Negative electrode for electricity storage device, and electricity storage device

By forming a multilayer structure on the negative electrode of a lithium-ion secondary battery and utilizing a layered design with different polymer compositions, the problem of insufficient adhesion caused by volume changes in silicon materials was solved, thereby improving electrode durability and battery performance.

CN118969952APending Publication Date: 2024-11-15ENEOS MATERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410587425.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-05-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In existing lithium-ion secondary battery anodes, silicon materials with high lithium-ion absorption capacity have large volume changes, resulting in insufficient sealing. During repeated charging and discharging, the active material falls off, affecting the electrode's durability and battery performance.

Method used

By forming a multilayer structure containing different polymers on the negative electrode current collector, the first layer contains 5-20% of unsaturated carboxylic acid repeating units (A) and the second layer contains 0.1-5% of unsaturated carboxylic acid repeating units (B), the adhesion between the negative electrode current collector and the active material and the adhesion between the active materials are improved, the electrode expansion is suppressed and the internal resistance is reduced.

Benefits of technology

It effectively suppressed electrode expansion, improved the adhesion of the negative electrode and the cycle characteristics of the electrode, and enhanced the battery capacity and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969952A_ABST
    Figure CN118969952A_ABST
Patent Text Reader

Abstract

Provided is a negative electrode for a power storage device, which is capable of effectively suppressing electrode expansion and reducing the internal resistance of the electrode by improving the adhesive force between a negative electrode current collector and a negative electrode mixture layer and the adhesive force between active materials. A negative electrode for a power storage device according to the present invention is provided with a negative electrode current collector and a negative electrode mixture layer formed on the negative electrode current collector, the negative electrode mixture layer including a first layer formed on the negative electrode current collector and a second layer formed on the first layer, the first layer including a first negative electrode active material and a polymer (A), and the second layer including a second negative electrode active material and a polymer (B). The first layer contains a first negative electrode active material and a polymer (B), the polymer (A) contains 5-20% by mass of a repeating unit (a1) derived from an unsaturated carboxylic acid when the total of the repeating units contained in the polymer (A) is 100% by mass, the second layer contains a second negative electrode active material and the polymer (B), and the third layer contains 5-20% by mass of a repeating unit (a2) derived from an unsaturated carboxylic acid when the total of the repeating units contained in the polymer (B) is 100% by mass. The polymer (B) contains 0.1 mass% or more but less than 5 mass% of a repeating unit (a1) derived from an unsaturated carboxylic acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative electrode for an electricity storage device and an electricity storage device including the negative electrode. Background Art

[0002] As technology related to mobile devices develops and demands increase, the demand for secondary batteries as energy sources is rapidly increasing. Among such secondary batteries, lithium ion secondary batteries having high energy density and voltage have been commercialized.

[0003] In order to overcome various problems of lithium ion secondary batteries, research has been conducted on technologies for forming electrodes used in lithium ion secondary batteries into multiple layers so that each layer has different physical properties (for example, see Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-5461 Summary of the invention

[0007] In the existing negative electrodes for power storage devices, new active materials represented by silicon materials with large lithium ion storage capacity and large volume changes accompanying lithium ion storage and release have been put into practical use, but the adhesion is still insufficient. Such negative electrodes for power storage devices may cause the negative electrode active material to fall off due to repeated charge and discharge, thereby causing electrode degradation, and therefore there is a problem that the durability required for practical use cannot be fully obtained.

[0008] Several aspects of the present invention provide a negative electrode for a power storage device, which can effectively suppress electrode expansion and reduce the internal resistance of the electrode by improving the bonding strength between the negative electrode collector and the negative electrode composite layer and the bonding strength between the active materials. In addition, several aspects of the present invention provide a power storage device having improved capacity and cycle characteristics by including the negative electrode for a power storage device.

[0009] The present invention has been made to solve at least a part of the above-mentioned problems, and can be implemented as any of the following aspects.

[0010] One embodiment of the negative electrode for an electric storage device according to the present invention comprises a negative electrode current collector and a negative electrode composite material layer formed on the negative electrode current collector, wherein:

[0011] The negative electrode composite layer includes a first layer formed on the negative electrode current collector and a second layer formed on the first layer.

[0012] The first layer comprises a first negative electrode active material and a polymer (A),

[0013] The polymer (A) contains 5 to 20% by mass of the repeating unit (a1) derived from an unsaturated carboxylic acid, when the total amount of the repeating units contained in the polymer (A) is 100% by mass.

[0014] The second layer comprises a second negative electrode active material and a polymer (B),

[0015] The polymer (B) contains 0.1% by mass or more and less than 5% by mass of the repeating unit (a1) derived from an unsaturated carboxylic acid, when the total of the repeating units contained in the polymer (B) is 100% by mass.

[0016] In one embodiment of the negative electrode for the power storage device,

[0017] When the total amount of the repeating units contained in the polymer (A) is 100% by mass, the polymer (A) may contain 1% by mass or more and less than 20% by mass of the repeating units (a3) ​​derived from an aromatic vinyl compound.

[0018] The polymer (B) may contain 20% by mass or more and less than 40% by mass of the repeating unit (a3) ​​derived from an aromatic vinyl compound, when the total of the repeating units contained in the polymer (B) is 100% by mass.

[0019] In any of the above-mentioned aspects of the negative electrode for an electricity storage device,

[0020] The polymer (A) may contain 15 to 60% by mass of the repeating unit (a2) derived from a conjugated diene compound, when the total amount of the repeating units contained in the polymer (A) is 100% by mass.

[0021] The polymer (B) may contain 15 to 60% by mass of the repeating unit (a2) derived from a conjugated diene compound, when the total of the repeating units contained in the polymer (B) is 100% by mass.

[0022] In any of the above-mentioned aspects of the negative electrode for an electricity storage device,

[0023] The polymer (A) may contain 1 to 20% by mass of the repeating unit (a4) derived from an unsaturated carboxylic acid ester, when the total amount of the repeating units contained in the polymer (A) is 100% by mass.

[0024] The polymer (B) may contain 1 to 20% by mass of the repeating unit (a4) derived from an unsaturated carboxylic acid ester, when the total of the repeating units contained in the polymer (B) is 100% by mass.

[0025] In any of the above-mentioned aspects of the negative electrode for an electricity storage device,

[0026] The polymer (A) may contain 5 to 40% by mass of the repeating unit (a5) derived from an α,β-unsaturated nitrile compound, when the total amount of the repeating units contained in the polymer (A) is 100% by mass.

[0027] The polymer (B) may contain 5 to 40% by mass of the repeating unit (a5) derived from the α,β-unsaturated nitrile compound, when the total of the repeating units contained in the polymer (B) is 100% by mass.

[0028] In any of the above-mentioned aspects of the negative electrode for an electricity storage device,

[0029] The polymer (A) and the polymer (B) are particles,

[0030] The number average particle size of the particles of the polymer (A) may be 150 nm to 300 nm.

[0031] The number average particle size of the particles of the polymer (B) may be 50 nm or more and less than 150 nm.

[0032] One aspect of an electric storage device according to the present invention includes the negative electrode for an electric storage device according to any of the above aspects.

[0033] According to the negative electrode for the power storage device involved in the present invention, the leveling property in the negative electrode composite layer is improved, so that the bonding force between the negative electrode collector and the negative electrode composite layer is improved, and the electrode expansion can be effectively suppressed, and the internal resistance of the electrode can be reduced because the bonding force between the active materials is improved. As a result, the capacity and cycle characteristics of the power storage device can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a cross-sectional view schematically showing the structure of a negative electrode for an electric storage device according to one embodiment of the present invention.

[0035] Explanation of symbols

[0036] 10···Negative electrode current collector, 20···Negative electrode composite material layer, 20a···First layer, 20b···Second layer, 100···Negative electrode for power storage device DETAILED DESCRIPTION

[0037] Hereinafter, preferred embodiments of the present invention will be described in detail. It should be noted that the present invention is not limited to the embodiments described below, and it should be understood that various modifications implemented within the scope of the present invention are also included.

[0038] In the present specification, "(meth)acrylic acid-" means "acrylic acid-" or "methacrylic acid-", and "-(meth)acrylate" means "-acrylate" or "-methacrylate".

[0039] In the present specification, a numerical range described in the format of "X to Y" can be interpreted as including the numerical value X as a lower limit and including the numerical value Y as an upper limit.

[0040] 1. Negative electrode for power storage device

[0041] Figure 1 1 is a cross-sectional view schematically showing the structure of a negative electrode 100 for an electric storage device according to an embodiment of the present invention. Figure 1 As shown, the negative electrode 100 for an electric storage device according to the present embodiment includes a negative electrode collector 10 and a negative electrode composite layer 20 formed on the negative electrode collector 10. The negative electrode composite layer 20 includes a first layer 20a formed on the negative electrode collector 10 and a second layer 20b formed on the first layer 20a. The first layer 20a includes a first negative electrode active material and a polymer (A), and when the total of the repeating units included in the polymer (A) is 100% by mass, the polymer (A) contains 5% to 20% by mass of a repeating unit (a1) derived from an unsaturated carboxylic acid. The second layer 20b includes a second negative electrode active material and a polymer (B), and when the total of the repeating units included in the polymer (B) is 100% by mass, the polymer (B) contains 0.1% by mass or more and less than 5% by mass of a repeating unit (a1) derived from an unsaturated carboxylic acid.

[0042] It should be explained that Figure 1 This is merely an example for explaining one embodiment of the present invention, and the present invention is not limited thereto. Hereinafter, the negative electrode for an electric storage device according to this embodiment will be described in detail.

[0043] 1.1. Negative electrode collector

[0044] As the negative electrode current collector 10, a material selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and a combination thereof can be used. Among these, copper foil and copper foam are preferred.

[0045] The thickness of the negative electrode current collector 10 is preferably 1 μm to 50 μm, more preferably 5 μm to 30 μm, and particularly preferably 8 μm to 20 μm.

[0046] 1.2. Negative electrode composite layer

[0047] The negative electrode mixed material layer 20 includes a first layer 20 a formed on the negative electrode current collector 10 and a second layer 20 b formed on the first layer 20 a .

[0048] The negative electrode 100 for the storage device involved in this embodiment can be manufactured by the following method, which includes: a step of forming a first layer 20a containing a first negative electrode active material and a polymer (A) on the negative electrode collector 10 (step 1); and a step of forming a second layer 20b containing a second negative electrode active material and a polymer (B) on the above-mentioned first layer 20a (step 2).

[0049] Step 1 is a step of forming the first layer 20a on the negative electrode collector 10. The first layer 20a is formed by coating the first negative electrode slurry for the negative electrode of the storage device, which is prepared by dissolving or dispersing the first negative electrode active material and the polymer (A) in a liquid medium, on the negative electrode collector 10 and drying the coating, or by coating the first negative electrode slurry for the storage device on another support and then laminating a film of the first negative electrode slurry for the storage device obtained by peeling off the support on the negative electrode collector 10.

[0050] The step of coating the first electricity storage device negative electrode slurry on the negative electrode current collector 10 can be performed by a conventional method, and specifically, can be performed by a method such as bar coating, casting, or spraying.

[0051] The step of drying after applying the first power storage device negative electrode slurry is a step for removing the liquid medium contained in the slurry, and can be performed by a common drying method such as hot air drying, natural drying or heating.

[0052] Next, step 2 is a step of forming a second layer 20b including a second negative electrode active material and a polymer (B) on the first layer 20a formed in the above step 1. The second layer 20b is formed by coating a second negative electrode slurry for a storage device produced by dissolving or dispersing the second negative electrode active material and the polymer (B) in a liquid medium on the first layer 20a and drying the slurry, or by coating the second negative electrode slurry for a storage device on another support and laminating a film obtained by peeling off the support on the first layer 20a.

[0053] In the negative electrode composite layer 20 having the above-mentioned structure, the thickness ratio of the first layer 20a can be 0.5 or less relative to the total thickness of the first layer 20a and the second layer 20b. When the thickness ratio of the first layer 20a is 0.5 or less, the migration of the polymer (A) of the first layer 20a can be suppressed, and the decrease in the adhesion between the negative electrode collector 10 and the first negative electrode active material can be prevented. Considering the reduction in the migration of the polymer (A) and the significant effect of improving the adhesion between the negative electrode collector 10 and the first negative electrode active material, the thickness ratio of the first layer 20a is preferably 0.1 to 0.5, and more preferably 0.1 to 0.4 relative to the total thickness of the first layer 20a and the second layer 20b.

[0054] In addition, under the condition that the above-mentioned thickness ratio range is satisfied, the average thickness of the first layer 20a can be 10 μm to 1000 μm. When the first layer 20a has a thickness within the above-mentioned range, the migration of the polymer (A) of the first layer 20a can be reduced, and a small amount of binder can be used to improve the adhesion between the negative electrode collector 10 and the first negative electrode active material and the performance of the storage device. Considering the reduction in the migration of the polymer (A) and the significant effect of the improvement in the adhesion between the negative electrode collector 10 and the first negative electrode active material, the average thickness of the first layer 20a is preferably 20 μm to 500 μm.

[0055] In the negative electrode composite layer 20 of the negative electrode for the storage device involved in this embodiment, the first layer 20a contains a polymer (A) with a relatively large acid content, and the second layer 20b contains a polymer (B) with a relatively small acid content. The first slurry for the negative electrode of the storage device used when forming the first layer 20a has a high viscosity because it contains a polymer (A) with a relatively large acid content, and sometimes the smoothness (leveling) of the surface of the first layer 20a is poor when applied and dried. On the other hand, the second slurry for the negative electrode of the storage device used when forming the second layer 20b has a low viscosity because it contains a polymer (B) with a relatively small acid content, and the coating property becomes good, so the smoothness (leveling) of the negative electrode composite layer 20 can be improved. In this way, by making the coating property of the second slurry for the negative electrode of the storage device good, the adhesion between the negative electrode collector 10 and the negative electrode composite layer 20 is excellent, and the cycle characteristics of the negative electrode for the storage device can be improved. In particular, the use of the polymer (A) contained in the first layer 20 a can play a role in improving the binding properties between the first negative electrode active material and the conductive additive and between the first negative electrode active materials, thereby reducing the internal resistance of the negative electrode for a power storage device.

[0056] The content of the polymer (B) in the second layer 20b is preferably 1% to 20% by mass relative to the total mass of the second layer 20b. By including the polymer (B) in the second layer 20b in an amount within the above range, the impregnation property of the electrolyte is excellent, and the adhesion between the negative electrode active materials in the second layer 20b is excellent, so that the conductivity and energy density in the second layer 20b can be improved. Considering the improvement of adhesion brought about by including the polymer (B) in the second layer 20b and the significance of the improvement effect of the conductivity and energy density in the negative electrode, the content of the polymer (B) is preferably 1% to 10% by mass, and more preferably 1% to 7% by mass relative to the total mass of the second layer 20b.

[0057] The second layer 20b having the above-described structure may have an average thickness whose thickness ratio relative to the average thickness of the first layer 20a is greater than 1. In view of the significance of the improvement effect brought about by optimizing the required binder properties by the thickness in the negative electrode, the thickness ratio of the first layer 20a to the second layer 20b is preferably 1 to 3:5 to 9.

[0058] Further, under the condition that the above-mentioned range of thickness ratio is satisfied, the average thickness of the second layer 20 b is preferably 10 μm to 1000 μm, more preferably 20 μm to 500 μm, and particularly preferably 30 μm to 300 μm.

[0059] In the negative electrode for a power storage device according to this embodiment, the thickness ratio of the first layer 20a to the total thickness of the first layer 20a and the second layer 20b may be 0.1 to 0.5, and the ratio of the thickness of the first layer 20a to the thickness of the second layer 20b may be 1 to 3:5 to 9.

[0060] In the negative electrode for a power storage device according to the present embodiment, the total amount of the first negative electrode active material and the second negative electrode active material contained in the first layer 20a and the second layer 20b is preferably 50 mg / 25 cm 2 ~1000mg / 25cm 2 , more preferably 50mg / 25cm 2 ~500mg / 25cm 2 .

[0061] In addition, the negative electrode for the storage device involved in the present embodiment includes the polymer (A) and the polymer (B) together with the particulate first negative electrode active material and the second negative electrode active material, so that fine pores can be formed in each active material layer. Specifically, the negative electrode for the storage device involved in the present embodiment can have a porosity of preferably 10% by volume to 50% by volume, more preferably 20% by volume to 40% by volume, relative to the total volume of the first layer 20a and the second layer 20b.

[0062] In the present invention, the porosity can be measured by BET (Brunauer-Emmett-Teller: specific surface area) measurement method or mercury porosimetry (Hg porosimetry).

[0063] Hereinafter, the first and second negative electrode slurries for power storage devices described above will be described in detail.

[0064] 1.2.1. First power storage device negative electrode slurry

[0065] The first negative electrode slurry for a power storage device contains a polymer (A) and a first negative electrode active material.

[0066] 1.2.1.1. Polymer (A)

[0067] The polymer (A) functions as a binder for demonstrating the binding ability between the first negative electrode active material, the adhesion ability between the negative electrode collector and the first layer, and the adhesion ability between the second layer and the first layer. The polymer (A) contained in the slurry for the negative electrode of the first storage device may be in the form of a latex dispersed in a liquid medium or in the form of a state dissolved in a liquid medium, but is preferably in the form of a latex dispersed in a liquid medium. If the polymer (A) is in the form of a latex dispersed in a liquid medium, the stability of the slurry for the negative electrode of the first storage device becomes good, and the coating property of the slurry on the negative electrode collector 10 becomes good, so it is preferred.

[0068] The content ratio of the polymer component in the slurry for the negative electrode of the first storage device is preferably 1 to 8 parts by mass, more preferably 1 to 7 parts by mass, and particularly preferably 1.5 to 6 parts by mass, relative to 100 parts by mass of the first negative electrode active material. If the content ratio of the polymer component is within the above range, the dispersibility of the first negative electrode active material in the slurry becomes good, and the coating property of the slurry also becomes excellent. Here, the polymer component includes a polymer (A), a polymer other than the polymer (A) added as needed, and a thickener, etc. Below, the repeating units constituting the polymer (A), the physical properties of the polymer (A), and the manufacturing method are described in turn.

[0069] <Repeating Unit Constituting Polymer (A)>

[0070] When the total of the repeating units contained in the polymer (A) is set to 100 mass%, the polymer (A) contains 5 mass% to 20 mass% of repeating units (a1) derived from unsaturated carboxylic acid (hereinafter also referred to as "repeating units (a1)".). The content of the repeating unit (a1) is preferably 6 mass% or more, more preferably 7 mass% or more. The content of the repeating unit (a1) is preferably 19 mass% or less, more preferably 18 mass% or less. By containing the repeating unit (a1) within the above range, the polymer (A) can increase the viscosity in the slurry and inhibit migration. In addition, the adhesion between the negative electrode collector and the first layer can be improved.

[0071] The unsaturated carboxylic acid is not particularly limited, and monocarboxylic acids and dicarboxylic acids (including anhydrides) such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid can be cited, and one or more selected from these can be used. As the unsaturated carboxylic acid, one or more selected from acrylic acid, methacrylic acid, and itaconic acid are preferably used.

[0072] In addition to the repeating unit (a1), the polymer (A) may contain repeating units derived from other monomers copolymerizable therewith. Examples of such repeating units include repeating units (a2) derived from a conjugated diene compound (hereinafter also referred to as "repeating unit (a2)"), repeating units (a3) ​​derived from an aromatic vinyl compound (hereinafter also referred to as "repeating unit (a3)"), repeating units (a4) derived from an unsaturated carboxylic acid ester (hereinafter also referred to as "repeating unit (a4)"), repeating units (a5) derived from an α,β-unsaturated nitrile compound (hereinafter also referred to as "repeating unit (a5)"), repeating units (a6) derived from (meth)acrylamide (hereinafter also referred to as "repeating unit (a6)"), and repeating units (a7) derived from a compound having a sulfonic acid group (hereinafter also referred to as "repeating unit (a7)"), etc.

[0073] When the total of the repeating units contained in the polymer (A) is set to 100% by mass, the content of the repeating unit (a2) from the conjugated diene compound is preferably 15% to 60% by mass. The content of the repeating unit (a2) is more preferably 17% by mass or more, and particularly preferably 20% by mass or more. The content of the repeating unit (a2) is more preferably 57% by mass or less, and particularly preferably 55% by mass or less. By making the polymer (A) contain the repeating unit (a2) within the above range, the dispersibility of the first negative electrode active material becomes good, and a homogeneous first layer can be produced without structural defects of the electrode plate, and sometimes good repeated charge and discharge characteristics are exhibited. In addition, the polymer (A) covering the surface of the first negative electrode active material can be given elasticity, and by stretching the polymer (A), the adhesion can be improved, and therefore sometimes good charge and discharge durability characteristics are exhibited.

[0074] The repeating unit (a2) derived from the conjugated diene compound is preferably not hydrogenated by an oil layer hydrogenation method or a water layer hydrogenation method. By containing the repeating unit (a2) derived from the conjugated diene compound that is not hydrogenated, the polymer (A) can be given elasticity, and by making the polymer (A) elastic, the adhesion can sometimes be further improved.

[0075] The conjugated diene compound is not particularly limited, and examples thereof include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, and 2-chloro-1,3-butadiene. One or more selected from these can be used. Among these, 1,3-butadiene is particularly preferred.

[0076] When the total of the repeating units contained in the polymer (A) is set to 100% by mass, the content ratio of the repeating unit (a3) ​​from the aromatic vinyl compound is preferably 1% by mass or more and less than 20% by mass. The content ratio of the repeating unit (a3) ​​is more preferably 2% by mass or more, and particularly preferably 3% by mass or more. The content ratio of the repeating unit (a3) ​​is more preferably 19% by mass or less, and particularly preferably 18% by mass or less. By making the polymer (A) contain repeating units (a3) ​​within the above range, the fusion of the polymers (A) dispersed in the electrode can be suppressed, and the permeability of the electrolyte is improved, so the repeated charge and discharge characteristics are sometimes improved. And, sometimes, good adhesion is shown to the graphite used as the first negative electrode active material.

[0077] The aromatic vinyl compound is not particularly limited, and examples thereof include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, chlorostyrene, divinylbenzene, and the like. One or more selected from these may be used.

[0078] When the total of the repeating units contained in the polymer (A) is set to 100% by mass, the total amount of the repeating units (a1), the repeating units (a2) and the repeating units (a3) ​​is preferably 50% by mass or more, and more preferably 55% by mass or more. If the total amount of the repeating units (a1), the repeating units (a2) and the repeating units (a3) ​​is within the above range, the dispersibility of the first negative electrode active material becomes good, and the fusion of the polymers (A) dispersed in the electrode can be suppressed, and the adhesion and the permeability of the electrolyte are improved, so sometimes good repeated charge and discharge characteristics and good charge and discharge durability characteristics are exhibited.

[0079] When the total of the repeating units contained in the polymer (A) is set to 100% by mass, the content of the repeating unit (a4) from the unsaturated carboxylic acid ester is preferably 1% to 20% by mass. The content of the repeating unit (a4) is more preferably 2% by mass or more, and particularly preferably 3% by mass or more. The content of the repeating unit (a4) is more preferably 18% by mass or less, and particularly preferably 15% by mass or less. By making the polymer (A) contain the repeating unit (a4) within the above range, the affinity of the polymer (A) and the electrolyte becomes good, and sometimes the internal resistance rise caused by the binder becoming a resistance component in the storage device can be suppressed, and the adhesion decrease caused by excessive absorption of the electrolyte can be prevented.

[0080] Among the unsaturated carboxylic acid esters, (meth)acrylates can be preferably used. Specific examples of (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, ethylene glycol di(meth)acrylate, di(meth)propylene glycol di(meth)acrylate, ethylene ... In some embodiments, the present invention relates to propylene glycol (meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, allyl (meth)acrylate, 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, glycerol mono(meth)acrylate, glycerol di(meth)acrylate, etc., and one or more selected from these can be used. Among them, one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, ethylene glycol di(meth)acrylate, and 2-hydroxyethyl (meth)acrylate are preferred, and methyl (meth)acrylate is particularly preferred.

[0081] When the total of the repeating units contained in the polymer (A) is set to 100% by mass, the content of the repeating unit (a5) from the α,β-unsaturated nitrile compound is preferably 5% to 40% by mass. The content of the repeating unit (a5) is more preferably 7% by mass or more, and particularly preferably 10% by mass or more. The content of the repeating unit (a5) is more preferably 35% by mass or less, and particularly preferably 30% by mass or less. By making the polymer (A) contain the repeating unit (a5) within the above range, it is sometimes possible to reduce the dissolution of the polymer (A) into the electrolyte, and it is possible to suppress the decrease in adhesion caused by the electrolyte. In addition, it is sometimes possible to suppress the internal resistance increase caused by the dissolved polymer component in the storage device becoming a resistance component.

[0082] The α,β-unsaturated nitrile compound is not particularly limited, and examples thereof include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-ethylacrylonitrile, vinylidene cyanide, and the like, and one or more selected from these can be used. Among these, one or more selected from acrylonitrile and methacrylonitrile is preferred, and acrylonitrile is particularly preferred.

[0083] When the total of the repeating units contained in the polymer (A) is set to 100% by mass, the content of the repeating unit (a6) from (meth) acrylamide is preferably 0 to 10% by mass. The content of the repeating unit (a6) is more preferably 1% by mass or more, and particularly preferably 2% by mass or more. The content of the repeating unit (a6) is preferably 8% by mass or less, and more preferably 5% by mass or less. By making the polymer (A) contain the repeating unit (a6) within the above range, the dispersibility of the first negative electrode active material in the slurry sometimes becomes good. In addition, sometimes the softness of the first layer obtained becomes appropriate, and the adhesion between the negative electrode collector and the first layer is improved. In addition, the ability of the first negative electrode active material containing a carbon material or a silicon material such as graphite to bind to each other can be improved, so sometimes a first layer with better softness or adhesion to the negative electrode collector can be obtained.

[0084] The (meth)acrylamide is not particularly limited, and examples thereof include acrylamide, methacrylamide, N-isopropylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N,N-diethylmethacrylamide, N,N-dimethylaminopropylacrylamide, N,N-dimethylaminopropylmethacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, diacetone acrylamide, maleamide, and tert-butylacrylamidesulfonic acid. At least one selected from these can be used.

[0085] When the total of the repeating units contained in the polymer (A) is set to 100% by mass, the content of the repeating unit (a7) derived from the compound having a sulfonic acid group is preferably 0 to 10% by mass. The content of the repeating unit (a7) is more preferably 0.5% by mass or more, and particularly preferably 1% by mass or more. The content of the repeating unit (a7) is more preferably 8% by mass or less, and particularly preferably 5% by mass or less.

[0086] The compound having a sulfonic acid group is not particularly limited, and examples thereof include compounds such as vinyl sulfonic acid, styrene sulfonic acid, allyl sulfonic acid, sulfoethyl (meth)acrylate, sulfopropyl (meth)acrylate, sulfobutyl (meth)acrylate, 2-acrylamide-2-methylpropanesulfonic acid, 2-hydroxy-3-acrylamidepropanesulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, and alkali salts thereof, and one or more selected from these compounds can be used.

[0087] <Physical properties of polymer (A)>

[0088] (Number average particle size)

[0089] When the polymer (A) is in the form of a latex (particle) dispersed in a liquid medium, the number average particle size of the particles is preferably 150 nm to 300 nm, more preferably 150 nm to 290 nm, and particularly preferably 150 nm to 280 nm. If the number average particle size of the particles of the polymer (A) is within the above range, the contact area with the liquid medium can be reduced, and the particles of the polymer (A) are easily adsorbed on the surface of the first negative electrode active material, so as the first negative electrode active material moves, the particles of the polymer (A) can also follow the movement. As a result, migration can be suppressed, so sometimes the degradation of electrical properties can be reduced.

[0090] The number average particle size of the particles of the polymer (A) is the average value of the particle sizes obtained from images of 50 particles observed using a transmission electron microscope (TEM). Examples of the transmission electron microscope include "H-7650" manufactured by Hitachi High-Tech Corporation.

[0091] <Method for producing polymer (A)>

[0092] The method for producing the polymer (A) is not particularly limited, and for example, an emulsion polymerization method carried out in the presence of a known emulsifier (surfactant), a chain transfer agent, a polymerization initiator, etc. can be used. As the emulsifier (surfactant), the chain transfer agent and the polymerization initiator, the compounds described in Japanese Patent No. 5999399 and the like can be used.

[0093] 1.2.1.2. First negative electrode active material

[0094] As the first negative electrode active material, a compound in which lithium can be reversibly inserted and removed can be used. As specific examples, carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon can be cited; metallic compounds that can be alloyed with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; metal oxides that can be doped and dedoped with lithium, such as SiOx (0<x<2), SnO2, vanadium oxide, and lithium vanadium oxide; composites such as Si-C complexes or Sn-C complexes that include the above-mentioned metallic compounds and carbonaceous materials, and any one of these or a mixture of two or more thereof can be used.

[0095] In the first negative electrode active material exemplified above, it is preferred to contain a metallic compound and / or a carbonaceous material, and more preferably a mixture of a silicon material and a carbonaceous material. Since the amount of lithium absorbed per unit weight of the silicon material is greater than that of other active materials, the storage capacity of the resulting power storage device can be increased, and as a result, the output and energy density of the power storage device can be increased. On the other hand, since the volume change of the carbonaceous material accompanying charging and discharging is smaller than that of the silicon material, by using a mixture of a silicon material and a carbonaceous material as the negative electrode active material, the influence of the volume change of the silicon material can be mitigated, and the adhesion between the negative electrode collector and the negative electrode composite layer can be further improved.

[0096] When silicon (Si) is used as the negative electrode active material, silicon has a high capacity, but on the other hand, it undergoes a large volume change when absorbing lithium. Therefore, the silicon material has the following properties: due to repeated expansion and contraction, it becomes micronized, causing peeling from the collector, separation of the negative electrode active materials, and easy destruction of the conductive network inside the negative electrode composite layer. Due to this property, the charge and discharge durability characteristics of the storage device deteriorate rapidly in a short period of time.

[0097] The negative electrode for the power storage device according to the present embodiment does not cause the above-mentioned problems even when a silicon material is used, and can exhibit good electrical properties. The reason for this is believed to be that the polymer (A) can firmly bind the silicon material, and even if the volume of the silicon material expands due to lithium absorption, the polymer (A) can expand and contract to maintain a state of firmly binding the silicon material.

[0098] The content ratio of the silicon material in 100% by mass of the first negative electrode active material is preferably 1% by mass or more, more preferably 2 to 50% by mass, further preferably 3 to 45% by mass, and particularly preferably 10 to 40% by mass. If the content ratio of the silicon material in 100% by mass of the first negative electrode active material is within the above range, an electric storage device having an excellent balance between the output and energy density of the electric storage device and the charge and discharge durability characteristics can be obtained.

[0099] The first negative electrode active material is preferably in the form of particles and has an average particle size of preferably 0.1 to 100 μm, more preferably 1 to 20 μm.

[0100] 1.2.1.3. Other ingredients

[0101] In addition to the above-mentioned components, other components may be added to the first negative electrode slurry of the power storage device as needed. Examples of such components include polymers other than the polymer (A), thickeners, liquid media, conductive additives, pH adjusters, preservatives, cellulose fibers, and the like.

[0102] <Polymers other than polymer (A)>

[0103] The first storage device negative electrode slurry may contain polymers other than polymer (A). Such polymers are not particularly limited, and examples thereof include acrylic polymers containing unsaturated carboxylic acid esters or their derivatives as constituent units, fluorine-based polymers such as PVDF (polyvinylidene fluoride), and the like. These polymers may be used alone or in combination of two or more. By containing these polymers, sometimes the flexibility and adhesion are further improved.

[0104] <Thickener>

[0105] The first negative electrode slurry for a power storage device may contain a thickener. By containing a thickener, the coating properties of the slurry, the charge and discharge characteristics of the resulting power storage device, etc. may be further improved.

[0106] Specific examples of thickeners include cellulose compounds such as carboxymethyl cellulose, methyl cellulose, and hydroxypropyl cellulose; poly(meth)acrylic acid; ammonium salts or alkali metal salts of the above cellulose compounds or poly(meth)acrylic acid; polyvinyl alcohol (co)polymers such as polyvinyl alcohol, modified polyvinyl alcohol, and ethylene-vinyl alcohol copolymers; and water-soluble polymers such as saponified copolymers of unsaturated carboxylic acids such as (meth)acrylic acid, maleic acid, and fumaric acid and vinyl esters. Among these, alkali metal salts of carboxymethyl cellulose and alkali metal salts of poly(meth)acrylic acid are preferred.

[0107] Examples of commercially available products of these thickeners include alkali metal salts of carboxymethylcellulose such as CMC1120, CMC1150, CMC2200, CMC2280, and CMC2450 (all manufactured by Daicel Corporation).

[0108] When the first negative electrode slurry for a storage device contains a thickener, the content of the thickener is preferably 5 parts by mass or less, more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the total solid content of the first negative electrode slurry for a storage device.

[0109] <Liquid medium>

[0110] The negative electrode slurry of the first power storage device contains a liquid medium. As the liquid medium, an aqueous medium containing water is preferred, and water is more preferred. The aqueous medium may contain a non-aqueous medium other than water. As the non-aqueous medium, for example, amide compounds, hydrocarbons, alcohols, ketones, esters, amine compounds, lactones, sulfoxides, sulfone compounds, etc. may be cited, and one or more selected from these may be used. By using an aqueous medium as the liquid medium, the negative electrode slurry of the first power storage device has a low degree of adverse effects on the environment and improves the safety of the operator.

[0111] In 100% by mass of the aqueous medium, the content ratio of the non-aqueous medium contained in the aqueous medium is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably substantially free of the non-aqueous medium. Here, "substantially free of" means that the non-aqueous medium is not intentionally added as a liquid medium, and may include the non-aqueous medium that is inevitably mixed in when preparing the negative electrode slurry for the first power storage device.

[0112] The content ratio of the liquid medium in the negative electrode slurry for the first power storage device is preferably a solid content concentration in the slurry (the ratio of the total mass of the components in the slurry excluding the liquid medium to the total mass of the slurry. The same applies hereinafter) of 30 to 70 mass %, more preferably 40 to 60 mass %.

[0113] <Conductive additive>

[0114] The first negative electrode slurry for a first power storage device may further contain a conductive auxiliary agent in order to impart conductivity and buffer the volume change of the first negative electrode active material caused by the entry and exit of lithium ions.

[0115] Specific examples of the conductive aid include activated carbon, acetylene black, Ketjen black, furnace black, graphite, carbon fiber, fullerene, carbon nanotubes and the like. Of these, acetylene black, Ketjen black, or carbon nanotubes can be preferably used. The conductive aid is preferably contained in an amount of 20 parts by mass or less, more preferably 1 to 15 parts by mass, and particularly preferably 2 to 10 parts by mass relative to 100 parts by mass of the first negative electrode active material.

[0116] <pH Adjuster>

[0117] The first electricity storage device negative electrode slurry may further contain a pH adjuster in order to suppress corrosion of the negative electrode collector depending on the type of the first negative electrode active material.

[0118] Examples of the pH adjuster include hydrochloric acid, phosphoric acid, sulfuric acid, acetic acid, formic acid, ammonium phosphate, ammonium sulfate, ammonium acetate, ammonium formate, ammonium chloride, sodium hydroxide, potassium hydroxide, etc. Among these, sulfuric acid, ammonium sulfate, sodium hydroxide, and potassium hydroxide are preferred.

[0119] <Preservatives>

[0120] The first electricity storage device negative electrode slurry may further contain an anticorrosive agent in order to suppress corrosion of the negative electrode collector depending on the type of the first negative electrode active material.

[0121] Examples of the preservative include ammonium metavanadate, sodium metavanadate, potassium metavanadate, ammonium metatungstate, sodium metatungstate, potassium metatungstate, ammonium paratungstate, sodium paratungstate, potassium paratungstate, ammonium molybdate, sodium molybdate, and potassium molybdate. Among these, ammonium paratungstate, ammonium metavanadate, sodium metavanadate, potassium metavanadate, and ammonium molybdate are preferred.

[0122] <Cellulose fiber>

[0123] The first storage device negative electrode slurry may further contain cellulose fibers. As the cellulose fibers, known cellulose fibers may be used. By containing cellulose fibers, the adhesion of the first negative electrode active material to the negative electrode collector can sometimes be improved. It is believed that the fibrous cellulose fibers can prevent the first negative electrode active material from falling off and improve the adhesion to the negative electrode collector by making the adjacent first negative electrode active materials bonded to each other in a fibrous manner by line bonding or line contact.

[0124] 1.2.1.4. Method for preparing negative electrode slurry for first power storage device

[0125] The first storage device negative electrode slurry can be manufactured by any method as long as it contains the polymer (A) and the first negative electrode active material. From the perspective of more effectively and cheaply manufacturing a slurry with better dispersibility and stability, it is preferred to add the first negative electrode active material and any additional components used as needed to the dispersion of the polymer (A) manufactured by the above-mentioned <method for manufacturing polymer (A)>, and mix them to manufacture. As a specific manufacturing method, for example, the method described in Japanese Patent Gazette No. 5999399 can be cited.

[0126] 1.2.2. Second power storage device negative electrode slurry

[0127] The second negative electrode slurry for a power storage device contains a polymer (B) and a second negative electrode active material.

[0128] 1.2.2.1. Polymer (B)

[0129] The polymer (B) functions as a binder for demonstrating the binding ability of the second negative electrode active material and the adhesion ability of the first layer and the second layer. The polymer (B) contained in the slurry for the negative electrode of the second power storage device may be in the form of a latex dispersed in a liquid medium or in the form of a state dissolved in a liquid medium, but preferably in the form of a latex dispersed in a liquid medium. If the polymer (B) is in the form of a latex dispersed in a liquid medium, the stability of the slurry for the negative electrode of the second power storage device becomes good, and the coating property of the slurry to the first layer becomes good, so it is preferred.

[0130] Relative to 100 parts by mass of the second negative electrode active material, the content ratio of the polymer component in the slurry for the negative electrode of the second storage device is preferably 1 to 8 parts by mass, more preferably 1 to 7 parts by mass, and particularly preferably 1.5 to 6 parts by mass. If the content ratio of the polymer component is within the above range, the dispersibility of the second negative electrode active material in the slurry becomes good, and the coating property of the slurry also becomes excellent. Here, the polymer component includes a polymer (B), a polymer other than the polymer (B) added as needed, and a thickener, etc. Below, the repeating units constituting the polymer (B), the physical properties of the polymer (B), and the manufacturing method are described in turn.

[0131] <Repeating units constituting polymer (B)>

[0132] When the total of the repeating units contained in the polymer (B) is set to 100% by mass, the polymer (B) contains 0.1% by mass or more and less than 5% by mass of repeating units (a1) from unsaturated carboxylic acids. The content of the repeating unit (a1) is preferably 0.2% by mass or more, more preferably 0.3% by mass or more. The content of the repeating unit (a1) is preferably 4% by mass or less, more preferably 3% by mass or less. By making the polymer (B) contain repeating units (a1) within the above range, the viscosity of the slurry can be reduced, so the smoothness (leveling) of the surface of the negative electrode composite layer becomes good when the coating is dried, and the thickness of the negative electrode composite layer can be made uniform. In addition, since the polymer composition of the polymer (A) is similar to that of the polymer (B), the adhesion between the first layer 20a and the second layer 20b can be improved. As an unsaturated carboxylic acid, one or more of the compounds listed in the description of the polymer (A) can be used.

[0133] In addition to the repeating unit (a1), the polymer (B) may contain repeating units derived from other monomers copolymerizable therewith. Examples of such repeating units include repeating units (a2) derived from conjugated diene compounds, repeating units (a3) ​​derived from aromatic vinyl compounds, repeating units (a4) derived from unsaturated carboxylic acid esters, repeating units (a5) derived from α,β-unsaturated nitrile compounds, repeating units (a6) derived from (meth)acrylamide, and repeating units (a7) derived from compounds having sulfonic acid groups.

[0134] When the total of the repeating units contained in the polymer (B) is set to 100% by mass, the content of the repeating unit (a2) from the conjugated diene compound is preferably 15% to 60% by mass. The content of the repeating unit (a2) is more preferably 17% by mass or more, and particularly preferably 20% by mass or more. The content of the repeating unit (a2) is more preferably 57% by mass or less, and particularly preferably 55% by mass or less. By making the polymer (B) contain the repeating unit (a2) within the above range, the dispersibility of the second negative electrode active material becomes good, and a homogeneous negative electrode composite layer can be made, so there are no structural defects of the electrode plate, and sometimes good repeated charge and discharge characteristics are exhibited. In addition, the polymer (B) covering the surface of the second negative electrode active material can be given elasticity, and by stretching the polymer (B), the adhesion can be improved, so sometimes good charge and discharge durability characteristics are exhibited. As a conjugated diene compound, one or more of the compounds listed in the description of the polymer (A) can be used.

[0135] The repeating unit (a2) derived from the conjugated diene compound is preferably not hydrogenated by an oil layer hydrogenation method or a water layer hydrogenation method. By making the polymer (B) not contain the repeating unit (a2) derived from the conjugated diene compound that is not hydrogenated, it is possible to impart stretchability to the polymer (B), and by making the polymer (B) stretchable, it is sometimes possible to further improve the adhesion.

[0136] When the total of the repeating units contained in the polymer (B) is set to 100% by mass, the content ratio of the repeating unit (a3) ​​from the aromatic vinyl compound is preferably 20% by mass or more and less than 40% by mass. The content ratio of the repeating unit (a3) ​​is more preferably 21% by mass or more, and particularly preferably 22% by mass or more. The content ratio of the repeating unit (a3) ​​is more preferably 35% by mass or less, and particularly preferably 30% by mass or less. By making the polymer (B) contain the repeating unit (a3) ​​within the above range, the fusion of the polymers (B) dispersed in the electrode can be suppressed, and the permeability of the electrolyte is improved, so the repeated charge and discharge characteristics are sometimes improved. And, sometimes good adhesion is shown to graphite used as the second negative electrode active material. As an aromatic vinyl compound, one or more of the compounds listed in the description of the polymer (A) can be used.

[0137] When the total of the repeating units contained in the polymer (A) is set to 100% by mass, the total amount of the repeating units (a1), repeating units (a2) and repeating units (a3) ​​is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more. If the total amount of the repeating units (a1), repeating units (a2) and repeating units (a3) ​​is within the above range, the dispersibility of the second negative electrode active material becomes good, and the fusion of the polymers (B) dispersed in the electrode can be suppressed, and the adhesion and the permeability of the electrolyte are improved, so sometimes good repeated charge and discharge characteristics and good charge and discharge durability characteristics are exhibited.

[0138] When the total of the repeating units contained in the polymer (B) is set to 100% by mass, the content of the repeating unit (a4) from the unsaturated carboxylic acid ester is preferably 1% to 20% by mass. The content of the repeating unit (a4) is more preferably 2% by mass or more, and particularly preferably 3% by mass or more. The content of the repeating unit (a4) is more preferably 18% by mass or less, and particularly preferably 15% by mass or less. By making the polymer (B) contain the repeating unit (a4) within the above range, the affinity of the polymer (B) and the electrolyte becomes good, and sometimes the internal resistance increase caused by the binder becoming a resistance component in the storage device can be suppressed, and the adhesion decrease caused by excessive absorption of the electrolyte can be prevented. As the unsaturated carboxylic acid ester, one or more of the compounds listed in the description of the polymer (A) can be used.

[0139] When the total of the repeating units contained in the polymer (B) is set to 100% by mass, the content of the repeating unit (a5) from the α,β-unsaturated nitrile compound is preferably 5% to 40% by mass. The content of the repeating unit (a5) is more preferably 7% by mass or more, and particularly preferably 10% by mass or more. The content of the repeating unit (a5) is more preferably 35% by mass or less, and particularly preferably 30% by mass or less. By making the polymer (B) contain the repeating unit (a5) within the above range, the dissolution of the polymer (B) into the electrolyte can be reduced, and the decrease in adhesion caused by the electrolyte can sometimes be suppressed. In addition, it is sometimes possible to suppress the increase in internal resistance caused by the dissolved polymer component in the storage device becoming a resistance component. As an α,β-unsaturated nitrile compound, one or more of the compounds listed in the description of the polymer (A) can be used.

[0140] When the total of the repeating units contained in the polymer (B) is set to 100% by mass, the content of the repeating unit (a6) from (meth) acrylamide is preferably 0 to 10% by mass. The content of the repeating unit (a6) is more preferably 1% by mass or more, and particularly preferably 2% by mass or more. The content of the repeating unit (a6) is preferably 8% by mass or less, and more preferably 5% by mass or less. By making the polymer (B) contain the repeating unit (a6) within the above range, the dispersibility of the second negative electrode active material in the slurry sometimes becomes good. In addition, sometimes the softness of the second layer obtained becomes appropriate, and the adhesion between the first layer and the second layer is improved. In addition, the ability to bind the second negative electrode active material containing a carbon material or a silicon material such as graphite to each other can be improved, so sometimes a second layer with better softness or adhesion to the first layer can be obtained. As (meth) acrylamide, one or more of the compounds listed in the description of the polymer (A) can be used.

[0141] When the total of the repeating units contained in the polymer (B) is set to 100% by mass, the content ratio of the repeating unit (a7) from the compound having a sulfonic acid group is preferably 0 to 10% by mass. The content ratio of the repeating unit (a7) is more preferably 0.5% by mass or more, and particularly preferably 1% by mass or more. The content ratio of the repeating unit (a7) is more preferably 8% by mass or less, and particularly preferably 5% by mass or less. As the compound having a sulfonic acid group, one or more of the compounds listed in the description of the polymer (A) can be used.

[0142] <Physical properties of polymer (B)>

[0143] (Number average particle size)

[0144] When the polymer (B) is in the form of a latex (particles) dispersed in a liquid medium, the number average particle size of the particles is preferably greater than 50 nm and less than 150 nm, more preferably 50 nm to 145 nm, and particularly preferably 50 nm to 140 nm. If the number average particle size of the particles of the polymer (B) is within the above range, the viscosity of the slurry for the negative electrode of the second power storage device can be reduced, so that the smoothness (leveling) of the surface of the second layer becomes good during coating and drying, and the thickness of the entire negative electrode composite layer becomes uniform. As a result, the adhesion of the negative electrode composite layer is improved, and sometimes good charge and discharge durability characteristics are exhibited. It should be noted that the number average particle size of the particles of the polymer (B) can be measured by the same method as the number average particle size of the particles of the polymer (A).

[0145] <Method for producing polymer (B)>

[0146] The method for producing the polymer (B) is not particularly limited, and for example, an emulsion polymerization method in the presence of a known emulsifier (surfactant), a chain transfer agent, a polymerization initiator, etc. can be used. As the emulsifier (surfactant), the chain transfer agent and the polymerization initiator, the compounds described in Japanese Patent No. 5999399 and the like can be used.

[0147] 1.2.2.2. Second negative electrode active material

[0148] As the second negative electrode active material, one or more compounds selected from the compounds listed in the description of the first negative electrode active material can be used. The second negative electrode active material may be the same as or different from the first negative electrode active material, but is preferably the same.

[0149] 1.2.2.3. Other ingredients

[0150] In addition to the above-mentioned components, other components may be added to the negative electrode slurry of the second power storage device as needed. Such components include, for example, polymers other than polymer (B), thickeners, liquid media, conductive aids, pH adjusters, preservatives, cellulose fibers, etc. These components may be selected from one or more of the compounds listed in the description of the negative electrode slurry of the first power storage device, and the amount used may be the same.

[0151] 2. Power storage device

[0152] An electric storage device according to one embodiment of the present invention comprises the above-mentioned negative electrode for electric storage device. In addition to the above-mentioned negative electrode for electric storage device, the electric storage device according to this embodiment may also comprise a positive electrode for electric storage device and a separator, may contain an electrolyte, and may be manufactured according to a conventional method. As a specific manufacturing method of the electric storage device according to this embodiment, for example, a method of overlapping the negative electrode for electric storage device and the positive electrode for electric storage device via a separator, winding and folding them according to the shape of a battery and then storing them in a battery container, injecting an electrolyte into the battery container and sealing it, etc. The shape of the battery may be a coin-shaped, cylindrical, square, laminated or other appropriate shape.

[0153] The above-mentioned power storage device can be used for lithium ion secondary batteries, double electric layer capacitors, lithium ion capacitors, etc. that need to be discharged at a high current density. Among these, lithium ion secondary batteries are particularly preferred. In the power storage device involved in this embodiment, the components other than the negative electrode for the power storage device can use the components for known lithium ion secondary batteries, double electric layer capacitors, and lithium ion capacitors.

[0154] 3. Example

[0155] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. "Parts" and "%" in Examples and Comparative Examples are based on mass unless otherwise specified.

[0156] 3.1. Example 1

[0157] 3.1.1. Polymer synthesis and physical property evaluation

[0158] (1) Synthesis of polymer (A1)

[0159] A particle dispersion of polymer (A1) was obtained by one-step polymerization as shown below. 400 parts by mass of water, a monomer mixture consisting of 50 parts by mass of 1,3-butadiene, 15 parts by mass of styrene, 5 parts by mass of acrylic acid, 5 parts by mass of methyl methacrylate, 25 parts by mass of acrylonitrile, 0.1 parts by mass of tert-dodecyl mercaptan as a chain transfer agent, 2 parts by mass of sodium alkyl diphenyl oxide disulfonate as an emulsifier, and 0.2 parts by mass of potassium persulfate as a polymerization initiator were added to a reactor, and polymerization was carried out at 70°C for 24 hours while stirring, and the reaction was terminated with a polymerization conversion rate of 98%. Unreacted monomers were removed from the particle dispersion of polymer (A1) obtained in this way, and after concentration, a 10% sodium hydroxide aqueous solution and water were added to obtain a particle dispersion of polymer (A1) having a solid content concentration of 20% and a pH of 8.0.

[0160] (2) Synthesis of polymer (B1)

[0161] A particle dispersion of polymer (B1) was obtained by one-step polymerization as shown below. 400 parts by mass of water, a monomer mixture consisting of 0.1 parts by mass of acrylic acid, 50 parts by mass of 1,3-butadiene, 24.9 parts by mass of styrene, 10 parts by mass of methyl methacrylate, 15 parts by mass of acrylonitrile, 0.1 parts by mass of tert-dodecyl mercaptan as a chain transfer agent, 2 parts by mass of sodium alkyl diphenyl oxide disulfonate as an emulsifier, and 0.2 parts by mass of potassium persulfate as a polymerization initiator were added to a reactor, and polymerization was carried out at 70°C for 24 hours while stirring, and the reaction was terminated at a polymerization conversion rate of 98%. Unreacted monomers were removed from the particle dispersion of polymer (B1) obtained in this way, and after concentration, a 10% sodium hydroxide aqueous solution and water were added to obtain a particle dispersion of polymer (B1) having a solid content concentration of 20% and a pH of 8.0.

[0162] (3) Determination of number average particle size

[0163] A drop of the polymer particle dispersion obtained above was diluted to 0.1 wt% latex by pipetting on the collodion support film, and a drop of 1 wt% phosphotungstic acid solution was further added on the collodion support film by pipetting, and air-dried for 12 hours to prepare a sample. The sample prepared in this way was observed at a magnification of 10K using a transmission electron microscope (TEM, manufactured by Hitachi High-Tech Corporation., model "H-7650"). Image analysis was performed using the HITACHI EMIP program, and the average particle size of 50 randomly selected polymer particles was calculated, and the average value was used as the number average particle size. The results are shown in Table 1 below.

[0164] 3.1.2. Preparation of negative electrode slurry for power storage device

[0165] (1) Synthesis of silicon material (negative electrode active material)

[0166] A mixture of crushed silica powder (average particle size 10 μm) and carbon powder (average particle size 35 μm) was heat treated for 10 hours in an electric furnace with a temperature adjusted to a range of 1100°C to 1600°C under a nitrogen flow (0.5 NL / min) to obtain a powder of silicon oxide represented by a composition formula SiOx (x = 0.5 to 1.1) (average particle size 8 μm). 300 g of the silicon oxide powder was placed in a batch heating furnace, and while maintaining an absolute pressure of 100 Pa with a vacuum pump, the temperature was raised from room temperature (25°C) to 1100°C at a heating rate of 300°C / h. Next, while maintaining the pressure in the heating furnace at 2000 Pa, methane gas was introduced at a flow rate of 0.5 NL / min, and a heating treatment (graphite coating treatment) was performed at 1100°C for 5 hours. After the graphite coating treatment was completed, the mixture was cooled to room temperature at a cooling rate of 50°C / h, thereby obtaining about 330g of graphite-coated silicon oxide powder. The graphite-coated silicon oxide is a conductive powder (negative electrode active material) in which the surface of silicon oxide is coated with graphite, and its average particle size is 10.5μm. When the total amount of the obtained graphite-coated silicon oxide is 100% by mass, the proportion of the graphite coating is 2% by mass.

[0167] (2) Preparation of Negative Electrode Slurry for First Electric Storage Device

[0168] Into a twin-shaft planetary mixer (manufactured by PRIMIX Co., Ltd., trade name “TK HIVIS MIX 2P-03”) were added 1 part by mass (solid content conversion value, added in the form of an aqueous solution with a concentration of 2% by mass) of a thickener (trade name “CMC2200”, manufactured by Daicel Co., Ltd.), 2 parts by mass (solid content conversion value, added in the form of a particle dispersion of the polymer (A1) obtained above) of the polymer (A1) obtained above, 80 parts by mass (solid content conversion value) of artificial graphite (manufactured by Resonac Co., Ltd.) which is a highly crystalline graphite as a negative electrode active material, 20 parts by mass (solid content conversion value) of the graphite-coated silicon oxide powder obtained above, and 1 part by mass of carbon (acetylene black, manufactured by Denka Co., Ltd.) as a conductive aid, and the mixture was stirred at 60 rpm for 1 hour to obtain a paste. Water was added to the obtained paste to adjust the solid content concentration to 48% by mass, and then the mixture was stirred and mixed at 200 rpm for 2 minutes and at 1800 rpm for 5 minutes using a stirring deaerator (manufactured by THINKY Co., Ltd., trade name "Defo Rentaro"), and then the mixture was further stirred and mixed under reduced pressure (about 2.5×10 4 The mixture was stirred and mixed at 1800 rpm for 1.5 minutes to prepare a first negative electrode slurry for a storage battery device containing 19.6 mass % of Si in the negative electrode active material (C / Si=80 / 20).

[0169] (3) Preparation of Negative Electrode Slurry for Second Electric Storage Device

[0170] A second slurry for negative electrodes of an electricity storage device was prepared in the same manner as in the first slurry for negative electrodes of an electricity storage device except that the polymer (A1) was changed to the polymer (B1).

[0171] 3.1.3. Manufacturing and evaluation of negative electrodes for power storage devices

[0172] (1) Manufacturing of negative electrodes for power storage devices

[0173] The first storage device negative electrode slurry obtained above was uniformly applied on the surface of a negative electrode collector made of copper foil with a thickness of 20 μm by a doctor blade method so that the film thickness after drying was 50 μm, and then dried at 60°C for 10 minutes and then at 120°C for 10 minutes. Then, the layer density was 1.5 g / cm 3 The first layer is obtained by performing pressing using a roller press.

[0174] The second negative electrode slurry for the power storage device obtained above was uniformly applied on the first layer obtained above by a doctor blade method so that the film thickness after drying was 50 μm, and then dried at 60° C. for 10 minutes and then at 120° C. for 10 minutes. Then, the layer density was 1.5 g / cm 3The negative electrode for an electricity storage device having a negative electrode composite layer composed of a first layer and a second layer is obtained by performing pressing using a roll press in a manner.

[0175] (2) Evaluation of the adhesion strength of the negative electrode composite layer

[0176] Use a cutter to make 10 deep cuts from the negative electrode composite layer to the negative electrode collector at 2 mm intervals in the vertical and horizontal directions on the surface of the negative electrode for the storage device obtained above to make a checkerboard cut. Paste an 18 mm wide adhesive tape (manufactured by NICHIBAN Co., Ltd., trade name "Cellotape" (registered trademark), specified in JIS Z1522: 2009) on the cut and immediately peel it off, and evaluate the degree of detachment of the negative electrode composite layer by visual judgment. The evaluation criteria are as follows. The evaluation results are shown in Table 1 below.

[0177] (Evaluation Criteria)

[0178] 5 points: No negative electrode composite layer was detached.

[0179] 4 points: 1 to 5 negative electrode composite layers are missing.

[0180] 3 points: 6 to 20 negative electrode composite layers have fallen off.

[0181] 2 points: 21 to 40 negative electrode composite layers have fallen off.

[0182] 1 point: 41 or more negative electrode composite layers were missing.

[0183] (3) Evaluation of the leveling properties of the negative electrode composite layer

[0184] The thickness of the negative electrode for the storage device obtained above was measured at 10 points in a range of 10 cm in length at both ends of the coating surface perpendicular to the coating direction of the first and second storage device negative electrode slurries. The deviation of the measured thickness was evaluated as leveling. The evaluation criteria were as follows. The evaluation results are shown in Table 1 below.

[0185] (Evaluation Criteria)

[0186] 5 points: Standard deviation less than 2μm

[0187] 4 points: Standard deviation is 2 μm or more and less than 3 μm

[0188] 3 points: Standard deviation is 3 μm or more and less than 4 μm

[0189] 2 points: Standard deviation is 4 μm or more and less than 5 μm

[0190] 1 point: Standard deviation is 5 μm or more

[0191] 3.1.4. Manufacturing and evaluation of power storage devices

[0192] (1) Manufacturing of the positive electrode

[0193] Into a twin-shaft planetary mixer (manufactured by PRIMIX Co., Ltd., trade name "TK HIVIS MIX 2P-03"), 4 parts by mass (solid content conversion value) of a binder for an electrochemical device electrode (manufactured by KUREHA Co., Ltd., trade name "KF polymer #1120"), 3 parts by mass of a conductive aid (manufactured by Denka Co., Ltd., trade name "Denka Black 50% pressed product"), 100 parts by mass (solid content conversion value) of LiCoO2 (manufactured by HAYASHI Chemical Co., Ltd.) having an average particle size of 5 μm as a positive electrode active material, and 36 parts by mass of N-methylpyrrolidone (NMP) were added and stirred at 60 rpm for 2 hours. NMP was added to the obtained paste to adjust the solid content concentration to 65% by mass, and then the mixture was stirred and mixed at 200 rpm for 2 minutes and at 1800 rpm for 5 minutes using a stirring degassing machine (manufactured by THINKY Co., Ltd., trade name "Degassing Rentaro"). The mixture was further stirred and mixed under reduced pressure (about 2.5×10 4 Pa) was stirred and mixed at 1800 rpm for 1.5 minutes to prepare a positive electrode slurry for a storage device. The positive electrode slurry for a storage device was uniformly coated on the surface of a positive electrode collector composed of aluminum foil by a doctor blade method in a manner such that the film thickness after removing the solvent was 80 μm, and heated at 120° C. for 20 minutes to remove the solvent. Thereafter, the density of the positive electrode active material layer was 3.0 g / cm 3 The counter electrode (positive electrode) was obtained by pressing the substrate using a roller press.

[0194] (2) Assembly of lithium-ion battery cells

[0195] In a glove box replaced by Ar in a manner that the dew point is below -80°C, the negative electrode of the above-made power storage device is punched into a molded product with a diameter of 16.16 mm, and it is placed on a 2-pole coin-type battery (manufactured by Hohsen Co., Ltd., trade name "HS Flat Cell"). Next, a separator (manufactured by Celgard Co., Ltd., trade name "Celgard#2400") punched into a 24 mm diameter polypropylene porous membrane is placed, and after further injecting 500 μL of electrolyte in a manner to avoid air entry, the counter electrode (positive electrode) punched into a molded product with a diameter of 15.95 mm is placed, and the outer casing of the above-mentioned 2-pole coin-type battery is tightened and sealed with screws, thereby assembling a lithium-ion battery cell (power storage device). The electrolyte used here is a solution in which LiPF6 is dissolved at a concentration of 1 mol / L in a solvent of ethylene carbonate / ethyl methyl carbonate = 1 / 1 (mass ratio).

[0196] (3) Evaluation of cycle characteristics

[0197] The lithium-ion battery cell manufactured as described above was charged at a constant current (1.0C) in a thermostatic chamber regulated at 25°C. When the voltage reached 4.2V, the charging was continued at a constant voltage (4.2V). The moment when the current value reached 0.05C was regarded as the end of charging (cut-off). Thereafter, discharge was started at a constant current (1.0C), and the moment when the voltage reached 3.0V was regarded as the end of discharge (cut-off), and the discharge capacity of the first cycle was calculated. This charge and discharge was repeated 300 times. The capacity retention rate was calculated by the following formula (1) and evaluated according to the following criteria. The evaluation results are shown in Table 1 below.

[0198] Capacity retention rate (%) = ((discharge capacity at the 300th cycle) / (discharge capacity at the 1st cycle)) × 100 (1)

[0199] (Evaluation Criteria)

[0200] 5 points: The capacity retention rate is 95% or more.

[0201] 4 points: The capacity retention rate is 90% or more and less than 95%.

[0202] 3 points: The capacity retention rate is 85% or more and less than 90%.

[0203] 2 points: The capacity retention rate is 80% or more and less than 85%.

[0204] 1 point: The capacity retention rate is 75% or more and less than 80%.

[0205] 0 points: The capacity retention rate is less than 75%.

[0206] (4) Evaluation of expansion characteristics

[0207] The lithium-ion battery cell manufactured as described above was charged at a constant current (1.0C) in a thermostatic chamber set at 45°C. When the voltage reached 4.2V, the charging was continued at a constant voltage (4.2V). The moment when the current value reached 0.05C was regarded as the end of charging (cut-off). Thereafter, discharge was started at a constant current (1.0C), and the moment when the voltage reached 3.0V was regarded as the end of discharge (cut-off), and the discharge capacity of the first cycle was calculated. After 300 times of charge and discharge, the lithium-ion battery cell was disassembled, and the negative electrode for the storage device was cleaned with dimethyl carbonate and dried. The inhibition rate of electrode expansion was calculated by the following formula (2), and the expansion characteristics were evaluated according to the following criteria. The evaluation results are shown in Table 1 below.

[0208] Electrode expansion suppression rate (%) = (1 - ((negative electrode film thickness at the 300th cycle) - (negative electrode film thickness at the 1st cycle)) ÷ negative electrode film thickness at the 1st cycle) × 100·····(2)

[0209] (Evaluation Criteria)

[0210] 5 points: The inhibition rate of electrode expansion was 95% or more.

[0211] 4 points: The suppression rate of electrode expansion is 90% or more and less than 95%.

[0212] 3 points: The suppression rate of electrode expansion is 85% or more and less than 90%.

[0213] 2 points: The suppression rate of electrode expansion is 80% or more and less than 85%.

[0214] 1 point: The suppression rate of electrode expansion was 75% or more and less than 80%.

[0215] 0 points: The inhibition rate of electrode expansion is less than 75%.

[0216] 3.2. Examples 2 to 18, Comparative Examples 1 to 6

[0217] In the above-mentioned "3.1.1. Synthesis and physical property evaluation of polymer", the types and amounts of each monomer were respectively as described in Tables 1 to 3 below, and the same procedures were followed to obtain polymer particle dispersions having a solid content concentration of 20% by mass and a pH of 8.0. In addition, a slurry for a negative electrode of a storage device was prepared in the same manner as in Example 1, and a negative electrode of a storage device and a storage device were prepared, respectively, and evaluated in the same manner as in Example 1.

[0218] 3.3. Evaluation results

[0219] The polymer compositions, the results of the measurement of physical properties, and the evaluation results used in Examples 1 to 18 and Comparative Examples 1 to 6 are shown in Tables 1 to 3 below. The numerical values ​​showing the polymer compositions shown in Tables 1 to 3 below represent parts by mass.

[0220]

[0221]

[0222]

[0223] In addition, the monomers in the above Table 1 to the above Table 3 respectively represent the following compounds.

[0224] <Unsaturated carboxylic acid>

[0225] AA: Acrylic acid

[0226] MAA: Methacrylic acid

[0227] TA: Itaconic acid

[0228] <Conjugated diene compounds>

[0229] BD: 1,3-Butadiene

[0230] <Aromatic vinyl compounds>

[0231] ·ST:Styrene

[0232] <Unsaturated carboxylic acid ester>

[0233] MMA: Methyl methacrylate

[0234] <α,β-Unsaturated nitrile compounds>

[0235] AN: Acrylonitrile

[0236] From the evaluation results of Table 1 to Table 3 above, it can be seen that according to Examples 1 to 18, by making the first layer contain a polymer (A) with a relatively large amount of acid and making the second layer contain a polymer (B) with a relatively small amount of acid, the leveling property in the negative electrode composite layer is excellent, and the adhesion between the negative electrode collector and the negative electrode composite layer is improved, so that the electrode expansion can be effectively suppressed. In addition, it can be seen that the binding force between the negative electrode active materials is improved, so the cycle characteristics of the storage device are improved.

[0237] The present invention is not limited to the above-mentioned embodiments, and various modifications are possible. The present invention includes a configuration substantially the same as the configuration described in the embodiments (for example, a configuration with the same function, method and result, or a configuration with the same purpose and effect). In addition, the present invention includes a configuration obtained by replacing the non-essential part of the configuration described in the above-mentioned embodiments with other configurations. In addition, the present invention also includes a configuration that can play the same role and effect as the configuration described in the above-mentioned embodiments, or a configuration that can achieve the same purpose. And the present invention also includes a configuration in which a known technology is added to the configuration described in the above-mentioned embodiments.

Claims

1. A negative electrode for an electric storage device, comprising a negative electrode current collector and a negative electrode composite layer formed on the negative electrode current collector, The negative electrode composite layer includes a first layer formed on the negative electrode current collector and a second layer formed on the first layer. The first layer comprises a first negative electrode active material and a polymer A, The polymer A contains 5 to 20% by mass of the repeating unit a1 derived from an unsaturated carboxylic acid, when the total amount of the repeating units contained in the polymer A is 100% by mass. The second layer comprises a second negative electrode active material and a polymer B, When the total of the repeating units contained in the polymer B is 100% by mass, the polymer B contains 0.1% by mass or more and less than 5% by mass of the repeating unit a1 derived from an unsaturated carboxylic acid.

2. The negative electrode for an electric storage device according to claim 1, in, When the total amount of the repeating units contained in the polymer A is 100% by mass, the polymer A contains 1% by mass or more and less than 20% by mass of the repeating unit a3 derived from an aromatic vinyl compound, When the total of the repeating units contained in the polymer B is 100 mass %, the polymer B contains 20 mass % or more and less than 40 mass % of the repeating units a3 derived from the aromatic vinyl compound.

3. The negative electrode for an electric storage device according to claim 1 or 2, in, When the total amount of the repeating units contained in the polymer A is 100% by mass, the polymer A contains 15% by mass to 60% by mass of the repeating unit a2 derived from the conjugated diene compound. When the total amount of the repeating units contained in the polymer B is 100% by mass, the polymer B contains 15% by mass to 60% by mass of the repeating unit a2 derived from the conjugated diene compound.

4. The negative electrode for an electric storage device according to claim 1 or 2, in, When the total amount of the repeating units contained in the polymer A is 100% by mass, the polymer A contains 1% by mass to 20% by mass of the repeating unit a4 derived from an unsaturated carboxylic acid ester. When the total amount of the repeating units contained in the polymer B is 100% by mass, the polymer B contains 1% by mass to 20% by mass of the repeating unit a4 derived from the unsaturated carboxylic acid ester.

5. The negative electrode for an electric storage device according to claim 1 or 2, in, When the total amount of the repeating units contained in the polymer A is 100% by mass, the polymer A contains 5% by mass to 40% by mass of the repeating unit a5 derived from the α,β-unsaturated nitrile compound. When the total amount of the repeating units contained in the polymer B is 100% by mass, the polymer B contains 5% by mass to 40% by mass of the repeating unit a5 derived from the α,β-unsaturated nitrile compound.

6. The negative electrode for an electric storage device according to claim 1 or 2, in, The polymer A and the polymer B are particles, The number average particle size of the particles of the polymer A is 150 nm to 300 nm, The number average particle size of the particles of the polymer B is 50 nm or more and less than 150 nm. 7 . An electric storage device comprising the negative electrode for an electric storage device according to claim 1 .