Method for preparing vanadium electrolyte from vanadium slag
Through sodium calcination and water immersion treatment of vanadium slag, combined with two-stage extraction processes and pH control, the problems of low vanadium yield and chromium resource utilization in vanadium battery preparation are solved, and the preparation of high-efficiency vanadium electrolyte and wastewater recycling are realized. , which has improved the application potential of vanadium batteries.
Patent Information
- Application Number
- CN202411288861.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The preparation process of existing vanadium batteries is complex, has low vanadium yield and high cost, and cannot achieve the maximum resource utilization of vanadium slag and the resource utilization of chromium, resulting in limited promotion and application of vanadium batteries.
After sodium calcination of vanadium slag, water-soaking treatment is performed with additives such as sodium metaaluminate. Combined with two-stage extraction processes and pH control, it can achieve efficient recycling of vanadium and chromium and preparation of electrolyte, and recycle sodium and wastewater.
The quality of vanadium electrolyte and vanadium recovery rate have been improved, the high value-added vanadium products and the resource utilization of chromium have been achieved, and the 0 emissions of three wastes have been basically achieved.
Smart Images

Figure CN118970127A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a method for preparing vanadium electrolyte from vanadium slag. Background Art
[0002] Vanadium batteries have the advantages of easy expansion, high safety, and long service life. They can well meet the conditions of large-scale energy storage applications and have become the most commercially promising liquid flow batteries. Vanadium electrolyte is a key component of vanadium batteries, and its production cost largely determines whether vanadium batteries can be applied on a large scale. At present, the preparation of commercial vanadium electrolytes uses high-purity vanadium pentoxide as the production raw material. The difference in the types of vanadium-containing materials makes the preparation process of high-purity vanadium pentoxide different, but they are all produced by hydrometallurgy. This "two-step" preparation method of vanadium-containing solution → high-purity vanadium pentoxide → vanadium electrolyte (liquid → solid → liquid) has a long process, complex process, low vanadium yield, and high cost, which seriously restricts the promotion and application of vanadium batteries. It is imperative to develop a new technology for preparing vanadium electrolytes by the "one-step" method (liquid → liquid) of vanadium-containing solutions.
[0003] The main raw material for vanadium extraction in my country is vanadium slag formed during the smelting process of vanadium-titanium magnetite. The current utilization of vanadium slag mainly adopts the sodium roasting-water leaching process to prepare 98% or 99% pure vanadium pentoxide, but this process cannot realize the resource utilization of chromium, and the vanadium recovery rate is also less than 85%. In addition, because the vanadium precipitation mother liquor cannot be reused, it can only be treated by evaporation, resulting in a large amount of ammonium sulfate & sodium sulfate hazardous solid waste containing a small amount of vanadium and chromium. How to achieve the maximum resource utilization of vanadium slag, the high added value of vanadium products and the recycling of wastewater has become a bottleneck restricting the sustainable development of vanadium extraction from vanadium slag. Summary of the invention
[0004] In view of the problems existing in the current utilization of vanadium slag, the purpose of the present invention is to provide a method for preparing vanadium electrolyte from vanadium slag, which has the advantages of high product added value, high vanadium and chromium extraction rate and waste water recycling.
[0005] A method for preparing vanadium electrolyte from vanadium slag, comprising the following steps:
[0006] Step (1):
[0007] The vanadium slag and sodium salt are subjected to sodium roasting, and then water leaching is carried out with the aid of an auxiliary agent, followed by solid-liquid separation to obtain leached slag and a vanadium-chromium-containing leaching solution; the auxiliary agent is an Al-containing compound;
[0008] Step (2):
[0009] The vanadium-chromium containing leachate is subjected to a first stage extraction with the organic phase O1 to obtain a chromium-loaded organic phase and a vanadium-containing raffinate;
[0010] The organic phase O1 is a hydrophobic solution containing an extractant of formula 1;
[0011]
[0012] The R1 to R3 are independently C8 to C 12 The straight chain alkane group; R4 is a C1-C3 alkyl group, the A - For CO3 2- or HCO3 - ;
[0013] The pH of the first extraction stage is above 13;
[0014] Step (3):
[0015] The vanadium-containing raffinate and the organic phase O2 are subjected to a second stage extraction to obtain a vanadium-carrying organic phase and a second stage raffinate; the vanadium-carrying organic phase is subjected to a back extraction treatment to obtain a vanadium electrolyte;
[0016] The organic phase O2 is a hydrophobic solution containing an extractant of formula 1; and the pH of the second extraction stage is between 8 and 10.
[0017] In view of the fact that the process of preparing vanadium electrolyte from vanadium slag faces the problems of too many impurities in the slag making it difficult for the vanadium electrolyte to meet the standards, and interference from impurities making it impossible to take into account both high-quality vanadium electrolyte and vanadium recovery rate, the present invention innovatively sodium-fermented and roasted the vanadium slag and then soaked it in water with the assistance of the auxiliary agent, and further cooperated with the subsequent two-stage extraction process and the joint control of conditions such as pH, so as to achieve synergy, solve the problems of low quality of vanadium electrolyte due to the complex components in the vanadium slag, and the impact of impurities on the recovery rate of vanadium electrolyte, and obtain vanadium electrolyte with high efficiency and high recovery rate; in addition, the process described in the present invention can realize efficient recycling of components, and basically achieve zero discharge of the three wastes.
[0018] Vanadium slag is a vanadium-chromium-containing material obtained by blast furnace smelting and converter blowing of vanadium-titanium magnetite. It has a complex composition, with vanadium oxide content of 10-20%, calcium oxide 1.5-3%, silicon oxide 10-24%, chromium oxide 1-8%, phosphorus 0.08-0.4%, titanium oxide 6-14%, magnesium oxide 1-4%, manganese oxide 6-14%, aluminum oxide 2-4%, and the rest mainly metallic iron and iron oxides.
[0019] In the present invention, in step (1), the vanadium slag is crushed and ground to -200 mesh, and then mixed with sodium salt for sodiumization roasting;
[0020] In the present invention, the sodium salt includes at least one of sodium carbonate and sodium bicarbonate.
[0021] In the present invention, the sodium salt accounts for 45-55% of the weight of the vanadium slag.
[0022] In the present invention, the temperature of the sodium calcination is 700-900°C, preferably 750-850°C.
[0023] In the present invention, the sodium roasting time is 1 to 2 hours.
[0024] In the present invention, an auxiliary agent is innovatively used to assist the water leaching treatment, which can optimize the leaching effect of V and the preparation quality of the prepared vanadium electrolyte.
[0025] In the present invention, the auxiliary agent is at least one of sodium aluminate, potassium aluminate, ammonium aluminate, aluminum hydroxide and aluminum oxide.
[0026] In the present invention, the auxiliary agent accounts for 10-25% of the weight of the sodium roasting product.
[0027] In the present invention, the liquid-to-solid ratio in the water immersion stage is 2 to 6:1 mL / g.
[0028] In the present invention, the temperature in the water immersion stage is 80-100°C.
[0029] In the present invention, the water immersion time is 1 to 3 hours.
[0030] In the present invention, the auxiliary agent-assisted water leaching process can optimize the recovery of vanadium and Cr in the leaching stage. In addition, the separation selectivity of vanadium, Cr and other impurities can be improved, which is beneficial to the subsequent extraction process and parameters such as pH, and can further enhance the quality and recovery rate of the vanadium electrolyte.
[0031] In the present invention, the pH of the vanadium-chromium containing leaching solution is adjusted to above 13 and then mixed with the organic phase O1 to perform the first stage extraction.
[0032] In the present invention, the volume content of the extractant of formula 1 in the organic phase O1 is 5-15%.
[0033] In the present invention, the organic phase O1 further comprises 5-15% of a phase regulator, and the phase regulator comprises, for example, at least one of sec-octanol, TBP, and nonylphenol.
[0034] In the present invention, the organic phase O1 further comprises at least one hydrophobic diluent selected from sulfonated kerosene, No. 260 solvent oil, aviation kerosene or other aliphatic hydrocarbon organic substances.
[0035] In the present invention, the flow ratio O / A in the first extraction stage is 1:3 to 5:1;
[0036] In the present invention, the first stage of extraction is performed by countercurrent extraction;
[0037] In the present invention, the number of stages of countercurrent extraction is 3 to 14.
[0038] In the present invention, the system consisting of the chromium-carrying organic phase, carbonate and alkaline liquid can be subjected to 2-14 levels of countercurrent stripping at a flow ratio of 2:1-1:10, and chromate precipitate and stripping organic phase O1" can be obtained by filtration and separation; the stripping organic phase O1" is returned to the chromium extraction process for recycling.
[0039] The carbonate includes at least one of calcium carbonate, barium carbonate, lead carbonate and copper carbonate, and the added amount thereof is 1.1 to 5 times the theoretical molar amount of the chromium in the chromium-carrying organic phase to react with it to generate the corresponding chromate.
[0040] The alkaline solution is an alkaline solution with a concentration of 0.5-5 mol / L obtained by dissolving at least one of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate in water.
[0041] In the present invention, the pH of the vanadium-containing raffinate is adjusted to 8-10 and then mixed with the organic phase O2 for the second stage extraction.
[0042] Preferably, carbon dioxide is used to control the pH of the vanadium-containing raffinate.
[0043] Preferably, in the organic phase O2, the volume content of the extractant of formula 1 is 20-40%;
[0044] Preferably, the organic phase O2 further comprises 5-15% of a phase regulator, wherein the phase regulator comprises at least one of octanol, TBP and nonylphenol;
[0045] Preferably, the organic phase O2 further comprises at least one hydrophobic diluent selected from sulfonated kerosene, No. 260 solvent oil, aviation kerosene or other aliphatic hydrocarbon organic substances;
[0046] Preferably, the flow ratio O / A in the second extraction stage is 1:2 to 5:1;
[0047] Preferably, the second stage of extraction is performed by countercurrent extraction;
[0048] Preferably, the number of countercurrent extraction stages is 4 to 14.
[0049] In the present invention, in step (3), the vanadium-loaded organic phase and the acidic solution are mixed and stripped to obtain a vanadium electrolyte and a stripped organic phase O2";
[0050] Preferably, the acidic solution is an aqueous solution containing an acidic solute, or an aqueous solution into which an acidic gas is introduced;
[0051] Preferably, the acidic solute includes at least one of H2SO3, V2(SO4)3 and H2C2O4; the acidic gas is SO2;
[0052] Preferably, in the acidic solution, the concentration of the acidic solute is 1 to 5 M;
[0053] Preferably, the acidic solute in the acidic solution is an acidic solute that can oxidize pentavalent vanadium in the vanadium-carrying organic phase to 1.1 to 2 times the theoretical amount of tetravalent vanadium.
[0054] In the present invention, the stripping organic phase O2" is mixed with the carbonic acid solution for transformation treatment and then reused;
[0055] Preferably, the carbonate solution is a solution containing 2-5 mol / L of at least one of sodium carbonate, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, potassium carbonate, and potassium bicarbonate;
[0056] Preferably, the ratio O / A of the stripping organic phase O2" to the carbonate solution is 1:1 to 4;
[0057] Preferably, the temperature in the transition stage is 20-40°C;
[0058] Preferably, the transformation treatment time is 0.5 to 5 hours.
[0059] In the present invention, the second-stage raffinate is cooled to 0-5°C and then crystallized for 1-5 hours, and then filtered and separated to obtain sodium carbonate and solution L3;
[0060] Preferably, sodium carbonate is returned to step (1) as sodium salt to participate in the sodium roasting process;
[0061] Preferably, solution L3 is returned to the leaching process of step (1) for recycling.
[0062] The process of the present invention can not only solve the problem of impurities in the vanadium slag preparation stage interfering with the electrolyte quality and recycling effect, but also realize the recycling of components and materials with almost zero emission.
[0063] Beneficial effects:
[0064] In view of the current shortcomings of vanadium slag such as low product value, low vanadium recovery, inability to recycle chromium, and high wastewater treatment costs, the present invention innovatively provides a method for preparing vanadium electrolyte from vanadium slag, which has the advantages of high vanadium extraction rate, high value-added vanadium electrolyte product, resource utilization of chromium, and ability to achieve the circulation of sodium and wastewater, without the generation of wastewater and hazardous solid waste. DETAILED DESCRIPTION
[0065] An optional method for preparing vanadium electrolyte from vanadium slag of the present invention, for example, comprises the following steps:
[0066] (1) Synchronous leaching of vanadium and chromium: after the vanadium slag is crushed and ground to -200 mesh, it is mixed with 45-55% of its mass of sodium carbonate, and roasted at 700-900°C, preferably 750-850°C for 1-2 hours to obtain a roasted material; the roasted material is ground to -100 mesh, and then aluminum salt and aqueous solution are added to leach at 80-100°C for 1-3 hours under the condition of solid-liquid ratio of 1:2-1:6 g / ml, and the leaching residue and leachate L are separated by filtration;
[0067] The aluminum salt is at least one of sodium aluminate, aluminum hydroxide and aluminum oxide, and the amount of the aluminum salt added is 10-25% of the weight of the sodium calcined product;
[0068] The aqueous solution used for the first leaching is ordinary water, and the aqueous solution used for the subsequent leaching is the aqueous solution obtained after step 4.
[0069] (2) Separation and extraction of chromium from the leachate: NaOH is added to the leachate L to adjust the pH of the solution to 13 or above, and then the leachate is contacted with the organic phase O1, and 3 to 14 levels of countercurrent extraction are performed at a flow ratio O / A of 1:3 to 5:1 to obtain a chromium-loaded organic phase O1' and a raffinate L1; the chromium-loaded organic phase O1' is subjected to 2 to 14 levels of countercurrent stripping at a flow ratio of 2:1 to 1:10 with a system consisting of carbonate and alkaline liquid, and chromate precipitate and stripping organic phase O1" are obtained by filtration and separation; the stripping organic phase O1" is returned to the chromium extraction process for recycling;
[0070] The organic phase O1 comprises an extractant A, a phase regulator B and a hydrophobic diluent C; the volume content of the extractant A is 5-15%, the volume content of the phase regulator B is 5-15%, and the rest is the hydrophobic diluent.
[0071] The extractant A comprises a structure of formula I;
[0072]
[0073] The R1 to R3 are independently C8 to C 12 A straight chain alkane group; R4 is CH3; A - For CO3 2- or HCO3 - ;
[0074] The phase regulator B is at least one of octanol, TBP and nonylphenol; the hydrophobic diluent is at least one of sulfonated kerosene, No. 260 solvent oil, aviation kerosene or other aliphatic hydrocarbon organic substances.
[0075] The carbonate is at least one of calcium carbonate, barium carbonate, lead carbonate and copper carbonate, and the amount of the carbonate added is 1.1 to 5 times the theoretical molar amount of the chromium in the loaded organic phase O1' to react with it to form the corresponding chromate; the alkaline solution refers to an alkaline solution with a concentration of 0.5 to 5 mol / L obtained by dissolving at least one of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate in water.
[0076] (3) Preparation of vanadium electrolyte: CO2 is introduced into the raffinate L1 to adjust the pH to 8-10, and then the raffinate L1 is mixed with an organic phase O2 containing an extractant of the structural formula 1 and subjected to 4-14 stages of countercurrent extraction at a flow ratio O / A of 1:2-5:1 to obtain a raffinate L2 and an organic phase O2' loaded with vanadium; the organic phase O2' is subjected to 3-14 stages of countercurrent stripping with an acidic solution at a flow ratio O / A of 2:1-1:2 to obtain a vanadium electrolyte and a stripping organic phase O2"; the stripping organic phase O2" is transformed and reused for vanadium extraction and separation.
[0077] The organic phase O2 comprises an extractant A', a phase regulator B' and a hydrophobic diluent C'; the volume content of the extractant A' is 20-40%, the volume content of the phase regulator B' is 5-15%, and the rest is the hydrophobic diluent.
[0078] The extractant A' of the present invention is the same as the extractant A described above;
[0079] The phase regulator B' is at least one of octanol, TBP and nonylphenol; the hydrophobic diluent is at least one of sulfonated kerosene, No. 260 solvent oil, aviation kerosene or other aliphatic hydrocarbon organic substances.
[0080] The acidic solution refers to a solution obtained by dissolving at least one of SO2, H2SO3, V2(SO4)3 and H2C2O4 in a 1-5 mol / L sulfuric acid solution. The amount of SO2, H2SO3, V2(SO4)3 and H2C2O4 added is 1.1-2 times the theoretical amount of tetravalent vanadium to oxidize pentavalent vanadium in the organic phase O2'.
[0081] The transformation of the stripping organic phase O2" refers to reacting the stripping organic phase O2" with a solution containing 2-5 mol / L of at least one of sodium carbonate, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, potassium carbonate, and potassium bicarbonate at a ratio O / A of 1:1-4 at 20-40°C for 0.5-5h.
[0082] (4) Recycling of sodium salt and waste liquid:
[0083] The raffinate L2 is cooled to 0-5°C and then crystallized for 1-5 hours, and then filtered to separate sodium carbonate and solution L3. The sodium carbonate is returned to the roasting process of step (1), and the solution L3 is returned to the leaching process of step (1) for recycling.
[0084] The following examples are intended to illustrate the present invention rather than to further limit the scope of protection of the present invention.
[0085] The extractant of the present invention can be a commercial product having The structured extractant is obtained by transformation of carbonate and / or bicarbonate solution.
[0086] Example 1
[0087] The main components of the vanadium slag used in the experiment are:
[0088] The vanadium oxide content is 19.5%, calcium oxide 2.5%, silicon oxide 16.1%, chromium oxide 6.1%, phosphorus 0.3%, titanium oxide 8.9%, magnesium oxide 3.7%, manganese oxide 8.1%, aluminum oxide 2.3%, and the rest is metallic iron and iron oxide.
[0089] Step 1:
[0090] 2000g of vanadium slag was crushed and ground to -200 mesh, and then evenly mixed with 55% of its mass of sodium carbonate, and roasted at 750°C for 2h to obtain a roasted material; the roasted material was ground to -100 mesh, and then 25% of the mass of the roasted material was added with sodium aluminate (auxiliary agent) and an aqueous solution at a solid-liquid ratio of 1:6g / ml, and leached at 100°C for 1h, and filtered and separated to obtain leached slag and leaching solution L; the leaching rate of vanadium was 95.2%, and the leaching rate of chromium was 91.3%.
[0091] Step 2:
[0092] NaOH was added to the leachate L to adjust the pH of the solution to 13.5, and then the leachate L was mixed with a 5% methyl trialkyl extractant (in Formula 1, R1-R3 are C8-C10 straight-chain alkane groups, R4 is CH3, A - For CO3 2- )+10% TBP+85% aviation kerosene organic phase O1, and then perform 3-stage countercurrent extraction at a flow ratio O / A of 5:1 to obtain raffinate L1 and chromium-loaded organic phase O1'. The chromium-loaded organic phase O1' is mixed with a system consisting of lead carbonate (the amount of lead carbonate added is 5 times the theoretical amount of lead chromate generated by the reaction of lead with chromium in the organic phase) and 0.5 mol / L sodium hydroxide solution, and perform 14-stage countercurrent stripping at a flow ratio (O / A) of 2:1. After filtration, separation and drying, lead chromate with a purity of 99.2% and stripping organic phase O1' are obtained. The recovery rate of chromium in the whole process is 89.3%.
[0093] Step 3:
[0094] The raffinate L1 was introduced into CO2 to adjust the pH to 8, and then mixed with a 20% methyl trialkyl extractant (in Formula 1, R1-R3 are C8-C10 straight-chain alkane groups, R4 is CH3, A - For CO3 2- )+15% TBP+65% sulfonated kerosene organic phase is mixed, and 14-stage countercurrent extraction is carried out at a flow ratio O / A of 1:2 to obtain a raffinate L2 and a vanadium-loaded organic phase O2'; the vanadium-loaded organic phase O2' is washed with ultrapure water, and then 2 times the theoretical amount of oxalic acid is dissolved in a 2.5M sulfuric acid solution, and 14-stage countercurrent stripping is carried out on the organic phase O2' at a flow ratio O / A of 2:1 to obtain a vanadium electrolyte and a stripped organic phase O2".
[0095] The Si content in the vanadium electrolyte is 5 mg / L, the P content is 0.4 mg / L, the Cr content is 12 mg / L, and the Al content is 30 mg / L, all of which are lower than the first-grade requirements of the national standard GB / T37204-2018. The contents of other impurities also meet the first-grade requirements of GB / T37204-2018.
[0096] The raffinate L2 was cooled to 0°C and crystallized for 1 hour, and then filtered to separate sodium carbonate and solution L3. The stripped organic phase O2" was reacted with 5 mol / L sodium carbonate solution at a ratio of O / A of 1:1 at 240°C for 0.5 hour to obtain the transformed organic phase O2"'.
[0097] The vanadium recovery rate in the whole process is 93.1%.
[0098] Comparative Example 1
[0099] Compared with Example 1, the only difference is that in step 1, no auxiliary agent is added, and the other operations and parameters are the same as those in Example 1. The results are:
[0100] In step 1, the leaching rate of vanadium is 93.8% and the leaching rate of chromium is 88.2%.
[0101] In step 2, the purity of the lead chromate prepared is 89.2%. The recovery rate of chromium in the whole process is 82.9%.
[0102] In step 3, the Si content of the prepared vanadium electrolyte is 150 mg / L, the P content is 20 mg / L, the Cr content is 30 mg / L, and the Al content is 25 mg / L, wherein the contents of silicon and chromium exceed the requirements of the first-grade product of the national standard GB / T37204-2018, and the phosphorus content is also far from Example 1. The recovery rate of vanadium in the whole process is 88.4%.
[0103] Comparative Example 2
[0104] Compared with Example 1, the only difference is that magnesium oxide of equal weight is used to replace the auxiliary agent, and other operations and parameters are the same as those of Example 1. The results are:
[0105] In step 1, the leaching rate of vanadium is 92.1% and the leaching rate of chromium is 87.3%.
[0106] In step 2, the purity of the lead chromate prepared is 92.6%. The recovery rate of chromium in the whole process is 83.7%.
[0107] In step 3, the Si content of the prepared vanadium electrolyte is 40 mg / L, the P content is 8 mg / L, the Cr content is 16 mg / L, and the Al content is 20 mg / L, wherein the contents of silicon and chromium exceed the requirements of the first-grade product of the national standard GB / T37204-2018, and the phosphorus content is also far from Example 1. The recovery rate of vanadium in the whole process is 88.9%.
[0108] Comparative Example 3
[0109] Compared with Example 1, the only difference is that in step 2, the pH is controlled at 10, and the other operations and parameters are the same as those in Example 1. The results are:
[0110] In step 2, the purity of the lead chromate prepared is 85.7%. The recovery rate of chromium in the whole process is 86.0%.
[0111] In step 3, the Si content of the prepared vanadium electrolyte is 6 mg / L, the P content is 0.9 mg / L, the Cr content is 1 g / L, and the Al content is 35 mg / L, wherein the chromium content exceeds the first-grade requirement of the national standard GB / T37204-2018. The vanadium recovery rate of the whole process is 87.2%.
[0112] Example 2
[0113] The vanadium slag used in the experiment is the same as that in Example 1.
[0114] 100g of vanadium slag was crushed and ground to -200 mesh, then mixed evenly with 55% of its mass of sodium carbonate, and roasted at 750°C for 2h to obtain a roasted material; the roasted material was ground to -100 mesh, and then 25% of the mass of the roasted material was added with sodium aluminate (auxiliary agent) and an aqueous solution at a solid-liquid ratio of 1:6g / ml, and leached at 100°C for 1h, and filtered and separated to obtain leached slag and leaching solution L; the leaching rate of vanadium was 95.2%, and the leaching rate of chromium was 91.3%.
[0115] NaOH was added to the leachate L to adjust the pH of the solution to 13.5, and then the leachate was mixed with the stripping organic phase O1" in Example 1, and then three-stage countercurrent extraction was performed at a flow ratio O / A of 5:1 to obtain a raffinate L1 and a chromium-loaded organic phase O1'. A system consisting of the chromium-loaded organic phase O1', lead carbonate (the amount of lead carbonate added was 5 times the theoretical amount of lead chromate generated by the reaction of lead with chromium in the organic phase) and 0.5 mol / L sodium hydroxide solution was mixed at a flow ratio (O / A) of 2:1 and 14-stage countercurrent stripping was performed. After filtration, separation and drying, lead chromate with a purity of 99.1% and stripping organic phase O1"' were obtained. The chromium recovery rate of the whole process was 89.4%.
[0116] The raffinate L1 was introduced with CO2 to adjust the pH to 8, and then mixed with the transformed organic phase O2"' in Example 1, and subjected to 4-stage countercurrent extraction at a flow ratio O / A of 5:1 to obtain the raffinate L2 and the vanadium-loaded organic phase O2'; the vanadium-loaded organic phase O2' was washed with ultrapure water, and then the organic phase O2' was subjected to 14-stage countercurrent stripping with 2 times the theoretical amount of oxalic acid dissolved in 2.5M sulfuric acid solution at a flow ratio O / A of 2:1 to obtain a vanadium electrolyte and a stripped organic phase.
[0117] The Si content in the vanadium electrolyte is 4.6 mg / L, the P content is 0.6 mg / L, and the Cr content is 11.9 mg / L, all of which are lower than the first-grade requirements of the national standard GB / T37204-2018. The contents of other impurities also meet the first-grade requirements of GB / T37204-2018. The recovery rate of vanadium in the whole process is 93.0%.
[0118] Example 3
[0119] The vanadium slag used in the experiment is the same as that in Example 1.
[0120] 100g of vanadium slag was crushed and ground to -200 mesh, and then sodium carbonate obtained by freeze crystallization in Example 1 was added in an amount of 55% of the mass of the vanadium slag. After mixing evenly, the mixture was roasted at 750°C for 2h to obtain a roasted material; the roasted material was ground to -100 mesh, and then sodium aluminate (auxiliary agent) of 25% of the mass of the roasted material and the solution L3 obtained in Example 1 were added, and the mixture was leached at 100°C for 1h at a solid-liquid ratio of 1:6g / ml, and the leached slag and the leaching solution L were obtained by filtration and separation; the leaching rate of vanadium was 98.1%, and the leaching rate of chromium was 94.2%.
[0121] NaOH was added to the leachate L to adjust the pH of the solution to 14, and then the leachate L was mixed with a 15% methyl trialkyl extractant (in Formula 1, R1-R3 are C8-C10 straight-chain alkane groups, R4 is CH3, A - For CO3 2-)+15% TBP+70% sulfonated kerosene organic phase O1, and then carry out 14-stage countercurrent extraction at a flow ratio O / A of 1:3 to obtain raffinate L1 and chromium-loaded organic phase O1'. The chromium-loaded organic phase O1 is mixed with a system consisting of barium carbonate (the amount of barium carbonate added is 1.1 times the theoretical amount of barium chromate generated by the reaction of barium with chromium in the organic phase) and 5 mol / L sodium hydroxide solution, and is subjected to 14-stage countercurrent stripping at a flow ratio (O / A) of 1:10. After filtration, separation and drying, a barium chromate product with a purity of 99.1% and a stripping organic phase O1' are obtained. The chromium recovery rate of the whole process is 92.8%.
[0122] The raffinate L1 was introduced into CO2 to adjust the pH to 10, and then mixed with a 40% methyl trialkyl extractant (in Formula 1, R1-R3 are C8-C10 straight-chain alkane groups, R4 is CH3, A - HCO3 - )+15% 2-octanol+45% sulfonated kerosene organic phase, and subjected to 4-stage countercurrent extraction at a flow ratio of O / A of 5:1 to obtain a raffinate L2 and a vanadium-loaded organic phase O2'; the vanadium-loaded organic phase O2' was washed with ultrapure water, and 1.1 times the theoretical amount of V2(SO4)3 was dissolved in 2.5M sulfuric acid solution, and the organic phase O2' was subjected to 14-stage countercurrent stripping at a flow ratio of O / A of 1:2 to obtain a vanadium electrolyte and a stripped organic phase O2".
[0123] The Si content in the vanadium electrolyte is 4 mg / L, the P content is 0.2 mg / L, and the Cr content is 10 mg / L, all of which are lower than the first-grade requirements of the national standard GB / T37204-2018. The contents of other impurities also meet the first-grade requirements of GB / T37204-2018. The raffinate L2 is cooled to 5°C for crystallization for 5 hours, and then filtered and separated to obtain sodium carbonate and solution L3.
[0124] The vanadium recovery rate in the whole process is 96.2%.
[0125] Example 4
[0126] The main components of the vanadium slag used in the experiment are:
[0127] The content of vanadium oxide is 10.3%, calcium oxide 1.5%, silicon oxide 20.6%, chromium oxide 1.5%, phosphorus 0.08%, titanium oxide 6.5%, magnesium oxide 1.1%, manganese oxide 10.3%, aluminum oxide 3.9%, and the rest is metallic iron and iron oxide.
[0128] Step 1:
[0129] 1000g of vanadium slag was crushed and ground to -200 mesh, and then mixed evenly with 45% of its mass of sodium carbonate, and roasted at 850°C for 1h to obtain a roasted material; the roasted material was ground to -100 mesh, and then 10% of the mass of the roasted material was added with aluminum hydroxide (auxiliary agent) and an aqueous solution, and leached at 80°C for 3h under the condition of a solid-liquid ratio of 1:2g / ml, and the leached slag and the leaching solution L were obtained by filtration and separation; the leaching rate of vanadium was 93.1%, and the leaching rate of chromium was 90.1%.
[0130] Step 2:
[0131] NaOH was added to the leachate L to adjust the pH of the solution to 15, and then the leachate L was mixed with a 15% methyl trialkyl extractant (in Formula 1, R1-R3 are C8-C10 straight-chain alkane groups, R4 is CH3, A - For CO3 2- )+10% nonylphenol+75% No. 260 solvent oil organic phase O1 is mixed, and then 12-stage countercurrent extraction is carried out at a flow ratio O / A of 1:3 to obtain a raffinate L1 and a chromium-loaded organic phase O1'. A system consisting of the chromium-loaded organic phase O1, copper carbonate (the amount of copper carbonate added is 1.1 times the theoretical amount of copper chromate generated by the reaction of copper with chromium in the organic phase) and 3 mol / L sodium carbonate solution is mixed at a flow ratio (O / A) of 1:3 and 11-stage countercurrent stripping is carried out. After filtration, separation and drying, a copper chromate product with a purity of 99.2% and a stripping organic phase O1' are obtained. The chromium recovery rate of the whole process is 89.5%.
[0132] Step 3:
[0133] The raffinate L1 was introduced into CO2 to adjust the pH to 9, and then mixed with a 20% methyl trialkyl extractant (in Formula 1, R1-R3 are C8-C10 straight-chain alkane groups, R4 is CH3, A - HCO3 - )+20% sec-octanol+50% sulfonated kerosene organic phase, and carry out 12-stage countercurrent extraction at a flow ratio O / A of 1:2 to obtain a raffinate L2 and a vanadium-loaded organic phase O2'; the vanadium-loaded organic phase O2' is washed with ultrapure water, and then 2 times the theoretical amount of sulfurous acid is dissolved in 1M sulfuric acid solution, and the organic phase O2' is subjected to 8-stage countercurrent stripping at a flow ratio O / A of 2:1 to obtain a vanadium electrolyte and a stripped organic phase O2".
[0134] The Si content in the vanadium electrolyte is 6 mg / L, the P content is 0.3 mg / L, the Cr content is 0.4 mg / L, and the Al content is 35 mg / L, all of which are lower than the first-grade requirements of the national standard GB / T37204-2018. The contents of other impurities also meet the first-grade requirements of GB / T37204-2018.
[0135] The vanadium recovery rate in the whole process is 91.6%.
Claims
1. A method for preparing vanadium electrolyte from vanadium slag, characterized in that the steps include: Step (1): The vanadium slag and sodium salt are subjected to sodium roasting, and then water leaching is carried out with the aid of an auxiliary agent, followed by solid-liquid separation to obtain leached slag and a vanadium-chromium-containing leaching solution; the auxiliary agent is an Al-containing compound; Step (2): The vanadium-chromium containing leachate is subjected to a first stage extraction with the organic phase O1 to obtain a chromium-loaded organic phase and a vanadium-containing raffinate; The organic phase O1 is a hydrophobic solution containing an extractant of formula 1; Formula 1 The R1 to R3 are independently C8 to C 12 The straight chain alkane group; R4 is a C1-C3 alkyl group, the A - For CO3 2- or HCO3 - ; The pH of the first extraction stage is above 13; Step (3): The vanadium-containing raffinate and the organic phase O2 are subjected to a second stage extraction to obtain a vanadium-carrying organic phase and a second stage raffinate; the vanadium-carrying organic phase is subjected to a back extraction treatment to obtain a vanadium electrolyte; The organic phase O2 is a hydrophobic solution containing an extractant of formula 1; and the pH of the second extraction stage is between 8 and 10.
2. The method for preparing vanadium electrolyte from vanadium slag according to claim 1, characterized in that: In step (1), the vanadium slag is crushed and ground to -200 mesh, and then mixed with sodium salt for sodium roasting; Preferably, the vanadium slag is a vanadium-chromium-containing material obtained by blast furnace smelting and converter blowing of vanadium-titanium magnetite, wherein the content of vanadium oxide is 10-20%, calcium oxide is 1.5-3%, silicon oxide is 10-24%, chromium oxide is 1-8%, phosphorus is 0.08-0.4%, titanium oxide is 6-14%, magnesium oxide is 1-4%, manganese oxide is 6-14%, aluminum oxide is 2-4%, and the rest is mainly metallic iron and iron oxide; Preferably, the sodium salt comprises at least one of sodium carbonate and sodium bicarbonate; Preferably, the sodium salt is 45-55% by weight of the vanadium slag; Preferably, the temperature of the sodium calcination is 700-900°C, preferably 750-850°C; Preferably, the sodium calcination time is 1-2 hours.
3. The method for preparing vanadium electrolyte from vanadium slag according to claim 1, characterized in that: The auxiliary agent is at least one of sodium aluminate, potassium aluminate, ammonium aluminate, aluminum hydroxide and aluminum oxide; Preferably, the auxiliary agent is 10-25% by weight of the sodium roasted product; Preferably, the liquid-to-solid ratio in the water immersion stage is 2 to 6:1 mL / g; Preferably, the temperature during the water immersion stage is 80-100°C; Preferably, the immersion time is 1-3 hours.
4. The method for preparing vanadium electrolyte from vanadium slag according to claim 1, characterized in that: The pH of the vanadium-chromium containing leaching solution is adjusted to above 13 and then mixed with the organic phase O1 to perform the first stage extraction; Preferably, in the organic phase O1, the volume content of the extractant of formula 1 is 5 to 15%; Preferably, the organic phase O1 further comprises 5-15% of a phase regulator, wherein the phase regulator comprises at least one of octanol, TBP and nonylphenol; Preferably, the organic phase O1 further comprises at least one hydrophobic diluent selected from sulfonated kerosene, No. 260 solvent oil, aviation kerosene or other aliphatic hydrocarbon organic substances; Preferably, the flow ratio O / A in the first extraction stage is 1:3-5:1; Preferably, the first stage of extraction is performed by countercurrent extraction; Preferably, the number of countercurrent extraction stages is 3-14 stages.
5. The method for preparing vanadium electrolyte from vanadium slag according to claim 1 or 4, characterized in that: The system consisting of the chromium-carrying organic phase, carbonate and alkaline liquid is subjected to 2-14 levels of countercurrent stripping at a flow ratio of 2:1-1:10, and chromate precipitate and stripping organic phase O1" are obtained by filtration and separation; the stripping organic phase O1" is returned to the chromium extraction process for recycling; Preferably, the carbonate comprises at least one of calcium carbonate, barium carbonate, lead carbonate and copper carbonate, and the amount thereof added is 1.1 to 5 times the theoretical molar amount of the chromium in the chromium-carrying organic phase that reacts with the chromium to form the corresponding chromate; Preferably, the alkaline solution is an alkaline solution having a concentration of 0.5 to 5 mol / L obtained by dissolving at least one of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate in water.
6. The method for preparing vanadium electrolyte from vanadium slag according to claim 1, characterized in that: The pH of the vanadium-containing raffinate is adjusted to 8-10 and then mixed with organic phase O2 for the second stage extraction; Preferably, carbon dioxide is used to control the pH of the vanadium-containing raffinate; Preferably, in the organic phase O2, the volume content of the extractant of formula 1 is 20-40%; Preferably, the organic phase O2 further comprises 5-15% of a phase regulator, wherein the phase regulator comprises at least one of octanol, TBP and nonylphenol; Preferably, the organic phase O2 further comprises at least one hydrophobic diluent selected from sulfonated kerosene, No. 260 solvent oil, aviation kerosene or other aliphatic hydrocarbon organic substances; Preferably, the flow ratio O / A in the second extraction stage is 1:2-5:1; Preferably, the second stage of extraction is performed by countercurrent extraction; Preferably, the number of countercurrent extraction stages is 4-14.
7. The method for preparing vanadium electrolyte from vanadium slag according to claim 1 or 6, characterized in that: In step (3), the vanadium-loaded organic phase and the acidic solution are mixed and stripped to obtain a vanadium electrolyte and a stripped organic phase O2"; Preferably, the acidic solution is an aqueous solution containing an acidic solute, or an aqueous solution into which an acidic gas is introduced; Preferably, the acidic solute includes at least one of H2SO3, V2(SO4)3 and H2C2O4; the acidic gas is SO2; Preferably, in the acidic solution, the concentration of the acidic solute is 1 to 5 M; Preferably, the acidic solute in the acidic solution is an acidic solute that can oxidize pentavalent vanadium in the vanadium-carrying organic phase to 1.1-2 times the theoretical amount of tetravalent vanadium.
8. The method for preparing vanadium electrolyte from vanadium slag according to claim 7, characterized in that: The stripping organic phase "O2" is mixed with the carbonic acid solution for transformation treatment and then reused; Preferably, the carbonate solution is a solution containing 2-5 mol / L of at least one of sodium carbonate, sodium bicarbonate, ammonium carbonate, ammonium bicarbonate, potassium carbonate, and potassium bicarbonate; Preferably, the ratio O / A of the stripping organic phase O2" to the carbonate solution is 1:1 to 4; Preferably, the temperature in the transition stage is 20-40°C; Preferably, the transformation treatment time is 0.5 to 5 hours.
9. The method for preparing vanadium electrolyte from vanadium slag according to claim 1, characterized in that: The second-stage raffinate is cooled to 0-5°C and then crystallized for 1-5 hours, and then filtered to separate and obtain sodium carbonate and solution L3; Preferably, sodium carbonate is returned to step (1) as sodium salt to participate in the sodium roasting process; Preferably, solution L3 is returned to the leaching process of step (1) for recycling.
Citation Information
Patent Citations
Two-stage extraction preparation method for high-purity vanadyl sulfate solution
CN103505903A
Method for separating and extracting vanadium and chromium from vanadium slag sodium-modified roasting water leachate
CN112442595A
Method for co-extraction-selective reverse extraction separation of vanadium and chromium from solution containing vanadium and chromium
CN113201657A
Method for preparing vanadium oxide from vanadium-containing solution
CN113604685A
Method for preparing high-purity vanadyl sulfate solution from industrial vanadium slag sodium salt roasting water leaching solution
CN115404361A
Cited By
Vanadium slag valence state regulation-based vanadyl sulfate electrolyte short-process preparation method and application thereof
CN119560602A
Preparation method of all-vanadium redox flow battery electrolyte
CN120565752A
Preparation method and application of carbon dioxide hydrogenation catalyst
CN120733745A