Preparation method and application of zinc negative electrode protection layer with hydrophilic-hydrophobic alternated structure

By depositing a block copolymer protective layer with a interfacial structure on the zinc negative electrode, the problems of zinc dendrites and side reactions in zinc ion batteries are solved, and the uniform deposition of zinc ions and high cycle life is achieved, which significantly improves the stability of the battery. Sex and safety.

CN118969946APending Publication Date: 2024-11-15TIANJIN UNIV OF SCI & TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411023162.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing aqueous zinc ion batteries tend to be dendritic and uneven due to the electrodeposition of zinc ions, which easily cause zinc dendrites to pierce the separator, causing the battery to fail short circuit. The aqueous electrolyte is prone to side reactions in the negative electrode of zinc, which has safety hazards and leads to circulation. Poor performance.

Method used

The block copolymer with a mutually friendly and alienated structure is used as the zinc negative electrode protective layer. The polyetheramide block copolymer is dissolved in ethanol/water to prepare a cast film liquid, and is uniformly deposited on the zinc surface. The hydrophobic polyamide segments are used to inhibit hydrogen evolution. Reaction and zinc dendrites growth, hydrophilic polyoxyethylene segments promote uniform deposition and rapid migration of zinc ions.

Benefits of technology

Achieve uniform deposition and high cycle life of zinc ions and ultra-long cycle performance. The cycle life of zinc ion batteries reaches more than 1300 hours under high current density, far exceeding the 2 hours of bare zinc plates, significantly improving the stability and safety of the battery sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969946A_ABST
    Figure CN118969946A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of new energy, and particularly relates to a preparation method and application of a zinc negative electrode protection layer with a hydrophilic-hydrophobic alternate structure. The preparation method comprises the following steps: dissolving a block copolymer with a hydrophilic-hydrophobic interphase structure in ethanol / water to form a membrane casting solution, and uniformly coating the surface of zinc with the prepared membrane casting solution to obtain a zinc plate with a hydrophilic-hydrophobic interphase block copolymer protective layer; the hydrophilic-hydrophobic segmented copolymer is commercial polyether amide, and has a hydrophilic polyoxyethylene chain segment and a relatively hydrophobic polyamide chain segment. Hydrated zinc ions are desolvated by utilizing strong electronegativity of amido bonds in polyamide chain segments, and high mechanical strength is shown; a polyoxyethylene flexible chain segment is used for conducting zinc ions and has good interface compatibility with the zinc surface; therefore, the interface side reaction and zinc dendrite growth are effectively inhibited, the zinc ion concentration is homogenized, and the zinc ion migration kinetics is improved; the obtained modified zinc negative electrode is used for an aqueous zinc ion battery, and has super-long cycle stability and good capacity retention rate under high current.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of new energy technology, and in particular relates to a method for preparing a zinc negative electrode protective layer with an alternating affinity and repellency structure and an application thereof. Background Art

[0002] Solar energy, wind energy, tidal energy and other new energy generation technologies are considered to be ideal substitutes for thermal power generation due to their advantages of being pollution-free and renewable. However, these new energy generation technologies have the disadvantage of poor stability and need to be used with large-scale energy storage devices. However, commercial lithium metal batteries cannot meet the requirements of large-scale energy storage due to their high cost and poor safety. Therefore, the development of a new generation of secondary energy storage devices suitable for large-scale energy storage equipment is of great significance and value to the new energy power generation industry and is a major demand for national development.

[0003] Similar to lithium metal batteries, aqueous zinc ion batteries use zinc metal as the negative electrode and materials such as MnO2 and V2O5 as the positive electrode. Thanks to the high hydrogen evolution overpotential of the zinc negative electrode (–0.76Vvs.SHE), zinc ion batteries can directly use aqueous solutions as electrolytes, which greatly improves the safety of zinc ion batteries. In addition, zinc metal negative electrodes have advantages that lithium metal negative electrodes cannot match, such as: high abundance of zinc resources in the earth's crust, low difficulty in zinc mining, low storage cost, and the production of aqueous zinc ion batteries does not rely on a highly anhydrous and oxygen-free environment. These advantages make aqueous zinc ion batteries far superior to lithium ion batteries in terms of production cost and safety. However, there are many problems in the direct use of zinc metal negative electrodes, which hinder their large-scale application: 1) The electrodeposition of zinc ions in the battery tends to be dendritic and uneven, and zinc dendrites are prone to pierce the diaphragm, causing the battery to short-circuit and fail; 2) Aqueous electrolytes are prone to side reactions at the zinc negative electrode, producing hydrogen, which causes safety hazards to the battery. Therefore, the existing technology needs to be further improved. Summary of the invention

[0004] In view of the above-mentioned deficiencies of the prior art, the present invention provides a method for preparing a zinc negative electrode protective layer with an affinity-dispersion alternating structure and its application, and assembles an aqueous zinc ion battery with a zinc negative electrode coated with the affinity-dispersion alternating structure, so as to solve the problem of poor cycle performance of existing aqueous zinc ion batteries.

[0005] The primary purpose of the present invention is to provide a method for preparing a zinc negative electrode coated with a hydrophilic-phobic phase structure, comprising the following steps: dissolving a hydrophilic-phobic phase block copolymer in ethanol / water to prepare a casting solution, and using a coating method to uniformly deposit the hydrophilic-phobic phase block copolymer on the zinc surface; the hydrophilic-phobic phase block copolymer is a polyetheramide block copolymer.

[0006] The second object of the present invention is to provide a block copolymer having a hydrophilic-hydrophobic phase structure, which is any one of a polyamide 6-polyoxyethylene block copolymer, a polyamide 11-polyoxyethylene block copolymer and a polyamide 12-polyoxyethylene block copolymer.

[0007] The third object of the present invention is to provide a method for preparing the zinc negative electrode protective layer with the hydrophilic-hydrophobic phase structure.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A method for preparing a zinc negative electrode protective layer of a hydrophilic-hydrophobic block copolymer comprises the following steps:

[0010] S1: adding the polyether amide block copolymer into a mixed solvent of anhydrous ethanol and deionized water to obtain a mixed solution;

[0011] S2: dissolving the mixed solution obtained in step S1 under heating and stirring conditions to obtain a polyether amide block copolymer casting solution.

[0012] As a preferred technical solution of the present invention, the molar ratio of anhydrous ethanol to deionized water in the mixed solvent in step S1 is 1:3 to 3:1.

[0013] Preferably, the reaction temperature in step S2 is 50° C.-100° C., and the reaction time is 2-12 hours.

[0014] Preferably, the mass percentage of the polyether amide block copolymer in step S2 is 1-15%.

[0015] The fourth object of the present invention is to provide a zinc negative electrode coated with a hydrophilic-hydrophobic phase structure obtained by the above preparation method.

[0016] Preferably, the coating method is any one of drop coating, spin coating and spray coating, and the solid content of the polymer deposited on the zinc surface is 0.5-5 mg·cm -2 .

[0017] The present invention also provides an aqueous zinc ion battery, comprising the zinc negative electrode coated with the hydrophilic-hydrophobic alternating structure as described above.

[0018] The present invention uses hydrophilic polyoxyethylene and relatively hydrophobic polyamide block copolymer as the zinc negative electrode protective layer. The amide bond in the relatively hydrophobic polyamide in the affinity-repellent interphase structure has strong electronegativity, strong binding energy with zinc ions, and can participate in the desolvation process of hydrated zinc ions. In addition, its hydrophobic structure can inhibit hydrogen evolution reaction and reduce the side reaction of the zinc negative electrode. The polyamide structure has high strength and can inhibit zinc dendrites. The hydrophilic polyoxyethylene segment in the affinity-repellent interphase structure has flexibility, which can realize the rapid migration of zinc ions after desolvation and improve the ion migration kinetics. The flexible structure can even the zinc ion flow rate and help the uniform deposition of zinc ions. By selecting the polyamide block copolymer, the mechanical strength and hydrophobic characteristics can also be improved, thereby meeting the requirements of different electrolyte systems and current densities.

[0019] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:

[0020] The present invention adopts a block copolymer with a hydrophilic-hydrophobic structure as the protective layer of the zinc negative electrode. The hydrophilic-hydrophobic structure of the protective layer has the functions of desolvation, promoting the migration kinetics of zinc ions and guiding the uniform deposition of zinc ions. The modified electrode has a high current density (10mA / cm 2 、10mAh / cm 2 ) achieved an ultra-high cycle life of more than 1300 hours in the symmetric battery cycle performance test, which is much longer than the cycle life of the current direct use of bare zinc plate as the negative electrode of aqueous zinc-ion batteries under high current density (symmetric battery test life <2 hours). So far, there has been no research report on the use of block copolymers with an interphilic and interphasic structure for zinc negative electrodes in aqueous zinc-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A digital picture of a zinc negative electrode coated with a protective layer of an interphasic structure prepared in Example 1 of the present invention;

[0022] Figure 2 This is a scanning electron microscope image of the surface of the zinc negative electrode coated with a protective layer having an affinity-repellency alternating structure prepared in Example 1 of the present invention;

[0023] Figure 3 This is an electron microscopic image of a cross-section of a zinc negative electrode coated with a protective layer having an affinity-repellency alternating structure prepared in Example 1 of the present invention;

[0024] Figure 4 This is an electron microscope image of the surface of the bare zinc negative electrode prepared in Comparative Example 4 of the present invention;

[0025] Figure 5 This is a scanning electron microscope image of the surface of the zinc negative electrode coated with a protective layer of an interphilic and interrephic structure prepared in Example 2 of the present invention;

[0026] Figure 6This is a scanning electron microscope image of the zinc negative electrode coated with a protective layer of an interphilic and interrepellent structure prepared in Example 2 of the present invention after ion beam sputtering;

[0027] Figure 7 This is a scanning electron microscope image of the bare zinc negative electrode prepared in Comparative Example 4 of the present invention after ion beam sputtering;

[0028] Figure 8 The cycle performance test diagram of the Zn-Zn symmetric battery prepared in Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention;

[0029] Fig. 9 This is a charge and discharge cycle test diagram of the Zn-V2O5 full battery prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] In the examples of the present invention, if the specific conditions are not specified, the preparation is carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are conventional products that can be purchased commercially.

[0032] In this embodiment, the zinc negative electrode refers to the negative electrode used for an aqueous zinc ion battery, which is an important component of an aqueous zinc ion rechargeable battery. During the discharge process, the negative electrode is oxidized due to the loss of electrons, thereby generating electrons in the external circuit, and the positive electrode material is reduced and consumes electrons. Electrons flow through the external circuit as current. The block copolymer of the inter-philic and inter-dispersive structure refers to a rubber block copolymer with polyamide (PA) as a relatively hydrophobic chain and aliphatic polyether as a hydrophilic chain. In this block copolymer, the hard segment has a large crystallinity and a high melting point, and the compatibility of the relatively hydrophobic / hard segment and the soft segment is very low, which helps to maintain the integrity of the hard segment micro-region at high temperature and can effectively increase the upper limit of the use temperature of the thermoplastic elastomer. The hydrophilic / soft segment gives the polymer softness and extensibility, while the glassy or semi-crystalline hard segment micro-region plays the role of a cross-linking point to prevent the polymer molecular chain from slipping and sticking. By changing the type and length of the soft segment and the hard segment and the proportion of the two segments, a series of polymers with different hardness can be obtained to meet the performance requirements of different fields. It should be noted that the polyetheramide block copolymer used in this embodiment can be a commercial polyetheramide block copolymer.

[0033] In the embodiment, the ethylene oxide groups in the polyetheramide block copolymer are coupled with zinc ions, and the thermal motion of the polyoxyethylene segments is used to conduct zinc ions, and the polyamide segments have high mechanical strength, which can effectively inhibit the growth of zinc dendrites and improve the cycle stability. It should be noted that the block copolymers with different affinity and repellency in this embodiment are directly deposited on the zinc plate by coating, which has the advantages of high efficiency and environmental protection, and is particularly suitable for large-scale preparation.

[0034] Example 1

[0035] The method comprises dissolving a commercial polyether amide block copolymer (PA6 / PEO) in ethanol / water to form a 5-10 wt % casting solution; uniformly coating the casting solution on a circular zinc plate with a diameter of 15 mm, and forming a film on the zinc plate by a solvent evaporation phase conversion method to obtain a zinc negative electrode (10) coated with a protective layer of an interphilic and interphilic structure. The digital photograph of the zinc negative electrode coated with the protective layer of an interphilic and interphilic structure is shown in FIG. Figure 1 The surface scanning electron microscopy image of the zinc negative electrode coated with the inter-philic and inter-repellent structure protective layer is shown in Figure 2 As shown in the figure, the cross-sectional scanning electron microscopy image of the zinc negative electrode coated with the protective layer of the interfacial structure is as follows Figure 3 shown.

[0036] Example 2

[0037] The preparation method is consistent with Example 1.

[0038] The prepared zinc negative electrode coated with the polyether amide block copolymer protective film was assembled into a Zn-Zn symmetric battery using a 2032 battery shell:

[0039] The Zn-Zn symmetric battery assembly process is as follows: negative electrode shell, spring, gasket, zinc negative electrode coated with a protective layer of an interfacial structure, glass fiber separator, zinc negative electrode coated with a protective layer of an interfacial structure, and positive electrode shell. At 25°C, 1 mA / cm 2 (1mAh / cm 2 ) conditions to test the performance of the protective film. After 60 hours of cycling, the surface of the zinc negative electrode coated with the protective layer of the interfacial and hydrophobic structure is shown in the scanning electron microscope image. Figure 4 The scanning electron microscope image after ion beam sputtering is shown in Figure 6 shown.

[0040] Example 3

[0041] The preparation method is consistent with that in Example 1. The prepared zinc negative electrode coated with the hydrophilic-hydrophobic interphase structure protective layer is assembled into a Zn-Zn symmetric battery and a Zn-V2O5 full battery using a 2032 battery shell:

[0042] The Zn-Zn symmetric battery assembly process is as follows: negative electrode shell, spring, gasket, zinc negative electrode coated with a protective layer of an interfacial structure, glass fiber separator, zinc negative electrode coated with a protective layer of an interfacial structure, and positive electrode shell. 2 (10mAh / cm 2 ) conditions, the cycle performance was tested. After 1300 hours of cycling, the symmetrical battery remained stable. The results are as follows Figure 8 shown.

[0043] The Zn-V2O5 full battery assembly process is as follows: negative electrode shell, spring, gasket, zinc negative electrode coated with a protective layer of inter-philic structure, glass fiber separator, V2O5 (active material loading is 0.68 mg / cm 2 ), positive electrode shell; at 25 ° C, the cycle performance test was carried out, and the current density was set to 3A / g. The results are as follows Fig. 9 As shown;

[0044] Comparative Example 1

[0045] A commercial polyamide polymer (PA6) is dissolved in anhydrous acetonitrile to form a casting solution, and the casting solution is evenly coated on a circular zinc plate with a diameter of 15 mm. After the acetonitrile is completely evaporated, a zinc negative electrode (20) coated with a polyetheramide polymer protective film is obtained.

[0046] The prepared zinc negative electrode coated with polyamide polymer protective film was assembled into a Zn-Zn symmetrical battery using a 2032 battery shell. 2 (10mAh / cm 2 ) conditions, the battery short-circuited after 16 hours of cycling. Figure 8 shown.

[0047] Comparative Example 2

[0048] In a glove box (O2≤0.01ppm; H2O≤0.01ppm), polyoxyethylene (PEO, molecular weight 300,000) is dissolved in anhydrous acetonitrile to obtain a casting solution, and the casting solution is evenly coated on a circular zinc plate with a diameter of 15mm. After the acetonitrile is evaporated, a zinc negative electrode (30) coated with polyoxyethylene polymer for protection is obtained.

[0049] The prepared polyoxyethylene polymer protected zinc anode was assembled into a Zn-Zn symmetrical battery using a 2032 battery shell. 2 (10mAh / cm 2 ) conditions, the battery short-circuited after 365 hours of cycling. Figure 8 shown.

[0050] Comparative Example 3

[0051] A 15 mm round zinc plate was directly used as the electrode (40) and assembled into a Zn-Zn symmetrical battery using a 2032 battery shell. 2 (10mAh / cm 2 ) conditions, the battery short-circuited after 2 hours of cycling. Figure 8 shown.

[0052] Comparative Example 4

[0053] The preparation process is the same as that of Comparative Example 3, and the test conditions are changed to: 25°C, 1 mA / cm 2 (1mAh / cm 2 ) condition, after 60 hours of circulation, the surface scanning electron microscope image of the zinc plate is as follows Figure 4 The scanning electron microscope image after ion beam sputtering is shown in Figure 7 shown.

[0054] In summary, the present invention provides a film casting liquid with a hydrophilic-dispersive interphase structure and a preparation method thereof, a method for preparing a zinc negative electrode coated with a hydrophilic-dispersive interphase structure, and an aqueous zinc ion battery assembled with the same. The hydrophobic polyamide segment in the polyetheramide block copolymer can inhibit the hydrogen evolution reaction, and the carbonyl group has a strong affinity for zinc ions, so as to achieve desolvation of zinc ions. In addition, the polyamide has high mechanical strength and can effectively inhibit the growth of zinc dendrites. The oxyethylene group couples with zinc ions, and the flexible segment of the polyoxyethylene segment is used to conduct zinc ions, strengthen the ion migration kinetics, regulate the zinc ion deposition behavior, and achieve no dendrite growth. The zinc negative electrode coated with the hydrophilic-dispersive interphase structure is used in an aqueous zinc ion battery to improve the cycle stability of the battery.

[0055] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

Claims

1. A method for preparing a zinc negative electrode coated with an affinitive and aphrodisiac alternating structure, characterized in that: The following steps are involved: The hydrophilic-phobic phase block copolymer is dissolved in ethanol / water to prepare a casting solution, and the hydrophilic-phobic phase block copolymer is uniformly deposited on the zinc surface by a coating method; The hydrophilic and hydrophobic block copolymer is a polyetheramide block copolymer.

2. The polyether amide block copolymer according to claim 1 is any one of polyamide 6-polyethylene oxide block copolymer, polyamide 11-polyethylene oxide block copolymer and polyamide 12-polyethylene oxide block copolymer.

3. A method for preparing the zinc negative electrode protective layer of the hydrophilic and hydrophobic interphase block copolymer according to claim 1, characterized in that: The following steps are involved: S1: adding the polyether amide block copolymer into a mixed solvent of anhydrous ethanol and deionized water to obtain a mixed solution; S2: dissolving the mixed solution obtained in step S1 under heating and stirring conditions to obtain a polyether amide block copolymer casting solution.

4. The method for preparing the hydrophilic-hydrophobic phase block copolymer zinc negative electrode protective film according to claim 3, characterized in that: The molar ratio of anhydrous ethanol to deionized water in the mixed solvent of step S1 is 1:3 to 3:

1.

5. The method for preparing the hydrophilic-hydrophobic phase block copolymer zinc negative electrode protective film according to claim 3, characterized in that: The reaction temperature in step S2 is 50°C-100°C, and the reaction time is 2-12 hours.

6. The method for preparing the hydrophilic-hydrophobic phase block copolymer zinc negative electrode protective film according to claim 3, characterized in that: The mass percentage of the polyether amide block copolymer in step S2 is 1-15%.

7. The method for preparing a zinc negative electrode coated with a hydrophilic-hydrophobic alternating structure according to claim 1, characterized in that: The coating method is any one of a drop coating method, a spin coating method and a spray coating method.

8. The method for preparing a zinc negative electrode coated with a hydrophilic alternating structure according to claim 1, characterized in that: The solid content of the polymer deposited on the zinc surface is 0.5-5 mg cm -2 .

9. The zinc negative electrode coated with a hydrophilic-hydrophobic alternating structure prepared by the method of claim 1.

10. An aqueous zinc ion battery, characterized in that: It includes the zinc negative electrode coated with the hydrophilic-hydrophobic phase structure as described in claim 9.

Citation Information

Cited By

  • Zinc negative electrode protective film constructed by in-situ inorganic hybrid polymer and preparation method and application thereof

    CN119993971A

  • A zinc anode protective film constructed by in-situ inorganic hybrid polymer, its preparation method and application

    CN119993971B

  • Hydrophobic-zinc-philic interface protection layer of high-magnification zinc metal negative electrode as well as preparation and application of hydrophobic-zinc-philic interface protection layer

    CN120388990A