Pole piece, electrochemical device and electronic device

By setting coatings with different adhesion forces on the edge of the electrode sheet, the balance between the electrical performance and volume energy density of the electrochemical device is solved, the electrical performance and safety performance of the electrochemical device are improved, and the electrode sheet is reduced. The cutter affects and maintains the stability of the volume energy density.

CN118969960AActive Publication Date: 2024-11-15NINGDE AMPEREX TECHNOLOGY LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411036303.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2020-08-31
Publication Date
2024-11-15
Estimated Expiration
2040-08-31

AI Technical Summary

Technical Problem

While improving the electrical properties of existing electrochemical devices, it is difficult to maintain volume energy density, and pole sheets are prone to burrs or debris when stripping, affecting the safety performance of electrochemical devices.

Method used

The edge area of ​​the electrode sheet is provided with different adhesion forces so that the adhesion force between it and the isolation film is greater than the adhesion force between the active material layer and the isolation film, reducing the influence of the cutting knife on the electrode sheet. , and improve the adhesion of edge areas, thereby improving the electrical and safety performance of electrochemical devices while minimizing the impact on volume energy density.

Benefits of technology

By setting a high-adhesion coating on the edge of the electrode sheet, the impact of the cutter during striping is reduced, the adhesion between the electrode sheet and the isolation film is improved, the electrical and safety performance of the electrochemical device is improved, while maintaining volume energy stability of density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969960A_ABST
    Figure CN118969960A_ABST
Patent Text Reader

Abstract

The invention provides a pole piece, an electrochemical device and an electronic device. The pole piece comprises a current collector; the first coating layer is arranged on the current collector, the first coating layer comprises an active material, and the first coating layer sequentially comprises a first edge part, a middle part and a second edge part in the width direction of the current collector; a second coating including a first portion and a second portion disposed on the first edge portion and the second edge portion, respectively; wherein the surface, far away from the first edge part, of the first part has a first bonding force, the surface, far away from the second edge part, of the second part has a second bonding force, the surface, far away from the current collector, of the middle part has a third bonding force, and the first bonding force and the second bonding force are both larger than the third bonding force. The embodiments of the present application improve the electrical performance and safety performance of the electrochemical device while minimizing the influence on the volumetric energy density of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent with application number 202080010007.5 (international application number: PCT / CN2020 / 112469) filed on August 31, 2020, whose invention name is "Electrode, electrochemical device and electronic device". Technical Field

[0002] The present application relates to the field of electronic technology, and in particular to pole pieces, electrochemical devices and electronic devices. Background Art

[0003] At present, in order to ensure the processing and safety performance of the electrode, a high-adhesion coating can be applied to cover the entire active material layer or current collector, but this will lose the volume energy density of the electrochemical device (for example, lithium-ion battery). How to improve the electrical performance of the electrochemical device while ensuring its volume energy density is a problem to be solved. Summary of the invention

[0004] The embodiment of the present application provides a high-adhesion coating in a specific area, which can improve the electrical performance and safety performance of the electrochemical device while minimizing the impact on the volume energy density of the electrochemical device.

[0005] An embodiment of the present application provides a pole piece, comprising: a current collector; a first coating, arranged on the current collector, the first coating comprising an active material, and the first coating comprising a first edge portion, a middle portion, and a second edge portion in sequence in the width direction of the current collector; a second coating, comprising a first portion and a second portion, respectively arranged on the first edge portion and the second edge portion; wherein a surface of the first portion away from the first edge portion has a first bonding force, a surface of the second portion away from the second edge portion has a second bonding force, a surface of the middle portion away from the current collector has a third bonding force, and both the first bonding force and the second bonding force are greater than the third bonding force.

[0006] In some embodiments, the first portion has a width d1, the second portion has a width d2, the first coating has a width D, and wherein 1%≤d1 / D≤10%, 1%≤d2 / D≤10%.

[0007] In some embodiments, the first bonding force and the second bonding force are both 2 to 10 times greater than the third bonding force; and / or the first bonding force and the second bonding force are both greater than 5 N / m.

[0008] In some embodiments, the thickness of the second coating layer is h, the thickness of the middle portion is H, 0.5 μm<h<8 μm, 20 μm<H<200 μm.

[0009] In some embodiments, the first coating includes a first binder, the content of the first binder is 0.5% to 6%, and the first binder includes at least one of polyvinylidene fluoride, vinylidene fluoride-fluorinated olefin copolymer, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl acrylate, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, fluorinated rubber or polyvinyl alcohol.

[0010] In some embodiments, the second coating includes a second binder, the content of the second binder is 30% to 80%, and the second binder includes at least one of polyvinylidene fluoride, vinylidene fluoride-fluorinated olefin copolymer, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl acrylate, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, fluorinated rubber or polyvinyl alcohol.

[0011] In some embodiments, in the length direction of the first coating, the first portion and / or the second portion are non-continuously coated, and the ratio of the total coating length of the first portion to the length of the first coating is greater than 80%, and the ratio of the total coating length of the second portion to the length of the first coating is greater than 80%.

[0012] In some embodiments, at least a portion of the current collector is etched.

[0013] In some embodiments, the regions of the current collector corresponding to the first edge portion and the second edge portion are etched, and the roughness of the regions of the current collector corresponding to the first edge portion and the second edge portion is 2 to 4 times the roughness of the region of the current collector corresponding to the middle portion.

[0014] Another embodiment of the present application provides an electrochemical device, comprising: a positive electrode sheet; a negative electrode sheet; and a separator, disposed between the positive electrode sheet and the negative electrode sheet; wherein the positive electrode sheet and / or the negative electrode sheet is any of the above-mentioned electrode sheets.

[0015] An embodiment of the present application further provides an electronic device, comprising the above-mentioned electrochemical device.

[0016] The embodiments of the present application provide coatings with different adhesive forces on the edge regions of the active material layer, so that the adhesive force between the coating and the isolation membrane is greater than the adhesive force between the active material layer and the isolation membrane, which can reduce the impact of the cutter on the pole piece when the pole piece is stripped (for example, generating burrs or debris). In addition, since the coating is provided on the edge region of the active material, the adhesive force between the edge region of the pole piece and the isolation membrane can be improved, thereby reducing the impact of the pole piece demolding on the electrode assembly at the level of the electrode assembly, thereby improving the electrical performance and safety performance of the electrochemical device, and since the coating is provided only on the edge region of the active material layer, the impact on the volume energy density of the electrochemical device can be minimized. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A front view of a pole piece according to an embodiment of the present application is shown.

[0018] Figure 2 A top view of a first coating layer (continuous) and a current collector according to an embodiment of the present application is shown.

[0019] Figure 3 A top view of a first coating layer (discontinuous) and a current collector according to another embodiment of the present application is shown.

[0020] Figure 4 A front view of an electrode assembly of an electrochemical device according to an embodiment of the present application is shown. DETAILED DESCRIPTION

[0021] The following embodiments may enable those skilled in the art to more fully understand the present application, but do not limit the present application in any way.

[0022] like Figure 1 As shown, a front view (cross-sectional view) of a pole piece of an embodiment of the present application is provided. The pole piece may include a current collector 1 and a first coating 2 disposed on the current collector 1. In some embodiments, the first coating 2 includes an active material. In some embodiments, the first coating 2 includes a first edge portion 4, a middle portion 6, and a second edge portion 5 in sequence in the width direction of the current collector 1, wherein the middle portion 6 is located between the first edge portion 4 and the second edge portion 5. It should be understood that although Figure 1 The first edge portion 4, the second edge portion 5 and the middle region 6 are distinguished by a dotted line, but in fact there may be no boundary at the dotted line. In some embodiments, the pole piece further includes a second coating 3, and the second coating 3 may include a first portion 7 and a second portion 8 respectively disposed on the first edge portion 4 and the second edge portion 5. In some embodiments, the material, width, thickness, etc. of the first portion 7 and the second portion 8 may be the same or different.

[0023] In some embodiments, the first portion 7 may have a first adhesive force away from the first edge portion, that is, the first portion 7 and the separator may have a first adhesive force; the second portion 8 may have a second adhesive force away from the surface of the second edge portion, that is, the second portion 8 and the separator may have a second adhesive force; the middle portion 6 may have a third adhesive force away from the surface of the current collector, that is, the middle portion 6 and the separator may have a third adhesive force, and the first adhesive force and the second adhesive force are both greater than the third adhesive force. In the embodiment of the present application, the first portion 7 and the second portion 8 of the second coating 3 are respectively arranged on the first edge portion 4 and the second edge portion 5 of the first coating 2, so as to reduce the influence of the cutter on the pole piece when the pole piece is stripped (for example, generating burrs or debris). In addition, since the first adhesive force and the second adhesive force are both greater than the third adhesive force, the adhesive force between the edge region of the pole piece and the separator can be improved, thereby reducing the influence of the pole piece demolding on the electrode assembly at the level of the electrode assembly, thereby improving the electrical performance and safety performance of the electrochemical device, and at the same time, since the second coating 3 is only arranged on the edge portion of the first coating 2, the influence on the volume energy density of the electrochemical device can be minimized.

[0024] In some embodiments, the first portion 7 has a width d1, the second portion 8 has a width d2, the first coating 2 has a width D, 1%≤d1 / D≤10%, 1%≤d2 / D≤10%. If the width of the first portion 7 or the second portion 8 is too small, for example, less than 1% of the width of the first coating 2, the second coating 3 has limited effect in improving the bonding force with the separator. If the width of the first portion 7 or the second portion 8 is too large, for example, greater than 10% of the width of the first coating 2, the volume energy density of the electrochemical device may be adversely affected.

[0025] In some embodiments, the first bonding force and the second bonding force are both 2 to 10 times of the third bonding force. In some embodiments, the first bonding force and the second bonding force are both greater than 5 N / m. In this way, a strong bonding force between the second coating 3 and the isolation film can be well ensured.

[0026] In some embodiments, the thickness of the second coating layer 3 is h, the thickness of the middle portion of the first coating layer 2 is H, 0.5 μm < h < 8 μm, 20 μm < H < 200 μm. In some embodiments, the thickness H of the middle portion of the second coating layer may be equal to the sum of the thicknesses of the first edge portion 4 and the first portion 7, or may be equal to the sum of the thicknesses of the second edge portion 5 and the second portion 8. If the thickness of the second coating layer 3 is too small, for example, less than 0.5 μm, a sufficiently strong bonding force between the second coating layer 3 and the separator cannot be ensured. If the thickness of the second coating layer is too large, the volume energy density of the electrochemical device may be adversely affected. If the thickness of the first coating layer 2 is too small, the amount of active material per unit area may be too small, affecting the volume energy density of the electrochemical device. If the thickness of the first coating layer 2 is too large, the insertion and extraction efficiency of lithium ions may be affected due to the long movement path of the insertion and extraction of lithium ions at the first coating layer 2 close to the current collector.

[0027] In some embodiments, the first coating 2 further includes a first binder. In some embodiments, the first binder includes at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-fluorinated olefin, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl acrylate, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, fluorinated rubber, or polyvinyl alcohol. In some embodiments, the content of the first binder in the first coating 2 is 0.5% to 6%. If the content of the first binder is too small, sufficient bonding force cannot be provided for the material of the first coating 2, and bonding between the first coating 2 and the current collector or between the first coating 2 and the isolation film is not conducive. If the content of the first binder is too large, the volume energy density of the electrochemical device is adversely affected.

[0028] In some embodiments, the second coating 3 includes a second binder. In some embodiments, the second binder includes at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-fluorinated olefin, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl acrylate, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, fluorinated rubber or polyvinyl alcohol. In some embodiments, the mass content of the second binder in the second coating 3 is 30% to 80%. If the mass content of the second binder is too small, sufficient bonding between the second coating 2 and the isolation film cannot be fully ensured. If the mass content of the second binder is too large, the conductive performance of the second coating 3 will be too low.

[0029] In some embodiments, the second coating 3 also includes a conductive agent. In some embodiments, the conductive agent in the second coating 3 may include at least one of conductive carbon black, carbon nanotubes, conductive graphite, graphene, acetylene black, or nano-carbon fibers. In some embodiments, the mass content of the conductive agent in the second coating 3 is 20% to 70%. If the mass content of the conductive agent in the second coating 3 is too small, the conductivity of the second coating 3 will be adversely affected. If the mass content of the conductive agent in the second coating 3 is too large, the mass content of the second binder will be too small, affecting the bonding performance of the second coating 3. In some embodiments, the second coating 3 also includes ceramic particles.

[0030] It should be understood that although Figure 1 It is shown that the first coating layer 2 and the second coating layer 3 are formed on both sides of the current collector 1 , but this is only exemplary, and the first coating layer 2 and the second coating layer 3 may be formed only on one side of the current collector 1 .

[0031] like Figure 2 , a top view of a second coating (continuous) and a first coating according to an embodiment of the present application is shown. For simplicity, only the middle portion 6 of the first coating 2 and the first portion 7 and the second portion 8 of the second coating 3 are shown. Figure 2 The dotted line in the figure shows the stripping position of the pole piece. By providing the second coating 3 on the edge portion of the first coating 2, the influence of stress during stripping and the generation of burrs of the current collector during stripping can be reduced. In addition, the bonding performance between the pole piece and the isolation film can also be improved. In some embodiments, in the length direction of the first coating 2, the first portion 7 and / or the second portion 8 can be continuously coated.

[0032] like Figure 3 As shown, in some embodiments, in the length direction of the first coating 2, the first portion 7 and / or the second portion 8 may be non-continuously coated, and the ratio of the total coating length of the first portion 7 to the length of the first coating 2 is greater than 80%, and the ratio of the total coating length of the second portion 8 to the length of the first coating 2 is greater than 80%. By adopting the non-continuous coating method, the impact on the volume energy density of the electrochemical device is further reduced. In addition, if the coating length of the first portion 7 and / or the second portion 8 is too small, it will affect the full play of the bonding performance of the second coating 3.

[0033] In some embodiments, at least part of the region or the entire region of the current collector 1 is etched. By etching the current collector 1, the roughness of the current collector 1 can be increased accordingly, thereby increasing the bonding force between the current collector 1 and the first coating 2. In some embodiments, the region of the current collector 1 corresponding to the first edge portion 4 and the second edge portion 5 is etched, and the roughness of the region of the current collector 1 corresponding to the first edge portion 4 and the second edge portion 5 is 2 to 4 times the roughness of the region of the current collector 1 corresponding to the middle portion 6. By etching the first edge portion 4 and the second edge portion 5, the bonding force between the current collector 1 and the first coating 2 is further enhanced, and the bonding force between the edge region of the overall pole piece and the isolation film is also enhanced. In some embodiments, etching is mainly performed by browning or blackening. Of course, other suitable methods can also be used for etching. In some embodiments, the roughness of the etched region of the current collector 1 is 2 to 4 times that of the unetched region. In some embodiments, the roughness of the unetched region is less than 2μm.

[0034] It should be understood that the electrode of the present application can be either a positive electrode or a negative electrode. Figure 4 As shown, an embodiment of the present application further provides an electrochemical device, which includes an isolation membrane 11, a positive electrode sheet 12 and a negative electrode sheet 13, wherein the isolation membrane 11 is arranged between the positive electrode sheet 12 and the negative electrode sheet 13, wherein the positive electrode sheet 12 and / or the negative electrode sheet 13 are the electrodes of the above structure.

[0035] In some embodiments, the positive electrode current collector of the positive electrode sheet 12 may be aluminum (Al) foil, and of course, other positive electrode current collectors commonly used in the art may also be used. In some embodiments, the thickness of the positive electrode current collector may be 1 μm to 200 μm.

[0036] In some embodiments, when the pole piece is a positive pole piece 12, the active material of the first coating 2 may include at least one of lithium cobaltate, lithium manganate, lithium iron phosphate, lithium nickel cobalt manganate, lithium nickel cobalt aluminum or lithium nickel manganate. In some embodiments, the first coating 2 also includes a conductive agent. In some embodiments, the conductive agent in the first coating 2 may include at least one of conductive carbon black, Ketjen black, lamellar graphite, graphene, carbon nanotubes or carbon fibers. In some embodiments, the mass ratio of the positive active material, the conductive agent and the binder in the first coating 2 may be 91 to 99: 0.5 to 3: 0.5 to 6. It should be understood that the above is only an example, and the positive active material layer may adopt any other suitable material, thickness and mass ratio.

[0037] In some embodiments, the negative electrode current collector of the negative electrode plate 13 may be at least one of copper foil, nickel foil or carbon-based current collector, and of course, other negative electrode current collectors commonly used in the art may also be used. In some embodiments, the thickness of the negative electrode current collector may be 1 μm to 200 μm.

[0038] In some embodiments, when the pole piece is a negative pole piece 13, the active material of the first coating 2 may include at least one of artificial graphite, natural graphite, hard carbon, mesophase carbon microspheres, silicon alloys, tin alloys or pure silicon. In some embodiments, the first coating 2 may also include a conductive agent. The conductive agent in the first coating 2 may include at least one of conductive carbon black, Ketjen black, lamellar graphite, graphene, carbon nanotubes or carbon fibers. It should be understood that the materials disclosed above are only exemplary, and any other suitable material may be used as the first coating 2 as the negative active material layer. In some embodiments, the mass ratio of the negative active material, the conductive agent and the binder in the first coating 2 may be 91 to 99:0 to 3:1 to 6. It should be understood that the above is only an example, and any other suitable mass ratio may be used.

[0039] In some embodiments, the isolation film 11 includes at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide or aramid. For example, polyethylene includes at least one selected from high-density polyethylene, low-density polyethylene or ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have a good effect on preventing short circuits and can improve the stability of the battery through the shutdown effect. In some embodiments, the thickness of the isolation film is in the range of about 5 μm to 20 μm.

[0040] In some embodiments, the surface of the isolation membrane may further include a porous layer, the porous layer is disposed on at least one surface of the isolation membrane, the porous layer includes inorganic particles and a binder, the inorganic particles are selected from at least one of aluminum oxide (Al2O3), silicon oxide (SiO2), magnesium oxide (MgO), titanium oxide (TiO2), hafnium dioxide (HfO2), tin oxide (SnO2), cerium dioxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. In some embodiments, the pores of the isolation membrane have a diameter in the range of about 0.01 μm to 1 μm. The binder of the porous layer is selected from at least one of polyvinylidene fluoride, copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The porous layer on the surface of the separator can improve the heat resistance, oxidation resistance and electrolyte wetting performance of the separator, and enhance the adhesion between the separator and the pole piece.

[0041] In some embodiments of the present application, the electrode assembly of the electrochemical device is a wound electrode assembly or a stacked electrode assembly.

[0042] In some embodiments, the electrochemical device includes a lithium ion battery, but the present application is not limited thereto. In some embodiments, the electrochemical device may further include an electrolyte. The electrolyte may be one or more of a gel electrolyte, a solid electrolyte, and an electrolyte, the electrolyte including a lithium salt and a non-aqueous solvent. The lithium salt is selected from one or more of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB or lithium difluoroborate. For example, the lithium salt is selected from LiPF6 because it can provide high ionic conductivity and improve cycle characteristics.

[0043] The non-aqueous solvent may be selected from carbonate compounds, carboxylate compounds, ether compounds, other organic solvents or combinations thereof.

[0044] The carbonate compound may be selected from a chain carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof.

[0045] The linear carbonate compound may be selected from diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. The cyclic carbonate compound may be selected from ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) or combinations thereof. The fluorocarbonate compound may be selected from fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate or combinations thereof.

[0046] The carboxylate compound may be selected from methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid lactone, valerolactone, mevalonolactone, caprolactone, methyl formate, or a combination thereof.

[0047] The ether compound may be selected from dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.

[0048] Other organic solvents may be selected from dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, and phosphate esters or combinations thereof.

[0049] In some embodiments of the present application, taking a lithium-ion battery as an example, a positive electrode sheet, a separator, and a negative electrode sheet are wound or stacked in sequence to form an electrode component, and then encapsulated in, for example, an aluminum-plastic film, injected with an electrolyte, formed, and encapsulated to form a lithium-ion battery. Then, the prepared lithium-ion battery is subjected to a performance test.

[0050] Those skilled in the art will appreciate that the above-described method for preparing an electrochemical device (eg, a lithium-ion battery) is only an example, and other methods commonly used in the art may be used without departing from the disclosure of the present application.

[0051] Embodiments of the present application also provide electronic devices including the above-mentioned electrochemical devices. The electronic devices of the embodiments of the present application are not particularly limited, and they can be any electronic devices known in the prior art. In some embodiments, the electronic device can include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0052] Some specific embodiments and comparative examples are listed below to better illustrate the present application, wherein a lithium-ion battery is used as an example.

[0053] Example 1

[0054] Preparation of positive electrode sheet: The positive electrode active material lithium cobalt oxide, conductive agent conductive carbon black, and binder polyvinylidene fluoride (PVDF) are dissolved in N-methylpyrrolidone (NMP) solution at a weight ratio of 97.6:1.1:1.3 to form positive electrode slurry. Aluminum foil is used as the positive electrode current collector, and the positive electrode slurry is coated on the positive electrode current collector with a coating thickness of 50μm. After drying, cold pressing, and slitting, the positive electrode sheet is obtained.

[0055] Preparation of negative electrode sheet: Dissolve the negative electrode active material artificial graphite and the binder styrene-butadiene rubber in deionized water at a weight ratio of 98:2 to form a first coating slurry. Use a copper foil with a thickness of 10 μm and a width of 80 mm as the negative electrode current collector, apply the first coating slurry on the negative electrode current collector to a coating thickness of 60 μm, and dry to obtain the first coating;

[0056] The first binder polyvinylidene fluoride and the first conductive agent conductive carbon black are dissolved in N-methylpyrrolidone (NMP) solution at a weight ratio of 60:40 to form a second coating slurry. The second coating slurry is applied to the two edge portions of the first coating, with a coating width of 5 mm and a thickness of 2 μm on the two edge portions, and then dried, cold pressed, and cut to obtain a negative electrode sheet.

[0057] Preparation of isolation membrane: The isolation membrane substrate is 8 μm thick polyethylene (PE), and a 2 μm alumina ceramic layer is coated on both sides of the isolation membrane substrate. Finally, 2.5 mg of binder polyvinylidene fluoride (PVDF) is coated on both sides of the ceramic layer and dried.

[0058] Preparation of electrolyte: In an environment with a water content of less than 10 ppm, lithium hexafluorophosphate and a non-aqueous organic solvent (ethylene carbonate (EC): dimethyl carbonate (DMC) = 40:60, weight ratio) are prepared in a weight ratio of 8:92 to form an electrolyte.

[0059] Preparation of lithium-ion battery: stack the positive electrode sheet, separator, and negative electrode sheet in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and wind them to obtain the electrode assembly. Place the electrode assembly in the outer packaging aluminum plastic film, remove moisture at 80°C, inject the above electrolyte and package, and obtain the lithium-ion battery through the process of formation, degassing, trimming, etc.

[0060] Other examples and comparative examples are based on the steps of Example 1 with parameter changes, wherein in Comparative Example 1, a bottom coating is first coated on the negative electrode current collector, the thickness of the bottom coating is 2 μm, and the material of the bottom coating is composed of polyvinylidene fluoride and conductive carbon black in a weight ratio of 60:40. The specific changed parameters are shown in the following table.

[0061] The test methods for various parameters of this application are described below.

[0062] Test method for volume energy density:

[0063] Place the lithium-ion battery in a 25℃ constant temperature box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge the lithium-ion battery that has reached a constant temperature at a constant current of 0.5C to a voltage of 4.4V, then charge it at a constant voltage of 4.4V to a current of 0.05C, and discharge it at 0.5C to a voltage of 3.0V, and record the discharge energy.

[0064] Volume energy density = discharge energy / (length*width*thickness of lithium-ion battery).

[0065] Cyclic expansion rate test:

[0066] The thickness of the plate of the lithium-ion battery after formation was measured. After the lithium-ion battery was placed in a constant temperature box at 45℃±2℃ for 2 hours, it was charged to 4.4V at a rate of 1C, and then charged to 0.05C at a constant voltage at 4.4V. It was then discharged to 3.0V at a rate of 1C. This process was considered as a cycle. After the lithium-ion battery was cycled 500 times, the thickness of the plate of the lithium-ion battery was tested. Four lithium-ion batteries were taken from each group, and the average value was taken to calculate the cycle expansion rate of the lithium-ion battery.

[0067] Cycle expansion ratio = (thickness of the lithium ion battery after 500 cycles / thickness of the lithium ion battery after formation - 1) x 100%.

[0068] Table 1 shows various parameters and evaluation results of Examples and Comparative Examples.

[0069] Table 1

[0070]

[0071]

[0072] By comparing Example 1 and Comparative Example 1, it can be seen that, relative to the lithium-ion battery in which the negative electrode plate in Comparative Example 1 has a bottom coating, the volume energy density in Example 1 is increased by 1.2% by eliminating the bottom coating. At the same time, because the high-viscosity coating is applied to the pole piece, it can not only reduce the influence of the cutter on the thickness of the edge of the pole piece during slitting, but also achieve a good bonding effect with the isolation membrane, inhibit the expansion process of the pole piece, and reduce the cycle expansion rate by 1%. Examples 2 to 4 can achieve slight regulation of the pole piece expansion rate and volume energy density by regulating the width of the applied high-viscosity coating. In addition, as the width of the second coating (i.e., the high-viscosity coating) increases, the volume energy density improvement rate tends to decrease.

[0073] By comparing Examples 5 to 7 with Comparative Example 1, it can be seen that for pole pieces with active material coatings of different thicknesses, the energy density and pole piece expansion rate can be improved by coating the high-viscosity coating on the active material layer. In addition, as the thickness of the first coating (i.e., the active material layer) increases, the volume energy density improvement rate tends to decrease, while the cycle expansion rate reduction rate tends to increase.

[0074] By comparing Examples 8, 9, 10 and Comparative Example 1, the thickness of the high-viscosity coating on the active material layer can also be adjusted, and the energy density and the expansion rate of the pole piece can be improved under different coating thicknesses. However, when the coating thickness is too thin, the good bonding between the pole piece and the isolation film cannot be guaranteed, and the control effect on the expansion rate of the pole piece is slightly limited, but the effect of improving the energy density is more obvious, which can reach 1.3%.

[0075] By comparing Examples 11 to 12 with Comparative Example 1, the adhesive force can be adjusted by adjusting the adhesive content of the high-viscosity coating, and the content of the adhesive has no effect on the effect of improving the volume energy density, which can reach 1.2%. However, different adhesive contents will affect the expansion rate of the pole piece.

[0076] By comparing Example 13 and Comparative Example 1, the intermittent coating method is used to apply the high-viscosity coating. This method can not only further improve the volume energy density of the battery, which can be increased to 1.4%, but also because it also has a limiting effect on the entire pole piece, the expansion rate of the pole piece can still achieve an improvement of 1%.

[0077] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of disclosure involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features. For example, the above features are replaced with the technical features with similar functions disclosed in the present application.

Claims

1. A pole piece, characterized in that: include: current collector; A first coating layer disposed on the current collector, the first coating layer comprising an active material, and the first coating layer sequentially comprising a first edge portion, a middle portion, and a second edge portion in a width direction of the current collector; a second coating layer comprising a first portion and a second portion disposed on the first edge portion and the second edge portion, respectively; Among them, the surface of the first part away from the first edge part has a first adhesion force, the surface of the second part away from the second edge part has a second adhesion force, the surface of the middle part away from the current collector has a third adhesion force, the first adhesion force and the second adhesion force are both greater than the third adhesion force, the first coating includes a first adhesive, the mass content of the first adhesive is 0.5% to 6%, and the second coating includes a second adhesive, the mass content of the second adhesive is 30% to 80%.

2. The pole piece according to claim 1, wherein: The first portion has a width d1, the second portion has a width d2, the first coating has a width D, and wherein 1%≤d1 / D≤10%, 1%≤d2 / D≤10%.

3. The pole piece according to claim 1, wherein: The first bonding force and the second bonding force are both 2 to 10 times of the third bonding force; and / or the first bonding force and the second bonding force are both greater than 5 N / m.

4. The pole piece according to claim 1, wherein: The thickness of the second coating layer is h, the thickness of the middle portion is H, 0.5 μm<h<8 μm, 20 μm<H<200 μm.

5. The pole piece according to claim 1, wherein: The first binder includes at least one of polyvinylidene fluoride, copolymer of vinylidene fluoride and fluorinated olefin, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl acrylate, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, fluorinated rubber or polyvinyl alcohol, and the second binder includes at least one of polyvinylidene fluoride, copolymer of vinylidene fluoride and fluorinated olefin, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl acrylate, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, fluorinated rubber or polyvinyl alcohol.

6. The pole piece according to claim 1, wherein: In the length direction of the first coating, the first part and / or the second part are non-continuously coated, and the ratio of the total coating length of the first part to the length of the first coating is greater than 80%, and the ratio of the total coating length of the second part to the length of the first coating is greater than 80%.

7. The pole piece according to claim 1, wherein: At least a portion of the current collector is etched.

8. The pole piece according to claim 7, wherein: The regions of the current collector corresponding to the first edge portion and the second edge portion are etched, and the roughness of the regions of the current collector corresponding to the first edge portion and the second edge portion is 2 to 4 times the roughness of the region of the current collector corresponding to the middle portion.

9. An electrochemical device, characterized in that: include: Positive electrode; Negative electrode; as well as A separator, disposed between the positive electrode sheet and the negative electrode sheet; Wherein, the positive electrode sheet and / or the negative electrode sheet is a sheet according to any one of claims 1 to 8.

10. An electronic device, characterized in that: Comprising the electrochemical device according to claim 9.

Citation Information

Patent Citations

  • Positive electrode plate, electrochemical device and electronic device containing same

    CN109244362A

  • Electrode plate and electrochemical device

    CN110943222A

  • Pole piece burr removing method, lithium ion battery pole pieces and lithium ion battery

    CN111293277A

  • Electrochemical apparatus and electronic apparatus

    US20230261200A1