapphire substrate is set to be inclined from the c-axis to the m-axis, and the inclination angle α is 0.5°.
[0069] The surface of the AlN epitaxial layer obtained by this embodiment has obvious macro-steps and no holes.
[0070] Embodiment 4
[0071] The difference between this embodiment and the third embodiment is that:
[0072] In the first step, c-plane (0001) sapphire is selected as the substrate, and the upper surface of the sapphire substrate is set to be inclined from the c-axis to the a-axis, and the inclination angle α is 0.8°.
[0073] The surface of the AlN epitaxial layer obtained by this embodiment has obvious macro-steps and no holes.
[0074] Embodiment 5
[0075] The difference between this embodiment and the third embodiment is that:
[0076] In the first step, c-plane (0001) sapphire is selected as the substrate, and the upper surface of the sapphire substrate is set to be inclined from the c-axis to the a-axis, and the inclination angle α is 0.9°.
[0077] The second step is to deposit an AlN layer on the upper surface of the sapphire substrate by using a high temperature magnetron technology, wherein the deposition thickness is controlled to be 600 nm and the sputtering temperature is controlled to be 800° C., so as to prepare an AlN layer without a macro-step surface morphology on the upper surface of the sapphire substrate, thereby forming a first wafer;
[0078] The third step is to place the first wafer into an annealing furnace for high-temperature thermal annealing. The surfaces of the AlN layers of every two first wafers are bonded together. The annealing temperature is 1800° C., the annealing atmosphere is nitrogen, and the annealing time in the high-temperature section is 10 hours.
[0079] In the fourth step, a 200nm SiO2 dielectric layer is deposited on the AlN layer, and then a layer of imprint glue is applied and dried; then, the pattern on the patterned template is transferred to the imprint glue; then, the imprint glue with the pattern is used as a mask, and the pattern is transferred to the SiO2 dielectric layer by RIE etching method; finally, the imprint glue is removed, and the SiO2 dielectric layer with the pattern is used as a new mask, and the AlN is etched out of the pattern by RIE etching method, and the etching gas is oxygen ions and boron trichloride, so that the AlN layer forms a patterned AlN layer with a hexagonal hole structure, the opposite side spacing of the hexagonal hole structure is 1000nm, the patterning period is 800nm, the depth of the hexagonal hole structure is greater than 100nm, and the six faces inside the hexagonal hole correspond to the six m-faces of AlN respectively.
[0080] In the fifth step, the sapphire substrate with the patterned AlN layer thereon is placed into the reaction chamber of the MOCVD equipment, and AlN epitaxy is performed at a temperature of 1350°C, the molar ratio of the N source and the Al source is controlled to be 1000, and the growth pressure is 100 mbar, so that the holes of the patterned AlN layer are closed.
[0081] The sixth step is to control the molar ratio of the N source and the (Al+Ga) source to 1500, the growth pressure to 200 mbar, prepare n-type AlGaN and AlGaN at a temperature of 1100°C to form an AlGaN structural layer, and control the Al composition difference of the well and barrier of the light-emitting layer in the AlGaN structural layer to be >10%, and the thickness of the well to be 1.5 nm.
[0082] The surface of the AlN epitaxial layer obtained by this embodiment has obvious macro-steps and no holes.
[0083] Embodiment 6
[0084] The difference between this embodiment and the third embodiment is that:
[0085] In the first step, c-plane (0001) sapphire is selected as the substrate, and the upper surface of the sapphire substrate is set to be inclined from the c-axis to the a-axis, and the inclination angle α is 1°.
[0086] The surface of the AlN epitaxial layer obtained by this embodiment has obvious macro-steps and no holes.
[0087] Embodiment 7
[0088] The difference between this embodiment and the first embodiment is that:
[0089] In the second step, an AlN layer is grown on the upper surface of the sapphire substrate by an MOCVD growth method. The growth process controls the deposition thickness to be 100 nm, the growth temperature to be 1000°C, the molar ratio of nitrogen to aluminum to be 500, and the growth rate to be 1 μm / h, so as to prepare an AlN layer without a macro-step surface morphology on the upper surface of the sapphire substrate to form a first wafer.
[0090] Embodiment 8
[0091] The difference between this embodiment and the first embodiment is that:
[0092] In the second step, an AlN layer is grown on the upper surface of the sapphire substrate by an MOCVD growth method. The growth process controls the deposition thickness to be 600 nm, the growth temperature to be 1150°C, the molar ratio of nitrogen to aluminum to be 1500, and the growth rate to be 5 μm / h, so as to prepare an AlN layer without a macro-step surface morphology on the upper surface of the sapphire substrate to form a first wafer.
[0093] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a high-efficiency deep ultraviolet light-emitting structure, characterized in that: The following steps are involved: S10: preparing an AlN layer on a substrate having a certain bevel angle, and controlling the surface of the AlN layer not to form a macro-step surface morphology, so as to obtain a first wafer; S20: performing high temperature thermal annealing on the first wafer to obtain an annealed wafer; S30: performing a patterning process on the AlN layer on the annealed wafer to form a patterned AlN layer; S40: performing epitaxial growth on the upper surface of the patterned AlN layer to prepare an AlN surface layer having a macro-step surface morphology; S50: preparing an AlGaN structural layer on the upper surface of the AlN surface layer, and ensuring that the surface of the AlGaN structural layer has a macro-step morphology.
2. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 1, characterized in that: In step S10, the AlN layer is prepared on a substrate having a certain off-cut angle by a high temperature magnetron sputtering method or a MOCVD growth method.
3. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 2, characterized in that: The thickness of the AlN layer is in the range of 100 nm to 600 nm; and / or The sputtering temperature range of the high-temperature magnetron sputtering method is 600°C to 800°C; or the preparation temperature of the MOCVD growth method is 1000°C to 1150°C, the N / Al molar ratio is 500 to 1500, and the preparation speed is 1 μm / h to 5 μm / h.
4. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 1, characterized in that: In step S10, the substrate is a sapphire substrate or a SiC substrate.
5. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 4, characterized in that: In step S10, the surface of the sapphire substrate or SiC substrate on which the AlN layer is grown has a c-plane (0001) with a bevel angle of α, wherein 0.2°<α≤1°, and the bevel direction is c-axis offset from m-axis or c-axis offset from a-axis.
6. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 1, characterized in that: In step S20, when the first wafer is subjected to high-temperature thermal annealing, the surfaces of the AlN layers of the two first wafers are bonded together, the annealing temperature is 1600°C to 1800°C, the annealing atmosphere is an inert gas or a nitrogen-containing gas, and the annealing time in the high-temperature section is 0h to 24h.
7. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 6, characterized in that: In step S20, the inert gas is helium, or the nitrogen-containing gas is nitrogen.
8. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 1, characterized in that: In step S30 , the AlN layer on the annealed wafer is patterned to prepare a patterned AlN layer having a hexagonal hole structure.
9. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 8, characterized in that: The hexagonal hole structure has an opposite side spacing of 500nm to 1000nm, a patterning period of 800nm to 1500nm, a depth of the hexagonal hole structure greater than 100nm, and six faces inside the hexagonal hole correspond to six a faces or six m faces of AlN respectively.
10. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to claim 8, characterized in that: In step S40, epitaxial growth is performed on the upper surface of the patterned AlN layer at 1150° C. to 1350° C. to prepare an AlN surface layer having a macro-step surface morphology.
11. The method for preparing a high-efficiency deep ultraviolet light-emitting structure according to any one of claims 1 to 10, characterized in that: The AlGaN structure layer is a composite structure layer of n-type AlGaN and AlGaN.