Pole piece, preparation method thereof and secondary battery

By introducing a transition coating of polyurethane adhesive into the electrode sheet, the problems of excessive adhesive usage and poor electrode flexibility in dry electrode preparation are solved, and the tensile strength and peel strength of the electrode sheet are improved, thereby reducing the tensile strength and peel strength of the electrode sheet. Resistors are used to optimize the cycle performance of the battery.

CN118970061APending Publication Date: 2024-11-15XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411028004.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the preparation process of existing dry electrodes, due to the large particle size of binders such as PTEF, the peel strength is poor, and the interface impedance between active substances and foils is large, resulting in the internal impedance of the battery. The tensile strength and flexibility are poor after the electrode thickness increases. It is prone to fragmentation problems.

Method used

The polyurethane adhesive is introduced into the electrode sheet to form a transition coating between the material layer and the current collector with the first conductive agent, reduce the use of polymer adhesive, increase the overall conductive agent content, and improve stretching Strength and peel strength.

Benefits of technology

Through the transition coating of polyurethane adhesive, the electrode sheet diaphragm resistance is reduced, the peel strength and tensile strength are improved, and the problems of excessive adhesive usage and poor electrode flexibility in dry electrode preparation are solved, and the battery is optimized cyclic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970061A_ABST
    Figure CN118970061A_ABST
Patent Text Reader

Abstract

The invention provides a pole piece and a preparation method thereof, and a secondary battery, the pole piece comprises a composite current collector and a material layer, the composite current collector comprises a current collector and a transition coating arranged on at least one surface of the current collector, the transition coating comprises a first binder and a first conductive agent, and the first binder and the first conductive agent are arranged on the surface of the material layer. The first binding agent comprises a polyurethane type binding agent; and the material layer is arranged on the surface of one side, deviating from the current collector, of the transition coating, and the material of the material layer comprises an active substance, a second binder and a second conductive agent. According to the pole piece disclosed by the invention, the polyurethane type binder is introduced, so that the polyurethane type binder and the first conductive agent form the transition coating between the material layer and the current collector, the usage amount of the polymer binder is reduced, the content ratio of the whole conductive agent in the pole piece is increased, further the resistance of a pole piece diaphragm can be reduced, and the tensile strength and the peel strength of the pole piece can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a pole piece and a preparation method thereof, and a secondary battery. Background Art

[0002] High energy density batteries are an urgent need in today's electric vehicle industry. The most effective and direct way to improve the battery is to increase the thickness of the electrode sheet. At present, the mainstream production technology for manufacturing thick electrodes is the wet process. This method consumes a lot of solvents and wastes energy during the production process; the subsequent solvent baking process will greatly increase the production cost and cause environmental pollution; when the thick electrode is wet-coated, the electrode sheet will have problems such as cracks, delamination and poor flexibility, which limits the thickness of the electrode. Compared with the wet coating technology, the dry electrode does not add any solvents in the process, which can greatly reduce costs; no baking is required and no toxic gases harmful to the environment are generated; dry film technology can control the uniformity of thick electrodes without cracks. The research on dry electrode technology has a very large role in promoting the development of the lithium battery industry.

[0003] Existing sodium ion dry-process electrodes mainly mix PTFE (polytetrafluoroethylene) and other binders, active materials and conductive agents at high speed under low temperature environment. The mixture relies on airflow or high-speed shear force to make PTFE and other micelles into silk. During the silk-making process, the electrode material and the conductive agent are trapped at the same time to form a sticky material similar to marshmallows. After hot pressing, the PTFE and other fibers in the sticky micelles are glued and crystallized to form a stable self-supporting thick film. The membrane and the current collector are hot-pressed and compounded to obtain the electrode pole piece.

[0004] However, there are still some problems in the dry electrode preparation process: due to the large particle size of binders such as PTEF, the adhesion effect is weakened, resulting in poor peel strength and easy powder loss after multiple cycles; the interface impedance between the active material and the foil is large, which leads to a larger impedance inside the battery; the thicker the electrode, the worse the tensile strength and flexibility of the electrode, which will cause problems such as breakage during the subsequent battery forming process. Summary of the invention

[0005] In view of this, one object of the present application is to provide a pole piece, introducing a polyurethane type adhesive into the pole piece so that it forms a transition coating with the first conductive agent between the material layer and the current collector, thereby reducing the amount of polymer adhesive used and increasing the overall conductive agent content ratio in the pole piece, thereby reducing the pole piece diaphragm resistance and improving the tensile strength and peel strength of the pole piece.

[0006] Another object of the present application is to provide a method for preparing a pole piece.

[0007] Another object of the present application is to provide a secondary battery.

[0008] To achieve the above objectives, the first aspect of the present application proposes a pole piece, comprising:

[0009] A composite current collector, the composite current collector comprising a current collector and a transition coating disposed on at least one surface of the current collector, the material of the transition coating comprising a first binder and a first conductive agent, the first binder comprising a polyurethane binder;

[0010] A material layer is provided on a surface of the transition coating layer facing away from the current collector, and the material of the material layer includes an active material, a second binder and a second conductive agent.

[0011] In some embodiments, the active material is a positive electrode active material of a secondary battery or a negative electrode active material of a secondary battery, preferably a positive electrode active material of a sodium ion battery.

[0012] In some embodiments, the current collector is a positive electrode current collector or a negative electrode current collector of a secondary battery, preferably a positive electrode current collector of a sodium ion battery.

[0013] In some embodiments, the polyurethane binder includes at least one high molecular weight polymer containing -NHCOO- on the main chain.

[0014] In some embodiments, the mass content of the polyurethane binder and the first conductive agent in the material of the transition coating is 40-60%.

[0015] In some embodiments, the second binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, nitrile rubber, sodium hydroxymethyl cellulose, polyacrylic acid, polyacrylonitrile, and sodium alginate.

[0016] In some embodiments, the mass content of the active substance in the material of the material layer is 90-98%.

[0017] In some embodiments, the mass content of the second binder in the material of the material layer is 1-5%.

[0018] In some embodiments, the mass content of the second conductive agent in the material of the material layer is 0.5-5%.

[0019] In some embodiments, the second conductive agent and the first conductive agent both include at least one of carbon black, graphene, carbon fiber, silicon, silicon oxide, and carbon nanotubes.

[0020] In some embodiments, the pole piece satisfies at least one of the following characteristics:

[0021] (1) The thickness of the transition coating is 4-6 μm;

[0022] (2) The thickness of the material layer is 100-400 μm;

[0023] (3) The thickness of the pole piece is 100-400 μm;

[0024] (4) The resistance of the electrode is 235-275 mΩ;

[0025] (5) The longitudinal tensile strength of the pole piece is 1.45-2.0 MPa, and / or the transverse tensile strength of the pole piece is 0.25-0.55 MPa

[0026] (6) The peel strength of the electrode is 48-60N / m.

[0027] The second aspect of the present application provides a method for preparing a pole piece, comprising:

[0028] Using the first conductive agent and the first binder as raw materials, forming the transition coating on the current collector to obtain the composite current collector;

[0029] The second binder and the second conductive agent are mixed to obtain a first mixed powder, and then the first mixed powder and the active material are sheared at a high speed to obtain a fiberized second mixed powder;

[0030] Extruding the fiberized second mixed powder at least once, and then rolling to obtain the material layer;

[0031] The material layer is hot-pressed and laminated on the surface of the transition coating layer that is away from the current collector to obtain the pole piece.

[0032] In some embodiments, the step of forming the transition coating on the current collector using the first conductive agent and the first binder as raw materials includes:

[0033] Mixing the first conductive agent, the first binder and a non-aqueous organic solvent to obtain a slurry;

[0034] The slurry is coated on at least one surface of the current collector and then dried to obtain the transition coating.

[0035] In some embodiments, the rotation speed of the high-speed shearing is 1000-4000 rpm, the temperature of the high-speed shearing is 40-100° C., and the time of the high-speed shearing is 0.5-1 h.

[0036] In some embodiments, the extrusion molding temperature is 40-200° C., and the extrusion molding speed is 5-50 mm / s.

[0037] In some embodiments, the temperature of the roller pressing is 25-100° C., and the speed of the roller pressing is 10-50 mm / s.

[0038] In some embodiments, the temperature of the hot pressing composite is 100-250° C., and the rotation speed of the hot pressing composite is 5-26 mm / s.

[0039] In some embodiments, the roll gap of the hot pressing composite is 0.1-2 mm.

[0040] In some embodiments, the extrusion molding obtains a dry powder tablet, and the thickness of the dry powder tablet is 500-800 μm.

[0041] The third aspect of the present application provides a secondary battery, comprising a positive electrode, a negative electrode and a separator, wherein the positive electrode or the negative electrode is the electrode sheet described in the present application or the electrode sheet prepared by the method for preparing the electrode sheet described in the present application.

[0042] The pole piece of the present application can at least bring the following beneficial effects:

[0043] The introduction of polyurethane binder into the pole piece allows it to form a transition coating with the first conductive agent between the material layer and the current collector, reducing the amount of polymer binder (i.e., the second binder) used in the formula, thereby increasing the proportion of the overall conductive agent in the pole piece, and further reducing the pole piece film resistance. At the same time, the transition coating containing polyurethane binder can also improve the tensile strength and peel strength of the pole piece.

[0044] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings.

[0046] in:

[0047] Figure 1 This is a schematic diagram of the structure of a pole piece shown in an exemplary embodiment of the present application.

[0048] Figure 2 The present invention is a flowchart of a method for preparing a pole piece according to an exemplary embodiment of the present application.

[0049] Figure 3 This is a schematic diagram of the structure of the pole piece of comparative example 1.

[0050] Figure 4 0.33C charge and discharge curves of the sodium ion batteries corresponding to the pole pieces of Example 1 and Comparative Example 1.

[0051] Figure 5 The 0.33C charge-discharge cycle performance curves of the sodium ion batteries corresponding to the pole pieces of Examples 1-4 and Comparative Examples 1-2 are shown.

[0052] Reference numerals:

[0053] 1-current collector; 2-transition coating; 3-material layer. DETAILED DESCRIPTION

[0054] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, but cannot be understood as limiting the present application.

[0055] In this application, the disclosure of numerical ranges includes all values ​​within the entire range and the disclosure of further subdivided ranges, including the endpoints and sub-ranges given in these ranges.

[0056] In this application, the raw materials, equipment, etc. involved, unless otherwise specified, are all raw materials and equipment that can be made through commercial channels or known methods; the methods involved, unless otherwise specified, are all conventional methods.

[0057] A pole piece and a method for preparing the pole piece according to an embodiment of the present application will be described below with reference to the accompanying drawings.

[0058] <Pole piece>

[0059] Figure 1 This is a schematic diagram of the structure of a pole piece shown in an exemplary embodiment of the present application.

[0060] like Figure 1 As shown, the pole piece of the embodiment of the present application includes a composite current collector and a material layer 3. Among them,

[0061] The composite current collector comprises a current collector 1 and a transition coating 2 arranged on at least one surface of the current collector 1. The material of the transition coating 2 comprises a first binder and a first conductive agent. The first binder comprises a polyurethane binder.

[0062] The material layer 3 is disposed on the surface of the transition coating layer 2 which faces away from the current collector 1 . The material of the material layer 3 includes an active material, a second binder and a second conductive agent.

[0063] In some embodiments, the current collector is a positive electrode current collector or a negative electrode current collector of a secondary battery.

[0064] Exemplarily, secondary batteries include, but are not limited to, sodium ion batteries, lithium ion batteries, potassium ion batteries, and the like.

[0065] In some embodiments, when the current collector is a positive electrode current collector of a secondary battery, the current collector includes but is not limited to at least one of aluminum foil, carbon-coated aluminum foil, copper foil, aluminum foil, nickel foil, iron foil, and the like.

[0066] In other embodiments, when the current collector is a negative electrode current collector of a secondary battery, the current collector includes but is not limited to at least one of copper foil, carbon-coated aluminum foil, aluminum foil, nickel foil, iron foil, and the like.

[0067] As a preferred example, the current collector is a positive electrode current collector of a sodium ion battery, and the current collector includes but is not limited to at least one of aluminum foil, carbon-coated aluminum foil, and the like.

[0068] It can be understood that, in the embodiments of the present application, the transition coating 2 can be provided on one surface of the current collector 1 , or on multiple (more than 2) surfaces of the current collector 1 .

[0069] As an optional example, the transition coating 2 is provided on two opposite surfaces of the current collector 1 (eg Figure 1 shown).

[0070] In some embodiments, the polyurethane binder includes at least one high molecular weight polymer containing -NHCOO- (urethane group) on the main chain.

[0071] Exemplarily, the polymer containing -NHCOO- on the main chain includes a polymer having a structure of Formula 1:

[0072]

[0073] Illustratively, in Formula 1, n is an integer of 1-100, including but not limited to 1, 10, 20, 30, 40, 50, 60, 70, 80 or 90, etc.

[0074] In some embodiments, the polymer having the structure of Formula 1 includes, but is not limited to, at least one of a monomeric polyisocyanate, a blocked polyisocyanate, and a prepolymerized polyisocyanate.

[0075] As a preferred example, the polymer having the structure of Formula 1 includes but is not limited to at least one of diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), and the like.

[0076] In some embodiments, the mass content of the polyurethane type binder and the first conductive agent in the material of the transition coating 2 is 40-60%, including but not limited to 40%, 45%, 50%, 55% or 60%. The mass content of the polyurethane type binder in the material of the transition coating is within the above range, which can improve the processing performance of the pole piece to the maximum extent; if it is less than 40%, it will affect the peeling and tensile strength of the pole piece; if it is higher than 60%, it will affect the uniformity and stability of the transition coating on the current collector.

[0077] In some embodiments, the first conductive agent includes, but is not limited to, at least one of carbon black (eg, SP), graphene, carbon fiber, silicon, carbon nanotubes, silicon dioxide, and the like.

[0078] In some embodiments, the active material is a positive electrode active material of a secondary battery or a negative electrode active material of a secondary battery.

[0079] As a non-limiting example, when the secondary battery is a sodium ion battery, the positive electrode active material of the sodium ion battery includes but is not limited to at least one of a polyanion compound, a layered oxide, a Prussian material, etc. Exemplarily, the polyanion compound includes but is not limited to at least one of a phosphate, a sulfate, a silicate, a mixed polyanion compound, etc.; the layered oxide includes a molecular formula of Na x M y O 2 At least one of the compounds (0.6≤x≤1, y=1, M includes at least one of Fe, Mn, Ni, Ti, Co, etc.), such as sodium nickel iron manganate active materials, etc.; Prussian materials include but are not limited to Prussian blue (Fe 4 [Fe(CN) 6 ] 3 ), Na 1.89 Mn[Fe(CN) 6 ] 0.97 、Na 1.85 Co[Fe(CN) 6 ] 0.99 1.9H 2 At least one of O, etc.

[0080] As a non-limiting example, when the secondary battery is a lithium-ion battery, the positive electrode active material of the lithium-ion battery includes but is not limited to at least one of lithium cobalt oxide, lithium iron phosphate, lithium manganese oxide, ternary materials lithium nickel cobalt manganese oxide (NCM) and lithium nickel cobalt aluminum oxide (NCA).

[0081] As a non-limiting example, when the secondary battery is a sodium ion battery, the negative electrode active material of the sodium ion battery includes but is not limited to at least one of hard carbon, soft carbon, graphite, and the like.

[0082] As a non-limiting example, when the secondary battery is a lithium-ion battery, the negative electrode active material of the lithium-ion battery includes but is not limited to at least one of graphite, silicon-based negative electrode materials, and the like.

[0083] As a preferred example, the active material is a positive electrode active material of a sodium ion battery.

[0084] In some embodiments, the second binder includes but is not limited to at least one of polyvinylidene fluoride, polytetrafluoroethylene (PTFE), styrene-butadiene rubber, nitrile rubber, sodium hydroxymethyl cellulose, polyacrylic acid, polyacrylonitrile, sodium alginate, and the like.

[0085] In some embodiments, the mass content of the active substance in the material layer 3 is 90-98%, including but not limited to 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97% or 98%, etc.

[0086] In some embodiments, the mass content of the second binder in the material of the material layer 3 is 1-5%, including but not limited to 1%, 2%, 3%, 4% or 5%, etc.

[0087] In some embodiments, the mass content of the second conductive agent in the material of the material layer 3 is 0.5-5%, including but not limited to 0.5%, 1%, 2%, 3%, 4% or 5%.

[0088] In some embodiments, the second conductive agent includes, but is not limited to, at least one of carbon black (eg, SP), graphene, carbon fiber, carbon nanotube, silicon, silicon oxide, and the like.

[0089] In some embodiments, the pole piece satisfies at least one of the following characteristics:

[0090] (1) The thickness of the transition coating 2 is 4-6 μm;

[0091] (2) The thickness of the material layer is 100-400 μm;

[0092] (3) The thickness of the pole piece is 100-400 μm;

[0093] (4) The resistance of the electrode is 235-275mΩ;

[0094] (5) The longitudinal tensile strength of the pole piece is 1.45-2.0Mpa, and / or the transverse tensile strength of the pole piece is 0.25-0.55Mpa

[0095] (6) The peel strength of the electrode is 48-60N / m.

[0096] Exemplarily, the thickness of the transition coating 2 includes but is not limited to 4 μm, 4.5 μm, 5 μm, 5.5 μm or 6 μm, etc. When the thickness of the transition coating 2 is within the above range, the processing performance of the pole piece can be improved without affecting the energy density of the battery; when the thickness is greater than 6 μm, the pole piece will affect the energy density of the battery.

[0097] Exemplarily, the thickness of the material layer 3 includes but is not limited to 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm or 400 μm.

[0098] Exemplarily, the thickness of the pole piece includes but is not limited to 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm or 400 μm, etc.

[0099] Exemplarily, the resistance of the electrode piece includes but is not limited to 240 mΩ, 250 mΩ, 260 mΩ or 270 mΩ, etc.

[0100] Exemplarily, the longitudinal tensile strength (MD) of the pole piece includes but is not limited to 1.50 MPa, 1.6 MPa, 1.7 MPa, 1.8 MPa, 1.9 MPa or 2.0 MPa, etc.

[0101] Exemplarily, the transverse tensile strength (TD) of the pole piece includes but is not limited to 0.3 MPa, 0.35 MPa, 0.4 MPa, 0.45 MPa, 0.5 MPa or 0.55 MPa, etc.

[0102] Exemplarily, the peel strength of the pole piece includes but is not limited to 50 N / m, 52 N / m, 55 N / m or 57 N / m, etc.

[0103] As a preferred example, the above-mentioned electrode sheet is a positive electrode sheet of a sodium ion battery, and more preferably a dry thick electrode sheet.

[0104] The pole piece of the embodiment of the present application introduces a polyurethane type binder into the pole piece, so that it forms a transition coating with the first conductive agent between the material layer and the current collector, reducing the amount of the polymer binder (i.e., the second binder) used in the formula, thereby increasing the content ratio of the overall conductive agent in the pole piece, thereby reducing the pole piece film resistance. At the same time, the presence of the transition coating can improve the tensile strength and peel strength of the pole piece.

[0105] <Method for preparing pole piece>

[0106] The method for preparing the pole piece of the embodiment of the present application can be used for preparing the pole piece of the embodiment of the present application.

[0107] Figure 2 The present invention is a flowchart of a method for preparing a pole piece according to an exemplary embodiment of the present application.

[0108] like Figure 2 As shown, the method for preparing the pole piece comprises the following steps:

[0109] S101, forming a transition coating on a current collector using a first conductive agent and a first binder as raw materials to obtain a composite current collector.

[0110] In some embodiments, forming a transition coating on a current collector using a first conductive agent and a first binder as raw materials includes:

[0111] Mixing the first conductive agent, the first binder and the non-aqueous organic solvent to obtain a slurry;

[0112] The slurry is coated on at least one surface of a current collector and then dried to obtain a transition coating.

[0113] In some embodiments, the non-aqueous organic solvent includes, but is not limited to, at least one of aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, lipids, and ketones.

[0114] Exemplarily, the non-aqueous organic solvent includes, but is not limited to, at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), propylene carbonate (PC), ethylene carbonate (EC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), methyl isopropyl carbonate (MiPC), 1,4-butyrolactone (GBL), dimethyltetrahydrofuran (2Me-THF), tetrahydrofuran (THF), butylene carbonate (BC), 1,2-dimethoxyethane (DME), dibutyl carbonate (DBC), methyl butyl carbonate (BMC), dipropyl carbonate (DPC), methyl ester (PA), ethyl acetate (MA), methyl formate (MF), methyl propionate (MP), etc.

[0115] As a preferred example, the non-aqueous organic solvent is carbonate.

[0116] S102, mixing a second binder and a second conductive agent to obtain a first mixed powder, and then shearing the first mixed powder with an active material at a high speed to obtain a fiberized second mixed powder.

[0117] In some embodiments, the mixing method of the first mixed powder obtained by mixing the second binder and the second conductive agent includes at least one of stirring mixing, high-speed mixing, etc.

[0118] In some embodiments, the rotation speed of high-speed shearing is 1000-4000 rpm, including but not limited to 1000 rpm, 1500 rpm, 2000 rpm, 2500 rpm, 3000 rpm, 3500 rpm or 4000 rpm.

[0119] In some embodiments, the high-speed shearing temperature is 40-100°C, including but not limited to 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C.

[0120] In some embodiments, the high-speed shearing time is 0.5-1 h, including but not limited to 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h or 1 h, etc.

[0121] S103, subjecting the fiberized second mixed powder obtained in step S102 to at least one extrusion molding, and then rolling to obtain a material layer.

[0122] It can be understood that in the embodiments of the present application, the fiberized second mixed powder obtained in step S102 can be extruded once or multiple times (more than 2 times) and can be reused (reuse here means that if the thickness does not meet the requirements, it can be refolded to become thicker and then pressed thinner).

[0123] In some embodiments, the extrusion molding temperature is 40-200°C, including but not limited to 50°C, 75°C, 100°C, 125°C, 150°C, 175°C or 200°C, etc.

[0124] In some embodiments, the extrusion speed is 5-50 mm / s, including but not limited to 10 mm / s, 20 mm / s, 30 mm / s, 40 mm / s or 50 mm / s.

[0125] In some embodiments, the fiberized second mixed powder obtained in step S102 is extruded at least once to obtain a dry powder sheet, and the thickness of the dry powder sheet is 500-800 μm, including but not limited to 550 μm, 600 μm, 650 μm, 700 μm or 750 μm.

[0126] In some embodiments, the temperature of the roller pressing is 25-100°C, including but not limited to 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, etc.

[0127] As a preferred example, the temperature of the roller pressing is 25-60°C.

[0128] In some embodiments, the rolling speed is 10-50 mm / s, including but not limited to 10 mm / s, 20 mm / s, 30 mm / s, 40 mm / s or 50 mm / s.

[0129] In the embodiments of the present application, the purpose of rolling is to reduce the thickness of the dry powder sheet (ie, to reduce the thickness).

[0130] S104, hot-pressing and compounding the material layer on the surface of the transition coating layer facing away from the current collector to obtain a pole piece.

[0131] In some embodiments, the temperature of hot pressing and laminating is 100-250°C, including but not limited to 110°C, 125°C, 150°C, 175°C, 200°C, 225°C or 250°C.

[0132] In some embodiments, the rotation speed of the hot pressing compound is 5-26 mm / s, including but not limited to 7 mm / s, 10 mm / s, 15 mm / s, 20 mm / s or 25 mm / s.

[0133] In some embodiments, the roll gap of the hot pressing composite is 0.1-2 mm, including but not limited to 0.2 mm, 0.5 mm, 0.8 mm, 1 mm, 1.3 mm, 1.5 mm or 1.8 mm, etc.

[0134] The method for preparing the pole piece of the embodiment of the present application belongs to the method for preparing the pole piece by dry process (for example, when the pole piece is the positive pole piece of a sodium ion battery, the method for preparing the pole piece of the embodiment of the application is the method for preparing the positive pole piece of a dry process sodium ion battery). The preparation method includes the preparation of a composite current collector, stirring and mixing of materials, fiberization and mixing of dry powders, thinning of the membrane and hot pressing compounding in sequence. The materials after high-speed mixing and stirring or air flow milling will have very good dispersibility: the materials are squeezed and stretched between the rotors to promote the fiberization of the second binder such as PTFE, and then rolled to the desired thickness by a cold roller. The cold pressing can well cool and shape the membrane. At the same time, the preparation method does not require the addition of any organic solvents, will not have the emission of toxic gases, and does not require a coating oven, which simplifies the process equipment, while also reducing the space used for plant construction and avoiding the process problems caused by slurry coating. In addition, in the preparation process, a transition coating containing a polyurethane binder is provided between the active material and the current collector, which can greatly improve the peel strength and tensile strength of the dry electrode pole piece. At the same time, since the addition of the polyurethane binder can enhance the bonding properties of the second binder such as PTFE, the content of the second binder such as PTFE can be reduced and the content of the conductive agent can be increased during the preparation of the dry electrode. This helps to reduce the diaphragm resistance of the pole piece and optimize the problem of poor rate performance caused by the dry electrode.

[0135] <Secondary Battery>

[0136] The secondary battery of the embodiment of the present application comprises a positive electrode, a negative electrode and a separator, wherein the positive electrode or the negative electrode is a pole piece of the embodiment of the present application, or is a pole piece prepared by the method for preparing a pole piece of the embodiment of the present application.

[0137] In some embodiments, the secondary battery includes but is not limited to a sodium ion battery, a lithium ion battery, a potassium ion battery, and the like.

[0138] In some embodiments, in the above-mentioned secondary battery, the positive electrode is the electrode of the embodiment of the present application, or is the electrode prepared by the preparation method of the electrode of the embodiment of the present application.

[0139] As a preferred example, the secondary battery is a sodium ion battery, and the positive electrode is the electrode of the embodiment of the present application, or is a electrode prepared by the method for preparing the electrode of the embodiment of the present application.

[0140] Certain features of the present technology are further illustrated in the following non-limiting examples.

[0141] 1. Examples and Comparative Examples

[0142] Example 1

[0143] <Pole piece>

[0144] like Figure 1 As shown, the pole piece of this embodiment includes a composite current collector and a material layer 3. Among them,

[0145] The composite current collector includes a current collector 1 and a transition coating 2 disposed on two opposite surfaces of the current collector 1. The material of the transition coating 2 includes a first binder and a first conductive agent. The first binder is a polyurethane-type binder diphenylmethane diisocyanate (MDI), and the first conductive agent is conductive carbon black (SP). The mass content of the polyurethane-type binder and the first conductive agent in the material of the transition coating 2 is 50%. The current collector 1 is an aluminum foil with a thickness of 10 μm. The thickness of the transition coating 2 on the two opposite surfaces of the current collector 1 is 5 μm. The total thickness of the composite current collector is 20 μm.

[0146] The material layer 3 is arranged on the surface of the transition coating 2 away from the current collector 1, and the material of the material layer 3 includes an active material, a second binder and a second conductive agent. Among them, the active material is sodium nickel iron manganese oxide, the second binder is a solid binder PTFE (polytetrafluoroethylene), and the second conductive agent is conductive carbon black (SP); the mass content of the active material in the material layer 3 is 96%, the mass content of the second binder in the material layer 3 is 2%, and the mass content of the second conductive agent in the material layer 3 is 2%. The thickness of the material layer 3 is 100 μm.

[0147] The thickness of the pole piece is 220 μm.

[0148] <Method for preparing pole piece>

[0149] The method for preparing the pole piece of this embodiment comprises the following steps:

[0150] (1) A first conductive agent, a polyurethane binder and N-methylpyrrolidone (NMP) were mixed in a weight percentage of 35%, 35% and 30% to obtain a slurry, and then the dispersed slurry was coated on two opposite surfaces of the current collector and dried to obtain a composite current collector with a thickness of 20 μm and a transition coating.

[0151] (2) The second conductive agent accounting for 4% of the total mass of the material layer and PTFE (solid binder) are placed in a stirring tank in a mass ratio of 1:1 and mixed and stirred at a speed of 200 rpm for 1 hour. The temperature is controlled at 25°C to obtain a uniformly mixed dry powder; the sodium nickel iron manganese oxide active substance accounting for 96% of the mass percentage of the material layer and the uniformly mixed dry powder are added to a high-speed stirring mixer, the stirring temperature is controlled at 50°C, the stirring speed is adjusted to 3000 r / min, and the stirring is carried out for 0.8 hours. The high-speed shear force generated by the high-speed stirring evenly disperses the active substance, the second conductive agent, and the second binder to achieve a fiberization effect, and a fiberized powder is obtained.

[0152] (3) The fibrous powder obtained in step (2) is extruded in a screw extruder at a speed of 20 mm / s and a temperature of 70°C to obtain a film (i.e., dry powder film) with a thickness of 600 μm; the obtained film is sent to a roller press for thinning, the rolling temperature is 25°C, the rolling speed is 15 mm / s, and the gap between the rollers is adjusted by 0.1 mm each time during the thinning process. After six times of rolling, a material layer (i.e., a dry electrode film) with a thickness of 100 μm is obtained; finally, the material layer and the composite current collector obtained in step (1) are hot-rolled and double-sidedly compounded at 150°C, a rotation speed of 15 mm / s, and a roll gap of 0.1 mm to obtain a sodium ion dry positive electrode sheet.

[0153] Example 2

[0154] This embodiment is basically the same as Embodiment 1, except that:

[0155] In the pole piece:

[0156] The mass content of the second binder PTFE (solid binder) in the material layer 3 is 1.6%, and the mass content of the second conductive agent conductive carbon black (SP) in the material layer 3 is 2.4%.

[0157] In the preparation method of the pole piece:

[0158] In step (2), the second conductive agent accounting for 4% of the total mass of the material layer and PTFE (solid binder) are placed in a stirring tank in a mass ratio of 3:2 and mixed and stirred at a speed of 200 rpm for 1 hour. The temperature is controlled at 25°C to obtain a uniformly mixed dry powder.

[0159] Example 3

[0160] This embodiment is basically the same as Embodiment 1, except that:

[0161] In the pole piece:

[0162] The mass content of the second binder PTFE (solid binder) in the material layer 3 is 1.33%, and the mass content of the second conductive agent conductive carbon black (SP) in the material layer 3 is 2.67%.

[0163] In the preparation method of the pole piece:

[0164] In step (2), the second conductive agent accounting for 4% of the total mass of the material layer and PTFE (solid binder) are placed in a stirring tank in a mass ratio of 2:1 and mixed and stirred at a speed of 200 rpm for 1 hour. The temperature is controlled at 25°C to obtain a uniformly mixed dry powder.

[0165] Example 4 (Content of polyurethane type binder in transition coating is close to the upper limit)

[0166] This embodiment is basically the same as Embodiment 1, except that:

[0167] In the pole piece:

[0168] The mass content of the polyurethane type adhesive in the material of the transition coating 2 is 57.14%, and the mass content of the first conductive agent in the material of the transition coating 2 is 42.86%.

[0169] In the preparation method of the pole piece:

[0170] In step (1), a first conductive agent, a polyurethane adhesive and N-methylpyrrolidone (NMP) are mixed in weight percentages of 40%, 30% and 30% to obtain a slurry.

[0171] Example 5 (Lower limit of content of polyurethane type binder in transition coating)

[0172] This embodiment is basically the same as Embodiment 1, except that:

[0173] In the pole piece:

[0174] The mass content of the polyurethane type adhesive in the material of the transition coating 2 is 40%, and the mass content of the first conductive agent in the material of the transition coating 2 is 60%.

[0175] In the preparation method of the pole piece:

[0176] In step (1), a first conductive agent, a polyurethane adhesive and N-methylpyrrolidone (NMP) are mixed in weight percentages of 28%, 42% and 30% to obtain a slurry.

[0177] Example 6 (Transition coating is provided only on one surface of the current collector)

[0178] This embodiment is basically the same as Embodiment 1, except that:

[0179] In the pole piece:

[0180] The transition coating 2 is disposed on one of the two opposite surfaces of the current collector 1;

[0181] The thickness of the transition coating 2 is 5 μm, and the total thickness of the composite current collector is 15 μm;

[0182] The thickness of the pole piece is 115 μm.

[0183] In the preparation method of the pole piece:

[0184] In step (1), a first conductive agent, a polyurethane binder and N-methylpyrrolidone (NMP) are mixed in weight percentages of 35%, 35% and 30% to obtain a slurry, and then the dispersed slurry is coated on one of the two opposite surfaces of the current collector and dried to obtain a composite current collector with a transition coating of 15 μm.

[0185] In step (3), the material layer and the composite current collector obtained in step (1) are finally composited on one side by hot rolling at 150° C., a rotation speed of 15 mm / s, and a roller gap of 0.1 mm to obtain a sodium ion dry-process positive electrode sheet.

[0186] Comparative Example 1 (First Adhesive is Non-Polyurethane Adhesive)

[0187] This comparative example is basically the same as Example 1, except that:

[0188] The first binder is PVDF (polyvinylidene fluoride).

[0189] Comparative Example 2 (no transition coating on the current collector surface)

[0190] This comparative example is basically the same as Example 1, except that:

[0191] like Figure 2 As shown, in the pole piece, the current collector itself is used instead of the composite current collector (that is, the transition coating 2 is not provided on the two opposite surfaces of the current collector 1, and the material layer 3 is directly provided), and the thickness of the pole piece is 210 μm.

[0192] In the preparation method of the pole piece:

[0193] Not including step (1);

[0194] In step (3), the material layer and the current collector (aluminum foil) are finally composited on both sides by hot rolling at 150° C., a rotation speed of 15 mm / s, and a roller gap of 0.1 mm to obtain a sodium ion dry-process positive electrode sheet.

[0195] Comparative Example 3 (Transition coating also contains active substances)

[0196] This comparative example is basically the same as Example 1, except that:

[0197] In the pole piece:

[0198] The material of the transition coating 2 also contains a first active substance, which is sodium nickel iron manganese oxide; in the transition coating 2, the mass ratio of the first binder, the first conductive agent and the first active substance is 1:1:1.

[0199] In the preparation method of the pole piece:

[0200] In step (1), the first conductive agent, the polyurethane binder, the first active material and N-methylpyrrolidone (NMP) are mixed in mass percentages of 20%, 20%, 20% and 30% to obtain a slurry, and then the dispersed slurry is coated on two opposite surfaces of the collector and dried to obtain a composite collector with a transition coating of 20 μm.

[0201] 2. Performance Test

[0202] 1. Test methods

[0203] (1) Mechanical properties test

[0204] The pole pieces prepared in each embodiment or comparative example were subjected to tensile strength and peel force tests. The test method was based on the standard GB / T36363-2018 "Polyolefin separators for lithium-ion batteries". The tensile strength and peel force of each pole piece were repeated three times and the average value was taken to obtain the tensile strength and peel force data.

[0205] (2) Diaphragm resistance test

[0206] The electrode pieces prepared in each embodiment or comparative example were cut into small discs with a diameter of 2 cm for membrane resistance testing. The electrode pieces were tested using a dual-plane controllable pressure disc electrode resistance method, with the pressure set to 20 MPa for measurement. Each electrode piece was tested four times and the average value was obtained.

[0207] (3) Electrochemical performance test

[0208] Battery Assembly:

[0209] The electrode sheets prepared in each embodiment or comparative example were cut into positive electrode sheets with a diameter of 12 mm, and then assembled into sodium ion button cells for electrochemical performance testing.

[0210] The assembly method of the sodium ion battery is as follows: the positive electrode sheet corresponding to each embodiment or comparative example is placed on one side of the diaphragm, and a Na metal sheet is placed on the other side of the diaphragm to obtain a mold; the mold is placed in a battery casing, an appropriate amount of electrolyte is dripped in, and the casing is tightened to obtain a mold battery for electrochemical performance testing. The separator is a glass fiber separator with a thickness of 9 μm; the electrolyte is composed of a solvent, an additive and a sodium salt, wherein: the solvent is composed of ethyl methyl carbonate (EMC), propylene carbonate (PC) and phenyl sulfone (PS), the mass content of ethyl methyl carbonate (EMC) in the electrolyte is 50.24%, the mass content of propylene carbonate (PC) in the electrolyte is 38.38%, and the mass content of phenyl sulfone (PS) in the electrolyte is 9.07%; the additive is composed of vinylene carbonate (VC) and fluoroethylene carbonate (FEC), the mass content of vinylene carbonate (VC) in the electrolyte is 0.54%, and the mass content of fluoroethylene carbonate (FEC) in the electrolyte is 1.77%; the sodium salt is sodium hexafluorophosphate, and its concentration in the electrolyte is 1 mol / L. The amount of electrolyte added is 0.1 g.

[0211] The method of electrochemical performance test is: connect the assembled mold battery to the charge and discharge tester, set the charge and discharge current (0.1C), test voltage (1.5-3.95V), and conduct the first week charge and discharge test. After 3 weeks of cycling at 0.1C, set the charge and discharge current to 0.33C and conduct the cycle performance test. The battery test temperature is 25℃.

[0212] 2. Test results

[0213] The mechanical property test results and diaphragm resistance test results of the electrode sheets prepared in each embodiment or comparative example are shown in Table 1.

[0214] Table 1 Mechanical properties and membrane resistance test results of the electrode sheets of various embodiments or comparative examples

[0215]

[0216] As can be seen from Table 1, the tensile strength and peel strength of the pole piece of the polyurethane composite current collector used are higher than the pole piece of the PVDF composite current collector in Comparative Example 2, indicating that the adhesion of the polyurethane type binder is higher than that of the PVDF binder; under the condition of similar surface density of sodium nickel cobalt manganate, the membrane resistance of the pole piece with the polyurethane composite current collector prepared in this application (Examples 1-4) is lower than that of the pole piece prepared using the PVDF current collector (Comparative Example 2), indicating that the pole piece provided in this application with a transition coating containing a polyurethane type binder between the current collector and the active substance has better ion transmission ability. The results of Examples 1-4 show that the transition coating containing a polyurethane type binder is provided between the current collector and the active substance, which can reduce the amount of polymer binder (for example, PTFE) used, increase the proportion of conductive carbon black, and the peel strength and peel force are significantly better than the pole piece (Comparative Example 1) without a transition coating between the current collector and the active substance.

[0217] The discharge specific capacity of the sodium ion battery corresponding to the electrode sheet prepared in each embodiment or comparative example and the test results of the capacity retention rate at 0.33C charge and discharge are shown in Table 2. Figure 4 0.33C charge and discharge curves of the sodium ion batteries corresponding to the pole pieces of Example 1 and Comparative Example 1, Figure 5 The 0.33C charge-discharge cycle performance curves of the sodium ion batteries corresponding to the pole pieces of Examples 1-4 and Comparative Examples 1-2 are shown.

[0218] Table 2 Test results of discharge specific capacity and capacity retention rate of sodium ion batteries corresponding to the pole pieces prepared in each embodiment or comparative example

[0219]

[0220]

[0221] From Table 2 and Figure 5 It can be seen that the life results show that the battery system has significantly improved cycle performance after a transition coating containing a polyurethane binder is set between the current collector and the active material. The pole pieces all have a transition coating containing a polyurethane binder and the SP to PTFE ratio of the pole piece membrane is (Example 3) 2:1. When the battery is cycled to 200 cycles at 0.33C, the battery discharge capacity is 124.63mAh / g, and the capacity retention rate is 96.32%; for the sodium ion battery without a transition coating between the current collector and the active material, when the battery is cycled to 200 cycles at 0.33C, the battery discharge capacity is only 123.46mAh / g, and the capacity retention rate is 93.9%. It can be concluded that the dry battery pole piece prepared by the present application scheme can effectively stabilize the battery structure during the battery cycle and improve the battery cycle life.

[0222] In the present application, the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0223] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0224] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A pole piece, characterized in that: include: A composite current collector, the composite current collector comprising a current collector and a transition coating disposed on at least one surface of the current collector, the material of the transition coating comprising a first binder and a first conductive agent, the first binder comprising a polyurethane binder; A material layer is provided on a surface of the transition coating layer facing away from the current collector, and the material of the material layer includes an active material, a second binder and a second conductive agent.

2. The pole piece according to claim 1, characterized in that: The active material is a positive electrode active material of a secondary battery or a negative electrode active material of a secondary battery; And / or, the current collector is a positive electrode current collector or a negative electrode current collector of a secondary battery.

3. The pole piece according to claim 2, characterized in that: The active material is a positive electrode active material of a sodium ion battery; And / or, the current collector is a positive electrode current collector of a sodium ion battery.

4. The pole piece according to claim 1, characterized in that: The polyurethane type binder includes at least one of the high molecular polymers containing -NHCOO- on the main chain; And / or, the mass content of the polyurethane type binder and the first conductive agent in the material of the transition coating is 40-60%.

5. The pole piece according to claim 1, characterized in that: The second binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, nitrile rubber, sodium hydroxymethyl cellulose, polyacrylic acid, polyacrylonitrile, and sodium alginate.

6. The pole piece according to claim 1, characterized in that: The mass content of the active substance in the material of the material layer is 90-98%; And / or, the mass content of the second binder in the material of the material layer is 1-5%; And / or, the mass content of the second conductive agent in the material of the material layer is 0.5-5%; And / or, the second conductive agent and the first conductive agent both include at least one of carbon black, graphene, carbon fiber, silicon, silicon oxide, and carbon nanotubes.

7. The pole piece according to claim 1, characterized in that: The pole piece meets at least one of the following characteristics: (1) The thickness of the transition coating is 4-6 μm; (2) The thickness of the material layer is 100-400 μm; (3) The thickness of the pole piece is 100-400 μm; (4) The resistance of the electrode is 235-275 mΩ; (5) The longitudinal tensile strength of the pole piece is 1.45-2.0 MPa, and / or the transverse tensile strength of the pole piece is 0.25-0.55 MPa; (6) The peel strength of the electrode is 48-60N / m.

8. A method for preparing a pole piece according to any one of claims 1 to 7, characterized in that: include: Using the first conductive agent and the first binder as raw materials, forming the transition coating on the current collector to obtain the composite current collector; The second binder and the second conductive agent are mixed to obtain a first mixed powder, and then the first mixed powder and the active material are sheared at a high speed to obtain a fiberized second mixed powder; Extruding the fiberized second mixed powder at least once, and then rolling to obtain the material layer; The material layer is hot-pressed and laminated on the surface of the transition coating layer that is away from the current collector to obtain the pole piece.

9. The preparation method according to claim 8, characterized in that: The step of forming the transition coating on the current collector using the first conductive agent and the first binder as raw materials comprises: Mixing the first conductive agent, the first binder and a non-aqueous organic solvent to obtain a slurry; Applying the slurry on at least one surface of the current collector, and then drying to obtain the transition coating; And / or, the rotation speed of the high-speed shearing is 1000-4000 rpm, the temperature of the high-speed shearing is 40-100° C., and the time of the high-speed shearing is 0.5-1 h; And / or, the extrusion molding temperature is 40-200°C, and the extrusion molding speed is 5-50mm / s; And / or, the temperature of the rolling is 25-100° C., and the speed of the rolling is 10-50 mm / s; And / or, the temperature of the hot pressing compound is 100-250° C., and the rotation speed of the hot pressing compound is 5-26 mm / s; And / or, the roll gap of the hot pressing composite is 0.1-2 mm; And / or, the extrusion molding obtains a dry powder tablet, and the thickness of the dry powder tablet is 500-800 μm.

10. A secondary battery comprising a positive electrode, a negative electrode and a separator, characterized in that: The positive electrode or negative electrode is the electrode piece according to any one of claims 1 to 7 or the electrode piece prepared by the preparation method according to claim 8 or 9.

Citation Information

Patent Citations

  • Electrode plate, electrode plate fabrication method and lithium ion battery

    CN109786658A

  • Composite current collector, electrode plate and lithium ion battery

    CN113036155A

  • Lithium ion battery positive plate, preparation method and lithium ion battery

    CN116454205A

  • Polyurethane binder for lithium ion battery pole piece as well as preparation method and application of polyurethane binder

    CN117363304A

  • Composite negative plate as well as preparation method and application thereof

    CN117525273A

Cited By

  • Negative pole piece and sodium ion battery

    CN121097017A