Doped and coated ternary positive electrode material as well as preparation method and application thereof

Through gallium-magnesium co-doping and magnesium coating the intermediate layer, combined with metal oxide-phosphate co-coated shell, the voltage attenuation and structural instability of the nickel-cobalt-manganese positive electrode material during the cycle process is solved, and the battery's plurality is improved Performance and cycle life extend the battery life.

CN118970016APending Publication Date: 2024-11-15JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411305339.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing nickel, cobalt, manganese ternary cathode materials have problems such as voltage attenuation, poor cycling performance of ratios, and unstable structural structure during the circulation process, resulting in degradation of battery capacity attenuation and cycle performance.

Method used

Doped coated ternary positive electrode material that uses gallium-magnesium co-doped nickel-cobalt manganese core, magnesium-coated intermediate layer and metal oxide-phosphate co-coated shell to improve electron conductivity and lithium ion diffusion through gallium elements , Magnesium element stabilizes the structure, and metal oxide-phosphate co-covering shell improves thermal stability and structural stability.

Benefits of technology

It significantly reduces voltage attenuation, improves the energy efficiency and cycle life of the battery, enhances the rate performance and thermal stability of the material, extends the service life of the battery, and slows down capacity attenuation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005048997940000201
    Figure BDA0005048997940000201
Patent Text Reader

Abstract

The invention provides a doped and coated ternary positive electrode material as well as a preparation method and application thereof. The doped and coated ternary positive electrode material comprises a gallium-magnesium co-doped nickel-cobalt-manganese core, a magnesium-coated intermediate layer and a metal oxide-phosphate co-coated shell, by taking the total mass of the ternary positive electrode material as a calculation reference, the mass ratio of the metal oxide-phosphate co-coated shell is 5-20wt%. According to the doped and coated ternary positive electrode material provided by the invention, the voltage attenuation of the positive electrode material in the use process of a battery is reduced, the electrochemical performance of the material and the cycle performance of the battery are improved, and large-scale popularization and application are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery material preparation, and relates to a ternary positive electrode material, and in particular to a doped coated ternary positive electrode material and a preparation method and application thereof. Background Art

[0002] Nickel-rich ternary positive electrode materials include nickel-rich lithium nickel cobalt manganese oxide and nickel cobalt aluminum oxide materials, and their nickel content is generally greater than 50wt%. Among them, nickel is mainly an electrochemically active element, and the increase in nickel content helps to increase the capacity of the material, thereby improving the energy density; the presence of cobalt can reduce the electrochemical polarization of the material and improve its rate characteristics, and too high a content will reduce the reversible capacity; manganese provides a guarantee for the structural stability and thermal stability of the material. The presence of manganese can reduce costs and improve safety performance, and too high a content can easily destroy the original layered structure of the material. Due to the high nickel content, nickel-rich ternary positive electrode materials have a higher reversible discharge specific capacity, but poor cycle performance. This is mainly due to the unstable surface properties, structural defects, lithium-nickel mixed arrangement, intergranular cracks and microstrain of the material. In order to solve the above problems, technicians have proposed many modification strategies, mainly including: surface interface engineering, bulk doping and morphology control and other modification methods.

[0003] The current nickel-cobalt-manganese ternary cathode materials still have other problems that need to be solved, such as low initial charge and discharge efficiency and poor rate cycle performance. These problems will be the focus of future research on the modification of nickel-cobalt-manganese ternary cathode materials. The conventional nickel-cobalt-manganese ternary cathode material precursor is a secondary spherical particle formed by the agglomeration of primary particles of fine grains. It has a dense structure and a low specific surface area. The ternary cathode materials prepared later will also inherit these characteristics. However, as the number of cycles of lithium-ion batteries increases, the primary particles in the secondary spheres have different crystal plane orientations and slip planes, and the anisotropy of lattice expansion and contraction between grains may cause secondary particles to expand or contract in the later stages of the cycle. The expansion or contraction may cause crushing, pulverization, and structural collapse, which in turn leads to an increase in battery impedance and a decrease in active ingredients. It will also aggravate its side reactions with the electrolyte, resulting in severe capacity decay, and a sharp decline in rate and cycle performance.

[0004] It can be seen that how to provide a nickel-cobalt-manganese ternary positive electrode material and a preparation method thereof, reduce the voltage attenuation of the positive electrode material during battery use, and improve the electrochemical properties of the material and the cycle performance of the battery has become an urgent problem that technical personnel in this field need to solve. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a doped and coated ternary positive electrode material and a preparation method and application thereof. The doped and coated ternary positive electrode material reduces the voltage attenuation of the positive electrode material during battery use, improves the electrochemical properties of the material and the cycle performance of the battery, and is conducive to large-scale promotion and application.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a doped and coated ternary positive electrode material, which comprises a gallium-magnesium co-doped nickel-cobalt-manganese core, a magnesium-coated intermediate layer and a metal oxide-phosphate co-coated outer shell.

[0008] Taking the total mass of the ternary positive electrode material as the calculation basis, the mass proportion of the metal oxide-phosphate co-coated shell is 5-20wt%, for example, it can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0009] The present invention performs gallium-magnesium co-doping in the nickel-cobalt-manganese core, which helps to improve the electrochemical properties of the ternary positive electrode material, wherein the doping of the gallium element can improve the electronic conductivity and lithium ion diffusivity of the material, thereby improving the rate performance of the material, and enabling the battery to operate at a higher current density without significantly reducing its performance; the doping of the magnesium element helps to stabilize the structure of the material, thereby improving its cycle stability, and at the same time, magnesium ions replace part of the nickel or manganese ions, reducing the lithium-nickel mixing phenomenon.

[0010] In addition, the presence of the magnesium-coated intermediate layer significantly increases the energy barrier for oxygen release in the nickel-cobalt-manganese positive electrode material, helps to stabilize the surface oxygen of the lithium-rich material, thereby reducing the voltage decay during charging and discharging and improving the energy efficiency of the battery; the metal oxide-phosphate co-coated shell has high thermal stability, which improves the performance of the ternary positive electrode material in high temperature environments and reduces the risk of thermal runaway. The co-coated shell further enhances the structural stability of the ternary positive electrode material and reduces the volume expansion and contraction during charging and discharging, thereby extending the cycle life of the battery.

[0011] Furthermore, the co-coated shell acts as a physical barrier, reducing the direct contact between the electrolyte and the ternary positive electrode material, thereby reducing the decomposition rate of the electrolyte and extending the service life of the battery. At the same time, it inhibits the dissolution of transition metals in the ternary positive electrode material during the charge and discharge process, reduces the concentration of metal ions in the electrolyte, thereby slowing down the attenuation of the battery capacity and improving the electrochemical performance of the material.

[0012] Preferably, the chemical formula of the gallium-magnesium co-doped nickel-cobalt-manganese core is: Li a Ni x Co y Mn z Ga m Mg n O2; wherein 1≤a≤1.5, for example, a=1, 1.1, 1.2, 1.3, 1.4 or 1.5, 0.6≤x≤0.8, for example, x=0.6, 0.62, 0.64, 0.66, 0.68, 0.7, 0.72, 0.74, 0.76, 0.78 or 0.8, x+y+z≤1, for example, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95 or 1, m:n=(1-3):1, for example, 1:1, 1.2:1, 1.4:1, 1.6:1, 1.8:1, 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1 or 3:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0013] Preferably, the average thickness of the magnesium-coated intermediate layer is 0.2-2 μm, for example, it can be 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm or 2 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] Preferably, in the metal oxide-phosphate co-coated shell, the metal oxide includes any one of aluminum oxide, zinc oxide or tin oxide, or a combination of at least two of them. Typical but non-limiting combinations include a combination of aluminum oxide and zinc oxide, a combination of zinc oxide and tin oxide, a combination of aluminum oxide and tin oxide, or a combination of aluminum oxide, zinc oxide and tin oxide, and aluminum oxide is further preferred.

[0015] Preferably, in the metal oxide-phosphate co-coated shell, the phosphate includes any one of lanthanum phosphate, aluminum phosphate or cerium phosphate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of lanthanum phosphate and aluminum phosphate, a combination of aluminum phosphate and cerium phosphate, a combination of lanthanum phosphate and cerium phosphate, or a combination of lanthanum phosphate, aluminum phosphate and cerium phosphate, and lanthanum phosphate is further preferred.

[0016] Preferably, in the metal oxide-phosphate co-coated shell, the mass ratio of metal oxide to phosphate is (0.2-2):1, for example, it can be 0.2:1, 0.4:1, 0.6:1, 0.8:1, 1:1, 1.2:1, 1.4:1, 1.6:1, 1.8:1 or 2:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] In the present invention, the mass ratio of metal oxide to phosphate affects the uniformity and integrity of the co-coated shell. Limiting the mass ratio to within the range of (0.2-2):1 helps to form a continuous and uniform co-coated shell, thereby effectively isolating the positive electrode material from direct contact with the electrolyte. At the same time, due to the different electrical conductivity of metal oxide and phosphate, a reasonable limitation of the mass ratio of the two helps to further optimize the ionic and electronic conductivity of the co-coated shell, thereby significantly improving the charge and discharge performance of the positive electrode material.

[0018] In a second aspect, the present invention provides a method for preparing the doped coated ternary cathode material as described in the first aspect, the preparation method comprising the following steps:

[0019] (1) mixing nickel salt, cobalt salt, manganese salt and deionized water to obtain a ternary salt solution;

[0020] (2) preparing a gallium salt solution, a magnesium salt solution, a precipitant solution and a complexing agent solution respectively;

[0021] (3) preparing a base liquid in a reaction kettle, then introducing a ternary salt solution, a precipitant solution and a complexing agent solution, controlling the pH of the mixed solution to a first target value, starting a coprecipitation reaction in a protective gas atmosphere, and then introducing a gallium salt solution, while continuing to introduce the ternary salt solution, the precipitant solution and the complexing agent solution, and controlling the pH of the mixed solution to a second target value; when the average particle size D50 of the precursor particles reaches a first set value, starting to gradually reduce the flow rate of the gallium salt solution until the flow rate is 0, and starting to introduce a magnesium salt solution, and gradually increasing the flow rate of the magnesium salt solution from 0; when the average particle size D50 of the precursor particles reaches a second set value, stopping the introduction of the ternary salt solution; when the average particle size D50 of the precursor particles reaches a third set value, stopping the introduction of the magnesium salt solution, the precipitant solution and the complexing agent solution, and obtaining a precursor material after solid-liquid separation;

[0022] (4) mixing the precursor material and the lithium salt for solid phase sintering to obtain an intermediate material;

[0023] (5) The intermediate material, metal oxide and phosphate are mixed and subjected to ball milling and heat treatment in sequence to obtain the doped and coated ternary positive electrode material.

[0024] There is no particular order in which steps (1) and (2) are performed.

[0025] Preferably, the nickel salt, cobalt salt and manganese salt in step (1) are any one of sulfate, nitrate or chloride salts of the corresponding metal ions, or a combination of at least two of them. Typical but non-limiting combinations include a combination of sulfate and nitrate, a combination of nitrate and chloride, a combination of sulfate and chloride, or a combination of sulfate, nitrate and chloride.

[0026] Preferably, the total concentration of metal ions in the ternary salt solution in step (1) is 0.5-10 mol / L, for example, it can be 0.5 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L or 10 mol / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] Preferably, the gallium salt solution in step (2) comprises any one of gallium sulfate solution, gallium nitrate solution or gallium chloride solution, or a combination of at least two of them. Typical but non-limiting combinations include a combination of gallium sulfate solution and gallium nitrate solution, a combination of gallium nitrate solution and gallium chloride solution, a combination of gallium sulfate solution and gallium chloride solution, or a combination of gallium sulfate solution, gallium nitrate solution and gallium chloride solution.

[0028] Preferably, the concentration of gallium ions in the gallium salt solution in step (2) is 1500-2500 ppm, for example, 1500 ppm, 1600 ppm, 1700 ppm, 1800 ppm, 1900 ppm, 2000 ppm, 2100 ppm, 2200 ppm, 2300 ppm, 2400 ppm or 2500 ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the magnesium salt solution in step (2) comprises any one of magnesium sulfate solution, magnesium nitrate solution or magnesium chloride solution, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of magnesium sulfate solution and magnesium nitrate solution, a combination of magnesium nitrate solution and magnesium chloride solution, a combination of magnesium sulfate solution and magnesium chloride solution, or a combination of magnesium sulfate solution, magnesium nitrate solution and magnesium chloride solution.

[0030] Preferably, the concentration of magnesium ions in the magnesium salt solution in step (2) is 800-1200 ppm, for example, 800 ppm, 850 ppm, 900 ppm, 950 ppm, 1000 ppm, 1050 ppm, 1100 ppm, 1150 ppm or 1200 ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the precipitant solution in step (2) comprises sodium hydroxide solution and / or sodium carbonate solution.

[0032] Preferably, the concentration of the precipitant solution in step (2) is 30-40wt%, for example, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt% or 40wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the complexing agent solution in step (2) comprises aqueous ammonia.

[0034] Preferably, the concentration of the complexing agent solution in step (2) is 10-20wt%, for example, it can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the base solution in step (3) is a mixed solution of a precipitant solution and a complexing agent solution, and the pH value of the base solution is 10-11, for example, it can be 10, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9 or 11, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the flow rate of the ternary salt solution in step (3) is 30-50 L / h, for example, 30 L / h, 32 L / h, 34 L / h, 36 L / h, 38 L / h, 40 L / h, 42 L / h, 44 L / h, 46 L / h, 48 L / h or 50 L / h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the pH of the mixed solution in step (3) is controlled by adjusting the flow rates of the precipitant solution and the complexing agent solution.

[0038] Preferably, the first target value in step (3) is 9.5-11.5, for example, it can be 9.5, 9.6, 9.7, 9.8, 9.9, 10, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9, 11, 11.1, 11.2, 11.3, 11.4 or 11.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the protective gas in step (3) includes nitrogen and / or argon, which is used to protect reactants and products from oxidation, thereby ensuring the purity and performance of the materials.

[0040] Preferably, the temperature of the coprecipitation reaction in step (3) is 40-65°C, for example, it can be 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C or 65°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Preferably, the coprecipitation reaction in step (3) is accompanied by stirring, and the stirring rate is 200-400 rpm, for example, it can be 200 rpm, 220 rpm, 240 rpm, 260 rpm, 280 rpm, 300 rpm, 320 rpm, 340 rpm, 360 rpm, 380 rpm or 400 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the flow rate of the gallium salt solution in step (3) is 1-3 L / h, for example, it can be 1 L / h, 1.2 L / h, 1.4 L / h, 1.6 L / h, 1.8 L / h, 2 L / h, 2.2 L / h, 2.4 L / h, 2.6 L / h, 2.8 L / h or 3 L / h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, in step (3), the second target value is 10.2-10.8, for example, it can be 10.2, 10.3, 10.4, 10.5, 10.6, 10.7 or 10.8, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the first set value in step (3) is 3-5 μm, for example, it can be 3 μm, 3.2 μm, 3.4 μm, 3.6 μm, 3.8 μm, 4 μm, 4.2 μm, 4.4 μm, 4.6 μm, 4.8 μm or 5 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the gradual reduction time of the gallium salt solution in step (3) is 0.5-1.5h, for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the flow rate of the magnesium salt solution in step (3) is 1-3 L / h, for example, 1 L / h, 1.2 L / h, 1.4 L / h, 1.6 L / h, 1.8 L / h, 2 L / h, 2.2 L / h, 2.4 L / h, 2.6 L / h, 2.8 L / h or 3 L / h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0047] Preferably, the gradual increase time of the magnesium salt solution in step (3) is 0.5-1.5h, for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, in step (3), the second set value is 8-10 μm, for example, it can be 8 μm, 8.2 μm, 8.4 μm, 8.6 μm, 8.8 μm, 9 μm, 9.2 μm, 9.4 μm, 9.6 μm, 9.8 μm or 10 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] Preferably, the third set value in step (3) is 11-13 μm, for example, it can be 11 μm, 11.2 μm, 11.4 μm, 11.6 μm, 11.8 μm, 12 μm, 12.2 μm, 12.4 μm, 12.6 μm, 12.8 μm or 13 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] Preferably, the solid-liquid separation in step (3) comprises centrifugation, washing and drying performed sequentially.

[0051] Preferably, the lithium salt in step (4) comprises lithium carbonate.

[0052] Preferably, the solid phase sintering in step (4) is carried out in an air atmosphere.

[0053] Preferably, the temperature of the solid phase sintering in step (4) is 900-1100°C, for example, it can be 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, 1020°C, 1040°C, 1060°C, 1080°C or 1100°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] Preferably, the solid-phase sintering time in step (4) is 20-30 h, for example, it can be 20 h, 21 h, 22 h, 23 h, 24 h, 25 h, 26 h, 27 h, 28 h, 29 h or 30 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] Preferably, the metal oxide in step (5) comprises any one of aluminum oxide, zinc oxide or tin oxide, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of aluminum oxide and zinc oxide, a combination of zinc oxide and tin oxide, a combination of aluminum oxide and tin oxide, or a combination of aluminum oxide, zinc oxide and tin oxide, and aluminum oxide is further preferred.

[0056] Preferably, the phosphate in step (5) includes any one of lanthanum phosphate, aluminum phosphate or cerium phosphate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of lanthanum phosphate and aluminum phosphate, a combination of aluminum phosphate and cerium phosphate, a combination of lanthanum phosphate and cerium phosphate, or a combination of lanthanum phosphate, aluminum phosphate and cerium phosphate, and lanthanum phosphate is further preferred.

[0057] Preferably, the heat treatment in step (5) is carried out in an air atmosphere.

[0058] Preferably, the temperature of the heat treatment in step (5) is 900-1100°C, for example, it can be 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, 1020°C, 1040°C, 1060°C, 1080°C or 1100°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] Preferably, the heat treatment time in step (5) is 8-12 h, for example, 8 h, 8.5 h, 9 h, 9.5 h, 10 h, 10.5 h, 11 h, 11.5 h or 12 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] As a preferred technical solution of the second aspect of the present invention, the preparation method comprises the following steps:

[0061] (1) mixing a nickel salt, a cobalt salt, a manganese salt and deionized water to obtain a ternary salt solution with a total metal ion concentration of 0.5-10 mol / L; wherein the nickel salt, the cobalt salt and the manganese salt are any one of sulfate, nitrate or chloride salts of the corresponding metal ions, or a combination of at least two of them;

[0062] (2) preparing a gallium salt solution, a magnesium salt solution, a precipitant solution and a complexing agent solution respectively; the gallium salt solution comprises any one of a gallium sulfate solution, a gallium nitrate solution or a gallium chloride solution or a combination of at least two thereof, and the concentration of gallium ions is 1500-2500 ppm; the magnesium salt solution comprises any one of a magnesium sulfate solution, a magnesium nitrate solution or a magnesium chloride solution or a combination of at least two thereof, and the concentration of magnesium ions is 800-1200 ppm; the precipitant solution comprises a sodium hydroxide solution and / or a sodium carbonate solution, and the concentration is 30-40 wt%; the complexing agent solution comprises ammonia water with a concentration of 10-20 wt%;

[0063] (3) Mixing the precipitant solution and the complexing agent solution in a reaction kettle to obtain a base solution with a pH value of 10-11, then introducing the ternary salt solution, the precipitant solution and the complexing agent solution, and controlling the flow rate of the ternary salt solution to 30-50 L / h, adjusting the flow rate of the precipitant solution and the complexing agent solution to control the pH of the mixed solution to 9.5-11.5, starting the coprecipitation reaction at 40-65° C. in a nitrogen and / or argon atmosphere, accompanied by stirring at a rate of 200-400 rpm, and then introducing the gallium salt solution at a flow rate of 1-3 L / h, while continuing to introduce the ternary salt solution, the precipitant solution and the complexing agent solution, and controlling the flow rate of the ternary salt solution to 30-50 L / h. The pH of the mixed solution is 10.2-10.8; when the average particle size D50 of the precursor particles reaches 3-5 μm, the flow rate of the gallium salt solution is gradually reduced within 0.5-1.5 hours until the flow rate is 0, and the magnesium salt solution is introduced at the same time, and the flow rate of the magnesium salt solution is gradually increased from 0 to 1-3 L / h within 0.5-1.5 hours; when the average particle size D50 of the precursor particles reaches 8-10 μm, the introduction of the ternary salt solution is stopped; when the average particle size D50 of the precursor particles reaches 11-13 μm, the introduction of the magnesium salt solution, the precipitant solution and the complexing agent solution is stopped, and the precursor material is obtained after centrifugation, washing and drying;

[0064] (4) mixing the precursor material and lithium carbonate, and performing solid phase sintering at 900-1100° C. for 20-30 h in an air atmosphere to obtain an intermediate material;

[0065] (5) The intermediate material, aluminum oxide and lanthanum phosphate are mixed and ball-milled, and then heat-treated at 900-1100° C. for 8-12 h in an air atmosphere to obtain the doped coated ternary positive electrode material.

[0066] There is no particular order in which steps (1) and (2) are performed.

[0067] In a third aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the doped and coated ternary positive electrode material as described in the first aspect.

[0068] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0069] Compared with the prior art, the present invention has the following beneficial effects:

[0070] (1) The present invention performs gallium-magnesium co-doping in the nickel-cobalt-manganese core, which helps to improve the electrochemical properties of the ternary positive electrode material. The doping of gallium can improve the electronic conductivity and lithium ion diffusivity of the material, thereby improving the rate performance of the material and enabling the battery to operate at a higher current density without significantly reducing its performance. The doping of magnesium helps to stabilize the structure of the material, thereby improving its cycle stability. At the same time, magnesium ions replace part of the nickel or manganese ions, reducing the lithium-nickel mixing phenomenon.

[0071] (2) The presence of the magnesium-coated intermediate layer significantly increases the energy barrier for oxygen release from the nickel-cobalt-manganese cathode material, helps stabilize the surface oxygen of the lithium-rich material, thereby reducing the voltage decay during the charge and discharge process and improving the energy efficiency of the battery; the metal oxide-phosphate co-coated shell has high thermal stability, improves the performance of the ternary cathode material in a high temperature environment, reduces the risk of thermal runaway, and the co-coated shell further enhances the structural stability of the ternary cathode material, reduces the volume expansion and contraction during the charge and discharge process, thereby extending the cycle life of the battery.

[0072] (3) The co-coated shell acts as a physical barrier, reducing the direct contact between the electrolyte and the ternary cathode material, thereby reducing the decomposition rate of the electrolyte and extending the service life of the battery. At the same time, it inhibits the dissolution of transition metals in the ternary cathode material during the charge and discharge process, reduces the concentration of metal ions in the electrolyte, thereby slowing down the attenuation of the battery capacity and improving the electrochemical performance of the material. DETAILED DESCRIPTION

[0073] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0074] Example 1

[0075] The present embodiment provides a doped and coated ternary positive electrode material and a preparation method thereof, wherein the doped and coated ternary positive electrode material comprises a gallium-magnesium co-doped nickel-cobalt-manganese core, a magnesium-coated intermediate layer, and a metal oxide-phosphate co-coated outer shell; taking the total mass of the ternary positive electrode material as a calculation basis, the mass proportion of the metal oxide-phosphate co-coated outer shell is 12wt%.

[0076] In this embodiment, the chemical formula of the gallium-magnesium co-doped nickel-cobalt-manganese core is: Li 1.2 Ni 0.64 Co0.08 Mn 0.08 Ga 0.0 2Mg 0.01 O2; the average thickness of the magnesium-coated intermediate layer is 1 μm; in the metal oxide-phosphate co-coated shell, the metal oxide is aluminum oxide, the phosphate is lanthanum phosphate, and the mass ratio of the metal oxide to the phosphate is 1.2:1.

[0077] The preparation method provided in this embodiment comprises the following steps:

[0078] (1) mixing nickel sulfate, cobalt sulfate, manganese sulfate and deionized water to obtain a ternary salt solution with a total metal ion concentration of 5 mol / L;

[0079] (2) preparing a gallium sulfate solution with a gallium ion concentration of 2000 ppm, a magnesium sulfate solution with a magnesium ion concentration of 1000 ppm, a sodium hydroxide solution with a concentration of 30 wt %, and an ammonia solution with a concentration of 20 wt % respectively;

[0080] (3) Mixing sodium hydroxide solution and ammonia water in a reactor to obtain a base liquid with a pH value of 10.8, then introducing a ternary salt solution, a sodium hydroxide solution and ammonia water, and controlling the introduction flow rate of the ternary salt solution to 40 L / h, and adjusting the introduction flow rate of the sodium hydroxide solution and ammonia water to control the pH of the mixed solution to 11±0.5, and starting a coprecipitation reaction at 52° C. in a nitrogen atmosphere, accompanied by stirring at a rate of 300 rpm, and then introducing a gallium sulfate solution at a flow rate of 2 L / h, while continuing to keep the ternary salt solution, sodium hydroxide solution and ammonia water to control the pH of the mixed solution The pH value is 10.6±0.2; when the average particle size D50 of the precursor particles reaches 4±1 μm, the flow rate of the gallium sulfate solution is gradually reduced within 1 hour until the flow rate is 0, and the magnesium sulfate solution is introduced at the same time, and the flow rate of the magnesium sulfate solution is gradually increased from 0 to 2 L / h within 1 hour; when the average particle size D50 of the precursor particles reaches 9±1 μm, the introduction of the ternary salt solution is stopped; when the average particle size D50 of the precursor particles reaches 12±1 μm, the introduction of the magnesium sulfate solution, the sodium hydroxide solution and the ammonia water is stopped, and the precursor material is obtained after centrifugation, washing and drying;

[0081] (4) mixing the precursor material and lithium carbonate, first heating to 50° C. in an air atmosphere for 8 h, and then continuing to heat to 1000° C. for solid phase sintering for 24 h to obtain an intermediate material;

[0082] (5) The intermediate material, aluminum oxide and lanthanum phosphate are mixed and ball-milled, and then heat-treated at 1000° C. for 10 h in an air atmosphere to obtain the doped coated ternary positive electrode material.

[0083] Example 2

[0084] The present embodiment provides a doped and coated ternary positive electrode material and a preparation method thereof, wherein the doped and coated ternary positive electrode material comprises a gallium-magnesium co-doped nickel-cobalt-manganese core, a magnesium-coated intermediate layer and a metal oxide-phosphate co-coated outer shell; taking the total mass of the ternary positive electrode material as a calculation basis, the mass proportion of the metal oxide-phosphate co-coated outer shell is 5wt%.

[0085] In this embodiment, the chemical formula of the gallium-magnesium co-doped nickel-cobalt-manganese core is: Li 1.5 Ni 0.6 Co 0.06 Mn 0.06 Ga 0.02 Mg 0.02 O2; the average thickness of the magnesium-coated intermediate layer is 0.2 μm; in the metal oxide-phosphate co-coated shell, the metal oxide is aluminum oxide, the phosphate is lanthanum phosphate, and the mass ratio of the metal oxide to the phosphate is 0.2:1.

[0086] The preparation method provided in this embodiment comprises the following steps:

[0087] (1) mixing nickel nitrate, cobalt nitrate, manganese nitrate and deionized water to obtain a ternary salt solution with a total metal ion concentration of 0.5 mol / L;

[0088] (2) preparing a gallium nitrate solution with a gallium ion concentration of 1500 ppm, a magnesium nitrate solution with a magnesium ion concentration of 800 ppm, a sodium carbonate solution with a concentration of 30 wt %, and an ammonia solution with a concentration of 10 wt % respectively;

[0089] (3) Mixing sodium carbonate solution and ammonia water in a reactor to obtain a base solution with a pH value of 10, then introducing a ternary salt solution, a sodium carbonate solution and ammonia water, and controlling the introduction flow rate of the ternary salt solution to 30 L / h, and adjusting the introduction flow rates of the sodium carbonate solution and ammonia water to control the pH of the mixed solution to 10±0.5, and starting a coprecipitation reaction at 40° C. in an argon atmosphere, accompanied by stirring at a rate of 200 rpm, and then introducing a gallium nitrate solution at a flow rate of 1 L / h, while continuing to introduce the ternary salt solution, sodium carbonate solution and ammonia water, and controlling the pH of the mixed solution to 1 0.4±0.2; when the average particle size D50 of the precursor particles reaches 4±1μm, the flow rate of the gallium nitrate solution is gradually reduced within 0.5h until the flow rate is 0, and at the same time, the magnesium nitrate solution is introduced, and the flow rate of the magnesium nitrate solution is gradually increased from 0 to 1L / h within 0.5h; when the average particle size D50 of the precursor particles reaches 9±1μm, the introduction of the ternary salt solution is stopped; when the average particle size D50 of the precursor particles reaches 12±1μm, the introduction of the magnesium nitrate solution, the sodium carbonate solution and the ammonia water is stopped, and the precursor material is obtained after centrifugation, washing and drying;

[0090] (4) mixing the precursor material and lithium carbonate, first heating to 50° C. in an air atmosphere for 8 h, and then continuing to heat to 900° C. for solid phase sintering for 30 h to obtain an intermediate material;

[0091] (5) The intermediate material, aluminum oxide and lanthanum phosphate are mixed and ball-milled, and then heat-treated at 900° C. for 12 h in an air atmosphere to obtain the doped coated ternary positive electrode material.

[0092] Example 3

[0093] The present embodiment provides a doped and coated ternary positive electrode material and a preparation method thereof, wherein the doped and coated ternary positive electrode material comprises a gallium-magnesium co-doped nickel-cobalt-manganese core, a magnesium-coated intermediate layer and a metal oxide-phosphate co-coated outer shell; taking the total mass of the ternary positive electrode material as a calculation basis, the mass proportion of the metal oxide-phosphate co-coated outer shell is 20wt%.

[0094] In this embodiment, the chemical formula of the gallium-magnesium co-doped nickel-cobalt-manganese core is: Li1Ni 0.8 Co 0.08 Mn 0.08 Ga 0.03 Mg 0.01 O2; the average thickness of the magnesium-coated intermediate layer is 2 μm; in the metal oxide-phosphate co-coated shell, the metal oxide is aluminum oxide, the phosphate is lanthanum phosphate, and the mass ratio of the metal oxide to the phosphate is 2:1.

[0095] The preparation method provided in this embodiment comprises the following steps:

[0096] (1) mixing nickel chloride, cobalt chloride, manganese chloride and deionized water to obtain a ternary salt solution with a total metal ion concentration of 10 mol / L;

[0097] (2) preparing a gallium chloride solution with a gallium ion concentration of 2500 ppm, a magnesium chloride solution with a magnesium ion concentration of 1200 ppm, a sodium hydroxide solution with a concentration of 40 wt %, and an ammonia solution with a concentration of 20 wt % respectively;

[0098] (3) Mixing sodium hydroxide solution and ammonia water in a reactor to obtain a base solution with a pH value of 11, then introducing a ternary salt solution, a sodium hydroxide solution and ammonia water, and controlling the introduction flow rate of the ternary salt solution to 50 L / h, and adjusting the introduction flow rates of the sodium hydroxide solution and ammonia water to control the pH of the mixed solution to 11±0.5, starting a coprecipitation reaction at 65° C. in a nitrogen atmosphere, accompanied by stirring at a rate of 400 rpm, and then introducing a gallium chloride solution at a flow rate of 3 L / h, while continuing to introduce the ternary salt solution, sodium hydroxide solution and ammonia water, and controlling the pH of the mixed solution to 10.6±0.2; when the average particle size D50 of the precursor particles reaches 4±1μm, the flow rate of the gallium chloride solution is gradually reduced within 1.5h until the flow rate is 0, and the magnesium chloride solution is introduced at the same time, and the flow rate of the magnesium chloride solution is gradually increased from 0 to 3L / h within 1.5h; when the average particle size D50 of the precursor particles reaches 9±1μm, the introduction of the ternary salt solution is stopped; when the average particle size D50 of the precursor particles reaches 12±1μm, the introduction of the magnesium chloride solution, the sodium hydroxide solution and the ammonia water is stopped, and the precursor material is obtained after centrifugation, washing and drying;

[0099] (4) mixing the precursor material and lithium carbonate, first heating to 50° C. in an air atmosphere for 8 h, and then continuing to heat to 1100° C. for solid phase sintering for 20 h to obtain an intermediate material;

[0100] (5) The intermediate material, aluminum oxide and lanthanum phosphate are mixed and ball-milled, and then heat-treated at 1100° C. for 8 h in an air atmosphere to obtain the doped coated ternary positive electrode material.

[0101] Example 4

[0102] This embodiment provides a doped coated ternary positive electrode material and a preparation method thereof. Except for replacing aluminum oxide with an equal mass of zinc oxide and replacing lanthanum phosphate with an equal mass of aluminum phosphate, the remaining steps and conditions are the same as those in Example 1, so they are not repeated here.

[0103] Example 5

[0104] This embodiment provides a doped coated ternary positive electrode material and a preparation method thereof. Except for replacing aluminum oxide with an equal mass of tin oxide and replacing lanthanum phosphate with an equal mass of cerium phosphate, the remaining steps and conditions are the same as those in Example 1, so they are not repeated here.

[0105] Example 6

[0106] This embodiment provides a doped coated ternary positive electrode material and a preparation method thereof. Except for changing the mass ratio of metal oxide to phosphate to 0.1:1, the remaining steps and conditions are the same as those in Example 1, so they are not repeated here.

[0107] Example 7

[0108] This embodiment provides a doped coated ternary positive electrode material and a preparation method thereof. Except for changing the mass ratio of metal oxide to phosphate to 2.5:1, the remaining steps and conditions are the same as those in Example 1, so they are not repeated here.

[0109] Example 8

[0110] This embodiment provides a doped coated ternary positive electrode material and a preparation method thereof. Except that the temperature of the coprecipitation reaction is changed to 35° C., the remaining steps and conditions are the same as those in Example 1, so they are not described here in detail.

[0111] Example 9

[0112] This embodiment provides a doped coated ternary positive electrode material and a preparation method thereof. Except that the temperature of the coprecipitation reaction is changed to 70° C., the remaining steps and conditions are the same as those in Example 1, so they are not described here in detail.

[0113] Example 10

[0114] This embodiment provides a doped coated ternary positive electrode material and a preparation method thereof. Except that the temperature of the heat treatment in step (5) is changed to 800° C., the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.

[0115] Comparative Example 1

[0116] This comparative example provides a ternary positive electrode material and a preparation method thereof, wherein the ternary positive electrode material comprises a gallium-magnesium co-doped nickel-cobalt-manganese core and a metal oxide-phosphate co-coated shell; taking the total mass of the ternary positive electrode material as a calculation basis, the mass proportion of the metal oxide-phosphate co-coated shell is 12wt%.

[0117] In this comparative example, the chemical formula of the gallium-magnesium co-doped nickel-cobalt-manganese core is: Li 1.2 Ni 0.64 Co 0.08 Mn 0.08 Ga 0.0 2Mg 0.01 O2; in the metal oxide-phosphate co-coated shell, the metal oxide is aluminum oxide, the phosphate is lanthanum phosphate, and the mass ratio of the metal oxide to the phosphate is 1.2:1.

[0118] The preparation method provided in this comparative example comprises the following steps:

[0119] (1) mixing nickel sulfate, cobalt sulfate, manganese sulfate and deionized water to obtain a ternary salt solution with a total metal ion concentration of 5 mol / L;

[0120] (2) preparing a gallium sulfate solution with a gallium ion concentration of 2000 ppm, a magnesium sulfate solution with a magnesium ion concentration of 1000 ppm, a sodium hydroxide solution with a concentration of 32 wt %, and an ammonia solution with a concentration of 18 wt % respectively;

[0121] (3) Mixing sodium hydroxide solution and ammonia water in a reactor to obtain a base solution with a pH value of 10.8, then introducing a ternary salt solution, a sodium hydroxide solution and ammonia water, and controlling the introduction flow rate of the ternary salt solution to 40 L / h, and adjusting the introduction flow rates of the sodium hydroxide solution and ammonia water to control the pH of the mixed solution to 11±0.5, and starting a coprecipitation reaction at 52° C. in a nitrogen atmosphere, accompanied by stirring at a rate of 300 rpm, and then introducing a gallium sulfate solution at a flow rate of 2 L / h, while maintaining the ternary salt solution and the sodium hydroxide solution at a constant flow rate of 1 L / h. The solution and ammonia water are continuously introduced, and the pH value of the mixed solution is controlled to be 10.6±0.2; when the average particle size D50 of the precursor particles reaches 4±1 μm, the flow rate of the gallium sulfate solution is gradually reduced within 1 hour until the flow rate is 0, and the magnesium sulfate solution is introduced at the same time, and the flow rate of the magnesium sulfate solution is gradually increased from 0 to 2 L / h within 1 hour; when the average particle size D50 of the precursor particles reaches 12±1 μm, the magnesium sulfate solution, sodium hydroxide solution and ammonia water are stopped, and the precursor material is obtained after centrifugation, washing and drying;

[0122] (4) mixing the precursor material and lithium carbonate, first heating to 50° C. in an air atmosphere for 8 h, and then continuing to heat to 1000° C. for solid phase sintering for 24 h to obtain an intermediate material;

[0123] (5) The intermediate material, aluminum oxide and lanthanum phosphate are mixed and ball-milled, and then heat-treated at 1000° C. for 10 h in an air atmosphere to obtain the ternary positive electrode material.

[0124] Comparative Example 2

[0125] This comparative example provides a ternary positive electrode material and a preparation method thereof, wherein the ternary positive electrode material comprises a nickel-cobalt-manganese core, a magnesium-coated intermediate layer and a metal oxide-phosphate co-coated outer shell; taking the total mass of the ternary positive electrode material as a calculation basis, the mass proportion of the metal oxide-phosphate co-coated outer shell is 12wt%.

[0126] In this comparative example, the chemical formula of the nickel-cobalt-manganese core is: Li 1.2 Ni 0.64 Co 0.08 Mn 0.08 O2; the average thickness of the magnesium-coated intermediate layer is 1 μm; in the metal oxide-phosphate co-coated shell, the metal oxide is aluminum oxide, the phosphate is lanthanum phosphate, and the mass ratio of the metal oxide to the phosphate is 1.2:1.

[0127] The preparation method provided in this comparative example comprises the following steps:

[0128] (1) mixing nickel sulfate, cobalt sulfate, manganese sulfate and deionized water to obtain a ternary salt solution with a total metal ion concentration of 5 mol / L;

[0129] (2) preparing a magnesium sulfate solution with a magnesium ion concentration of 1000 ppm, a sodium hydroxide solution with a concentration of 32 wt %, and an ammonia solution with a concentration of 18 wt % respectively;

[0130] (3) Mixing sodium hydroxide solution and ammonia water in a reactor to obtain a base liquid with a pH value of 10.8, then introducing a ternary salt solution, a sodium hydroxide solution and ammonia water, and controlling the flow rate of the ternary salt solution to 40 L / h, adjusting the flow rate of the sodium hydroxide solution and ammonia water to control the pH of the mixed solution to 11±0.5, and starting a coprecipitation reaction at 52° C. in a nitrogen atmosphere, accompanied by stirring at a rate of 300 rpm; when the average particle size D50 of the precursor particles reaches 9±1 μm, starting to introduce a magnesium sulfate solution at a flow rate of 2 L / h, and stopping the introduction of the ternary salt solution; when the average particle size D50 of the precursor particles reaches 12±1 μm, stopping the introduction of the magnesium sulfate solution, the sodium hydroxide solution and the ammonia water, and obtaining the precursor material after centrifugation, washing and drying;

[0131] (4) mixing the precursor material and lithium carbonate, first heating to 50° C. in an air atmosphere for 8 h, and then continuing to heat to 1000° C. for solid phase sintering for 24 h to obtain an intermediate material;

[0132] (5) The intermediate material, aluminum oxide and lanthanum phosphate are mixed and ball-milled, and then heat-treated at 1000° C. for 10 h in an air atmosphere to obtain the doped coated ternary positive electrode material.

[0133] Comparative Example 3

[0134] This comparative example provides a ternary positive electrode material and a preparation method thereof, except that no aluminum oxide is added in step (5), that is, only lanthanum phosphate is coated on the intermediate material, and the remaining steps and conditions are the same as those in Example 1, so they are not repeated here.

[0135] Comparative Example 4

[0136] This comparative example provides a ternary positive electrode material and a preparation method thereof, except that lanthanum phosphate is not added in step (5), that is, only the intermediate material is coated with alumina, and the remaining steps and conditions are the same as those in Example 1, so they are not repeated here.

[0137] Comparative Example 5

[0138] This comparative example provides a ternary positive electrode material and a preparation method thereof. Except for deleting step (5), that is, directly using the intermediate material as the ternary positive electrode material, the remaining steps and conditions are the same as those in Example 1, and therefore are not described in detail here.

[0139] Performance Test:

[0140] Button-type lithium-ion batteries were prepared using the ternary positive electrode materials obtained in Examples 1-10 and Comparative Examples 1-5, respectively. The specific preparation methods included: dropping the positive electrode material, acetylene black and polyvinylidene fluoride into N-methyl-2-pyridine alkanone in a mass ratio of 8:1:1 to prepare a solution, and then evenly applying the solution on an aluminum foil, drying and stamping it into a thin sheet; assembling the battery pole piece, single lithium sheet, glass fiber diaphragm, electrolyte (LiClO4) gasket, shrapnel and battery shell into a button-type battery in an argon glove box.

[0141] Table 1 below shows the electrochemical performance test data of button-type batteries prepared using the ternary positive electrode materials obtained in Examples 1-10 and Comparative Examples 1-5, respectively.

[0142] Table 1

[0143]

[0144] It can be seen that the co-doping of gallium and magnesium in the nickel-cobalt-manganese core of the present invention is helpful to improve the electrochemical properties of the ternary positive electrode material, wherein the doping of gallium element can improve the electronic conductivity and lithium ion diffusion of the material, thereby improving the rate performance of the material, and enabling the battery to operate at a higher current density without significantly reducing its performance; the doping of magnesium element helps to stabilize the structure of the material, thereby improving its cycle stability, and at the same time, magnesium ions replace part of the nickel or manganese ions, reducing the lithium-nickel mixing phenomenon.

[0145] In addition, the presence of the magnesium-coated intermediate layer significantly increases the energy barrier for oxygen release in the nickel-cobalt-manganese positive electrode material, helps to stabilize the surface oxygen of the lithium-rich material, thereby reducing the voltage decay during charging and discharging and improving the energy efficiency of the battery; the metal oxide-phosphate co-coated shell has high thermal stability, which improves the performance of the ternary positive electrode material in high temperature environments and reduces the risk of thermal runaway. The co-coated shell further enhances the structural stability of the ternary positive electrode material and reduces the volume expansion and contraction during charging and discharging, thereby extending the cycle life of the battery.

[0146] Furthermore, the co-coated shell acts as a physical barrier, reducing the direct contact between the electrolyte and the ternary positive electrode material, thereby reducing the decomposition rate of the electrolyte and extending the service life of the battery. At the same time, it inhibits the dissolution of transition metals in the ternary positive electrode material during the charge and discharge process, reduces the concentration of metal ions in the electrolyte, thereby slowing down the attenuation of the battery capacity and improving the electrochemical performance of the material.

[0147] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A doped coated ternary positive electrode material, characterized in that: The doped and coated ternary positive electrode material comprises a gallium-magnesium co-doped nickel-cobalt-manganese core, a magnesium-coated intermediate layer, and a metal oxide-phosphate co-coated outer shell; Taking the total mass of the ternary positive electrode material as a calculation basis, the mass proportion of the metal oxide-phosphate co-coated shell is 5-20wt%.

2. The doped coated ternary positive electrode material according to claim 1, characterized in that: The chemical formula of the gallium-magnesium co-doped nickel-cobalt-manganese core is: Li a Ni x Co y Mn z Ga m Mg n O2; wherein, 1≤a≤1.5, 0.6≤x≤0.8, x+y+z≤1, m:n=(1-3):

1.

3. The doped coated ternary positive electrode material according to claim 1 or 2, characterized in that: The average thickness of the magnesium-coated intermediate layer is 0.2-2 μm; Preferably, in the metal oxide-phosphate co-coated shell, the metal oxide comprises any one or a combination of at least two of aluminum oxide, zinc oxide or tin oxide, and more preferably aluminum oxide; Preferably, in the metal oxide-phosphate co-coated shell, the phosphate includes any one or a combination of at least two of lanthanum phosphate, aluminum phosphate or cerium phosphate, and is further preferably lanthanum phosphate; Preferably, in the metal oxide-phosphate co-coated shell, the mass ratio of metal oxide to phosphate is (0.2-2):

1.

4. A method for preparing a doped and coated ternary positive electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) mixing nickel salt, cobalt salt, manganese salt and deionized water to obtain a ternary salt solution; (2) preparing a gallium salt solution, a magnesium salt solution, a precipitant solution and a complexing agent solution respectively; (3) preparing a base liquid in a reaction kettle, then introducing a ternary salt solution, a precipitant solution and a complexing agent solution, controlling the pH of the mixed solution to a first target value, starting a coprecipitation reaction in a protective gas atmosphere, and then introducing a gallium salt solution, while continuing to introduce the ternary salt solution, the precipitant solution and the complexing agent solution, and controlling the pH of the mixed solution to a second target value; when the average particle size D50 of the precursor particles reaches a first set value, starting to gradually reduce the flow rate of the gallium salt solution until the flow rate is 0, and starting to introduce a magnesium salt solution, and gradually increasing the flow rate of the magnesium salt solution from 0; when the average particle size D50 of the precursor particles reaches a second set value, stopping the introduction of the ternary salt solution; when the average particle size D50 of the precursor particles reaches a third set value, stopping the introduction of the magnesium salt solution, the precipitant solution and the complexing agent solution, and obtaining a precursor material after solid-liquid separation; (4) mixing the precursor material and the lithium salt for solid phase sintering to obtain an intermediate material; (5) mixing the intermediate material, the metal oxide and the phosphate, and performing ball milling and heat treatment in sequence to obtain the doped and coated ternary positive electrode material; There is no particular order in which steps (1) and (2) are performed.

5. The preparation method according to claim 4, characterized in that: The nickel salt, cobalt salt and manganese salt in step (1) are any one of sulfate, nitrate or chloride salts of the corresponding metal ions, or a combination of at least two thereof; Preferably, the total concentration of metal ions in the ternary salt solution in step (1) is 0.5-10 mol / L; Preferably, the gallium salt solution in step (2) comprises any one of gallium sulfate solution, gallium nitrate solution or gallium chloride solution, or a combination of at least two thereof; Preferably, the concentration of gallium ions in the gallium salt solution in step (2) is 1500-2500 ppm; Preferably, the magnesium salt solution in step (2) comprises any one of magnesium sulfate solution, magnesium nitrate solution or magnesium chloride solution, or a combination of at least two thereof; Preferably, the concentration of magnesium ions in the magnesium salt solution in step (2) is 800-1200 ppm; Preferably, the precipitant solution in step (2) comprises sodium hydroxide solution and / or sodium carbonate solution; Preferably, the concentration of the precipitant solution in step (2) is 30-40 wt %; Preferably, the complexing agent solution in step (2) comprises aqueous ammonia; Preferably, the concentration of the complexing agent solution in step (2) is 10-20 wt%.

6. The preparation method according to claim 4 or 5, characterized in that: The base solution in step (3) is a mixed solution of a precipitant solution and a complexing agent solution, and the pH value of the base solution is 10-11; Preferably, the flow rate of the ternary salt solution in step (3) is 30-50 L / h; Preferably, the pH of the mixed solution in step (3) is controlled by adjusting the flow rates of the precipitant solution and the complexing agent solution; Preferably, in step (3), the first target value is 9.5-11.5; Preferably, the protective gas in step (3) comprises nitrogen and / or argon; Preferably, the temperature of the coprecipitation reaction in step (3) is 40-65°C; Preferably, the coprecipitation reaction in step (3) is accompanied by stirring, and the stirring rate is 200-400 rpm; Preferably, the flow rate of the gallium salt solution in step (3) is 1-3 L / h; Preferably, in step (3), the second target value is 10.2-10.8; Preferably, in step (3), the first set value is 3-5 μm; Preferably, the gallium salt solution in step (3) is gradually reduced for 0.5-1.5 h; Preferably, the flow rate of the magnesium salt solution in step (3) is 1-3 L / h; Preferably, the gradual increase time of the magnesium salt solution in step (3) is 0.5-1.5h; Preferably, the second set value in step (3) is 8-10 μm; Preferably, the third set value in step (3) is 11-13 μm; Preferably, the solid-liquid separation in step (3) comprises centrifugation, washing and drying performed sequentially.

7. The preparation method according to any one of claims 4 to 6, characterized in that: The lithium salt in step (4) comprises lithium carbonate; Preferably, the solid phase sintering in step (4) is carried out in an air atmosphere; Preferably, the temperature of the solid phase sintering in step (4) is 900-1100° C. Preferably, the solid phase sintering time in step (4) is 20-30 hours.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The metal oxide in step (5) comprises any one of aluminum oxide, zinc oxide or tin oxide, or a combination of at least two thereof, and aluminum oxide is more preferably used; Preferably, the phosphate in step (5) comprises any one or a combination of at least two of lanthanum phosphate, aluminum phosphate or cerium phosphate, and more preferably lanthanum phosphate; Preferably, the heat treatment in step (5) is carried out in an air atmosphere; Preferably, the temperature of the heat treatment in step (5) is 900-1100°C; Preferably, the heat treatment time in step (5) is 8-12 hours.

9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises the following steps: (1) mixing a nickel salt, a cobalt salt, a manganese salt and deionized water to obtain a ternary salt solution with a total metal ion concentration of 0.5-10 mol / L; wherein the nickel salt, the cobalt salt and the manganese salt are any one of sulfate, nitrate or chloride salts of the corresponding metal ions, or a combination of at least two of them; (2) preparing a gallium salt solution, a magnesium salt solution, a precipitant solution and a complexing agent solution respectively; the gallium salt solution comprises any one of a gallium sulfate solution, a gallium nitrate solution or a gallium chloride solution or a combination of at least two thereof, and the concentration of gallium ions is 1500-2500 ppm; the magnesium salt solution comprises any one of a magnesium sulfate solution, a magnesium nitrate solution or a magnesium chloride solution or a combination of at least two thereof, and the concentration of magnesium ions is 800-1200 ppm; the precipitant solution comprises a sodium hydroxide solution and / or a sodium carbonate solution, and the concentration is 30-40 wt%; the complexing agent solution comprises ammonia water with a concentration of 10-20 wt%; (3) Mixing the precipitant solution and the complexing agent solution in a reaction kettle to obtain a base solution with a pH value of 10-11, then introducing the ternary salt solution, the precipitant solution and the complexing agent solution, and controlling the flow rate of the ternary salt solution to 30-50 L / h, adjusting the flow rate of the precipitant solution and the complexing agent solution to control the pH of the mixed solution to 9.5-11.5, starting the coprecipitation reaction at 40-65° C. in a nitrogen and / or argon atmosphere, accompanied by stirring at a rate of 200-400 rpm, and then introducing the gallium salt solution at a flow rate of 1-3 L / h, while continuing to introduce the ternary salt solution, the precipitant solution and the complexing agent solution, and controlling the flow rate of the ternary salt solution to 30-50 L / h. The pH of the mixed solution is 10.2-10.8; when the average particle size D50 of the precursor particles reaches 3-5 μm, the flow rate of the gallium salt solution is gradually reduced within 0.5-1.5 hours until the flow rate is 0, and the magnesium salt solution is introduced at the same time, and the flow rate of the magnesium salt solution is gradually increased from 0 to 1-3 L / h within 0.5-1.5 hours; when the average particle size D50 of the precursor particles reaches 8-10 μm, the introduction of the ternary salt solution is stopped; when the average particle size D50 of the precursor particles reaches 11-13 μm, the introduction of the magnesium salt solution, the precipitant solution and the complexing agent solution is stopped, and the precursor material is obtained after centrifugation, washing and drying; (4) mixing the precursor material and lithium carbonate, and performing solid phase sintering at 900-1100° C. for 20-30 h in an air atmosphere to obtain an intermediate material; (5) mixing the intermediate material, aluminum oxide and lanthanum phosphate for ball milling, and then heat treating at 900-1100° C. for 8-12 h in an air atmosphere to obtain the doped coated ternary cathode material; There is no particular order in which steps (1) and (2) are performed.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the doped and coated ternary positive electrode material as described in any one of claims 1 to 3.