Composite pole piece and preparation method and application thereof
Through the composite pole sheet preparation method, the safety and circulation performance of the secondary battery are improved, the fire and explosion risks caused by the unstable pole sheet structure are solved, and the battery capacity retention rate and assembly efficiency are achieved.
Patent Information
- Application Number
- CN202410902590.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-07
- Publication Date
- 2024-11-15
AI Technical Summary
Existing high-compression active materials can easily lead to unstable pole sheet structure in secondary batteries, increase the risk of fire or explosion, and have low circulation and safety performance.
A composite electrode sheet preparation method is adopted to prepare a slurry by mixing active materials, adhesives and conductive agents and then coat them on both sides of the current collector. After heating and rolling, organic polymer glue and diaphragm are added to lift the electrode sheet. mechanical properties and ion transport capability of electrolyte.
It effectively reduces the occurrence of pole segment fracture and short circuit, improves the safety and circulation performance of the battery, reduces assembly difficulty and time, and improves the capacity retention rate of the battery.
Smart Images

Figure CN118969966A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of batteries, and in particular to a composite pole piece and a preparation method and application thereof. Background Art
[0002] At present, in order to meet the needs of high capacity and long cycle of secondary batteries, the application of high-density active materials has received widespread attention. When the compaction density of the active material is high, the damage of the membrane to the current collector foil will increase, causing the mechanical properties of the pole piece to change, and then causing the cycle performance and safety performance of the secondary battery to be reduced. For example, hot pressing can easily cause the pole piece to break and short-circuit. Since the pole piece is structurally unstable at high temperatures, when the secondary battery is used at high temperatures, the pole piece and the electrolyte produce a large number of side reactions, causing thermal runaway, and there is a risk of causing fire or explosion. Summary of the invention
[0003] The purpose of the present invention is to address the deficiencies in the prior art and provide a composite electrode and its preparation method and application that can effectively improve the mechanical properties of the electrode, effectively reduce electrode breakage and wrinkles, and thereby improve the safety performance and cycle performance of secondary batteries.
[0004] To achieve the above object, the technical solution adopted by the present invention is:
[0005] The first aspect of the present invention is to provide a method for preparing a composite pole piece, the steps comprising:
[0006] S1. Weigh a certain amount of active material, adhesive and conductive agent, mix to prepare slurry, apply the slurry to both sides of the current collector, and dry to obtain a composite electrode primary product;
[0007] S2. Weigh a certain amount of organic polymer and organic solvent, mix to obtain glue, apply it on both sides of the composite pole piece initial product, attach the diaphragm to both sides of the composite pole piece initial product coated with glue, and then heat and roll press to obtain the composite pole piece.
[0008] Preferably, in step S1, in the slurry, the mass ratio of the active material, the binder and the conductive agent is (96-98): (1-2): (1-2).
[0009] More preferably, the active material is lithium iron phosphate or graphite;
[0010] The binder comprises: at least one of polyvinylidene fluoride, carboxymethyl cellulose or polyacrylic acid;
[0011] The conductive agent includes at least one of graphene, carbon nanotubes or carbon black.
[0012] Preferably, in step S1, the drying process is carried out at a temperature of 100-150°C and for a time of 2-4 minutes.
[0013] Preferably, in step S2, in the glue solution, the mass ratio of the organic polymer to the organic solvent is (5-15): (85-95).
[0014] More preferably, the organic polymer includes at least one of polyvinylidene fluoride, polyethylene glycol, polyimide or polyurethane; and the organic solvent includes at least one of N-methylpyrrolidone, dimethylformamide, dimethylacetamide or dimethyl sulfoxide.
[0015] Preferably, in step S2, the diaphragm comprises: a substrate layer and a ceramic layer; the substrate layer comprises: at least one of polypropylene or polyethylene; the thickness of the substrate layer is 10-14 μm; the thickness of the ceramic layer is 1-4 μm.
[0016] More preferably, in step S2, the temperature of the heated roller pressing is 70-90°C, the time is 30-60s, and the pressure is 4000-6000kg.F.
[0017] The second aspect of the present invention is to provide a composite pole piece obtained by the above preparation method.
[0018] The third aspect of the present invention is to provide a composite pole piece obtained by the above preparation method or the application of the above composite pole piece in a sodium ion battery.
[0019] The present invention adopts the above technical solution, and has the following technical effects compared with the prior art:
[0020] The composite pole piece provided by the present invention does not need to add a diaphragm when being assembled into a battery, and the negative pole piece and the positive pole piece can be directly stacked or wound, which effectively reduces the difficulty and time of assembly; the present invention supports the composite pole piece by adding a highly flexible glue, which effectively improves the mechanical properties of the composite pole piece, reduces the probability of pole piece breakage and short circuit during battery cycling, and improves the safety performance of the battery; the diaphragm on the surface of the composite pole piece after heating and rolling can fully contact with the active material in the electrolyte, thereby improving the ion transmission capacity in the electrolyte, reducing the DC internal resistance of the battery, and improving the cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of the basic structure of a composite pole piece in one embodiment of the present invention;
[0022] Figure 2 is a surface diagram of the composite pole piece; Figure 2A The surface diagram of the composite pole piece assembled in the traditional way. Figure 2B This is a surface diagram of the composite pole piece obtained by the preparation method of the present invention.
[0023] Reference numerals in the figures include:
[0024] The first diaphragm layer 1; the first adhesive layer 2; the first membrane layer 3; the current collector 4; the second membrane layer 5; the second adhesive layer 6; the second diaphragm layer 7. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0027] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but they are not intended to limit the present invention.
[0028] Example 1
[0029] This embodiment provides a method for preparing a composite electrode, the steps comprising:
[0030] S1. After mixing 96wt% lithium iron phosphate, 2wt% adhesive and 2wt% conductive agent to prepare slurry, the slurry is coated on both sides of the current collector and dried at 150°C for 2min to obtain a composite electrode primary product;
[0031] S2, after mixing 15wt% polyvinylidene fluoride and 85wt% N-methylpyrrolidone to prepare a glue solution, apply it on both sides of the composite pole piece primary product, and attach the diaphragm to both sides of the composite pole piece primary product coated with the glue solution, and then heat and roll press, so as to obtain the composite pole piece;
[0032] Wherein, the diaphragm comprises a substrate layer with a thickness of 10 μm and a ceramic layer with a thickness of 4 μm; the substrate layer is made of polypropylene;
[0033] The temperature of the heated roller pressing is 90°C, the time is 30s, and the pressure is 6000kg.F;
[0034] The composite electrode comprises: a first diaphragm layer 1, a first adhesive layer 2, a first membrane layer 3, a current collector 4, a second membrane layer 5, a second adhesive layer 6 and a second diaphragm layer 7 which are arranged in sequence.
[0035] Example 2
[0036] This embodiment provides another method for preparing a composite electrode, the steps comprising:
[0037] S1. After mixing 98 wt% of graphite, 1 wt% of an adhesive and 1 wt% of a conductive agent to prepare a slurry, the slurry is applied to both sides of a current collector and dried at 100° C. for 4 min to obtain a composite electrode primary product;
[0038] S2, after mixing 5wt% polyethylene glycol and 95wt% dimethylacetamide to prepare a glue solution, apply it on both sides of the composite pole piece initial product, and attach the diaphragm to both sides of the composite pole piece initial product coated with the glue solution, and then heat and roll press, so as to obtain the composite pole piece;
[0039] Wherein, the diaphragm comprises a substrate layer with a thickness of 14 μm and a ceramic layer with a thickness of 1 μm; the substrate layer is made of polyethylene;
[0040] The temperature of the heated roller pressing is 70°C, the time is 60s, and the pressure is 4000kg.F.
[0041] Example 3
[0042] This embodiment provides another method for preparing a composite electrode, the steps comprising:
[0043] S1. After mixing 97wt% lithium iron phosphate, 1wt% adhesive and 2wt% conductive agent to prepare slurry, the slurry is coated on both sides of the current collector and dried at 120°C for 3min to obtain a composite electrode primary product;
[0044] S2, after mixing 5wt% polyethylene glycol, 5wt% polyimide and 90wt% dimethyl sulfoxide to prepare a glue solution, apply it on both sides of the composite pole piece preliminary product, and attach the diaphragm to both sides of the composite pole piece preliminary product coated with the glue solution, and then heat and roll press, so as to obtain the composite pole piece;
[0045] The diaphragm includes a substrate layer with a thickness of 12 μm and a ceramic layer with a thickness of 3 μm; the substrate layer is made of polypropylene and polyethylene;
[0046] The temperature of the heated roller pressing is 79°C, the time is 50s, and the pressure is 5000kg.F.
[0047] Detection Example
[0048] The composite electrode stacks prepared by the preparation methods described in Example 1 and Example 2 were used to prepare batteries, and performance tests were performed. The test results are shown in Table 1.
[0049] Table 1
[0050] serial number Capacity retention rate at room temperature Capacity retention at 45°C Traditional Batteries 82% 63% Example 1+Example 2 98% 86%
[0051] Note: The percentage of 500 discharge capacity to the first discharge capacity is taken as the capacity retention rate.
[0052] In summary, compared with the battery manufactured by stacking or winding the negative electrode sheet, separator and positive electrode sheet on a stacking machine or a winding machine by the conventional method, the battery assembled with the composite electrode sheet described in the embodiment of the present invention only needs to stack or wind the negative electrode sheet and the positive electrode sheet, which effectively reduces the difficulty of assembly and saves assembly time; as shown in Figure 2, the preparation method of the present invention can reduce the hot pressing breakage of the composite electrode sheet, and effectively improve the cycle performance and safety performance of the assembled battery.
[0053] The above description is only a preferred embodiment of the present invention, and does not limit the implementation mode and protection scope of the present invention. For those skilled in the art, it should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the description and illustrations of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite electrode. It is characterized in that the steps include: S1. Weigh a certain amount of active material, adhesive and conductive agent, mix to prepare slurry, apply the slurry to both sides of the current collector, and dry to obtain a composite electrode primary product; S2. Weigh a certain amount of organic polymer and organic solvent, mix to obtain glue, apply it on both sides of the composite pole piece initial product, attach the diaphragm to both sides of the composite pole piece initial product coated with glue, and then heat and roll press to obtain the composite pole piece.
2. The preparation method according to claim 1, It is characterized in that In step S1, in the slurry, the mass ratio of the active material, the binder and the conductive agent is (96-98): (1-2): (1-2).
3. The preparation method according to claim 2, It is characterized in that The active material is lithium iron phosphate or graphite; The binder comprises: at least one of polyvinylidene fluoride, carboxymethyl cellulose or polyacrylic acid; The conductive agent includes at least one of graphene, carbon nanotubes or carbon black.
4. The preparation method according to claim 1, It is characterized in that In step S1, the drying process is carried out at a temperature of 100-150°C and for a time of 2-4 minutes.
5. The preparation method according to claim 1, It is characterized in that In step S2, in the glue solution, the mass ratio of the organic polymer to the organic solvent is (5-15): (85-95).
6. The preparation method according to claim 5, It is characterized in that The organic polymer includes at least one of polyvinylidene fluoride, polyethylene glycol, polyimide or polyurethane; the organic solvent includes at least one of N-methylpyrrolidone, dimethylformamide, dimethylacetamide or dimethyl sulfoxide.
7. The preparation method according to claim 1, It is characterized in that In step S2, the diaphragm includes: a substrate layer and a ceramic layer; the substrate layer includes: at least one of polypropylene or polyethylene; the thickness of the substrate layer is 10-14 μm; the thickness of the ceramic layer is 1-4 μm.
8. The preparation method according to claim 7, It is characterized in that In step S2, the temperature of the heated roller pressing is 70-90°C, the time is 30-60s, and the pressure is 4000-6000kg.F.
9. A composite electrode produced by the method according to any one of claims 1 to 8.
10. Use of the composite pole piece obtained by the preparation method according to any one of claims 1 to 8 or the composite pole piece according to claim 9 in a sodium ion battery.