High-conductivity graphite negative electrode material and preparation method thereof
By using polyimide and polysulfur nitride to heat-treated wrapping materials on graphite negative electrode materials, a highly conductive amorphous carbon layer is formed, which solves the problem of vulnerability in graphite negative electrode materials and improves the cycle stability of the battery and conductivity.
Patent Information
- Application Number
- CN202411137829.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-15
AI Technical Summary
The conductivity of graphite negative electrode materials is easily damaged during use, affecting the cycle stability of lithium-ion batteries. The existing coating technology has problems such as high energy consumption, low environmental protection and low efficiency.
Using a combination of graphite powder, boric acid, encapsulation material (polyimide and polysulfur nitride) and conductive agent, a highly conductive amorphous carbon layer is formed through heat treatment, which improves the efficiency of lithium ion embedding/deintercalation channels and the conductivity of the material. sex.
It significantly improves the conductivity and structural stability of graphite negative electrode materials, extends the service life of the battery, and meets the development needs of the next generation of lithium-ion batteries.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of graphite negative electrode materials, and in particular to a high-conductivity graphite negative electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, environmental friendliness, and good cycle performance. They are widely used in mobile electronic devices, new energy vehicles and other products. The working principle of lithium-ion batteries mainly depends on the migration of lithium ions between the positive and negative electrodes. Specifically, when the battery is charging, lithium ions are released from the positive electrode material and migrate to the negative electrode through the electrolyte, making the negative electrode lithium-rich. The discharge process is the opposite. Lithium ions are released from the negative electrode material and return to the positive electrode through the electrolyte. This process is actually a chemical redox reaction. Voltage is generated through the migration of lithium ions and the chemical reaction between the electrodes, allowing the battery to store and release electrical energy.
[0003] Graphite negative electrode material is one of the negative electrode materials widely used in lithium-ion batteries. It has the advantages of high stability, good conductivity, and abundant resources. It is the most widely used negative electrode material for lithium-ion batteries in the market. However, graphite has a layered structure, and the layers are bound by van der Waals forces, which have weak bonding forces. Therefore, lithium ions will damage the structure of graphite during the embedding-de-embedding process, which is not conducive to the cycle stability of the battery. In order to solve this problem, other materials can be used to coat the graphite surface to modify the graphite, thereby changing the negative electrode surface structure of graphite, optimizing the lithium ion embedding and de-embedding channels, and avoiding the problem of the conductivity of graphite negative electrode materials being damaged and reduced during long-term use.
[0004] In the existing technology, the technology of coating non-graphite carbon layer with carbon-containing precursor materials such as asphalt is very mature, and it is still the technology used by most graphite negative electrode companies today. However, with the development of technology and the development of next-generation batteries, the shortcomings of asphalt coating, such as high energy consumption, low environmental protection, low efficiency and health hazards, make it increasingly unable to meet the development needs of graphite negative electrode materials. Summary of the invention
[0005] The present invention provides a high-conductivity graphite negative electrode material and a preparation method thereof, which solves the problem in the related art that the conductivity of the graphite negative electrode material is easily damaged and reduced during use.
[0006] The technical solution of the present invention is as follows: In the first aspect, the present invention proposes a highly conductive graphite negative electrode material, comprising the following raw materials in parts by weight: 95-105 parts of graphite powder, 3-5 parts of boric acid, 5-8 parts of wrapping material, 5-10 parts of binder, and 5-10 parts of conductive agent; wherein the wrapping material comprises polyimide and polysulfur nitride, and the mass ratio of the two is 1:(0.8-1.2).
[0007] Preferably, graphite powder is 98-102 parts, boric acid is 3.5-4.5 parts, wrapping material is 6-7 parts, binder is 6-9 parts, and conductive agent is 6-9 parts; the mass ratio of polyimide and polysulfur nitride in the wrapping material is 1: (0.9-1.1); More preferably, the graphite powder is 100 parts, the boric acid is 4 parts, the wrapping material is 6.5 parts, the binder is 7 parts, and the conductive agent is 7 parts; the mass ratio of polyimide to polysulfur nitride in the wrapping material is 1:1.
[0008] As a further technical solution, petroleum coke is added into a pulverizing device to prepare a powder with a particle size of 5-15 μm, and then the obtained powder is graphitized to obtain the graphite powder.
[0009] As a further technical solution, the method for graphitizing the powder is: adding the powder to a high-temperature graphitization furnace, heating it to 3000-3200°C at a heating rate of 10-15°C / min under inert gas protection, and keeping it at this temperature for 4.5-5h.
[0010] As a further technical solution, the method for preparing the wrapping material is as follows: polyimide and polysulfur nitride are added to a pulverizing device in proportion to form powders, and then added together to a container for ultrasonic stirring to obtain the wrapping material.
[0011] For example, polyimide and polysulfur nitride are added to a ball mill respectively and ground into powder, and then added together into an ultrasonic mixer and stirred at 20-30 Hz for 0.5-1 h. Under the premise of fully stirring the polyimide and polysulfur nitride, the polysulfur nitride can be adsorbed on the surface of the polyimide to form a blend of polyimide and polysulfur nitride.
[0012] Polyimide is a type of high molecular polymer containing an imide ring (-CO-NR-CO-) in the main chain. It has a certain degree of conductivity. Its conductivity is mainly related to the π electrons in its molecular structure. These π electrons can be responsible for the conductivity of polyimide to a certain extent, but this conductivity is relatively weak. However, through thermal decomposition treatment, the structure and conductivity of polyimide can be significantly changed, which can be greatly improved; polysulfur nitride is a synthetic pure single crystal inorganic polymer composed of chains of alternating sulfur and nitrogen atoms. It has high conductivity. At extremely low temperatures (such as 0.26kPa, -262.7℃), polysulfur nitride also shows superconductivity, that is, there is no measurable resistance.
[0013] As a further technical solution, the binder is one or a combination of hydroxymethyl cellulose or styrene-butadiene rubber.
[0014] As a further technical solution, the conductive agent is acetylene black, Ketjen black or Super-P carbon black.
[0015] In a second aspect, the present invention further discloses a method for preparing the highly conductive graphite negative electrode material as described above, comprising the following steps: S1: Add N-methylpyrrolidone to the encapsulating material and stir thoroughly to form an encapsulating liquid; wherein the optimal ratio of the encapsulating material to N-methylpyrrolidone is 1 g: (15-20) mL.
[0016] S2: adding graphite powder to the coating liquid and stirring well, then adding boric acid and stirring well to obtain a mixed solution; S3: heat-treating the mixed solution at 1000°C or above, and then adding the mixture to a crushing device to make it into powder to obtain coated graphite; S4: Add a binder, a conductive agent and coated graphite to water in turn, stir thoroughly and evenly to obtain a negative electrode slurry, wherein the optimal ratio of water to the sum of the amounts of the binder, the conductive agent and the coated graphite is (120-140) mL: (110-140) g.
[0017] The negative electrode slurry is evenly coated on the copper foil, and taken out after vacuum drying to obtain a highly conductive graphite negative electrode material.
[0018] Specifically, after the polyimide and polysulfur nitride in the encapsulating material are dissolved in N-methylpyrrolidone, since the polyimide carries the polysulfur nitride to form a blend, the two have excellent dispersibility in N-methylpyrrolidone; after adding graphite powder and boric acid, a stable homogeneous mixed liquid is formed, and the polyimide and polysulfur nitride in the encapsulating liquid are initially encapsulated on the surface of the graphite powder, and the boric acid is attached to the surface of the encapsulating liquid.
[0019] During the heat treatment process, polyimide first loses CO at around 600°C and undergoes intramolecular cyclization to form a small aromatic system. At this time, the conductivity is still within the semiconductor range, but has been enhanced. As the temperature rises, when the temperature reaches 700°C, polyimide continues to pyrolyze to form a large aromatic structure. At this time, the conductivity is significantly improved, but it may still be lower than the level of high conductivity materials. When the temperature reaches 800°C, at this stage, polyimide undergoes deep pyrolysis to form a high conductivity aromatic graphite structure. This structure is similar to graphite and has excellent conductive properties. When the temperature reaches 1000°C, polyimide undergoes deep pyrolysis to form a high conductivity aromatic structure. An amorphous carbon layer with a conjugated structure is formed on the graphite surface. The carbon layer has a larger interlayer spacing than graphite, which can provide more diffusion channels for lithium ions, thereby improving the conductivity of the negative electrode material.
[0020] At the same time, the polysulfur nitride carried on the surface of polyimide has a large conjugated π electron system and high carrier mobility, which can promote the flow of lithium ions in the negative electrode material. At the same time, the N atoms can provide additional active sites for lithium ion adsorption for the amorphous carbon layer, and the connection of S atoms reduces the energy gap between the highest occupied molecular orbital and the lowest unoccupied molecular orbital, further enhancing the interlayer spacing of the amorphous carbon layer, making it easier for electrons to shuttle, thereby greatly enhancing the conductivity of the graphite negative electrode material.
[0021] In addition, during the heat treatment process, when the temperature reaches above 300°C, boric acid slowly vaporizes and escapes, forming pores on the surface of the wrapping material. When the wrapping material continues to be heated to form a carbon layer, these pores are distributed on the surface of the amorphous carbon layer, which can construct a more effective lithium ion embedding / de-embedding network structure, thereby improving the conductivity of the graphite negative electrode material.
[0022] As a further technical solution, in step S2, graphite powder is added to the coating liquid and stirred at 500-800 rpm for 0.5-1.5 min until uniform, and then boric acid is added and stirred at 400-500 rpm for 1-2 h until uniform.
[0023] Preferably, the graphite powder is added to the coating liquid and stirred at 600-700 rpm for 0.8-1.2 hours until uniform, and then the boric acid is added and stirred at 420-480 rpm for 1.2-1.8 hours until uniform; more preferably, the graphite powder is added to the coating liquid and stirred at 650 rpm for 1 hour until uniform, and then the boric acid is added and stirred at 450 rpm for 1.5 hours until uniform; As a further technical solution, in step S3, the specific method for heat treatment of the mixed liquid at above 1000°C is: under the protection of inert gas, the mixed liquid is heated to 120-150°C at a heating rate of 5-10°C / min, kept warm for 0.5-1h, then heated to 500-600°C at a heating rate of 1-2°C / min, kept warm for 1-2h, and finally heated to 1000-1200°C at a heating rate of 5-8°C / min, and kept warm for 2-3h.
[0024] As a further technical solution, in step S4, the vacuum drying conditions are: vacuum drying at 60-80°C for 10-12h.
[0025] The working principle and beneficial effects of the present invention are: 1. In the present invention, a wrapping material is used outside the graphite powder for modification. During the heat treatment process, the polyimide in the wrapping material first loses CO at about 600°C and undergoes intramolecular cyclization to form a small aromatic system. At this time, the conductivity is still within the semiconductor range, but has been enhanced. As the temperature increases, when the temperature reaches 700°C, the polyimide continues to pyrolyze to form a large aromatic structure. At this time, the conductivity is significantly improved, but it may still be lower than the level of high conductivity materials. When the temperature reaches 800°C, at this stage, the polyimide undergoes deep pyrolysis to form an aromatic graphite structure with high conductivity. This structure is similar to graphite and has excellent conductive properties. When the temperature reaches 1000°C, the polyimide undergoes deep pyrolysis to form an aromatic structure with high conductivity. An amorphous carbon layer with a conjugated structure is formed on the graphite surface. The carbon layer has a larger interlayer spacing than graphite, which can provide more diffusion channels for lithium ions, thereby improving the conductivity of the negative electrode material.
[0026] 2. In the present invention, a wrapping material is used outside the graphite powder for modification. The polysulfur nitride in the wrapping material has a large conjugated π electron system and a high carrier mobility, which can promote the flow of lithium ions in the negative electrode material. At the same time, the N atoms therein can provide additional lithium ion adsorption active sites for the amorphous carbon layer, and the connection of the S atoms reduces the energy gap between the highest occupied molecular orbital and the lowest unoccupied molecular orbital, further enhancing the interlayer spacing of the amorphous carbon layer, making it easier for electrons to shuttle, thereby greatly enhancing the conductivity of the graphite negative electrode material.
[0027] 3. In the present invention, boric acid is added to the mixed solution of the negative electrode material. During the heat treatment process, when the temperature reaches above 300°C, the boric acid slowly vaporizes and escapes, forming pores on the surface of the wrapping material. When the wrapping material continues to be heated to form a carbon layer, these pores are distributed on the surface of the amorphous carbon layer, which can construct a more effective lithium ion embedding / de-embedding network structure, provide more diffusion channels for lithium ions, and thus improve the conductivity of the graphite negative electrode material; at the same time, the pores on the surface also enhance the friction between adjacent amorphous carbon layers, making the structure of the negative electrode material more stable. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0030] Example 1 Preparation of graphite powder 1000g of graphite powder was added to a planetary ball mill and ground into powder. After screening, a powder with a particle size of 5-15um and an average particle size of 10um was obtained. The powder was then added to a high-temperature graphitization furnace and heated to 3100℃ at a heating rate of 10℃ / min under argon protection, and kept at this temperature for 5h to obtain graphite powder.
[0031] Example 2 Preparation of packaging materials 25g of polyimide and 25g of polysulfur nitride were added to a planetary ball mill and ground into powder. After screening, powders with a particle size of less than 30um and an average particle size of 20um were obtained. Then, various powders were added to an ultrasonic mixer and stirred at 20HZ for 1h to obtain the packaging material.
[0032] Example 3 Preparation of highly conductive graphite anode materials Add 5g of the encapsulating material obtained in Example 2 to a stirring tank, then add 100mL of N-methylpyrrolidone, stir at 400rpm for 20min to form an encapsulating liquid, then add 95g of the graphite powder obtained in Example 1, stir at 600rpm for 1.2h, then add 3g of boric acid, stir at 420rpm for 1.8h to obtain a mixed solution, transfer the mixed solution to a crucible, add the crucible to a high-temperature electric furnace, fill the high-temperature electric furnace with helium, adjust the temperature of the high-temperature electric furnace for heat treatment, first heat to 120°C at a heating rate of 5°C / min, keep warm for 1h, then heat to 500°C at a heating rate of 1°C / min, keep warm for 2h, finally heat to 1000°C at a heating rate of 5°C / min, keep warm for 3h, take out the crucible after the end, cool to room temperature to obtain a block solid, break the block solid into small pieces and add them to a ball mill to grind into a coated graphite with a particle size of less than 60um; Add 120 mL of water to a beaker, and then add 5 g of hydroxymethyl cellulose, 5 g of Super-P-Li carbon black, and the above-mentioned coated graphite in turn, and stir quickly with a glass rod for 10 minutes to obtain a negative electrode slurry. The negative electrode slurry is evenly coated on a copper foil with a thickness of 150 um. After cutting, a negative electrode sheet with a length of 4 cm and a width of 1.5 cm is formed. The negative electrode sheet is placed in a vacuum box at 60°C and heated for 12 hours. After drying, it is taken out to obtain a highly conductive graphite negative electrode material.
[0033] Example 4 Add 6g of the encapsulating material obtained in Example 2 to a stirring tank, then add 105mL of N-methylpyrrolidone, stir at 400rpm for 20min to form an encapsulating liquid, then add 98g of the graphite powder obtained in Example 1, stir at 650rpm for 1h, then add 3.5g of boric acid, stir at 450rpm for 1.5h to obtain a mixed solution, transfer the mixed solution to a crucible, add the crucible to a high-temperature electric furnace, fill the high-temperature electric furnace with helium, adjust the temperature of the high-temperature electric furnace for heat treatment, first heat to 130°C at a heating rate of 6°C / min, keep warm for 0.8h, then heat to 500°C at a heating rate of 1°C / min, keep warm for 2h, finally heat to 1100°C at a heating rate of 6°C / min, keep warm for 2.5h, take out the crucible after the end, cool to room temperature to obtain a block solid, break the block solid into small pieces and add them to a ball mill to grind into a coated graphite with a particle size of less than 60um; Add 125 mL of water to a beaker, and then add 6 g of hydroxymethyl cellulose, 6 g of Super-P-Li carbon black, and the above-mentioned coated graphite in turn, and stir quickly with a glass rod for 10 minutes to obtain a negative electrode slurry. The negative electrode slurry is evenly coated on a copper foil with a thickness of 150 um. After cutting, a negative electrode sheet with a length of 4 cm and a width of 1.5 cm is formed. The negative electrode sheet is placed in a vacuum box at 70°C and heated for 11 hours. After drying, it is taken out to obtain a highly conductive graphite negative electrode material.
[0034] Example 5 Add 6.5g of the encapsulating material obtained in Example 2 to a stirring tank, then add 110mL of N-methylpyrrolidone, stir at 400rpm for 20min to form an encapsulating liquid, then add 100g of the graphite powder obtained in Example 1, stir at 650rpm for 1h, then add 4g of boric acid, stir at 450rpm for 1.5h to obtain a mixed solution, transfer the mixed solution to a crucible, add the crucible to a high-temperature electric furnace, fill the high-temperature electric furnace with helium, adjust the temperature of the high-temperature electric furnace for heat treatment, first heat to 135°C at a heating rate of 8°C / min, keep warm for 0.7h, then heat to 500°C at a heating rate of 1°C / min, keep warm for 2h, finally heat to 1100°C at a heating rate of 6°C / min, keep warm for 2.5h, take out the crucible after the end, cool to room temperature to obtain a block solid, break the block solid into small pieces and add them to a ball mill to grind into a coated graphite with a particle size of less than 60um; Add 130 mL of water to a beaker, and then add 7 g of hydroxymethyl cellulose, 7 g of Super-P-Li carbon black, and the above-mentioned coated graphite in turn, and stir quickly with a glass rod for 10 minutes to obtain a negative electrode slurry. The negative electrode slurry is evenly coated on a copper foil with a thickness of 150 um. After cutting, a negative electrode sheet with a length of 4 cm and a width of 1.5 cm is formed. The negative electrode sheet is placed in a vacuum box at 70°C and heated for 11 hours. After drying, it is taken out to obtain a highly conductive graphite negative electrode material.
[0035] Example 6 7 g of the encapsulating material obtained in Example 2 was added to a stirring tank, and then 115 mL of N-methylpyrrolidone was added, and the mixture was stirred at 400 rpm for 20 min to form an encapsulating liquid. Subsequently, 102 g of the graphite powder obtained in Example 1 was added, and the mixture was stirred at 650 rpm for 1 h. Then, 4.5 g of boric acid was added, and the mixture was stirred at 450 rpm for 1.5 h to obtain a mixed solution. The mixed solution was transferred to a crucible, and the crucible was added to a high-temperature electric furnace. Helium was filled into the high-temperature electric furnace, and the temperature of the high-temperature electric furnace was adjusted for heat treatment. First, the mixture was heated to 140° C. at a heating rate of 9° C. / min, and the mixture was kept warm for 0.6 h. Then, the mixture was heated to 600° C. at a heating rate of 2° C. / min, and the mixture was kept warm for 1 h. Finally, the mixture was heated to 1100° C. at a heating rate of 6° C. / min, and the mixture was kept warm for 2.5 h. After the mixture was finished, the crucible was taken out, and the mixture was cooled to room temperature to obtain a block solid. The block solid was broken into small pieces and added to a ball mill to grind into a coated graphite with a particle size of less than 60 μm. Add 135 mL of water to a beaker, and then add 9 g of hydroxymethyl cellulose, 9 g of Super-P-Li carbon black, and the above-mentioned coated graphite in turn, and stir quickly with a glass rod for 10 minutes to obtain a negative electrode slurry. The negative electrode slurry is evenly coated on a copper foil with a thickness of 150 um. After cutting, a negative electrode sheet with a length of 4 cm and a width of 1.5 cm is formed. The negative electrode sheet is placed in a vacuum box at 70°C and heated for 11 hours. After drying, it is taken out to obtain a highly conductive graphite negative electrode material.
[0036] Example 7 8 g of the encapsulating material obtained in Example 2 was added to a stirring tank, and then 120 mL of N-methylpyrrolidone was added, and the mixture was stirred at 400 rpm for 20 min to form an encapsulating liquid. Subsequently, 105 g of the graphite powder obtained in Example 1 was added, and the mixture was stirred at 700 rpm for 0.8 h. Then, 5 g of boric acid was added, and the mixture was stirred at 480 rpm for 1.2 h to obtain a mixed solution. The mixed solution was transferred to a crucible, and the crucible was added to a high-temperature electric furnace. Helium was filled into the high-temperature electric furnace, and the temperature of the high-temperature electric furnace was adjusted for heat treatment. First, the mixture was heated to 150° C. at a heating rate of 10° C. / min, and the mixture was kept warm for 0.5 h. Then, the mixture was heated to 600° C. at a heating rate of 2° C. / min, and the mixture was kept warm for 1 h. Finally, the mixture was heated to 1200° C. at a heating rate of 8° C. / min, and the mixture was kept warm for 2 h. After the mixture was finished, the crucible was taken out, and the mixture was cooled to room temperature to obtain a block solid. The block solid was broken into small pieces and added to a ball mill to grind into a coated graphite with a particle size of less than 60 um. Add 140 mL of water to a beaker, and then add 10 g of hydroxymethyl cellulose, 10 g of Super-P-Li carbon black, and the above-mentioned coated graphite in turn, and stir quickly with a glass rod for 10 minutes to obtain a negative electrode slurry. The negative electrode slurry is evenly coated on a copper foil with a thickness of 150 um. After cutting, a negative electrode sheet with a length of 4 cm and a width of 1.5 cm is formed. The negative electrode sheet is placed in a vacuum box at 80°C and heated for 10 hours. After drying, it is taken out to obtain a highly conductive graphite negative electrode material.
[0037] Example 8 Compared with Example 5, the only difference is: (1) The preparation method of graphite powder is as follows: 1000 g of graphite powder is added to a planetary ball mill and ground into powder, and after screening, a powder with a particle size of 5-15 μm and an average particle size of 10 μm is obtained, and then the powder is added to a high-temperature graphitization furnace, and heated to 3200°C at a heating rate of 10°C / min under argon protection, and kept at this temperature for 4.5 hours to obtain graphite powder; (2) The preparation method of the encapsulating material is as follows: 27 g of polyimide and 22 g of polysulfur nitride are added to a planetary ball mill and ground into powder respectively. After screening, a powder with a particle size of less than 30 μm and an average particle size of 20 μm is obtained. Then, various powders are added to an ultrasonic mixer and stirred at 20 Hz for 1 hour to obtain the encapsulating material.
[0038] Example 9 Compared with Example 5, the only difference is: The preparation method of the encapsulating material is as follows: 22.7 g of polyimide and 27.2 g of polysulfur nitride are respectively added to a planetary ball mill and ground into powder, and after screening, a powder with a particle size of less than 30 um and an average particle size of 20 μm is obtained, and then various powders are added together to an ultrasonic mixer and stirred at 20 Hz for 1 hour to obtain the encapsulating material.
[0039] Comparative Example 1 Compared with Example 5, the only difference is that the packaging material prepared in Example 2 is replaced by polyimide, and finally a graphite negative electrode material is prepared.
[0040] Comparative Example 2 Compared with Example 5, the only difference is that the packaging material prepared in Example 2 is replaced by polysulfur nitride, and finally a graphite negative electrode material is prepared.
[0041] Comparative Example 3 Compared with Example 5, the only difference is that no boric acid is added, and a graphite negative electrode material is finally obtained.
[0042] Comparative Example 4 Add 6.5 g of asphalt PD and 100 g of graphite powder obtained in Example 1 into a stirring tank, stir at 650 rpm for 2 h to obtain a mixed solution, transfer the mixed solution to a crucible, and keep it at 1200° C. for 4 h. After the mixture is finished, take out the crucible, cool it to room temperature to obtain a block solid, break the block solid into small pieces, add it to a ball mill and grind it into coated graphite with a particle size of less than 60 μm; Add 130 mL of water to a beaker, and then add 7 g of hydroxymethyl cellulose, 7 g of Super-P-Li carbon black, and the above-mentioned coated graphite in turn, and stir quickly with a glass rod for 10 minutes to obtain a negative electrode slurry. The negative electrode slurry is evenly coated on a copper foil with a thickness of 150 um. After cutting, a negative electrode sheet with a length of 4 cm and a width of 1.5 cm is formed. The negative electrode sheet is placed in a vacuum box at 70°C and heated for 11 hours. After drying, it is taken out to obtain a graphite negative electrode material.
[0043] The graphite negative electrode material samples prepared in Examples 3-9 and Comparative Examples 1-4 were assembled into button cells and then subjected to performance tests, including impedance testing and the first charge and discharge capacity and first coulomb efficiency testing of the samples at a rate of 0.1C. The testing method was as follows: Impedance test: Use an electrochemical workstation (CHI660e) to test the charge transfer impedance R ct and Warbury impedance Q p , the CV voltage test range is 0-2V, the scan speed is 0.1mV / s, the EIS test frequency is 0.01-10000Hz, and the amplitude is mV.
[0044] First charge and discharge capacity test at 0.1C rate: using LAND test system, First coulombic efficiency test: Calculated based on the first charge and discharge capacity, the coulombic efficiency is the ratio between the actual amount of charge released during the discharge process and the amount of charge input during the charging process.
[0045] The calculation results are listed in Table 1. Table 1 is as follows: Table 1
[0046] By analyzing the data in Table 1, it can be seen that the graphite negative electrode materials prepared in Examples 3-9 have stronger conductivity than those in Comparative Examples 1-4, which indicates that the graphite negative electrode materials prepared in the present invention have high conductivity.
[0047] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A highly conductive graphite negative electrode material, characterized in that: The invention comprises the following raw materials in parts by weight: 95-105 parts of graphite powder, 3-5 parts of boric acid, 5-8 parts of wrapping material, 5-10 parts of binder and 5-10 parts of conductive agent; wherein the wrapping material comprises polyimide and polysulfur nitride, and the mass ratio of the two is 1:(0.8-1.2).
2. The highly conductive graphite negative electrode material according to claim 1, characterized in that: The preparation method of the graphite powder is as follows: petroleum coke is added into a pulverizing device to prepare a powder with a particle size of 5-15 μm, and then the obtained powder is graphitized to obtain the graphite powder.
3. The highly conductive graphite negative electrode material according to claim 2, characterized in that: The method for graphitizing the powder is as follows: adding the powder into a high-temperature graphitization furnace, heating to 3000-3200° C. at a heating rate of 10° C. / min under the protection of an inert gas, and keeping the temperature at this temperature for 4.5-5 hours.
4. The highly conductive graphite negative electrode material according to claim 1, characterized in that: The preparation method of the wrapping material is as follows: polyimide and polysulfur nitride are added into a pulverizing device in proportion to be made into powder, and then added into a container together for ultrasonic stirring to obtain the wrapping material.
5. The highly conductive graphite negative electrode material according to claim 1, characterized in that: The binder is one or a combination of hydroxymethyl cellulose or styrene-butadiene rubber.
6. The highly conductive graphite negative electrode material according to claim 1, characterized in that: The conductive agent is acetylene black, Ketjen black or Super-P carbon black.
7. A method for preparing a highly conductive graphite negative electrode material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: Add N-methylpyrrolidone to the encapsulating material and stir thoroughly to form an encapsulating liquid; S2: adding graphite powder to the coating liquid and stirring well, then adding boric acid and stirring well to obtain a mixed solution; S3: heat-treating the mixed solution at 1000°C or above, and then adding the mixture to a crushing device to make it into powder to obtain coated graphite; S4: Add a binder, a conductive agent and coated graphite to water in sequence, stir thoroughly to obtain a negative electrode slurry, evenly coat the negative electrode slurry on a copper foil, vacuum dry and take out to obtain a highly conductive graphite negative electrode material.
8. The method for preparing a highly conductive graphite negative electrode material according to claim 7, characterized in that: In step S2, graphite powder is added to the coating liquid and stirred at 500-800 rpm for 0.5-1.5 hours until it is uniform, and then boric acid is added and stirred at 400-500 rpm for 1-2 hours until it is uniform.
9. The method for preparing a highly conductive graphite negative electrode material according to claim 7, characterized in that: In step S3, the specific method for heat treatment of the mixed liquid at above 1000°C is as follows: under the protection of inert gas, the mixed liquid is heated to 120-150°C at a heating rate of 5-10°C / min, kept warm for 0.5-1h, then heated to 500-600°C at a heating rate of 1-2°C / min, kept warm for 1-2h, and finally heated to 1000-1200°C at a heating rate of 5-8°C / min, kept warm for 2-3h.