Carbon-compounded sodium ferric pyrophosphate positive electrode material and preparation method thereof
By adding organic phosphonic acid and carbon material to the positive electrode material of sodium ferric phosphate, a carbon composite structure is formed, the problem of heterophase generation in synthesis is solved, the electronic conductivity and cycle stability of the material are improved, and the sodium ion battery is realized High magnification and long cycle performance of the cathode material.
Patent Information
- Application Number
- CN202411163559.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
AI Technical Summary
The existing sodium ferric phosphate positive electrode material produces more electrochemically active NaFePO4 heterophase during the synthesis process, resulting in poor electrochemical performance and failure to meet the requirements.
Using carbon composite sodium ferric phosphate positive electrode material, the carbon coating layer is formed to improve the electron conductivity and Na+ ions by adding organic phosphonic acid and carbon material precursor during the synthesis process, and adjusting the heat treatment temperature and time. diffusion kinetics.
It significantly reduces the formation of NaFePO4 heterophase, improves the electronic conductivity and cyclic stability of the material, improves the rate performance and long cycle stability of the cathode material of sodium ion battery, and performs well in a wide temperature range.
Smart Images

Figure CN118970009A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a carbon-composite sodium iron pyrophosphate positive electrode material and also relates to a method for preparing the carbon-composite sodium iron pyrophosphate positive electrode material. Background Art
[0002] With the booming development of the global new energy industry, sodium-ion batteries are considered to have great development potential. As an important component of sodium-ion batteries, cathode materials have a direct impact on the various properties of sodium-ion batteries. At present, the main types of cathode materials for sodium-ion batteries are layered metal oxides, polyanionic compounds, Prussian blue analogs and organic compounds. Among them, polyanionic compounds have attracted widespread attention due to their high stability, good safety and high operating voltage.
[0003] Among the polyanionic compound materials, iron-based polyanionic cathode materials have attracted extensive attention due to their abundant iron resources, low cost, environmental friendliness, and stable structure. Among the iron-based polyanionic cathode materials, sodium iron pyrophosphate [Na4Fe3(PO4)2P2O7, Na3Fe2PO4P2O7, denoted as NFPP] has a high theoretical specific capacity, and P2O7 with strong electronegativity 4- The average voltage of the material reaches 3.1V, showing a high energy density, so it is considered to be a very promising sodium-ion battery positive electrode material.
[0004] However, when synthesizing sodium ferric pyrophosphate, the existing method always inevitably produces a large amount of NaFePO4 (denoted as NFP) impurities in the final product, which has no electrochemical activity, thus seriously affecting the electrochemical performance of sodium ferric pyrophosphate. In addition, due to the low intrinsic electronic conductivity of sodium ferric pyrophosphate, Na + The ion diffusion kinetics are poor, resulting in its rate performance and long cycle stability failing to meet people's requirements. These problems have greatly hindered the practical application of sodium iron pyrophosphate. Summary of the invention
[0005] Purpose of the invention: One purpose of the present invention is to provide a carbon-composite sodium iron pyrophosphate positive electrode material, and another purpose is to provide a method for preparing the above-mentioned carbon-composite sodium iron pyrophosphate positive electrode material, which method can, on the one hand, significantly improve the NaFePO4 impurity problem generated during the synthesis process, and on the other hand, can greatly improve the electronic conductivity of the prepared material, so that it has good rate performance and long cycle stability when used as a positive electrode material for sodium ion batteries.
[0006] Technical solution: The carbon composite sodium iron pyrophosphate positive electrode material of the present invention comprises an active component and a carbon coating layer in situ grown outside the active component, and also comprises a conductive structure for connecting each active site into a conductive network. The active component is sodium iron pyrophosphate.
[0007] The preparation method of the carbon composite sodium iron pyrophosphate positive electrode material comprises the following steps:
[0008] (1) at room temperature, mixing an organic phosphonic acid, a sodium source, an iron source, and a carbon source to obtain a solid mixture;
[0009] (2) The solid mixture is heat treated at 500-600° C. in an inert gas atmosphere to obtain a carbon-composite sodium iron pyrophosphate positive electrode material.
[0010] Wherein, in step (1), the sodium source, the iron source and the organic phosphonic acid are mixed in a molar ratio of Na, Fe and P of 4:3:4.2-4.8 or 3:2:3.1-3.6 based on the mass of the sodium, iron and phosphorus elements.
[0011] Wherein, in step (1), the mass of the added carbon source is 10-20% of the mass of the iron source.
[0012] Wherein, in step (1), the sodium source is one or more of sodium acetate, sodium carbonate, sodium formate, sodium citrate, sodium oxalate, sodium dihydrogen phosphate, disodium hydrogen phosphate or sodium phosphate.
[0013] Wherein, in step (1), the iron source is ferrous salt.
[0014] Wherein, the ferrous salt is one or more of ferrous nitrate, ferrous oxalate, ferrous acetate, ferrous citrate or ferrous oxide, preferably ferrous oxalate.
[0015] Wherein, in step (1), the organic phosphonic acid is one or more of aminotrimethylenephosphonic acid (ATMPA), ethylenediaminetetramethylenephosphonic acid (EDTMPA) or hexamethylenediaminetetramethylenephosphonic acid (HDTMPA).
[0016] Wherein, in step (1), the carbon source is a carbon material or a carbon material precursor.
[0017] The carbon material is one or more of graphene oxide (GO), multi-walled carbon nanotubes (MWCNT), single-walled carbon nanotubes (SWCNT), Ketjen black (KB), Super P, graphyne, hollow carbon nanocages, graphite, wood charcoal or activated carbon; the carbon material precursor is one or more of sucrose, glucose, dicyandiamide, melamine, cellulose or biomass.
[0018] Wherein, in step (2), the inert gas is argon or nitrogen.
[0019] Wherein, in step (2), the heat treatment time is 8 to 16 hours.
[0020] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The present invention uses organic phosphonic acid as the phosphorus source required for synthesizing high-phase-purity sodium iron pyrophosphate, and at the same time, by adjusting the amount of organic phosphonic acid in the raw material, the NaFePO4 impurity problem generated during the synthesis process is significantly improved; (2) The present invention adds carbon material or carbon material precursor to the raw material, and at the same time, by adjusting the amount of organic phosphonic acid and the heat treatment temperature, the electronic conductivity and Na + The ion diffusion kinetics have been significantly improved, thereby effectively improving the rate performance and long-cycle stability when used as a positive electrode material for sodium ion batteries; (3) Thanks to the good electrochemical activity of the active component sodium iron pyrophosphate in a wide temperature range, the positive electrode material of the present invention has good electrochemical properties in a wide temperature range. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The X-ray diffraction pattern of NFP0 prepared in Comparative Example 1;
[0022] Figure 2 is the X-ray diffraction pattern of NFPP1 prepared in Example 1;
[0023] Figure 3 is the X-ray diffraction pattern of NFPP2 prepared in Example 2;
[0024] Figure 4 The rate performance curve of NFPP0 prepared in Comparative Example 1 as a positive electrode material for a sodium ion battery at 25°C and a voltage range of 1.7 to 4.3V;
[0025] Figure 5 The rate performance curve of the sodium iron pyrophosphate positive electrode material prepared in Comparative Example 2 as a positive electrode material for a sodium ion battery at 25° C. and a voltage range of 1.7 to 4.3 V;
[0026] Figure 6 The rate performance curve of the sodium iron pyrophosphate positive electrode material prepared in Comparative Example 3 as a positive electrode material for a sodium ion battery at 25° C. and a voltage range of 1.7 to 4.3 V;
[0027] Figure 7 The rate performance curve of NFPP3 prepared in Example 3 as a positive electrode material for a sodium ion battery at 25°C and a voltage range of 1.7 to 4.3V;
[0028] Figure 8The rate performance curve of NFPP3-10% GO prepared in Example 5 as a positive electrode material for sodium ion batteries at 25°C and a voltage range of 1.7 to 4.3V;
[0029] Fig. 9 The rate performance curve of NFPP4-10% CNT prepared in Example 6 as a positive electrode material for sodium ion batteries at 25°C and a voltage range of 1.7 to 4.3V;
[0030] Fig.10 The rate performance curve of NFPP3-20% CNT prepared in Example 7 as a positive electrode material for sodium ion batteries at 25°C and a voltage range of 1.7 to 4.3V;
[0031] Fig.11 The NFPP0 prepared in Comparative Example 1 was used as a positive electrode material for a sodium ion battery at 25°C, a voltage range of 1.7 to 4.3V, and 100mA g -1 Cyclic performance curve under current density;
[0032] Fig.12 The sodium iron pyrophosphate positive electrode material prepared in Comparative Example 2 is used as a positive electrode material for a sodium ion battery at 25°C, a voltage range of 1.7 to 4.3V, and 100mA g -1 Cyclic performance curve under current density;
[0033] Fig.13 The sodium iron pyrophosphate positive electrode material prepared in Comparative Example 3 is used as a positive electrode material for a sodium ion battery at 25°C, a voltage range of 1.7 to 4.3V, and 100mA g -1 Cyclic performance curve under current density;
[0034] Fig.14 The NFPP4 prepared in Example 4 was used as a positive electrode material for sodium ion batteries at 25°C, 1.7-4.3V voltage range, 100mA g -1 Cyclic performance curve under current density;
[0035] Fig.15 The NFPP3-10% GO prepared in Example 5 was used as a positive electrode material for sodium ion batteries at 25°C, 1.7-4.3V voltage range, 100mA g -1 Cyclic performance curve under current density;
[0036] Fig.16 The NFPP3-20% CNT prepared in Example 7 was used as a positive electrode material for a sodium ion battery at 25°C, a voltage range of 1.7 to 4.3V, and 5000mA g -1 Cyclic performance curve under current density;
[0037] Fig.17The NFPP4-10% CNT prepared in Example 6 was used as a positive electrode material for sodium ion batteries at 0°C, 1.7-4.3V voltage range, 100mA g -1 Cyclic performance curve under current density;
[0038] Fig.18 The NFPP4-10% CNT prepared in Example 6 was used as a positive electrode material for sodium ion batteries at -20°C, 1.7-4.3V voltage range, 50mA g -1 Cyclic performance curve under current density;
[0039] Fig.19 This is the rate performance curve of NFPP3-10% GO prepared in Example 5 as a positive electrode material for sodium ion batteries at 50°C and a voltage range of 1.7 to 4.3V.
[0040] Fig. 20 This is a high-magnification transmission electron microscopy image of NFPP4-10% CNT prepared in Example 6;
[0041] Fig.21 This is a high-magnification transmission electron microscopy image of NFPP3-20% CNT prepared in Example 7. DETAILED DESCRIPTION
[0042] Example 1
[0043] A method for preparing a carbon composite sodium iron pyrophosphate positive electrode material comprises the following steps:
[0044] (1) mixing ethylenediaminetetramethylenephosphonic acid, sodium acetate and ferrous oxalate in a molar ratio of Na, Fe and P of 4:3:4.2 (the molar ratio of sodium, iron and phosphorus atoms in Na4Fe3(PO4)2P2O7 is 4:3:4, and the phosphorus content in the raw materials is 5% in excess) and adding the mixture into a mortar and grinding them to obtain a solid mixture;
[0045] (2) The fully ground solid phase powder was heated to 550° C. at a heating rate of 5° C. / min in a tube furnace under a nitrogen atmosphere and calcined for 12 h to obtain a carbon-composite sodium iron pyrophosphate positive electrode material, which was recorded as NFPP1.
[0046] Example 2
[0047] A method for preparing a carbon composite sodium iron pyrophosphate positive electrode material comprises the following steps:
[0048] (1) mixing ethylenediaminetetramethylenephosphonic acid, sodium acetate and ferrous oxalate in a molar ratio of Na, Fe and P of 4:3:4.4 (with an excess of 10% phosphorus) based on the mass of the sodium, iron and phosphorus elements, and adding the mixture into a mortar and grinding it to obtain a solid mixture;
[0049] (2) The fully ground solid phase powder was heated to 550° C. at a heating rate of 5° C. / min in a tube furnace under a nitrogen atmosphere and calcined for 12 h to obtain a carbon-composite sodium iron pyrophosphate positive electrode material, which was recorded as NFPP2.
[0050] Example 3
[0051] A method for preparing a carbon composite sodium iron pyrophosphate positive electrode material comprises the following steps:
[0052] (1) mixing ethylenediaminetetramethylenephosphonic acid, sodium acetate and ferrous oxalate in a molar ratio of Na, Fe and P of 4:3:4.6 (phosphorus excess 15%) based on the mass of sodium, iron and phosphorus elements, and adding the mixture into a mortar and grinding it to obtain a solid mixture;
[0053] (2) The fully ground solid phase powder was heated to 600° C. at a heating rate of 5° C. / min in a tube furnace under a nitrogen atmosphere and calcined for 8 h to obtain a carbon-composite sodium iron pyrophosphate positive electrode material, which was recorded as NFPP3.
[0054] Example 4
[0055] A method for preparing a carbon composite sodium iron pyrophosphate positive electrode material comprises the following steps:
[0056] (1) mixing ethylenediaminetetramethylenephosphonic acid, sodium acetate and ferrous oxalate in a molar ratio of Na, Fe and P of 4:3:4.8 (phosphorus excess 20%) based on the mass of sodium, iron and phosphorus elements, and adding the mixture into a mortar and grinding it to obtain a solid mixture;
[0057] (2) The fully ground solid phase powder was heated to 600° C. at a heating rate of 5° C. / min in a tube furnace under a nitrogen atmosphere and calcined for 8 h to obtain a carbon-composite sodium iron pyrophosphate positive electrode material, which was recorded as NFPP4.
[0058] Example 5
[0059] A method for preparing a carbon composite sodium iron pyrophosphate positive electrode material comprises the following steps:
[0060] (1) Ethylenediaminetetramethylenephosphonic acid, sodium acetate and ferrous oxalate are mixed in a ratio of Na, Fe and P of 4:3:4.6 (15% excess phosphorus) based on the mass of sodium, iron and phosphorus elements, and added to a mortar; at this time, graphene oxide (GO) of 10% by mass of ferrous oxalate is added to the mortar, and a solid mixture is obtained after grinding;
[0061] (2) The fully ground solid phase powder was heated to 500° C. at a heating rate of 5° C. / min in a tube furnace under a nitrogen atmosphere and calcined for 16 h to obtain a carbon-composite sodium iron pyrophosphate positive electrode material, which was recorded as NFPP3-10wt% GO.
[0062] Example 6
[0063] A method for preparing a carbon composite sodium iron pyrophosphate positive electrode material comprises the following steps:
[0064] (1) mixing ethylenediaminetetramethylenephosphonic acid, sodium acetate and ferrous oxalate in a molar ratio of 4:3:4.8 (phosphorus excess 20%) based on the mass of sodium, iron and phosphorus elements, and adding them to a mortar; at this time, adding multi-walled carbon nanotubes (MWCNT) in an amount of 10% by mass of ferrous oxalate to the mortar, and grinding to obtain a solid mixture;
[0065] (2) The fully ground solid phase powder was heated to 500° C. at a heating rate of 5° C. / min in a tubular furnace under a nitrogen atmosphere and calcined for 16 h to obtain a carbon-composite sodium iron pyrophosphate positive electrode material, which was recorded as NFPP4-10wt% CNT.
[0066] Example 7
[0067] A method for preparing a carbon composite sodium iron pyrophosphate positive electrode material comprises the following steps:
[0068] (1) mixing ethylenediaminetetramethylenephosphonic acid, sodium acetate and ferrous oxalate in a molar ratio of 4:3:4.6 (15% excess phosphorus) based on the mass of sodium, iron and phosphorus elements, and adding them to a mortar; at this time, adding multi-walled carbon nanotubes (MWCNT) in an amount of 20% by mass of ferrous oxalate to the mortar, and grinding to obtain a solid mixture;
[0069] (2) The fully ground solid phase powder was heated to 600° C. at a heating rate of 5° C. / min in a tubular furnace under a nitrogen atmosphere and calcined for 8 h to obtain a carbon-composite sodium iron pyrophosphate positive electrode material, which was recorded as NFPP3-20wt% CNT.
[0070] Comparative Example 1
[0071] A method for preparing a sodium iron pyrophosphate positive electrode material comprises the following steps:
[0072] (1) Based on the mass of sodium, iron and phosphorus elements, ethylenediaminetetramethylenephosphonic acid, sodium acetate and ferrous oxalate are mixed in a Na:Fe:P molar ratio of 4:3:4 (phosphorus is not excessive), and added to a mortar and ground to obtain a solid mixture;
[0073] (2) The fully ground solid phase powder was heated to 550° C. at a heating rate of 5° C. / min in a tube furnace under a nitrogen atmosphere and calcined for 8 h to obtain a sodium iron pyrophosphate positive electrode material, which was recorded as NFPP0.
[0074] Comparative Example 2
[0075] The preparation method of Comparative Example 2 is basically the same as that of Example 6, with the only difference being that the calcination temperature is 400° C. to obtain a sodium iron pyrophosphate positive electrode material.
[0076] Comparative Example 3
[0077] The preparation method of Comparative Example 3 is basically the same as that of Example 6, with the only difference being that the calcination temperature is 700° C. to obtain sodium iron pyrophosphate positive electrode material.
[0078] XRD was used to characterize the phase and structure of the samples prepared in Examples 1-2 and Comparative Example 1. Figure 1 , Figure 2 and Figure 3 The XRD spectra of NFPP0 prepared in Comparative Example 1, NFPP1 prepared in Example 1, and NFPP2 prepared in Example 2 are respectively given. From the XRD spectrum, it can be seen that there is an obvious diffraction peak belonging to the hetero-NFP in NFPP0 of Comparative Example 1, and the peak intensity is relatively strong, while the diffraction peak belonging to NFPP exists but the intensity is relatively weak, indicating that there are more hetero phases in the material at this time; while in the NFPP1 and NFPP2 samples of Examples 1 and 2, the diffraction peak belonging to the hetero-phase NFP gradually weakens, and the diffraction peak belonging to NFPP gradually strengthens, proving that the formation of hetero-phase NFP can be effectively inhibited by regulating the amount of organic phosphonic acid in the raw material.
[0079] Electrochemical performance test: The materials of each embodiment and comparative examples 1 to 3 were mixed with the conductive agent SP and the binder PVDF in a mass ratio of 7:2:1, formed into a slurry in N-methylpyrrolidone solvent and coated on an aluminum foil, and then dried in a vacuum oven at 90°C for 12 hours. The loading amount of active substances on the aluminum foil was finally obtained to be about 0.65-0.71 mg / cm 2 In an argon-filled glove box with water and oxygen contents less than 0.1 ppm, a CR2032 button half-cell was prepared with sodium metal as the negative electrode and glass fiber (Whatman, GF / D) as the separator. + / Na) potential range, the battery was electrochemically tested.
[0080] Figures 4 to 7 The rate performance curves of the CR2032 button half-cells formed by the above method at room temperature are respectively the sodium iron pyrophosphate positive electrode materials prepared in Comparative Examples 1, 2 and 3 and the NFPP3 prepared in Example 3. Figures 4 to 7 It can be clearly seen that, compared with the three groups of comparative examples, the rate performance of NFPP3 prepared in Example 3 is significantly improved.
[0081] Figure 8 The rate performance curve of NFPP3-10% GO prepared in Example 5 as a positive electrode material for a sodium ion battery at 25°C. Compared with Example 3, Example 5 introduces GO with a 10% mass% of ferrous oxalate under the premise of an excess of 15% phosphorus, which further improves the electronic conductivity of the positive electrode material. It can be observed that the material has excellent rate performance as a positive electrode material for sodium ion batteries, and has a high discharge specific capacity even at high rates, which can meet the fast charging requirements. The rate performance results of the NFPP4-10% CNT prepared in Example 6 and the NFPP3-20% CNT prepared in Example 7 also have excellent rate performance, as shown Figures 9-10 shown.
[0082] Figures 11 to 14 The sodium iron pyrophosphate positive electrode materials prepared in Comparative Examples 1, 2 and 3 and the NFPP4 prepared in Example 4 were heated to 25°C and 100 mAg. -1 The first cycle discharge capacity of NFPP0 prepared in Comparative Example 1 is only 51.1 mAh g -1 After 200 cycles, the discharge capacity retention rate was only 76.5%; the first cycle discharge capacity of the sodium iron pyrophosphate cathode material prepared in comparative example 2 was only 46.7 mAhg -1 After 200 cycles, the discharge capacity retention rate was only 51.6%; the first cycle discharge capacity of the sodium iron pyrophosphate cathode material prepared in comparative example 3 was only 39.3 mAhg -1 After 200 cycles, the discharge capacity retention rate was only 71.2%; while the discharge capacity of NFPP4 prepared in Example 4 was 82.3 mAhg -1 After 200 cycles, the discharge capacity retention rate is 85.8%.
[0083] Based on the above, it can be seen that by regulating the amount of organic phosphonic acid in the raw material and the heat treatment temperature, not only can the formation of NFP impurities in the material be inhibited, but also the cycle stability and rate performance of the material can be effectively improved.
[0084] Fig.15 The NFPP3-10% GO prepared in Example 5 was used as a positive electrode material for sodium ion batteries at 25°C and 100 mAg -1 The first cycle discharge capacity is 91.2 mAh g -1 After 200 cycles, the discharge capacity retention rate is as high as 96.5%, proving that carbon materials can further improve the electrochemical properties of materials.
[0085] Fig.16 The NFPP3-20% CNT prepared in Example 7 was used as a positive electrode material for sodium ion batteries at 25°C and 5000 mAg -1 The cycle performance curve below. Fig.16 It can be seen that even at 5000mAg -1 At this current density, the first cycle discharge capacity of the material can still reach 72.0 mAh g -1 After 10,000 cycles, the discharge capacity retention rate of the material is still about 92.2%, showing an excellent long cycle life.
[0086] Fig.17 The NFPP4-10% CNT prepared in Example 6 was used as a positive electrode material for sodium ion batteries at 0°C and 100 mAg -1 The cycle performance curve below. Fig.17 It can be seen that even at 0°C and 100mAg -1 The first cycle discharge capacity of the material is still 78.3 mAh g -1 After 300 cycles, there is basically no loss in discharge capacity, and the retention rate of discharge capacity reaches 100%.
[0087] Fig.18 The NFPP4-10% CNT prepared in Example 6 was used as a positive electrode material for sodium ion batteries at -20°C and 50 mAg. -1 The cycle performance curve below. Fig.18 It can be seen that even at -20℃ and 50mAg -1 The first cycle discharge capacity of the material can reach 66.7 mAh g -1 After 150 cycles, the capacity has no obvious decay, and the discharge capacity retention rate is close to 100%. The NFPP4-10% CNT prepared in Example 6 has excellent low-temperature cycle performance.
[0088] Fig.19 The rate performance curve of NFPP3-10% GO prepared in Example 5 as a positive electrode material for sodium ion batteries at 50°C. Fig.19 It can be seen that at 50°C, the discharge specific capacity of the material is slightly improved. With the increase of current density, the change trend of the discharge specific capacity is basically consistent with that at 25°C, and there is no sharp capacity decay, which proves that the material has good high temperature resistance. Therefore, the carbon composite sodium iron pyrophosphate positive electrode material prepared by the present invention not only has excellent rate and stable long cycle performance, but also has high specific capacity and stable electrochemical performance in a wide temperature range, especially at low temperature.
[0089] Figures 20-21The high-magnification transmission electron microscopy images of NFPP4-10% CNT prepared in Example 6 and NFPP3-20% CNT prepared in Example 7 are shown in FIG. Figures 20-21 It can be observed that CNT and NFPP materials are closely interwoven to form a highly conductive network, which is beneficial to the Na + Quick insertion / removal.
Claims
1. A carbon-composite sodium iron pyrophosphate positive electrode material, characterized in that: The invention comprises an active component and a carbon coating layer in-situ grown outside the active component, and also comprises a conductive structure for connecting each active component into a conductive network; wherein the active component is sodium ferric pyrophosphate.
2. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 1, characterized in that: The steps include: (1) at room temperature, mixing an organic phosphonic acid, a sodium source, an iron source, and a carbon source to obtain a solid mixture; (2) The solid mixture is heat treated at 500-600° C. in an inert gas atmosphere to obtain a carbon-composite sodium iron pyrophosphate positive electrode material.
3. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 2, characterized in that: In step (1), the sodium source, the iron source and the organic phosphonic acid are mixed in a molar ratio of Na, Fe and P of 4:3:4.2-4.8 or 3:2:3.1-3.6 based on the mass of the sodium, iron and phosphorus elements; the mass of the added carbon source is 10-20% of the mass of the iron source.
4. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 2, characterized in that: In step (1), the sodium source is one or more of sodium acetate, sodium carbonate, sodium formate, sodium citrate, sodium oxalate, sodium dihydrogen phosphate, disodium hydrogen phosphate or sodium phosphate.
5. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 2, characterized in that: In step (1), the iron source is a ferrous salt.
6. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 5, characterized in that: The ferrous salt is one or more of ferrous nitrate, ferrous oxalate, ferrous acetate, ferrous citrate or ferrous oxide.
7. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 2, characterized in that: In step (1), the organic phosphonic acid is one or more of aminotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid or hexamethylenediaminetetramethylenephosphonic acid.
8. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 2, characterized in that: In step (1), the carbon source is a carbon material or a carbon material precursor.
9. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 8, characterized in that: The carbon material is one or more of graphene oxide, multi-walled carbon nanotubes, single-walled carbon nanotubes, Ketjen black, Super P, graphyne, hollow carbon nanocages, graphite, wood charcoal or activated carbon; the carbon material precursor is one or more of sucrose, glucose, dicyandiamide, melamine, cellulose or biomass.
10. The method for preparing the carbon composite sodium iron pyrophosphate positive electrode material according to claim 2, characterized in that: In step (2), the inert gas is argon or nitrogen; and the heat treatment time is 8 to 16 hours.
Citation Information
Cited By
Pyrophosphate ferric phosphate sodium positive electrode material and preparation method thereof, positive electrode plate and secondary battery