Mixed conductor with continuous ion and electron transmission channel and preparation method and application thereof

The instability of the electrode-electrolyte interface and lithium is solved by using a hybrid conductor composed of a lithium-philic modified titanium nitride nanotube array and a solid electrolyte interface film in a solid lithium metal battery to form a continuous lithium ion and electron transport channel. Dentite growth problems significantly improve the cycle stability and safety performance of the battery.

CN118970046AActive Publication Date: 2024-11-15FUJIAN NORMAL UNIV

Patent Information

Application Number
CN202411025493.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Solid-state lithium metal batteries face problems such as instability of the electrode-electrolyte interface, accumulation of internal stress of lithium and growth of lithium dendrites, resulting in poor battery performance and safety risks.

Method used

A hybrid conductor composed of a lithium-philic modified titanium nitride nanotube array and a solid electrolyte interface film forms a continuous lithium ion and electron transport channel through a titanium nitride nanotube array and a solid electrolyte interface film, promoting uniform deposition and peeling of lithium , adapt to volume changes during charging and discharging, and reduce side reactions.

Benefits of technology

It improves the electrochemical stability and overall conductivity of the electrode material, significantly improves the diffusion and transmission capacity of lithium ions, extends the cycling stability and rate performance of the battery, reduces side reactions, and enhances the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970046A_ABST
    Figure CN118970046A_ABST
Patent Text Reader

Abstract

The invention discloses a mixed conductor with continuous ion and electron transmission channels and a preparation method and application thereof, and belongs to the technical field of solid-state lithium metal batteries. The lithium-philic modified titanium nitride nanotube array and the solid electrolyte interface film are adopted to form a mixed conductor with a continuous ion and electron transmission channel, so that uniform deposition and stripping of lithium in nanotubes through a creep mechanism can be promoted, stress is effectively released, and the electrochemical performance of the battery is improved; the titanium nitride nanotube array not only can improve the overall conductivity of the electrode material, but also can adapt to the volume change of the negative electrode in the charge-discharge cycle; and titanium nitride is stable to lithium, so that side reactions in the cycle process are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid-state lithium metal batteries, and in particular relates to a mixed conductor with continuous ion and electron transmission channels, and a preparation method and application thereof. Background Art

[0002] With the development of electric vehicles and large-scale grid energy storage technology, people's demand for batteries with high energy density, long cycle life and superior safety performance is increasing day by day. However, traditional lithium-ion batteries have serious safety issues such as thermal runaway and flammability, and their energy density cannot meet the requirements of various advanced applications. Lithium metal anodes have extremely high theoretical capacity (3860mAh g -1 , while the theoretical capacity of traditional graphite anode is 372 mAh g -1 ), low electrochemical potential (-3.04 V, compared with the standard hydrogen electrode) and low density (0.53 g·cm -3 ). Solid electrolytes (SE) have excellent safety characteristics and can inhibit the growth of lithium dendrites due to their high mechanical strength, thereby improving the cycle life and stability of the battery. Therefore, solid-state lithium metal batteries are considered to be one of the most promising energy storage devices and have attracted extensive research.

[0003] However, the practical application of solid-state lithium metal batteries is severely hindered by several key challenges, including the instability of the electrode-electrolyte interface, the accumulation of stress inside lithium, and the growth of lithium dendrites. Specifically, during the lithium deposition and stripping process, huge volume changes occur, generating voids at the interface and triggering a sharp increase in polarization with cycles. The electrochemical reactions occurring during the cycle will generate huge stress inside the lithium metal (approximately 1GPa of stress per 135mV of potential), which is then transferred to the SE. This huge stress can cause the SE to break and form a channel for lithium dendrites to penetrate due to the "tip effect", ultimately leading to a battery short circuit.

[0004] In the face of these challenges, researchers have made a lot of efforts and achieved encouraging progress. One effective strategy is to create an artificial solid electrolyte interface (SEI) on the lithium metal anode. For example, porous organic polymers are integrated into polyethylene oxide (PEO)-based SEs to form a lithium fluoride-rich SEI that improves the uniformity of lithium deposition. Although this artificial SEI layer can provide protection, it often fails under the huge volume changes during lithium deposition and stripping. Another promising approach is to use three-dimensional electronic conductors as lithium metal hosts. This approach has several benefits: (1) the three-dimensional structure can buffer the volume changes during lithium plating or stripping, thereby enhancing the structural stability of the anode; (2) the electronic conductor can accelerate electron transport and reduce the polarization phenomenon of the battery. For example, carbon cloth modified with MOF nanorod arrays is used as a lithium metal host, thereby reducing the local current density and enhancing the electrochemical deposition behavior of lithium. However, at high current density, excessive operating current will promote lithium deposition outside the framework, thereby weakening its ability to control lithium deposition. Using ionic conductors as lithium metal hosts is another effective strategy. When lithium ions are deposited in ionic conductors, electron conduction is inhibited, allowing lithium ions to deposit in a "bottom-up" manner. A typical example is the use of a three-dimensional garnet-type ionic conductor framework as a lithium metal host to guide lithium deposition from the bottom, thereby preventing the formation of dendrites. However, the insulating nature of the framework limits electron transport and may lead to "dead lithium". Neither a single electronic conductor nor an ionic conductor can completely solve the challenges posed by solid-state lithium metal batteries. From a kinetic point of view, the rapid transport of lithium ions and electrons is crucial to the performance of solid-state lithium metal batteries.

[0005] Therefore, it is necessary to provide a conductor material with stable structure, good cycle performance, and excellent lithium ion and electron transport properties for solid-state lithium metal batteries. Summary of the invention

[0006] In order to solve the above technical problems, the present invention proposes a mixed conductor with continuous ion and electron transmission channels, a preparation method and application thereof. The mixed conductor with continuous ion and electron transmission channels provided by the present invention has high lithium affinity, excellent lithium ion diffusion and electron transmission capabilities, can improve the deposition and stripping of lithium metal, and has extremely high application value in the field of high-performance solid-state lithium metal batteries.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] The invention provides a mixed conductor with continuous ion and electron transmission channels. The mixed conductor comprises a lithium-philic modified titanium nitride nanotube array and a solid electrolyte interface film deposited on the surface of the lithium-philic modified titanium nitride nanotube array.

[0009] Preferably, the diameter of the titanium nitride nanotubes in the lithium-philic modified titanium nitride nanotube array is 50-200 nm.

[0010] Preferably, the lithiophilic modified lithiophilic material comprises one or more of nanosilver particles, nanogold particles, nanozinc particles and nanosilicon particles.

[0011] Preferably, the chemical composition of the solid electrolyte interface film includes one or more of lithium fluoride, lithium oxide, lithium carbonate, and lithium nitride.

[0012] Preferably, the method for constructing the solid electrolyte interface film is a pre-lithiation method; the pre-lithiation method includes electrochemical deposition or atomic layer deposition.

[0013] Preferably, the solid electrolyte interface film has a thickness of 5-50 nm.

[0014] Preferably, the method for preparing the titanium nitride nanotube array comprises: annealing the titanium dioxide nanotube array in ammonia to obtain the titanium nitride nanotube array.

[0015] Preferably, the annealing temperature is 750-850°C, the annealing time is 0.5-5h, and the rate of heating to the annealing temperature is 1-5°C·min -1 .

[0016] The present invention provides a method for preparing a mixed conductor having continuous ion and electron transmission channels as described in the above technical solution, comprising the following steps:

[0017] (1) performing lithium-philic modification on the titanium nitride nanotube array to obtain a lithium-philic modified titanium nitride nanotube array;

[0018] (2) constructing a solid electrolyte interface film on the surface of the lithium-philic modified titanium nitride nanotube array obtained in step (1) to obtain the mixed conductor with continuous ion and electron transport channels.

[0019] The present invention also provides the use of the mixed conductor with continuous ion and electron transmission channels described in the above technical solution in the preparation of battery electrode materials.

[0020] Compared with the prior art, the present invention has the following advantages and technical effects:

[0021] 1. The present invention adopts a lithium-philic modified titanium nitride nanotube array and a solid electrolyte interface membrane to form a mixed conductor with continuous ion and electron transmission channels, which can promote the uniform deposition and stripping of lithium in the nanotubes through a creep mechanism, and help improve the electrochemical stability of the electrode material; the titanium nitride nanotube array can not only improve the overall conductivity of the electrode material, but also adapt to the volume change of the negative electrode during the charge and discharge cycle; and titanium nitride is stable to lithium, reducing side reactions during the cycle.

[0022] 2. In the mixed conductor with continuous ion and electron transmission channels provided by the present invention, the solid electrolyte interface film SEI with high lithium affinity and high lithium ion diffusion rate forms a continuous lithium ion transmission channel, which significantly improves the diffusion and transmission capacity of lithium ions; the titanium nitride nanotube array with excellent electronic conductivity and SEI jointly form a continuous lithium ion and electron transmission channel, which is beneficial to the uniform deposition and stripping of lithium metal.

[0023] 3. The mixed conductor with continuous ion and electron transmission channels provided by the present invention is applied to solid-state lithium metal electrode materials. The assembled solid-state lithium metal battery exhibits the characteristics of high specific capacity, good rate performance, and strong cycle stability, indicating that the mixed conductor provided by the present invention has important application prospects in the field of high-performance solid-state lithium metal batteries.

[0024] 4. The preparation method of the mixed conductor with continuous ion and electron transport channels provided by the present invention has the advantages of simplicity, high efficiency, easy operation, low cost, etc., and is suitable for further promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0026] Figure 1 This is a SEM image of the titanium nitride nanotube array prepared in Example 1;

[0027] Figure 2 is an X-ray diffraction pattern of the titanium nitride nanotube array prepared in Example 1;

[0028] Figure 3 HRTEM image of the mixed conductor with continuous ion and electron transport channels prepared in Example 1;

[0029] Figure 4 Mapping diagram of the mixed conductor with continuous ion and electron transport channels prepared in Example 1;

[0030] Figure 5 The electrochemical performance diagram of the solid-state lithium metal full battery in Application Example 1;

[0031] Figure 6 Graph showing the electrochemical performance of the solid-state lithium metal half-cells in Application Example 2 and Comparative Application Examples 1-3. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0034] An embodiment of the present invention provides a mixed conductor with continuous ion and electron transmission channels, wherein the mixed conductor comprises a lithium-philic modified titanium nitride nanotube array and a solid electrolyte interface film deposited on the surface of the lithium-philic modified titanium nitride nanotube array.

[0035] The present invention adopts lithium-philic modified titanium nitride nanotube array and solid electrolyte interface film to form a mixed conductor with continuous ion and electron transmission channels, which can promote the uniform deposition and stripping of lithium in the nanotubes through the creep mechanism, and help to improve the electrochemical stability of the electrode material; the titanium nitride nanotube array can not only improve the overall conductivity of the electrode material, but also adapt to the volume change of the negative electrode during the charge and discharge cycle; and titanium nitride is stable to lithium, reducing side reactions during the cycle process.

[0036] In a preferred embodiment, the diameter of the titanium nitride nanotubes in the lithium-philic modified titanium nitride nanotube array is 50-200nm, more preferably 100-200nm. The present invention uses a titanium nitride nanotube array with a diameter in the above range, and the diffusion of lithium metal in the nanotubes is mainly based on Coble creep, which can effectively release stress and promote uniform deposition of lithium. If the diameter of the titanium nitride nanotube is too large, significant dislocation creep will occur, which is a mixed diffusion-displacement mechanism that will cause stress accumulation and endanger the safety performance of the battery.

[0037] In a preferred embodiment, the lithium-affinity modified lithium-affinity material comprises one or more of nanosilver particles, nanogold particles, nanozinc particles and nanosilicon particles. The present invention can improve the lithium affinity of the titanium nitride nanotube array by performing lithium-affinity modification on the titanium nitride nanotube array, thereby promoting uniform lithium deposition and slowing down the growth of lithium dendrites.

[0038] In a preferred embodiment, the method for preparing the titanium nitride nanotube array comprises: annealing the titanium dioxide nanotube array in ammonia to obtain the titanium nitride nanotube array.

[0039] In a preferred embodiment, the preparation method of the titanium dioxide nanotube array includes a template method, a hydrothermal method or an anodic oxidation method, and more preferably an anodic oxidation method; the titanium dioxide nanotube array obtained by the anodic oxidation method has a more uniform size, which is beneficial to improving its electrochemical stability.

[0040] In a preferred embodiment, the annealing temperature is 750-850°C, the annealing time is 0.5-5h, and the rate of heating to the annealing temperature is 1-5°C·min -1 The present invention performs annealing under the above conditions, which is conducive to obtaining a titanium nitride nanotube array that is stable to lithium metal.

[0041] In a preferred embodiment, the chemical composition of the solid electrolyte interface film includes one or more of lithium fluoride, lithium oxide, lithium carbonate, and lithium nitride. The solid electrolyte interface film in the present invention has high lithium affinity and high lithium ion diffusion rate, which improves the deposition and stripping of lithium metal.

[0042] In a preferred embodiment, the construction method of the solid electrolyte interface film is a pre-lithiation method; the pre-lithiation method includes electrochemical deposition or atomic layer deposition; the electrolyte used in the electrochemical deposition method is prepared by an organic solvent, a lithium salt and an additive, the concentration of the lithium salt in the electrolyte is 0.8-1.5 mol / L, and the mass concentration of the additive is 2%; the organic solvent includes one or more of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl ether (DME), and 1,3-dioxolane (DOL); the lithium salt includes one or more of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium perchlorate (LiClO4), and lithium hexafluorophosphate (LiPF6); the additive includes one or more of lithium nitrate (LiNO3), triphenyl phosphate (TPP), and dimethyl methylphosphonate (DMMP).

[0043] In a preferred embodiment, the thickness of the solid electrolyte interface film is 5-50nm. The present invention controls the thickness of the solid electrolyte interface film within the above range, which has the advantages of continuous and rapid transmission of lithium ions. If the solid electrolyte interface film is too thin, its mechanical stability and lithium ion transmission capacity cannot be guaranteed. If the solid electrolyte interface film is too thick, the internal resistance of the battery will be increased, and the charging and discharging efficiency of the battery will be reduced.

[0044] The present invention provides a method for preparing a mixed conductor having continuous ion and electron transmission channels as described in the above technical solution, comprising the following steps:

[0045] (1) performing lithium-philic modification on the titanium nitride nanotube array to obtain a lithium-philic modified titanium nitride nanotube array;

[0046] (2) constructing a solid electrolyte interface film on the surface of the lithium-philic modified titanium nitride nanotube array obtained in step (1) to obtain the mixed conductor with continuous ion and electron transport channels.

[0047] In a preferred embodiment, in step (1), the lithium-philic modification is specifically as follows: using the titanium nitride nanotube array as a cathode, the titanium sheet as an anode, and the lithium-philic material precursor solution as an electrolyte, electrolysis is performed to obtain a pretreated titanium nitride nanotube array; and the pretreated titanium nitride nanotube array is calcined to obtain a lithium-philic modified titanium nitride nanotube array.

[0048] In a preferred embodiment, the solvent of the lithium-philic material precursor solution is water and ethylene glycol; the amount ratio of the lithium-philic material precursor, water and ethylene glycol in the lithium-philic material precursor solution is (2.0-3.6) g:10 mL:240 mL; the lithium-philic material precursor includes silver nitrate, gold chloride or zinc sulfate.

[0049] In a preferred embodiment, the electrolysis current is 15 mA constant current, the electrolysis time is 1 min, and the number of electrolysis is 2 times.

[0050] In a preferred embodiment, the calcination temperature is 400°C, the calcination time is 3 hours, and the rate of heating to the calcination temperature is 2°C·min -1 The calcination atmosphere is nitrogen atmosphere.

[0051] In a preferred embodiment, in step (2), the process parameters for constructing the solid electrolyte interface film include: temperature is room temperature, voltage is 0-1V, current density is 0.01-2mA·cm -1 .

[0052] The present invention also provides the use of the mixed conductor with continuous ion and electron transmission channels described in the above technical solution in the preparation of battery electrode materials.

[0053] The room temperature in the embodiments of the present invention refers to "25±2°C".

[0054] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.

[0055] Example 1

[0056] A mixed conductor with continuous ion and electron transmission channels, consisting of a titanium nitride nanotube array modified by nanosilver particles and a solid electrolyte interface film deposited on the surface of the titanium nitride nanotube array modified by nanosilver particles; the diameter of the titanium nitride nanotubes in the titanium nitride nanotube array modified by nanosilver particles is 100nm, the chemical composition of the solid electrolyte interface film includes lithium fluoride, lithium oxide, lithium carbonate and lithium nitride, and the thickness of the solid electrolyte interface film is 5-50nm.

[0057] The preparation process is:

[0058] (1) Add 2.75 g of ammonium fluoride to 15 mL of deionized water and stir to obtain solution A; add solution A to 500 mL of ethylene glycol and stir to obtain solution B;

[0059] (2) using a 1×7 cm rectangular titanium sheet as the anode and cathode, and using the solution B obtained in step (1) as the electrolyte, electrolyzing at a constant voltage of 60 V for 2 h to form a titanium dioxide nanotube array at the anode;

[0060] (3) The titanium dioxide nanotube array obtained in step (2) was placed in a tube furnace and heated at 5°C min under an ammonia atmosphere. -1 The temperature was raised to 750°C at a rate of 100 °C and annealed for 1 h to obtain a titanium nitride nanotube array;

[0061] (4) dissolving 2.1 g of silver nitrate in 10 mL of deionized water, adding 240 mL of ethylene glycol, and stirring evenly to obtain solution C; using the titanium nitride nanotube array obtained in step (3) as the cathode, the titanium sheet as the anode, and solution C as the electrolyte, electrolyzing at a constant current of 15 mA for 1 min, and then washing the titanium nitride nanotube array with anhydrous ethanol, repeating the above electrolysis process once to obtain a pretreated titanium nitride nanotube array; placing the above pretreated titanium nitride nanotube array in a tube furnace, and heating it at 2 °C min under a nitrogen atmosphere. -1 The temperature was raised at a rate of 1.5 ℃ and maintained at 400℃ for 3 hours to obtain a titanium nitride nanotube array modified with nanosilver particles;

[0062] (5) The titanium nitride nanotube array modified with nanosilver particles obtained in step (4) is used as a working electrode and lithium metal is used as a counter electrode, and electrochemical deposition is performed in an electrolyte prepared by DOL, DME, LiTFSI and LiNO3 (the concentration of LiTFSI in the electrolyte is 1.0 mol / L, the mass concentration of LiNO3 is 2.0%, and the volume ratio of DOL and DME is 1:1) to obtain a mixed conductor with continuous ion and electron transport channels; the process parameters of the electrochemical deposition are: temperature 25°C, voltage 0-1V, current density 0.1 mA cm -1 .

[0063] Figure 1This is a SEM image of the titanium nitride nanotube array prepared in Example 1. Figure 1 It can be seen that the titanium nitride nanotubes in the titanium nitride nanotube array prepared in Example 1 are arranged vertically and have a diameter of about 100 nm.

[0064] Figure 2 This is the X-ray diffraction pattern of the titanium nitride nanotube array prepared in Example 1. Figure 2 It can be seen that the chemical composition of the obtained titanium nitride nanotube array is pure titanium nitride.

[0065] Figure 3 HRTEM image of the mixed conductor with continuous ion and electron transport channels prepared in Example 1. Figure 3 It can be seen that the SEI layer is deposited on the surface of titanium nitride nanotubes.

[0066] Figure 4 This is a mapping diagram of the mixed conductor with continuous ion and electron transport channels prepared in Example 1. Figure 4 It can be seen that C, N, O, F and Ag elements are evenly distributed on the surface of titanium nitride nanotubes.

[0067] Example 2

[0068] A mixed conductor with continuous ion and electron transmission channels, consisting of a titanium nitride nanotube array modified by nanogold particles and a solid electrolyte interface film deposited on the surface of the titanium nitride nanotube array modified by nanogold particles; the diameter of the titanium nitride nanotubes in the titanium nitride nanotube array modified by nanogold particles is 100nm, the chemical composition of the solid electrolyte interface film includes lithium fluoride, lithium oxide, lithium carbonate and lithium nitride, and the thickness of the solid electrolyte interface film is 5-50nm.

[0069] The preparation process is:

[0070] (1) Add 2.5 g of ammonium fluoride to 15 mL of deionized water and stir to obtain solution A; add solution A to 500 mL of ethylene glycol and stir to obtain solution B;

[0071] (2) using a 1×7 cm rectangular titanium sheet as the anode and cathode, and using the solution B obtained in step (1) as the electrolyte, electrolyzing at a constant voltage of 60 V for 2 h to form a titanium dioxide nanotube array at the anode;

[0072] (3) The titanium dioxide nanotube array obtained in step (2) was placed in a tube furnace and heated at 5°C min under an ammonia atmosphere. -1 The temperature was raised to 750°C at a rate of 100 °C and annealed for 1 h to obtain a titanium nitride nanotube array;

[0073] (4) 3.6 g of gold chloride was dissolved in 10 mL of deionized water, and 240 mL of ethylene glycol was added and stirred to obtain solution C; the titanium nitride nanotube array obtained in step (3) was used as the cathode, the titanium sheet was used as the anode, and solution C was used as the electrolyte. After electrolysis at a constant current of 15 mA for 1 min, the titanium nitride nanotube array was cleaned with anhydrous ethanol, and the above electrolysis process was repeated once to obtain a pretreated titanium nitride nanotube array; the pretreated titanium nitride nanotube array was placed in a tube furnace and heated at 2 °C min under a nitrogen atmosphere. -1 The temperature was raised at a rate of 1.5 ℃ and maintained at 400℃ for 3 hours to obtain a titanium nitride nanotube array modified with nano-gold particles;

[0074] (5) The titanium nitride nanotube array modified with the nano-gold particles obtained in step (4) is used as a working electrode and lithium metal is used as a counter electrode, and electrochemical deposition is performed in an electrolyte prepared by DOL, DME, LiTFSI and LiNO3 (the concentration of LiTFSI in the electrolyte is 1.5 mol / L, the mass concentration of LiNO3 is 2.0%, and the volume ratio of DOL and DME is 1:1) to obtain a mixed conductor with continuous ion and electron transport channels; the process parameters of the electrochemical deposition are: temperature 25°C, voltage 0-1V, current density 0.2 mA cm -1 .

[0075] Example 3

[0076] A mixed conductor with continuous ion and electron transmission channels, consisting of a titanium nitride nanotube array modified by nano-zinc particles and a solid electrolyte interface film deposited on the surface of the titanium nitride nanotube array modified by nano-zinc particles; the diameter of the titanium nitride nanotubes in the titanium nitride nanotube array modified by nano-zinc particles is 100nm, the chemical composition of the solid electrolyte interface film includes lithium fluoride, lithium oxide, lithium carbonate and lithium nitride, and the thickness of the solid electrolyte interface film is 5-50nm.

[0077] The preparation process is:

[0078] (1) Add 2.8 g of ammonium fluoride to 15 mL of deionized water and stir to obtain solution A; add solution A to 500 mL of ethylene glycol and stir to obtain solution B;

[0079] (2) using a 1.5×7 cm rectangular titanium sheet as the anode and cathode, and using the solution B obtained in step (1) as the electrolyte, electrolyzing at a constant voltage of 60 V for 2 h to form a titanium dioxide nanotube array at the anode;

[0080] (3) The titanium dioxide nanotube array obtained in step (2) was placed in a tube furnace and heated at 3°C ​​min under an ammonia atmosphere. -1 The temperature was raised to 750°C at a rate of 100 °C and annealed for 1 h to obtain a titanium nitride nanotube array;

[0081] (4) dissolving 2 g of zinc sulfate in 10 mL of deionized water, adding 240 mL of ethylene glycol, and stirring evenly to obtain solution C; using the titanium nitride nanotube array obtained in step (3) as the cathode, the titanium sheet as the anode, and solution C as the electrolyte, electrolyzing at a constant current of 15 mA for 1 min, and then washing the titanium nitride nanotube array with anhydrous ethanol, repeating the above electrolysis process once to obtain a pretreated titanium nitride nanotube array; placing the above pretreated titanium nitride nanotube array in a tube furnace, and heating it at 2 °C min under a nitrogen atmosphere. -1 The temperature was raised at a rate of 1.5 ℃ and maintained at 400℃ for 3 hours to obtain a titanium nitride nanotube array modified with nano-zinc particles;

[0082] (5) The titanium nitride nanotube array modified with the nano-zinc particles obtained in step (4) is used as a working electrode and lithium metal is used as a counter electrode, and electrochemical deposition is performed in an electrolyte prepared by DOL, DME, LiTFSI and LiNO3 (the concentration of LiTFSI in the electrolyte is 0.8 mol / L, the mass concentration of LiNO3 is 2.0%, and the volume ratio of DOL and DME is 1:1) to obtain a mixed conductor with continuous ion and electron transport channels; the process parameters of the electrochemical deposition are: temperature 25°C, voltage 0-1V, current density 0.3 mA cm -1 .

[0083] Comparative Example 1

[0084] The only difference from Example 1 is that step (4) and step (5) are omitted.

[0085] Comparative Example 2

[0086] The only difference from Example 1 is that step (5) is omitted.

[0087] Comparative Example 3

[0088] The only difference from Example 1 is that step (4) is omitted.

[0089] Application Example 1

[0090] A solid-state lithium metal full battery, comprising a working electrode, a counter electrode and a solid electrolyte; the working electrode is the mixed conductor with continuous ion and electron transmission channels in Example 1;

[0091] The preparation method of the solid-state lithium metal full battery comprises the following steps:

[0092] (1) Lithium iron phosphate powder, super P, polyethylene oxide PEO, and lithium bis(trifluoromethanesulfonyl)imide LiTFSI were mixed in acetonitrile in a weight ratio of 6:1:2:1 to obtain lithium iron phosphate slurry, and then the obtained lithium iron phosphate slurry was coated on a carbon-coated aluminum foil and vacuum dried at 70°C for 12 hours to obtain a lithium iron phosphate positive electrode material.

[0093] (2) 686 mg of polyethylene oxide (PEO, Mw≈600,000, purchased from Sigma), 343 mg of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 36 mg of lithium aluminum titanium phosphate (LATP) were added to 15 mL of anhydrous acetonitrile and stirred for 12 h; the resulting solution was then poured into a mold, and a celgard separator was added, and dried at 60 °C for 24 h to obtain a polymer composite electrolyte; the above processes were all carried out in a glove box filled with Ar, and O2 and H2O were less than 0.1 ppm.

[0094] (3) The mixed conductor with continuous ion and electron transport channels in Example 1 is used as the working electrode, the lithium iron phosphate positive electrode material obtained in step (1) is used as the counter electrode, and the polymer composite electrolyte obtained in step (2) is used as the solid electrolyte to assemble into a full battery.

[0095] The electrochemical performance of Application Example 1 was tested at 60°C. The results are shown in Figure 5 . Figure 5 This is the electrochemical performance diagram of the solid-state lithium metal full battery in Application Example 1. Figure 5 It can be seen that when the mixed conductor with continuous ion and electron transport channels in Example 1 is used as the negative electrode and lithium iron phosphate is used as the positive electrode to assemble a full battery, when the charge and discharge performance is tested at a rate of 1C, it can be stably cycled for 300 times and the capacity attenuation rate is 0.2%.

[0096] Application Example 2 and Comparative Examples Application Examples 1-3

[0097] A solid-state lithium metal half-cell, comprising a working electrode, a counter electrode and a solid electrolyte; the working electrode is the mixed conductor in Example 1 or Comparative Examples 1-3;

[0098] The preparation method of the solid-state lithium metal half-cell comprises the following steps:

[0099] (1) 686 mg of polyethylene oxide (PEO, Mw ≈ 600,000, purchased from Sigma), 343 mg of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 36 mg of lithium aluminum titanium phosphate (LATP) were added to 15 mL of anhydrous acetonitrile and stirred for 12 h; the resulting solution was then poured into a mold, and a celgard separator was added, and dried at 60 ° C for 24 h to obtain a polymer composite electrolyte; the above processes were all carried out in a glove box filled with Ar, and O2 and H2O were less than 0.1 ppm.

[0100] (2) The mixed conductor in Example 1 or Comparative Examples 1-3 is used as the working electrode, the lithium metal sheet is used as the counter electrode, and the polymer composite electrolyte obtained in step (1) is used as the solid electrolyte to assemble into a half-cell.

[0101] The electrochemical performance of Application Example 2 and Comparative Example Application Examples 1-3 was tested at 60°C. The results are shown in Figure 6 . Figure 6 The electrochemical performance diagram of the solid-state lithium metal half-cell in Application Example 2 and Comparative Example Application Examples 1-3. Figure 6 It can be seen that at 0.2 mA cm -1 , 0.2mAh·cm -1 Under the cycle conditions, the cycle performance of the half-cell made of the composite material in Example 1 is 450h, the cycle performance of the half-cell made of the composite material in Comparative Example 1 is 100h, the cycle performance of the half-cell made of the composite material in Comparative Example 2 is 185h, and the cycle performance of the half-cell made of the composite material in Comparative Example 3 is 210h.

[0102] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A mixed conductor having continuous ion and electron transport channels, characterized in that: The mixed conductor comprises a lithium-philic modified titanium nitride nanotube array and a solid electrolyte interface film deposited on the surface of the lithium-philic modified titanium nitride nanotube array.

2. The mixed conductor with continuous ion and electron transport channels according to claim 1, characterized in that: The diameter of the titanium nitride nanotubes in the lithium-philic modified titanium nitride nanotube array is 50-200 nm.

3. The mixed conductor with continuous ion and electron transport channels according to claim 1 or 2, characterized in that: The lithium-philic modified lithium-philic material comprises one or more of nano-silver particles, nano-gold particles, nano-zinc particles and nano-silicon particles.

4. The mixed conductor with continuous ion and electron transport channels according to claim 1, characterized in that: The chemical composition of the solid electrolyte interface film includes one or more of lithium fluoride, lithium oxide, lithium carbonate and lithium nitride.

5. The mixed conductor with continuous ion and electron transport channels according to claim 1, characterized in that: The method for constructing the solid electrolyte interface film is a pre-lithiation method; the pre-lithiation method includes electrochemical deposition or atomic layer deposition.

6. The mixed conductor with continuous ion and electron transport channels according to claim 1, characterized in that: The thickness of the solid electrolyte interface film is 5-50 nm.

7. The mixed conductor with continuous ion and electron transport channels according to claim 1, characterized in that: The preparation method of the titanium nitride nanotube array comprises: annealing the titanium dioxide nanotube array in ammonia to obtain the titanium nitride nanotube array.

8. The mixed conductor with continuous ion and electron transport channels according to claim 7, characterized in that: The annealing temperature is 750-850°C, the annealing time is 0.5-5h, and the rate of heating to the annealing temperature is 1-5°C·min -1 .

9. The method for preparing a mixed conductor having continuous ion and electron transport channels according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) performing lithium-philic modification on the titanium nitride nanotube array to obtain a lithium-philic modified titanium nitride nanotube array; (2) constructing a solid electrolyte interface film on the surface of the lithium-philic modified titanium nitride nanotube array obtained in step (1) to obtain the mixed conductor with continuous ion and electron transport channels.

10. Use of the mixed conductor having continuous ion and electron transport channels according to any one of claims 1 to 8 in preparing battery electrode materials.

Citation Information

Patent Citations

  • Oxygen electrode of lithium air battery as well as preparation method and application thereof

    CN102034985A

  • Lithium intercalation manganese dioxide-titanium nitride nanotube composite material and preparing method and application thereof

    CN103985563A

  • Method for inhibiting lithium dendrites by constructing polymer electrolyte film with flaky nano molybdenum carbide filler

    CN114824464A

  • Surface-stabilized and prelithiated anode active materials for lithium batteries and production method

    US20190088930A1

Cited By

  • Directional double-layer structure mixed ion / electron conductor intermediate layer and preparation method and application thereof

    CN121460586A

  • Artificial solid electrolyte interface layer and preparation method thereof

    CN122118061A