Secondary battery, battery module, battery pack, and electric device
By doping elements A and R in lithium manganese phosphate, coating the core surface, combining organic solvents in the non-aqueous electrolyte, the problem of poor rate performance of lithium manganese phosphate is solved, and the high-temperature cycle of secondary batteries is significantly improved and rate performance enhances the stability and safety of the battery.
Patent Information
- Application Number
- CN202410985090.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-04-29
AI Technical Summary
As the positive electrode active material of lithium ion secondary batteries, lithium manganese phosphate has poor rate performance, which limits its commercial application.
Using a core-shell structure, a doped lithium manganese phosphate positive electrode active material is used to form a doped lithium manganese phosphate core by doping element A and phosphorus doping element R at the manganese position, and a layer of coat is applied on the core surface, combined with The organic solvent in the nonaqueous electrolyte improves the high-temperature cycle performance, cycle stability and rate performance of secondary batteries.
It significantly improves the high-temperature cycling performance, cycle stability and rate performance of the secondary battery, reduces the interface side reaction between the positive electrode material and the electrolyte, and improves the energy density and safety performance of the battery.
Smart Images

Figure CN118970143A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a secondary battery, a battery module, a battery pack and an electrical device. Background Art
[0002] In recent years, with the development of lithium-ion secondary battery technology, lithium-ion secondary batteries are widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, and are widely used in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. As lithium-ion secondary batteries have made great progress, higher requirements have been put forward for their energy density, cycle performance and safety performance.
[0003] As the positive electrode active material of lithium-ion secondary batteries, lithium manganese phosphate has the advantages of high capacity, good safety and low cost. However, the rate performance of lithium manganese phosphate is poor, which restricts its commercial application. Summary of the invention
[0004] The present application provides a secondary battery, a battery module, a battery pack and an electric device to solve the problem of poor rate performance of a secondary battery when lithium manganese phosphate is used as a positive electrode active material of a lithium ion secondary battery.
[0005] A first aspect of the present invention provides a secondary battery, the secondary battery comprising a positive electrode sheet and a non-aqueous electrolyte, wherein:
[0006] The positive electrode sheet includes a positive electrode active material having a core-shell structure, wherein the positive electrode active material includes a core and a shell covering the core.
[0007] The chemical formula of the core is Li 1+x Mn 1-y A y P 1-z R z O4, wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, z is any value in the range of 0.001-0.100, A includes one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be one or more elements selected from Fe, Ti, V, Ni, Co and Mg, R includes one or more elements selected from B, Si, N and S, and R includes one element selected from B, Si, N and S; the values of x, y and z satisfy the following conditions: keep the entire core electrically neutral;
[0008] The shell includes a first coating layer covering the core;
[0009] The first coating layer includes crystalline pyrophosphate LiaMP2O7 and / or Mb(P2O7) c , wherein 0≤a≤2, 1≤b≤4, 1≤c≤6, and the values of a, b and c satisfy the following conditions: making the crystalline pyrophosphate LiaMP2O7 or Mb(P2O7) c Maintaining electrical neutrality, crystalline pyrophosphate LiaMP2O7 and Mb(P2O7) c Each of the M's independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al;
[0010] The non-aqueous electrolyte includes an organic solvent, the organic solvent includes a first solvent, the first solvent includes one or more of the compounds shown in Formula 1,
[0011]
[0012] R1 and R2 are each independently one of C1-C10 alkyl and C1-C10 haloalkyl. Optionally, R1 and R2 are each independently one of methyl, ethyl, propyl, butyl, pentyl, hexyl, fluoromethyl, fluoroethyl, fluoropropyl, fluorobutyl, fluoropentyl and fluorohexyl. Further, R1 and R2 are each independently one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl and fluoropropyl.
[0013] The surface oxygen valence state of the positive electrode active material having a core-shell structure is -1.90 or less.
[0014] Unless otherwise specified, in the above chemical formula, when A is more than two elements, the above-mentioned limitation on the numerical range of y is not only a limitation on the stoichiometric number of each element as A, but also a limitation on the sum of the stoichiometric numbers of each element as A. For example, when A is more than two elements A1, A2...An, the stoichiometric numbers y1, y2...yn of A1, A2...An each need to fall within the numerical range of y defined in this application, and the sum of y1, y2...yn also needs to fall within the numerical range. Similarly, for the case where R is more than two elements, the limitation on the numerical range of the stoichiometric number of R in this application also has the above meaning.
[0015] Herein, crystalline means that the crystallinity is above 50%, i.e., 50%-100%. Crystallinity less than 50% is called glassy state. The crystallinity of the crystalline pyrophosphate and crystalline phosphate described in this application is 50% to 100%. Pyrophosphate and phosphate with a certain degree of crystallinity are not only conducive to giving full play to the pyrophosphate coating layer's ability to hinder the dissolution of manganese ions and the phosphate coating layer's excellent ability to conduct lithium ions and reduce interface side reactions, but also enable the pyrophosphate coating layer and the phosphate coating layer to better perform lattice matching, thereby achieving a close combination between the coating layers.
[0016] The present application provides a novel lithium manganese phosphate positive electrode active material with a core-shell structure by doping element A at the manganese position of lithium manganese phosphate and doping element R at the phosphorus position to obtain a doped lithium manganese phosphate core and coating the core surface. The positive electrode active material is applied to a secondary battery, which can significantly improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the secondary battery.
[0017] At the same time, the first solvent in the non-aqueous electrolyte has a good ability to dissociate lithium salts, but compared with carbonates, the first organic solvent has a poor affinity with Li + The force of Li + The desolvation energy will gradually decrease, which is beneficial to Li + Rapid embedding and extraction at the interface, thereby improving the rate performance of the secondary battery. In addition, the first solvent has a low viscosity, which can quickly migrate and embed the lithium ions extracted from the positive electrode active material into the negative electrode side. Driven by concentration polarization, the lithium ions at the interface of the positive electrode material are quickly transferred to the electrolyte, further improving the rate performance of the secondary battery.
[0018] Moreover, by limiting the surface oxygen valence state of the positive electrode active material within the above range, the interface side reaction between the positive electrode material and the electrolyte can be reduced, thereby improving the cycle performance, high temperature storage gas generation performance and the like of the battery cell.
[0019] In any embodiment of the first aspect, the shell further includes a second coating layer coating the first coating layer.
[0020] In any embodiment of the first aspect, the second coating layer comprises crystalline phosphate XPO4, wherein X comprises one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al.
[0021] In any embodiment of the first aspect, the shell further includes a third coating layer coating the second coating layer.
[0022] In any embodiment of the first aspect, the third coating layer comprises carbon.
[0023] In any embodiment of the first aspect, the first solvent comprises at least one of the following compounds:
[0024]
[0025] In any embodiment of the first aspect, optionally, the first solvent comprises at least one of the following compounds:
[0026]
[0027] When the first solvent is selected from the above substances, the electrolyte viscosity is lower and the wettability is better, so the lithium ion transmission capacity is better, thereby better improving the rate performance of the secondary battery; at the same time, the above first solvents have better chemical stability and better oxidation tolerance to the positive electrode active material.
[0028] In any embodiment of the first aspect, based on the total mass of the organic solvent, the mass percentage of the first solvent is w1, and the range of w1 is 20% to 80%; optionally, the range of w1 is 30% to 75%. By controlling the above mass percentage, the first solvent can be used to improve the fast charging performance of the battery while making the secondary battery have good cycle performance and storage performance.
[0029] In any embodiment of the first aspect, optionally, the organic solvent further comprises a second solvent, and the second solvent comprises one or more of the group consisting of linear carbonates and cyclic carbonates; further optionally, based on the total mass of the organic solvent, the mass percentage of the second solvent is w2, and the range of w2 is 20% to 80%; optionally, the range of w2 is 25% to 70%. The second solvent is used in combination with the first solvent to improve the cycle performance of the secondary battery.
[0030] In any embodiment of the first aspect, the non-aqueous electrolyte further includes a first additive, and the first additive includes one or more of the group consisting of sultones and cyclic sulfates. Sultones or cyclic sulfates are introduced into the non-aqueous electrolyte, and during the charging process of the secondary battery, they form a layer of polymers with strong ion conductivity, such as ester-based sulfates, on the surface of the positive electrode active material. The polymer can not only further improve the rate performance of the secondary battery, but also effectively inhibit the catalytic oxidation of the positive electrode active material to the first solvent, thereby improving the circulation and storage performance of the secondary battery. In addition, sultones or cyclic sulfates can be superior to the first solvent in film formation at the negative electrode, reducing the reaction of α-H on the first solvent with the active lithium obtained by reduction of the negative electrode, thereby further improving the circulation and storage performance of the secondary battery.
[0031] In any embodiment of the first aspect, the sultone comprises at least one of the compounds represented by Formula 2,
[0032]
[0033] p means 1, 2 or 3,
[0034] R 11 represents one of a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, and a C1-C12 haloalkoxy group; optionally, R 11 represents one of a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, and a C1-C3 haloalkoxy group; the alkoxy group may be a chain alkoxy group or a cyclic alkoxy group, the cyclic alkoxy group may share a carbon atom with the parent ring of the sultone, and the cyclic alkoxy group may have 4, 5 or 6 carbon atoms;
[0035] Each R 12 Each independently represents a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, or a 4- to 7-membered sultone group; optionally, each R 12 Each independently represents one of a hydrogen atom, a halogen atom, a C1-C3 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, and a 5- to 6-membered sultone group; optionally, the sultone group shares a carbon atom with the parent ring of the sultone group, and optionally the sultone group is a 5-membered ring;
[0036] R 11 and R 12 The carbon atoms to which they are attached may form a 5- to 10-membered cycloalkyl group;
[0037] R 13 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a C2-C6 ester group, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C2-C12 alkenyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, a C6-C20 aryl group or a benzyl group; optionally, R 13 It represents one of hydrogen atom, halogen atom, carbonyl group, C2-C3 ester group, C1-C3 alkyl group, C1-C3 haloalkyl group, C2-C6 alkenyl group, C1-C3 alkoxy group, C1-C3 haloalkoxy group, C6-C10 aryl group or benzyl group. The above sultone is commonly used in the art, with wide sources and low cost.
[0038] In any embodiment of the first aspect, the cyclic sulfate ester comprises at least one of the compounds represented by Formula 3,
[0039]
[0040] q means 1, 2 or 3,
[0041] R 14 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C2-C12 alkenyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, a C2-C6 ester group, and a 4- to 7-membered cyclic sulfate group; optionally, R 14 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a double bond, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C2-C3 ester group, and a 4- to 5-membered cyclic sulfate group; optionally, the cyclic sulfate group and the cyclic sulfate ester share a carbon atom;
[0042] Each R 15 Each independently represents a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, or a C6-C20 aryl group; optionally, each R 15 Each independently represents one of a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, and a C6-C10 aryl group;
[0043] or R 14 and R 15 Together with the carbon atoms to which they are linked, they form a 4- to 7-membered cyclic sulfate group. 14 and R 15 Together with the carbon atoms to which they are linked, they form a 5-membered cyclic sulfate group.
[0044] The above-mentioned cyclic sulfate is a commonly used cyclic sulfate in the art, with a wide source and low cost.
[0045] In any embodiment of the first aspect, optionally, the sultone comprises at least one of the following compounds:
[0046]
[0047] In any embodiment of the first aspect, optionally, the cyclic sulfate comprises at least one of the following compounds:
[0048]
[0049] Further optionally, the sultone comprises at least one of the following compounds:
[0050]
[0051] Further optionally, the cyclic sulfate comprises at least one of the following compounds:
[0052]
[0053] The above-mentioned sultone and cyclic sulfate are more likely to form a polymer at the positive electrode.
[0054] In any embodiment of the first aspect, based on the total mass of the non-aqueous electrolyte, the content of the first additive is W3, and 0.01%≤W3≤20%, optionally 0.1%≤W3≤10%, and further optionally 0.3%≤W3≤5%. The increase in positive and negative electrode impedance caused by the introduction of too much sultone or cyclic sulfate is avoided, thereby ensuring a significant improvement in the capacity and rate performance of the lithium-ion battery.
[0055] In any embodiment of the first aspect, the non-aqueous electrolyte further comprises a second additive, and the second additive comprises one or more of the group consisting of a sulfite compound, a disulfonate compound, a nitrile compound, an aromatic compound, a phosphazene compound, an anhydride compound, a phosphite compound, a phosphate compound, and a borate compound. The second additive helps to form a more compact and stable interface film on the surface of the positive and / or negative electrode active material, thereby further improving at least one of the cycle performance, storage performance, and rate performance of the secondary battery.
[0056] In any embodiment of the first aspect, based on the total mass of the non-aqueous electrolyte, the content of the second additive is W4, 0.01%≤W4≤20%, optionally 0.05%≤W4≤5%, further optionally 0.1%≤W4≤3%, so that the effect of the second additive can be fully exerted.
[0057] In any embodiment of the first aspect, based on the weight of the inner core, the coating amount of the first coating layer is C1 weight %, C1 is greater than 0 and less than or equal to 6, can be greater than 0 and less than or equal to 5.5, and can be greater than 0 and less than or equal to 2.
[0058] In any embodiment of the first aspect, based on the weight of the inner core, the coating amount of the second coating layer is C2 weight %, C2 is greater than 0 and less than or equal to 6, can be greater than 0 and less than or equal to 5.5, and can be more optionally 2-4.
[0059] In any embodiment of the first aspect, based on the weight of the inner core, the coating amount of the third coating layer is C3 weight %, C3 is greater than 0 and less than or equal to 6, can be greater than 0 and less than or equal to 5.5, and can be greater than 0 and less than or equal to 2.
[0060] In the positive electrode active material with a core-shell structure of the above embodiment, the coating amount of the three coating layers is preferably within the above range, thereby being able to fully coat the inner core and at the same time further improve the kinetic performance and safety performance of the secondary battery without sacrificing the gram capacity of the positive electrode active material.
[0061] In any embodiment of the first aspect, the interplanar spacing of the crystalline pyrophosphate in the first coating layer is in the range of 0.293-0.470 nm, and the angle of the crystal orientation (111) is in the range of 18.00°-32.00°.
[0062] In any embodiment of the first aspect, the interplanar spacing of the crystalline phosphate in the second coating layer is in the range of 0.244-0.425 nm, and the angle of the crystal orientation (111) is in the range of 20.00°-37.00°.
[0063] The first coating layer and the second coating layer in the positive electrode active material of the above embodiment both use crystalline materials, and their crystal plane spacing and angle range are within the above range, which can more effectively avoid impurity phases in the coating layers, thereby further improving the material's specific capacity, cycle performance and rate performance.
[0064] In any embodiment of the first aspect, in the core, the ratio of y to 1-y is 1:10 to 1:1, and can be 1:4 to 1:1. Thus, the cycle performance and rate performance of the secondary battery are further improved.
[0065] In any embodiment of the first aspect, in the core, the ratio of z to 1-z is 1:999 to 1:9, and can be 1:499 to 1:249. Thus, the cycle performance and rate performance of the secondary battery are further improved.
[0066] In any embodiment of the first aspect, the carbon of the third coating layer is a mixture of SP2 carbon and SP3 carbon, and optionally, the molar ratio of SP2 carbon to SP3 carbon is any value in the range of 0.1-10, and can be any value in the range of 2.0-3.0. The above embodiment better improves the comprehensive performance of the secondary battery by limiting the molar ratio of SP2 carbon to SP3 carbon within the above range.
[0067] In any embodiment of the first aspect, the thickness of the first coating layer is 1-10 nm. In the above embodiment, when the thickness of the first coating layer ranges from 1-10 nm, it is possible to avoid the adverse effect on the kinetic properties of the material that may be caused when it is too thick, and it is possible to avoid the problem of not being able to effectively hinder the migration of transition metal ions when it is too thin.
[0068] In any embodiment of the first aspect, the thickness of the second coating layer is 2-15nm. In the above embodiment, when the thickness of the second coating layer is in the range of 2-15nm, the surface structure of the second coating layer is stable, and the side reaction with the electrolyte is small, so the interface side reaction can be more effectively reduced, thereby more significantly improving the high temperature performance of the secondary battery.
[0069] In any embodiment of the first aspect, the thickness of the third coating layer is 2-25 nm. In the above embodiment, when the thickness of the third coating layer is in the range of 2-20 nm, the electrical conductivity of the material can be further improved and the compaction density performance of the battery pole piece prepared using the positive electrode active material can be improved.
[0070] In any embodiment of the first aspect, based on the weight of the positive electrode active material having a core-shell structure, the manganese content is in the range of 10 wt%-35 wt%, optionally in the range of 15 wt%-30 wt%, and more optionally in the range of 17 wt%-20 wt%, the phosphorus content is in the range of 12 wt%-25 wt%, optionally in the range of 15 wt%-20 wt%, and the weight ratio of manganese to phosphorus is in the range of 0.90-1.25, and optionally in the range of 0.95-1.20.
[0071] In the positive electrode active material with a core-shell structure of the above-mentioned embodiment, the content of manganese element is within the above-mentioned range, which can effectively avoid the problems such as poor material structure stability and decreased density that may be caused by excessive manganese content, thereby more effectively improving the secondary battery's cycle, storage and compaction density and other performances; and can avoid the problems such as low voltage platform that may be caused by too low manganese content, thereby improving the energy density of the secondary battery.
[0072] In the positive electrode active material with a core-shell structure of the above-mentioned embodiment, the content of phosphorus is within the above-mentioned range, which can effectively avoid the following situations: if the content of phosphorus is too large, the covalency of PO may be too strong and affect the conductivity of small polarons, thereby affecting the electrical conductivity of the material; if the content of phosphorus is too small, the stability of the pyrophosphate lattice structure in the inner core, the first coating layer and / or the phosphate in the second coating layer may be reduced, thereby affecting the overall stability of the material.
[0073] In the positive electrode active material with a core-shell structure of the above-mentioned embodiment, the weight ratio of manganese element to phosphorus element is within the above-mentioned range, which can effectively avoid the following situations: if the weight ratio is too large, it may lead to increased dissolution of transition metals, affecting the stability of the material and the cycle and storage performance of the secondary battery; if the weight ratio is too small, the discharge voltage platform of the material may decrease, thereby reducing the energy density of the secondary battery.
[0074] In any embodiment of the first aspect, the lattice change rate of the positive electrode active material having a core-shell structure before and after complete lithium deintercalation is 4% or less, optionally 3.8% or less, and more optionally 2.0-3.8%. The positive electrode active material having a core-shell structure of the above embodiment can achieve a lattice change rate of less than 4% before and after lithium deintercalation. Therefore, the use of positive electrode active materials can more effectively improve the gram capacity and rate performance of secondary batteries.
[0075] In any embodiment of the first aspect, the Li / Mn antisite defect concentration of the positive electrode active material having a core-shell structure is less than 4%, optionally less than 2.2%, and more optionally 1.5-2.2%. By having the Li / Mn antisite defect concentration within the above range, the Mn 2+ Obstacles + transmission, while further improving the gram capacity and rate performance of the positive electrode active materials.
[0076] In any embodiment of the first aspect, the positive electrode active material having a core-shell structure has a compaction density of 2.2 g / cm at 3 T (tons). 3 Above, optionally 2.2 g / cm 3 Above and 2.8g / cm 3 Therefore, by increasing the compaction density, the weight of the active material per unit volume increases, which is more conducive to improving the volume energy density of the secondary battery.
[0077] In any embodiment of the first aspect, the surface oxygen valence state of the positive electrode active material having a core-shell structure is -1.90 to -1.98. Thus, by limiting the surface oxygen valence state of the positive electrode active material to the above range as above, the interfacial side reaction between the positive electrode material and the electrolyte can be further reduced, thereby improving the cycle of the battery cell, high temperature storage gas production and other performances.
[0078] A second aspect of the present application further provides a battery module, the battery module comprising a secondary battery, the secondary battery being any one of the above-mentioned secondary batteries of the present application.
[0079] The third aspect of the present application also provides a battery pack, which includes a battery module, and the battery module is the above-mentioned battery module of the present application.
[0080] The fourth aspect of the present application also provides an electrical device, which includes at least one of a secondary battery, a battery module or a battery pack, and the above-mentioned secondary batteries, battery modules and battery packs are all the secondary batteries, battery modules and battery packs provided in the present application.
[0081] Therefore, the battery module and battery pack of the present application have higher cycle performance and rate characteristics, and thus provide higher power cycle stability and rate characteristics for the electrical device having the secondary battery, battery module or battery pack of the present application.
[0082] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0083] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.
[0084] Figure 1 is a schematic diagram of a secondary battery according to one embodiment of the present application.
[0085] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown.
[0086] Figure 3 is a schematic diagram of a battery module according to an embodiment of the present application.
[0087] Figure 4 It is a schematic diagram of a battery pack according to one embodiment of the present application.
[0088] Figure 5 yes Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown.
[0089] Figure 6 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.
[0090] In the drawings, the drawings are not drawn to scale.
[0091] Description of reference numerals:
[0092] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION
[0093] The following detailed description and drawings of the embodiments of the present application are used to illustrate the principles of the present application, but cannot be used to limit the scope of the present application, that is, the present application is not limited to the described embodiments.
[0094] Below, the embodiments of the secondary battery, battery module, battery pack and power device of the present application are specifically disclosed with appropriate reference to the accompanying drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0095] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0096] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0097] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0098] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0099] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0100] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0101] In this article, the term "coating" refers to the material layer coated on the kernel, and the material layer can completely or partially coat the kernel. The use of "coating" is just for the convenience of description and is not intended to limit the present invention. Similarly, the term "thickness of coating" refers to the thickness of the material layer coated on the kernel in the kernel radial direction.
[0102] As used herein, the term "source" refers to a compound that is the source of a certain element. Examples of the "source" include, but are not limited to, carbonates, sulfates, nitrates, simple substances, halides, oxides, and hydroxides.
[0103] [Secondary battery]
[0104] Secondary batteries, also known as rechargeable batteries or storage batteries, refer to batteries that can continue to be used by recharging the active materials after the battery is discharged.
[0105] Normally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. During the battery charging and discharging process, active ions (such as lithium ions) are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte is between the positive electrode sheet and the negative electrode sheet, mainly to conduct active ions.
[0106] A first aspect of the present invention provides a secondary battery, the secondary battery comprising a positive electrode sheet and a non-aqueous electrolyte, wherein:
[0107] The positive electrode sheet includes a positive electrode active material having a core-shell structure, wherein the positive electrode active material includes a core and a shell covering the core.
[0108] The chemical formula of the core is Li 1+x Mn 1-y A y P 1-z R z O4, wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, z is any value in the range of 0.001-0.100, A includes one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be one or more elements selected from Fe, Ti, V, Ni, Co and Mg, R includes one or more elements selected from B, Si, N and S, and optionally, R includes an element selected from B, Si, N and S; the values of x, y and z satisfy the following conditions: keep the entire core electrically neutral;
[0109] The shell includes a first coating layer covering the core;
[0110] The first coating layer includes crystalline pyrophosphate LiaMP2O7 and / or Mb(P2O7) c , wherein 0≤a≤2, 1≤b≤4, 1≤c≤6, and the values of a, b and c satisfy the following conditions: making the crystalline pyrophosphate LiaMP2O7 or Mb(P2O7) c Maintaining electrical neutrality, crystalline pyrophosphate LiaMP2O7 and Mb(P2O7) c Each of the M's independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al;
[0111] The non-aqueous electrolyte includes an organic solvent, the organic solvent includes a first solvent, the first solvent includes one or more of the compounds shown in Formula 1,
[0112]
[0113] R1 and R2 are each independently one of C1-C10 alkyl and C1-C10 haloalkyl. Optionally, R1 and R2 are each independently one of methyl, ethyl, propyl, butyl, pentyl, hexyl, fluoromethyl, fluoroethyl, fluoropropyl, fluorobutyl, fluoropentyl and fluorohexyl. Further, R1 and R2 are each independently one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl and fluoropropyl.
[0114] The surface oxygen valence state of the positive electrode active material having a core-shell structure is -1.90 or less.
[0115] Unless otherwise specified, in the above chemical formula, when A is more than two elements, the above-mentioned limitation on the numerical range of y is not only a limitation on the stoichiometric number of each element as A, but also a limitation on the sum of the stoichiometric numbers of each element as A. For example, when A is more than two elements A1, A2...An, the stoichiometric numbers y1, y2...yn of A1, A2...An each need to fall within the numerical range of y defined in this application, and the sum of y1, y2...yn also needs to fall within the numerical range. Similarly, for the case where R is more than two elements, the limitation on the numerical range of the stoichiometric number of R in this application also has the above meaning.
[0116] The secondary battery of the present application utilizes the positive electrode active material with a coating layer and the improvement of the electrolyte composition, which not only effectively improves the rate performance of the secondary battery, but also improves the cycle performance of the secondary battery. Specifically:
[0117] The positive electrode active material of the present application can improve the gram capacity, cycle performance and safety performance of the secondary battery. Although the mechanism is not clear, it is speculated that the lithium manganese phosphate positive electrode active material of the present application is a core-shell structure, wherein the manganese position and phosphorus position of the lithium manganese phosphate core are doped with elements A and R respectively, which can not only effectively reduce manganese dissolution, thereby reducing the manganese ions migrating to the negative electrode, reducing the electrolyte consumed by the decomposition of the SEI film, and improving the cycle performance and safety performance of the secondary battery, but also can promote the adjustment of the Mn-O bond, reduce the lithium ion migration barrier, promote lithium ion migration, and improve the rate performance of the secondary battery; by coating the core with a first coating layer including crystalline pyrophosphate, the migration resistance of manganese can be further increased, its dissolution can be reduced, and the surface impurity lithium content can be reduced, and the contact between the core and the electrolyte can be reduced, thereby reducing the interface side reaction, reducing the gas production, and improving the high temperature storage performance, cycle performance and safety performance of the secondary battery.
[0118] In addition, in the core, the element A doped at the manganese position of the lithium manganese phosphate also helps to reduce the lattice change rate of the lithium manganese phosphate during the lithium insertion and extraction process of the material, improves the structural stability of the lithium manganese phosphate positive electrode material, greatly reduces the dissolution of manganese and reduces the oxygen activity on the surface of the particles; the element R doped at the phosphorus position also helps to change the difficulty of the Mn-O bond length change, thereby improving electronic conductivity and reducing the lithium ion migration barrier, promoting lithium ion migration, and improving the rate performance of the secondary battery.
[0119] In addition, the entire core system maintains electrical neutrality, which can ensure that there are as few defects and impurities in the positive electrode active material as possible. If there is an excess of transition metal (such as manganese) in the positive electrode active material, since the material system itself has a relatively stable structure, the excess transition metal is likely to precipitate in the form of a single substance or form an impurity phase inside the lattice. Maintaining electrical neutrality can minimize such impurities. In addition, ensuring the electrical neutrality of the system can also produce lithium vacancies in the material in some cases, thereby making the material's kinetic properties more excellent.
[0120] It can be seen that the present application provides a new type of lithium manganese phosphate positive electrode active material with a core-shell structure by doping element A at the manganese position of lithium manganese phosphate and doping element R at the phosphorus position to obtain a doped lithium manganese phosphate core and performing a layer of coating on the surface of the core. The positive electrode active material is applied to secondary batteries, which can significantly improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the secondary batteries.
[0121] At the same time, the first solvent in the non-aqueous electrolyte has a good ability to dissociate lithium salts, but compared with carbonates, the first organic solvent has a poor affinity with Li + The force of Li + The desolvation energy will gradually decrease, which is beneficial to Li + Rapid embedding and extraction at the interface, thereby improving the rate performance of the secondary battery. In addition, the first solvent has a low viscosity, which can quickly migrate and embed the lithium ions extracted from the positive electrode active material into the negative electrode side. Driven by concentration polarization, the lithium ions at the interface of the positive electrode material are quickly transferred to the electrolyte, further improving the rate performance of the secondary battery.
[0122] Moreover, the stable valence state of oxygen is -2. The closer the valence state is to -2, the stronger its electron-acquiring ability is, that is, the stronger its oxidizing property is. Under normal circumstances, its surface valence state is below -1.7. By limiting the surface oxygen valence state of the positive electrode active material to the above range as described above, the interface side reaction between the positive electrode material and the electrolyte can be reduced, thereby improving the cycle of the battery cell, high-temperature storage gas production and other performances.
[0123] The surface oxygen valence state can be measured by methods known in the art, such as by electron energy loss spectroscopy (EELS).
[0124] In any embodiment of the first aspect, the shell further comprises a second coating layer coating the first coating layer.
[0125] By further coating with a crystalline phosphate coating layer having excellent lithium ion conductivity, the interfacial side reactions on the surface of the positive electrode active material can be effectively reduced, thereby improving the high temperature cycle and storage performance of the secondary battery.
[0126] In any embodiment of the first aspect, the second coating layer comprises crystalline phosphate XPO4, wherein X comprises one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al.
[0127] In any embodiment of the first aspect, the shell further comprises a third coating layer coating the second coating layer.
[0128] By further coating with a third coating layer (such as a carbon layer), the safety performance and dynamic performance of the secondary battery can be further improved.
[0129] In any embodiment of the first aspect, the third coating layer comprises carbon.
[0130] [Non-aqueous electrolyte]
[0131] The first solvent used in the present application may be any carboxylic acid ester included in the aforementioned formula 1. In some embodiments, the first solvent includes at least one of the following compounds:
[0132]
[0133]
[0134] In some embodiments, optionally, the first solvent includes at least one of the following compounds:
[0135]
[0136] When the first solvent is selected from the above substances, the electrolyte viscosity is lower and the wettability is better, so the lithium ion transmission capacity is better, thereby better improving the rate performance of the secondary battery; at the same time, the above first solvents have better chemical stability and better oxidation tolerance to the positive electrode active material.
[0137] Although the first solvent has the advantages of low viscosity and high conductivity, it is easy to react chemically with the positive and negative electrodes of the secondary battery, thereby affecting the cycle performance of the secondary battery. In some embodiments, based on the total mass of the organic solvent, the mass percentage of the first solvent is w1, and the range of w1 is 20% to 80% (such as 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%); Optionally, the range of w1 is 30% to 75%. Through the control of the above mass percentage, the first solvent can be used to improve the fast charging performance of the battery while making the secondary battery have good cycle performance and storage performance.
[0138] When the first solvent is used as the solvent of the non-aqueous electrolyte, in order to ensure that the secondary battery has high cycle performance and storage performance as much as possible, in some embodiments, optionally, the organic solvent also includes a second solvent, and the second solvent includes one or more of the group consisting of linear carbonates and cyclic carbonates; further optionally, based on the total mass of the organic solvent, the mass percentage of the second solvent is w2, and the range of w2 is 20% to 80% (such as 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%); optionally, the range of w2 is 25% to 70%. The second solvent is used in combination with the first solvent to improve the cycle performance of the secondary battery.
[0139] There is no particular restriction on the types of the linear carbonate and cyclic carbonate of the above-mentioned second solvent, and they can be selected according to actual needs. Optionally, the second solvent can include one or more of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, and methyl propionate.
[0140] In some embodiments of the first aspect, the solvent of the non-aqueous electrolyte may also include common solvents such as tetrahydrofuran, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone, which are not described in detail in this application.
[0141] Typically, the non-aqueous electrolyte may also optionally include additives. As an example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0142] Furthermore, in some embodiments, the non-aqueous electrolyte further includes a first additive, and the first additive includes one or more of the group consisting of sultones and cyclic sulfates. Sultones or cyclic sulfates are introduced into the non-aqueous electrolyte, and during the charging process of the secondary battery, they form a layer of polymers with strong ion conductivity, such as ester-based sulfates, on the surface of the positive electrode active material. The polymer can not only further improve the rate performance of the secondary battery, but also effectively inhibit the catalytic oxidation of the positive electrode active material to the first solvent, thereby improving the circulation and storage performance of the secondary battery. In addition, sultones or cyclic sulfates can be superior to the first solvent in film formation at the negative electrode, reducing the reaction of α-H on the first solvent with the active lithium obtained by reduction of the negative electrode, thereby further improving the circulation and storage performance of the secondary battery.
[0143] The sultone and cyclic sulfate used in the above embodiments of the present application may be corresponding substances commonly used in the prior art. In some embodiments, the sultone includes at least one of the compounds shown in Formula 2.
[0144]
[0145] p means 1, 2 or 3,
[0146] R 11 represents one of a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, and a C1-C12 haloalkoxy group; optionally, R 11 represents one of a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, and a C1-C3 haloalkoxy group; the alkoxy group may be a chain alkoxy group or a cyclic alkoxy group, the cyclic alkoxy group may share a carbon atom with the parent ring of the sultone, and the cyclic alkoxy group may have 4, 5 or 6 carbon atoms;
[0147] Each R 12 Each independently represents a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, or a 4- to 7-membered sultone group; optionally, each R 12 Each independently represents one of a hydrogen atom, a halogen atom, a C1-C3 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, and a 5- to 6-membered sultone group; optionally, the sultone group shares a carbon atom with the parent ring of the sultone group, and optionally the sultone group is a 5-membered ring;
[0148] R 11 and R 12 The carbon atoms to which they are attached may form a 5- to 10-membered cycloalkyl group;
[0149] R13 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a C2-C6 ester group, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C2-C12 alkenyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, a C6-C20 aryl group or a benzyl group; optionally, R 13 It represents one of a hydrogen atom, a halogen atom, a carbonyl group, a C2-C3 ester group, a C1-C3 alkyl group, a C1-C3 haloalkyl group, a C2-C6 alkenyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C6-C10 aryl group or a benzyl group.
[0150] The above-mentioned sultone is a commonly used sultone in the art, with a wide source and low cost.
[0151] In some embodiments, the cyclic sulfate ester comprises at least one of the compounds shown in Formula 3,
[0152]
[0153] q means 1, 2 or 3,
[0154] R 14 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C2-C12 alkenyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, a C2-C6 ester group, and a 4- to 7-membered cyclic sulfate group; optionally, R 14 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a double bond, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C2-C3 ester group, and a 4- to 5-membered cyclic sulfate group; optionally, the cyclic sulfate group and the cyclic sulfate ester share a carbon atom;
[0155] Each R 15 Each independently represents a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, or a C6-C20 aryl group; optionally, each R 15 Each independently represents one of a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, and a C6-C10 aryl group;
[0156] or R 14 and R 15 Together with the carbon atoms to which they are linked, they form a 4- to 7-membered cyclic sulfate group. 14 and R 15 Together with the carbon atoms to which they are linked, they form a 5-membered cyclic sulfate group.
[0157] The above-mentioned cyclic sulfate is a commonly used cyclic sulfate in the art, with a wide source and low cost.
[0158] In some embodiments, optionally, the sultone comprises at least one of the following compounds:
[0159]
[0160] In some embodiments, optionally, the cyclic sulfate comprises at least one of the following compounds:
[0161]
[0162] Further optionally, the sultone comprises at least one of the following compounds:
[0163]
[0164] Further optionally, the cyclic sulfate comprises at least one of the following compounds:
[0165]
[0166] The above-mentioned sultone and cyclic sulfate are more likely to form a polymer at the positive electrode.
[0167] Although sultone and cyclic sulfate can improve the cycle performance and storage performance of the secondary battery relative to the first solvent, if the amount is too much, it may cause the positive and negative impedance of the secondary battery to increase, affecting the rate of the secondary battery. Those skilled in the art can select their amount in the non-aqueous electrolyte of the present application based on the conventional amount of existing sultone and cyclic sulfate. In some embodiments, based on the total mass of the non-aqueous electrolyte, the content of the above-mentioned first additive is W3, and 0.01%≤W3≤20% (such as 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 1%, 2%, 3%, 4%, 5%, 10%, 15% or 20%), optionally 0.1%≤W3≤10%, and further optionally 0.3%≤W3≤5%. On the basis of effectively suppressing the decrease in cycle performance caused by the first solvent, the increase in positive and negative electrode impedance caused by the introduction of too much sultone or cyclic sulfate is avoided, thereby ensuring a significant improvement in the capacity and rate performance of the lithium-ion battery.
[0168] In some embodiments, the non-aqueous electrolyte used in the present application further includes a second additive, which includes one or more of the group consisting of sulfite compounds, disulfonate compounds, nitrile compounds, aromatic compounds, phosphazene compounds, anhydride compounds, phosphite compounds, phosphate compounds, and borate compounds. The above-mentioned second additive helps to form a more compact and stable interface film on the surface of the positive and / or negative electrode active material, thereby further improving at least one of the cycle performance, storage performance, and rate performance of the secondary battery.
[0169] In some embodiments, based on the total mass of the non-aqueous electrolyte, the content of the second additive is W4, 0.01%≤W4≤20%, optionally 0.05%≤W4≤5%, further optionally 0.1%≤W4≤3%, so that the effect of the second additive can be fully exerted.
[0170] Some of the second additives are exemplified below.
[0171] Sulfite compounds
[0172] The sulfite compound is preferably a cyclic sulfite compound, and specifically can be selected from one or more of the compounds shown in Formula 4.
[0173]
[0174] In formula 4, R 28 It is selected from substituted or unsubstituted C1-C6 alkylene groups, substituted or unsubstituted C2-C6 alkenylene groups, wherein the substituent is selected from one or more of a halogen atom, a C1-C3 alkyl group, and a C2-C4 alkenyl group.
[0175] In Formula 4, optionally, R 28 It is selected from substituted or unsubstituted C1-C4 alkylene groups, substituted or unsubstituted C2-C4 alkenylene groups, wherein the substituent is selected from one or more of a halogen atom, a C1-C3 alkyl group, and a C2-C4 alkenyl group.
[0176] Optionally, the sulfite compound can be selected from one or more of ethylene sulfite (abbreviated as ES), propylene sulfite (abbreviated as PS), and butylene sulfite (abbreviated as BS).
[0177] Disulfonate compounds
[0178] The disulfonate compound is a compound containing two sulfonic acid groups (-S(=O)2O-), preferably selected from disulfonic acid methylene ester compounds, and the disulfonic acid methylene ester compound can be selected from one or more of the compounds shown in Formula 5. In Formula 5, R 24 , R 25 , R 26 , R 27Each is independently selected from a hydrogen atom, a halogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C2-C10 alkenyl group, wherein the substituent is selected from one or more of a halogen atom, a C1-C3 alkyl group, and a C2-C4 alkenyl group.
[0179]
[0180] In Formula 5, optionally, R 24 , R 25 , R 26 , R 27 Each is independently selected from a hydrogen atom, a halogen atom, a substituted or unsubstituted C1-C4 alkyl group, a substituted or unsubstituted C2-C6 alkenyl group, wherein the substituent is selected from one or more of a halogen atom, a C1-C3 alkyl group, and a C2-C4 alkenyl group.
[0181] Optionally, the disulfonate compound may be specifically selected from one or more of the following compounds, but the present application is not limited thereto:
[0182]
[0183] Further optionally, the disulfonate compound can be selected from methylene disulfonate (abbreviated as MMDS), and the specific structure is as follows:
[0184]
[0185] Nitrile compounds
[0186] The nitrile compound may be any one or more of the compounds shown in Formula 6 or Formula 7,
[0187]
[0188] In Formula 6 and Formula 7: R5 is selected from substituted or unsubstituted C1~C12 alkylene, substituted or unsubstituted C2~C12 alkenylene, substituted or unsubstituted C2~C12 alkynylene, R6, R7, R8 are each independently selected from substituted or unsubstituted C0~C12 alkylene, substituted or unsubstituted C2~C12 alkenylene, substituted or unsubstituted C2~C12 alkynylene, wherein the substituent is selected from one or more of a halogen atom, a nitrile group, a C1~C6 alkyl group, a C2~C6 alkenyl group, and a C1~C6 alkoxy group. Optionally, R5 is selected from substituted or unsubstituted C1~C10 alkylene, substituted or unsubstituted C2~C10 alkenylene, substituted or unsubstituted C2~C10 alkynylene, R6, R7, R8 are each independently selected from substituted or unsubstituted C0~C10 alkylene, substituted or unsubstituted C2~C10 alkenylene, substituted or unsubstituted C2~C10 alkynylene, wherein the substituents are selected from halogen atoms.
[0189] Further optionally, in formula 6, R5 is selected from C1~C6 alkylene, C2~C6 alkenylene, C2~C6 alkynylene, optionally, R5 is selected from C2~C4 alkylene, C2~C4 alkenylene, C2~C4 alkynylene; in formula 7, R6, R7, R8 are each independently selected from C0~C6 alkylene, C2~C6 alkenylene, C2~C6 alkynylene, optionally, R6 is selected from C0~C1 alkylene, R7, R8 are each independently selected from C2~C4 alkylene, C2~C4 alkenylene, C2~C4 alkynylene.
[0190] In some embodiments, the nitrile compound is selected from one or more of ethanedinitrile, succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, octanedinitrile, azelaic acid dinitrile, decanedinitrile, undecane dinitrile, dodecane dinitrile, tetramethylsuccinonitrile, methylglutaronitrile, butene dinitrile, 2-pentene dinitrile, hex-2-enedinitrile, hex-3-enedinitrile, oct-4-enedinitrile, oct-4-ynedinitrile, 1,2,3-propanetricarbonitrile, 1,3,5-pentanetricarbonitrile, and 1,3,6-hexanetrinitrile.
[0191] Aromatic compounds
[0192] The aromatic compound can be selected from one or more of cyclohexylbenzene, fluorocyclohexylbenzene compounds (1-fluoro-2-cyclohexylbenzene, 1-fluoro-3-cyclohexylbenzene, 1-fluoro-4-cyclohexylbenzene), tert-butylbenzene, tert-amylbenzene, 1-fluoro-4-tert-butylbenzene, biphenyl, terphenyl (ortho-, meta-, para-), diphenyl ether, fluorobenzene, difluorobenzene (ortho-, meta-, para-), anisole, 2,4-difluoroanisole, and partial hydrogenation of terphenyl (1,2-dicyclohexylbenzene, 2-phenylbicyclohexyl, 1,2-diphenylcyclohexane, ortho-cyclohexylbiphenyl).
[0193] Optionally, the aromatic compound can be selected from one or more of biphenyl, terphenyl (ortho-, meta-, para-), fluorobenzene, cyclohexylbenzene, tert-butylbenzene, and tert-amylbenzene. Further optionally, the aromatic compound can be selected from one or more of biphenyl, ortho-terphenyl, fluorobenzene, cyclohexylbenzene, and tert-amylbenzene.
[0194] Phosphazene compounds
[0195] The phosphazene compound is preferably a cyclic phosphazene compound. The cyclic phosphazene compound can be selected from one or more of methoxypentafluorocyclotriphosphazene, ethoxypentafluorocyclotriphosphazene, phenoxypentafluorocyclotriphosphazene, and ethoxyheptafluorocyclotetraphosphazene.
[0196] Optionally, the cyclic phosphazene compound may be selected from one or more of methoxypentafluorocyclotriphosphazene, ethoxypentafluorocyclotriphosphazene, and phenoxypentafluorocyclotriphosphazene.
[0197] Further alternatively, the cyclic phosphazene compound may be selected from methoxypentafluorocyclotriphosphazene or ethoxypentafluorocyclotriphosphazene.
[0198] Acid anhydride compounds
[0199] The anhydride compound may be a chain anhydride or a cyclic anhydride. Specifically, the anhydride compound may be selected from one or more of acetic anhydride, propionic anhydride, succinic anhydride, maleic anhydride, 2-allylsuccinic anhydride, glutaric anhydride, itaconic anhydride, and 3-sulfo-propionic anhydride.
[0200] Optionally, the anhydride compound can be selected from one or more of succinic anhydride, maleic anhydride, and 2-allylsuccinic anhydride. Further optionally, the anhydride compound can be selected from one or two of succinic anhydride and 2-allylsuccinic anhydride.
[0201] Phosphite compounds
[0202] The phosphite compound may be selected from silane phosphite compounds, and specifically may be selected from one or more of the compounds shown in Formula 8. In Formula 8, R 31 , R 32 , R 33 , R 34 , R 35 , R 36 , R 37 , R 38 , R 39 Each is independently selected from halogen-substituted or unsubstituted C1-C6 alkyl.
[0203]
[0204] Optionally, the silane phosphite compound may be specifically selected from one or more of the following compounds, but the present application is not limited thereto:
[0205]
[0206] Phosphate compounds
[0207] The phosphate compound may be selected from silane phosphate compounds, and specifically may be selected from one or more of the compounds shown in Formula 9. In Formula 9, R 41 , R 42 , R 43 , R 44 , R 45 , R 46 , R 47 , R 48 , R 49 Each is independently selected from halogen-substituted or unsubstituted C1-C6 alkyl.
[0208]
[0209] Optionally, the silane phosphate compound may be specifically selected from one or more of the following compounds, but the present application is not limited thereto:
[0210]
[0211] Boric acid ester compounds
[0212] The borate compound may be selected from silane borate compounds, and specifically may be selected from one or more of the compounds shown in Formula 10. In Formula 10, R 51 , R 52 , R 53 , R 54 , R 55 , R 56 , R 57 , R 58 , R 59 Each is independently selected from halogen-substituted or unsubstituted C1-C6 alkyl.
[0213]
[0214] Optionally, the silane borate compound may be specifically selected from one or more of the following compounds, but the present application is not limited thereto:
[0215]
[0216] In addition, the non-aqueous electrolyte of the secondary battery of the present application also includes a lithium salt. The type of lithium salt is not particularly limited and can be selected according to actual needs. For example, the lithium salt can be selected from LiN(C x’ F 2x’+1 SO2)(C y’ F 2y ' +1 SO2), LiPF6, LiBF4, LiBOB, LiAsF6, Li(FSO2)2N, LiCF3SO3 and LiClO4, wherein x' and y' are natural numbers, such as independently 0, 1, 2, 3, 4, 5 or 6. In some embodiments, the concentration range of the lithium salt is 0.5 mol / L to 2.5 mol / L, preferably 0.8 mol / L to 2 mol / L.
[0217] [Positive electrode]
[0218] The positive electrode sheet generally includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0219] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0220] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0221] In the above-mentioned positive electrode active material having a core and a shell covering the core in the secondary battery of the present application, the main characteristic peak position in the XRD diagram of lithium manganese phosphate doped with A element and R element is consistent with that of undoped LiMnPO4, indicating that the doping process does not introduce an impurity phase. Therefore, the improvement in the core performance is mainly caused by element doping, rather than impurity phase. After preparing the above-mentioned positive electrode active material, the inventor of the present application cut the middle area of the prepared positive electrode active material particles by focused ion beam (FIB for short), and tested by transmission electron microscopy (TEM for short) and X-ray energy spectrum analysis (EDS for short) and found that the elements were evenly distributed without aggregation.
[0222] In an alternative embodiment, when A comprises one, two, three or four elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, A y Q n1 D n2 E n3 K n4 , wherein n1+n2+n3+n4=y, and n1, n2, n3, n4 are all positive numbers and not zero at the same time, Q, D, E, K are each independently selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and optionally, at least one of Q, D, E, K is Fe. Optionally, one of n1, n2, n3, n4 is zero, and the others are not zero; more optionally, two of n1, n2, n3, n4 are zero, and the others are not zero; further optionally, three of n1, n2, n3, n4 are zero, and the others are not zero. The kernel Li 1+x Mn 1-y A y P 1-z R zIn O4, it is advantageous to dope one, two, three or four of the above A elements at the manganese position, and optionally, one, two or three of the above A elements; in addition, it is advantageous to dope one or two R elements at the phosphorus position, which is conducive to uniform distribution of the doping elements.
[0223] The kernel Li 1+x Mn 1-y A y P 1-z R z In O4, the size of x is affected by the valence of A and R and the size of y and z to ensure that the entire system is electrically neutral. If the value of x is too small, the lithium content of the entire core system will be reduced, affecting the gram capacity of the material. The y value will limit the total amount of all doping elements. If y is too small, that is, the doping amount is too little, the doping element will not work. If y exceeds 0.5, the Mn content in the system will be less, affecting the voltage platform of the material. The R element is doped in the position of P. Since the PO tetrahedron is relatively stable, and the z value is too large, it will affect the stability of the material, so the z value is limited to 0.001-0.100.
[0224] Through process control (for example, fully mixing and grinding the materials of various sources), it is possible to ensure that each element is evenly distributed in the lattice without aggregation. The main characteristic peak position in the XRD diagram of lithium manganese phosphate doped with A element and R element is consistent with that of undoped LiMnPO4, indicating that the doping process does not introduce impurity phases. Therefore, the improvement in the core performance mainly comes from element doping, rather than impurity phases. After preparing the positive electrode active material described in this application, the inventors of the present application cut the middle area of the prepared positive electrode active material particles by focused ion beam (FIB for short), and tested by transmission electron microscopy (TEM for short) and X-ray energy spectrum analysis (EDS for short) and found that each element is evenly distributed without aggregation.
[0225] In the present application, crystalline means a crystallinity of more than 50%, i.e., 50%-100%. A crystallinity of less than 50% is called a glassy state. The crystallinity of the crystalline pyrophosphate and crystalline phosphate in the present application is 50% to 100%. Pyrophosphates and phosphates with a certain degree of crystallinity are not only conducive to giving full play to the pyrophosphate coating layer's ability to hinder the dissolution of manganese ions and the phosphate coating layer's excellent ability to conduct lithium ions and reduce interface side reactions, but also enable the pyrophosphate coating layer and the phosphate coating layer to better lattice match, thereby achieving a tighter combination of the coating layers.
[0226] In the present application, the crystallinity of the first coating layer material crystalline pyrophosphate and the second coating layer material crystalline phosphate of the positive electrode active material can be tested by conventional technical means in the art, such as density method, infrared spectroscopy, differential scanning calorimetry and nuclear magnetic resonance absorption method, and can also be tested by, for example, X-ray diffraction method.
[0227] A specific method for testing the crystallinity of the first coating layer crystalline pyrophosphate and the second coating layer crystalline phosphate of the positive electrode active material by X-ray diffraction method may include the following steps:
[0228] Take a certain amount of positive electrode active material powder and measure the total scattering intensity by X-ray. It is the sum of the scattering intensities of all matter in space and is only related to the intensity of the primary rays, the chemical structure of the positive electrode active material powder, and the total number of electrons participating in the diffraction, i.e. the mass, but has nothing to do with the order state of the sample. Then separate the crystalline scattering and non-crystalline scattering from the diffraction pattern, and the degree of crystallinity is the ratio of the scattering of the crystalline part to the total scattering intensity.
[0229] It should be noted that, in the present application, the crystallinity of the pyrophosphate and phosphate in the coating layer can be adjusted by, for example, adjusting the process conditions of the sintering process, such as the sintering temperature, the sintering time, and the like.
[0230] In the present application, since metal ions are difficult to migrate in pyrophosphate, pyrophosphate as the first coating layer can effectively isolate the doped metal ions from the electrolyte. The structure of crystalline pyrophosphate is stable, so crystalline pyrophosphate coating can effectively inhibit the dissolution of transition metals and improve cycle performance.
[0231] The bonding between the first coating layer and the core is similar to a heterojunction, and the strength of the bonding is limited by the degree of lattice matching. When the lattice mismatch is below 5%, the lattice matching is better, and the two are easy to bond tightly. Tight bonding can ensure that the coating will not fall off during subsequent cycles, which is beneficial to ensure the long-term stability of the material. The degree of bonding between the first coating layer and the core is mainly measured by calculating the mismatch between the core and each lattice constant of the coating. In the present application, after A and R elements are doped into the core, the matching degree between the core and the first coating layer is improved compared to undoped elements, and the core and the pyrophosphate coating layer can be more tightly bonded together.
[0232] The reason why crystalline phosphate is chosen as the second coating layer is, firstly, because it has a high lattice matching degree with the first coating material, crystalline pyrophosphate (the mismatch degree is only 3%); secondly, the stability of phosphate itself is better than that of pyrophosphate, and using it to coat pyrophosphate is beneficial to improve the stability of the material. The structure of crystalline phosphate is very stable, and it has excellent lithium ion conductivity. Therefore, the use of crystalline phosphate for coating can effectively reduce the interfacial side reactions on the surface of the positive electrode active material, thereby improving the high-temperature cycle and storage performance of the secondary battery. The lattice matching mode between the second coating layer and the first coating layer is similar to the bonding between the first coating layer and the core mentioned above. When the lattice mismatch is less than 5%, the lattice matching is better, and the two are easy to combine tightly.
[0233] The main reason for using carbon as the third layer is that the carbon layer has good electronic conductivity. Since electrochemical reactions occur when used in secondary batteries, the participation of electrons is required. Therefore, in order to increase the electron transfer between particles and the electron transfer at different positions on the particles, carbon with excellent conductive properties can be used to coat the positive electrode active material. Carbon coating can effectively improve the conductivity and desolvation ability of the positive electrode active material.
[0234] Each coating layer of the present application may be a complete coating or a partial coating.
[0235] In some embodiments, based on the weight of the inner core, the coating amount of the first coating layer is C1 weight %, C1 is greater than 0 and less than or equal to 6, optionally greater than 0 and less than or equal to 5.5, and more optionally greater than 0 and less than or equal to 2.
[0236] In any embodiment of the first aspect, based on the weight of the inner core, the coating amount of the second coating layer is C2 weight %, C2 is greater than 0 and less than or equal to 6, can be greater than 0 and less than or equal to 5.5, and can be more optionally 2-4.
[0237] In any embodiment of the first aspect, based on the weight of the inner core, the coating amount of the third coating layer is C3 weight %, C3 is greater than 0 and less than or equal to 6, can be greater than 0 and less than or equal to 5.5, and can be greater than 0 and less than or equal to 2.
[0238] In the positive electrode active material with a core-shell structure of the above embodiment, the coating amount of the three coating layers is preferably within the above range, thereby being able to fully coat the inner core and at the same time further improve the kinetic performance and safety performance of the secondary battery without sacrificing the gram capacity of the positive electrode active material.
[0239] For the first coating layer, by keeping the coating amount within the above range, the following situations can be avoided: too little coating amount means that the coating layer is thin and may not be able to effectively hinder the migration of transition metals; too much coating amount means that the coating layer is too thick, which will affect the migration of Li+ and further affect the rate performance of the material.
[0240] For the second coating layer, by keeping the coating amount within the above range, the following situations can be avoided: too much coating amount may affect the platform voltage of the entire material; too little coating amount may not achieve sufficient coating effect.
[0241] For the third coating layer, the carbon coating mainly plays the role of enhancing the electron transfer between particles. However, since the structure also contains a large amount of amorphous carbon, the carbon density is relatively low. Therefore, if the coating amount is too large, it will affect the compaction density of the electrode.
[0242] In the positive electrode active material with a core-shell structure of the above embodiment, the coating amount of the three coating layers is preferably within the above range, thereby being able to fully coat the inner core and at the same time further improve the kinetic performance and safety performance of the secondary battery without sacrificing the gram capacity of the positive electrode active material.
[0243] In any embodiment, the interplanar spacing of the crystalline pyrophosphate in the first coating layer is in the range of 0.293-0.470 nm, and the angle of the crystal orientation (111) is in the range of 18.00°-32.00°.
[0244] In any embodiment, the interplanar spacing of the crystalline phosphate in the second coating layer is in the range of 0.244-0.425 nm, and the angle of the crystal orientation (111) is in the range of 20.00°-37.00°.
[0245] The crystalline pyrophosphate and crystalline phosphate in the coating layer can be characterized by conventional techniques in the art, or by transmission electron microscopy (TEM). Under TEM, the core and the coating layer can be distinguished by testing the interplanar spacing.
[0246] The specific test method for the interplanar spacing and angle of the crystalline pyrophosphate and crystalline phosphate in the coating layer may include the following steps:
[0247] Take a certain amount of coated positive electrode active material sample powder in a test tube, inject a solvent such as alcohol into the test tube, and then stir and disperse it thoroughly. Then use a clean disposable plastic pipette to take an appropriate amount of the above solution and drop it on a 300-mesh copper grid. At this time, some powder will remain on the copper grid. Transfer the copper grid and the sample to the TEM sample chamber for testing, obtain the original TEM test image, and save the original image.
[0248] The original image obtained by the above TEM test is opened in the diffractometer software and Fourier transformed to obtain the diffraction pattern. The distance from the diffraction spot to the center position in the diffraction pattern is measured to obtain the crystal plane spacing, and the angle is calculated according to the Bragg equation.
[0249] The difference between the interplanar spacing range of crystalline pyrophosphate and the existence of crystalline phosphate can be directly judged by the value of the interplanar spacing.
[0250] The first coating layer and the second coating layer in the positive electrode active material of the above embodiment both use crystalline materials, and their interplanar spacing and angle ranges are within the above ranges. As a result, the impurity phase in the coating layer can be effectively avoided, thereby improving the gram capacity, cycle performance and rate performance of the material. Moreover, the crystalline pyrophosphate and crystalline phosphate within the above interplanar spacing and angle ranges can more effectively inhibit the lattice change rate and manganese ion dissolution of lithium manganese phosphate during lithium insertion and extraction, thereby improving the high temperature cycle performance, cycle stability and high temperature storage performance of the secondary battery.
[0251] In some embodiments, in the core, the ratio of y to 1-y is 1:10 to 1:1, and optionally 1:4 to 1:1. When the above conditions are met, the energy density and cycle performance of a secondary battery using the positive electrode active material can be further improved.
[0252] In some embodiments, in the core, the ratio of z to 1-z is 1:999 to 1:9, optionally 1:499 to 1:249. Here, z represents the sum of the stoichiometric numbers of the P-site doping elements R. When the above conditions are met, the energy density and cycle performance of the secondary battery using the positive electrode active material can be further improved.
[0253] In some embodiments, the carbon of the third coating layer is a mixture of SP2 carbon and SP3 carbon. Optionally, the molar ratio of SP2 carbon to SP3 carbon is any value in the range of 0.1-10, and can be any value in the range of 2.0-3.0.
[0254] In some embodiments, the molar ratio of SP2 carbon to SP3 carbon may be about 0.1, about 0.2, about 0.3, about 0.4, about 0.5, about 0.6, about 0.7, about 0.8, about 0.9, about 1, about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9, or about 10, or any range of any of the above values.
[0255] In the present application, "about" a certain numerical value indicates a range, which means a range of ±10% of the numerical value.
[0256] By selecting the form of carbon in the carbon coating layer, the comprehensive electrical performance of the secondary battery is improved. Specifically, by using a mixed form of SP2 carbon and SP3 carbon and limiting the ratio of SP2 carbon to SP3 carbon within a certain range, the following situations can be avoided: if the carbon in the coating layer is all amorphous SP3, the conductivity is poor; if it is all graphitized SP2, although the conductivity is good, there are few lithium ion pathways, which is not conducive to lithium deintercalation. In addition, limiting the molar ratio of SP2 carbon to SP3 carbon within the above range can achieve good conductivity and ensure the passage of lithium ions, which is beneficial to the optimization of secondary battery functions and the improvement of their cycle performance.
[0257] The mixing ratio of the SP2 form and the SP3 form of the third coating layer carbon can be controlled by sintering conditions such as sintering temperature and sintering time. For example, when using sucrose as a carbon source to prepare the third coating layer, after sucrose is cracked at high temperature, it is deposited on the second coating layer and at high temperature, a carbon coating layer having both SP3 form and SP2 form is produced. The ratio of SP2 form carbon and SP3 form carbon can be regulated by selecting high temperature cracking conditions and sintering conditions.
[0258] The structure and characteristics of the third coating layer carbon can be measured by Raman spectroscopy. The specific test method is as follows: by decomposing the energy spectrum of the Raman test, Id / Ig is obtained (where Id is the peak intensity of SP3 form carbon, and Ig is the peak intensity of SP2 form carbon), thereby confirming the molar ratio of the two.
[0259] In some embodiments, the first cladding layer has a thickness of 1-10 nm; and / or the second cladding layer has a thickness of 2-15 nm; and / or the third cladding layer has a thickness of 2-25 nm.
[0260] In some embodiments, the thickness of the first coating layer can be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, or about 10 nm, or any range thereof.
[0261] In some embodiments, the thickness of the second coating layer may be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, about 10 nm, about 11 nm, about 12 nm, about 13 nm, about 14 nm, about 15 nm, or within any range of any of the above values.
[0262] In some embodiments, the thickness of the third coating layer may be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, about 10 nm, about 11 nm, about 12 nm, about 13 nm, about 14 nm, about 15 nm, about 16 nm, about 17 nm, about 18 nm, about 19 nm, about 20 nm, about 21 nm, about 22 nm, about 23 nm, about 24 nm or about 25 nm, or within any range of any of the above values.
[0263] When the thickness of the first coating layer is in the range of 1-10 nm, it is possible to avoid the adverse effect on the dynamic properties of the material that may be caused when it is too thick, and it is possible to avoid the problem that the migration of transition metal ions may not be effectively hindered when it is too thin.
[0264] When the thickness of the second coating layer is within the range of 2-15 nm, the surface structure of the second coating layer is stable and the side reaction with the electrolyte is small, so the interface side reaction can be more effectively reduced, thereby further improving the high temperature performance of the secondary battery.
[0265] When the thickness of the third coating layer is in the range of 2-25 nm, the electrical conductivity of the material can be further improved and the compression performance of the battery pole piece prepared using the positive electrode active material can be better improved.
[0266] The thickness test of the coating layer is mainly carried out by FIB. The specific method may include the following steps: randomly select a single particle from the positive electrode active material powder to be tested, cut a thin slice with a thickness of about 100nm from the middle position or near the middle position of the selected particle, and then perform TEM test on the thin slice to measure the thickness of the coating layer, measure 3-5 positions, and take the average value.
[0267] In some embodiments, based on the weight of the positive electrode active material, the manganese content is in the range of 10 wt%-35 wt%, optionally in the range of 15 wt%-30 wt%, and more optionally in the range of 17 wt%-20 wt%, the phosphorus content is in the range of 12 wt%-25 wt%, optionally in the range of 15 wt%-20 wt%, and the weight ratio of manganese to phosphorus is in the range of 0.90-1.25, and optionally in the range of 0.95-1.20.
[0268] In the present application, in the case where manganese is contained only in the core of the positive electrode active material, the content of manganese may correspond to the content of the core.
[0269] In the above embodiment, limiting the content of manganese element within the above range can effectively avoid problems such as poor material structure stability and decreased density that may be caused by excessive manganese content, thereby effectively improving the cycle, storage and compaction performance of the secondary battery; and can avoid problems such as low voltage platform that may be caused by too low manganese content, thereby further improving the energy density of the secondary battery.
[0270] In the above embodiment, limiting the content of phosphorus within the above range can effectively avoid the following situations: if the content of phosphorus is too high, the covalency of PO may be too strong and affect the conductivity of small polarons, thereby affecting the electrical conductivity of the material; if the phosphorus content is too low, the stability of the pyrophosphate lattice structure in the core, the first coating layer and / or the phosphate in the second coating layer may be reduced, thereby affecting the overall stability of the material.
[0271] The weight ratio of manganese to phosphorus has the following effects on the performance of secondary batteries: if the weight ratio is too large, it means that there is too much manganese, and the dissolution of manganese ions increases, affecting the stability and gram capacity of the positive electrode active material, and thus affecting the cycle performance and storage performance of the secondary battery; if the weight ratio is too small, it means that there is too much phosphorus, which is easy to form an impurity phase, which will reduce the discharge voltage platform of the material, thereby reducing the energy density of the secondary battery.
[0272] The measurement of manganese and phosphorus can be carried out by conventional technical means in the art. In particular, the following method is used to determine the content of manganese and phosphorus: the material is dissolved in dilute hydrochloric acid (concentration 10-30%), the content of each element in the solution is tested by ICP, and then the content of manganese is measured and converted to obtain its weight percentage.
[0273] In some embodiments, the lattice change rate of the positive electrode active material having a core-shell structure before and after complete lithium deintercalation is 4% or less, optionally 3.8% or less, and more optionally 2.0-3.8%.
[0274] The lithium insertion and extraction process of lithium manganese phosphate (LiMnPO4) is a two-phase reaction. The interfacial stress of the two phases is determined by the lattice change rate before and after lithium insertion and extraction. The smaller the lattice change rate, the smaller the interfacial stress, and the easier the Li+ transmission. Therefore, reducing the lattice change rate of the inner core will help enhance the transmission capacity of Li+, thereby improving the rate performance of the secondary battery. The positive electrode active material with a core-shell structure of the above-mentioned embodiment can achieve a lattice change rate before and after lithium insertion and extraction of less than 4%, so the use of the positive electrode active material can improve the rate performance of the secondary battery. The lattice change rate can be measured by methods known in the art, such as X-ray diffraction patterns (XRD).
[0275] In some embodiments, the Li / Mn antisite defect concentration of the positive electrode active material having a core-shell structure is 4% or less, optionally 2.2% or less, and more optionally 1.5-2.2%.
[0276] The Li / Mn antisite defect in this application refers to the LiMnPO4 lattice. + With Mn 2+ The positions of Li / Mn are interchanged. Correspondingly, the Li / Mn antisite defect concentration refers to the concentration of Li / Mn antisite defect with Mn 2+ Li exchange + Occupy + In the present application, the Li / Mn antisite defect concentration can be measured according to JIS K 0131-1996, for example.
[0277] The core-shell structured positive electrode active material of the above embodiment can achieve the above-mentioned low Li / Mn antisite defect concentration. Although the mechanism is not yet clear, the inventors of the present application speculate that due to the LiMnPO4 lattice, Li + With Mn 2+ There will be a position swap, and Li + The transmission channel is a one-dimensional channel, so Mn 2+ In Li + It will be difficult to migrate in the channel, thus hindering Li + Therefore, the positive electrode active material with a core-shell structure described in the present application can avoid Mn due to the low concentration of Li / Mn antisite defects within the above range. 2+ Obstacles + transmission, while improving the gram capacity and rate performance of the positive electrode active material.
[0278] In some embodiments, the compaction density of the positive electrode active material at 3T is 2.2 g / cm 3 Above, optionally 2.2 g / cm 3 Above and 2.8g / cm 3 The higher the compaction density, the greater the weight of the active material per unit volume, so increasing the compaction density is beneficial to increasing the volume energy density of the battery cell. The compaction density can be measured according to GB / T24533-2009.
[0279] In some embodiments, the surface oxygen valence state of the positive electrode active material having a core-shell structure is -1.90 to -1.98. The stable valence state of oxygen is -2. The closer the valence state is to -2, the stronger its electron-acquiring ability is, that is, the stronger its oxidizing property is. Under normal circumstances, its surface valence state is below -1.7. The above embodiment can reduce the interfacial side reactions between the positive electrode material and the electrolyte by limiting the surface oxygen valence state of the positive electrode active material to the above range as described above, thereby improving the cycle of the battery cell, high-temperature storage gas production and other performances.
[0280] The present application also provides a method for preparing a positive electrode active material, comprising the following steps:
[0281] Step of providing a core material: the core chemical formula is Li 1+x Mn 1-y A y P 1-z R z O4, wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, z is any value in the range of 0.001-0.100, the A comprises one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be one or more elements selected from Fe, Ti, V, Ni, Co and Mg, the R comprises one or more elements selected from B, Si, N and S, and can be one element selected from B, Si, N and S;
[0282] Coating step: provide LiaMP2O7 and / or Mb(P2O7) respectively c and XPO4 suspension, adding the core material to the suspension and mixing, and sintering to obtain a positive electrode active material, wherein 0≤a≤2, 1≤b≤4, 1≤c≤6, and the values of a, b and c satisfy the following conditions: making the crystalline pyrophosphate LiaMP2O7 or Mb(P2O7) c Maintain electrical neutrality; M each independently includes one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al; X includes one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al;
[0283] The positive electrode active material has a core-shell structure, which includes the core and a shell covering the core, the shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer, the first coating layer includes crystalline pyrophosphate LiaMP2O7 and / or Mb(P2O7)c , the second coating layer includes crystalline phosphate XPO4, and the third coating layer includes carbon.
[0284] In some embodiments, the step of providing a core material comprises the following steps:
[0285] Step (1): mixing a manganese source, a dopant of element A and an acid in a container and stirring to obtain manganese salt particles doped with element A;
[0286] Step (2): mixing the manganese salt particles doped with element A with a lithium source, a phosphorus source and a dopant of element R in a solvent to obtain a slurry, and sintering the slurry under the protection of an inert gas atmosphere to obtain a core doped with element A and element R, wherein the core doped with element A and element R is Li 1+x Mn 1-y A y P 1-z R z O4, wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, z is any value in the range of 0.001-0.100, the A includes one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be one or more elements selected from Fe, Ti, V, Ni, Co and Mg, the R includes one or more elements selected from B, Si, N and S, and can be selected from B, Si, N and S.
[0287] The preparation method of the present application has no particular restrictions on the source of materials. The source of a certain element may include one or more of the element's simple substance, sulfate, halide, nitrate, organic acid salt, oxide or hydroxide. The precursor is the source that can achieve the purpose of the preparation method of the present application.
[0288] In some embodiments, the dopant of element A includes one or more of the single substance, carbonate, sulfate, chloride, nitrate, organic acid salt, oxide, and hydroxide of one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge.
[0289] In some embodiments, the dopant of the element R comprises one or more of an inorganic acid, a subacid, an organic acid, a sulfate, a chloride, a nitrate, an organic acid salt, an oxide, and a hydroxide of one or more elements selected from B, Si, N, and S;
[0290] In the present application, the manganese source may be a manganese-containing substance known in the art that can be used to prepare lithium manganese phosphate. As an example, the manganese source may be one or more selected from elemental manganese, manganese dioxide, manganese phosphate, manganese oxalate, and manganese carbonate.
[0291] In the present application, the acid may be one or more selected from organic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, silicic acid, silicic acid, and organic acids such as oxalic acid. In some embodiments, the acid is a dilute organic acid with a concentration of 60 wt % or less.
[0292] In the present application, the lithium source may be a lithium-containing substance known in the art that can be used to prepare lithium manganese phosphate. As an example, the lithium source is one or more selected from lithium carbonate, lithium hydroxide, lithium phosphate, and lithium dihydrogen phosphate.
[0293] In the present application, the phosphorus source may be a phosphorus-containing substance known in the art that can be used to prepare lithium manganese phosphate. As an example, the phosphorus source is one or more selected from diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate and phosphoric acid.
[0294] In some optional embodiments, after the manganese source, the dopant of element A and the acid react in a solvent to obtain a manganese salt suspension doped with element A, the suspension is filtered, dried, and sand-milled to obtain manganese salt particles doped with element A having a particle size of 50-200 nm.
[0295] In some optional embodiments, the slurry in step (2) is dried to obtain a powder, and then the powder is sintered to obtain a core doped with element A and element R.
[0296] In some embodiments, the step (1) is mixed at a temperature of 20-120° C., optionally 40-120° C.; and / or
[0297] The stirring in step (1) is carried out at 400-700 rpm for 1-9 hours, optionally for 3-7 hours.
[0298] Optionally, the reaction temperature in step (1) can be carried out at about 30°C, about 50°C, about 60°C, about 70°C, about 80°C, about 90°C, about 100°C, about 110°C or about 120°C; the stirring in step (1) can be carried out for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours or about 9 hours; optionally, the reaction temperature and stirring time in step (1) can be in any range of the above-mentioned arbitrary values.
[0299] In some embodiments, the step (2) is mixed at a temperature of 20-120° C., optionally 40-120° C. for 1-12 hours. Optionally, the reaction temperature in the step (2) can be about 30° C., about 50° C., about 60° C., about 70° C., about 80° C., about 90° C., about 100° C., about 110° C., or about 120° C.; the mixing in the step (2) is carried out for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, about 10 hours, about 11 hours, or about 12 hours; optionally, the reaction temperature and mixing time in the step (2) can be in any range of the above-mentioned arbitrary values.
[0300] When the temperature and time during the preparation of the core particles are within the above range, the core obtained and the positive electrode active material prepared therefrom have fewer lattice defects, which is beneficial to inhibiting the dissolution of manganese ions and reducing the interfacial side reactions between the positive electrode active material and the electrolyte, thereby improving the cycle performance and safety performance of the secondary battery.
[0301] In some embodiments, optionally, in the process of preparing the diluted acid manganese particles doped with A element and R element, the pH of the solution is controlled to be 3.5-6, optionally, the pH of the solution is controlled to be 4-6, and more optionally, the pH of the solution is controlled to be 4-5. It should be noted that in the present application, the pH of the obtained mixture can be adjusted by methods commonly used in the art, for example, by adding acid or alkali.
[0302] In some embodiments, optionally, in step (2), the molar ratio of the manganese salt particles to the lithium source and the phosphorus source is 1:0.5-2.1:0.5-2.1, and more optionally, the molar ratio of the manganese salt particles doped with element A to the lithium source and the phosphorus source is about 1:1:1.
[0303] In some embodiments, optionally, the sintering conditions in the process of preparing lithium manganese phosphate doped with A element and R element are: sintering at 600-950°C for 4-10 hours in an inert gas or a mixed atmosphere of inert gas and hydrogen; optionally, the sintering can be sintered at about 650°C, about 700°C, about 750°C, about 800°C, about 850°C or about 900°C for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours or about 10 hours; optionally, the sintering temperature and sintering time can be within any range of the above-mentioned any numerical values. In the process of preparing lithium manganese phosphate doped with A elements and R elements, when the sintering temperature is too low and the sintering time is too short, the crystallinity of the material core will be low, which will affect the overall performance. When the sintering temperature is too high, impurities will easily appear in the material core, thus affecting the overall performance. When the sintering time is too long, the particles in the material core will be larger, thus affecting the gram capacity, compaction density and rate performance.
[0304] In some optional embodiments, optionally, the protective atmosphere is a mixed gas of 70-90 volume % nitrogen and 10-30 volume % hydrogen.
[0305] In some embodiments, the coating step comprises:
[0306] The first coating step: dissolving the source of element M, the phosphorus source and the acid and optionally the lithium source in a solvent to obtain a first coating layer suspension; fully mixing the core obtained in the core step with the first coating layer suspension obtained in the first coating step, drying, and then sintering to obtain a material coated with the first coating layer;
[0307] The second coating step: dissolving the source of element X, the phosphorus source and the acid in a solvent to obtain a second coating layer suspension; fully mixing the first coating layer-coated material obtained in the first coating step with the second coating layer suspension obtained in the second coating step, drying, and then sintering to obtain a material coated with two coating layers;
[0308] The third coating step: dissolving the carbon source in a solvent and fully dissolving it to obtain a third coating layer solution; then adding the two-layer coating material obtained in the second coating step to the third coating layer solution, mixing evenly, drying, and then sintering to obtain a three-layer coating material, i.e., a positive electrode active material.
[0309] In some embodiments, the source of the element M includes one or more of the elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al, each of which is a single substance, carbonate, sulfate, chloride, nitrate, organic acid salt, oxide, and hydroxide.
[0310] In some embodiments, the source of the element X includes one or more of a single substance, carbonate, sulfate, chloride, nitrate, organic acid salt, oxide, and hydroxide of one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, or Al.
[0311] The amount of each source of the elements A, R, M, and X added depends on the target doping amount, and the ratio of the amount of the lithium source, the manganese source, and the phosphorus source conforms to the stoichiometric ratio.
[0312] As an example, the carbon source is one or more selected from starch, sucrose, glucose, polyvinyl alcohol, polyethylene glycol, and citric acid.
[0313] In some embodiments, in the first coating step, the pH of the solution containing the source of element M, the phosphorus source and the acid, and optionally the lithium source, is controlled to be 3.5-6.5, and then stirred and reacted for 1-5 hours, and then the solution is heated to 50-120°C and maintained at this temperature for 2-10 hours, and / or sintered at 650-800°C for 2-6 hours.
[0314] Optionally, in the first coating step, the reaction is fully carried out. Optionally, in the first coating step, the reaction is carried out for about 1.5 hours, about 2 hours, about 3 hours, about 4 hours, about 4.5 hours or about 5 hours. Optionally, in the first coating step, the reaction time of the reaction can be within any range of the above-mentioned arbitrary values.
[0315] Optionally, in the first coating step, the pH of the solution is controlled to be 4-6. Optionally, in the first coating step, the solution is heated to about 55°C, about 60°C, about 70°C, about 80°C, about 90°C, about 100°C, about 110°C or about 120°C, and maintained at this temperature for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours or about 10 hours; Optionally, in the first coating step, the temperature of the heating and the holding time can be in any range of any of the above values.
[0316] Optionally, in the first coating step, the sintering may be performed at about 650°C, about 700°C, about 750°C, or about 800°C for about 2 hours, about 3 hours, about 4 hours, about 5 hours, or about 6 hours; optionally, the sintering temperature and sintering time may be within any range of the above-mentioned values.
[0317] In the first coating step, by controlling the sintering temperature and time within the above range, the following situations can be avoided: when the sintering temperature in the first coating step is too low and the sintering time is too short, the first coating layer will have low crystallinity and more amorphous substances, which will lead to a decrease in the effect of inhibiting metal dissolution, thereby affecting the cycle performance and high-temperature storage performance of the secondary battery; when the sintering temperature is too high, the first coating layer will contain impurities, which will also affect its effect of inhibiting metal dissolution, thereby affecting the cycle and high-temperature storage performance of the secondary battery; when the sintering time is too long, the thickness of the first coating layer will increase, affecting the migration of Li+, thereby affecting the material's gram capacity and rate performance, etc.
[0318] In some embodiments, in the second coating step, the source of element X, the phosphorus source and the acid are dissolved in a solvent, stirred and reacted for 1-10 hours, and then the solution is heated to 60-150° C. and maintained at this temperature for 2-10 hours, and / or sintered at 500-700° C. for 6-10 hours.
[0319] Optionally, in the second coating step, the reaction is fully carried out. Optionally, in the second coating step, the reaction is carried out for about 1.5 hours, about 2 hours, about 3 hours, about 4 hours, about 4.5 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours or about 10 hours. Optionally, in the second coating step, the reaction time of the reaction can be in any range of the above arbitrary numerical values.
[0320] Optionally, in the second coating step, the solution is heated to about 65°C, about 70°C, about 80°C, about 90°C, about 100°C, about 110°C, about 120°C, about 130°C, about 140°C or about 150°C, and maintained at this temperature for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours or about 10 hours; optionally, in the second coating step, the heated temperature and the holding time may be within any range of any of the above values.
[0321] In the step of providing the core material and the first coating step and the second coating step, before sintering, that is, in the preparation of the core material for chemical reaction (steps (1)-(2)) and in the preparation of the first coating layer suspension and the second coating layer suspension, by selecting appropriate reaction temperature and reaction time as described above, the following situations can be avoided: when the reaction temperature is too low, the reaction cannot occur or the reaction rate is slow; when the temperature is too high, the product decomposes or forms a mixed phase; when the reaction time is too long, the product particle size is large, which may increase the time and difficulty of subsequent processes; when the reaction time is too short, the reaction is incomplete and the obtained product is small.
[0322] Optionally, in the second coating step, the sintering may be performed at about 550°C, about 600°C or about 700°C for about 6 hours, about 7 hours, about 8 hours, about 9 hours or about 10 hours; optionally, the sintering temperature and sintering time may be within any range of the above-mentioned values.
[0323] In the second coating step, by controlling the sintering temperature and time within the above range, the following situations can be avoided: when the sintering temperature in the second coating step is too low and the sintering time is too short, the second coating layer will have low crystallinity and more amorphous state, and the performance of reducing the surface reaction activity of the material will be reduced, thereby affecting the circulation and high-temperature storage performance of the secondary battery; when the sintering temperature is too high, the second coating layer will have impurities, which will also affect its effect of reducing the surface reaction activity of the material, thereby affecting the circulation and high-temperature storage performance of the secondary battery; when the sintering time is too long, the thickness of the second coating layer will increase, affecting the voltage platform of the material, thereby reducing the energy density of the material, etc.
[0324] In some embodiments, the sintering in the third coating step is performed at 700-800° C. for 6-10 hours. Alternatively, in the third coating step, the sintering may be performed at about 700° C., about 750° C., or about 800° C. for about 6 hours, about 7 hours, about 8 hours, about 9 hours, or about 10 hours; alternatively, the sintering temperature and sintering time may be within any range of the above values.
[0325] In the third coating step, by controlling the sintering temperature and time within the above range, the following situations can be avoided: when the sintering temperature in the third coating step is too low, the degree of graphitization of the third coating layer will decrease, affecting its conductivity, thereby affecting the specific capacity of the material; when the sintering temperature is too high, the degree of graphitization of the third coating layer will be too high, affecting the transmission of Li+, thereby affecting the specific capacity of the material, etc.; when the sintering time is too short, the coating layer will be too thin, affecting its conductivity, thereby affecting the specific capacity of the material; when the sintering time is too long, the coating layer will be too thick, affecting the compaction density of the material, etc.
[0326] In the above-mentioned first coating step, second coating step and third coating step, the drying is carried out at a drying temperature of 100°C to 200°C, optionally 110°C to 190°C, more optionally 120°C to 180°C, even more optionally 120°C to 170°C, most optionally 120°C to 160°C, and the drying time is 3-9 hours, optionally 4-8 hours, more optionally 5-7 hours, and most optionally about 6 hours.
[0327] The positive electrode active material prepared by the preparation method of the positive electrode active material described in the present application has a secondary battery prepared therefrom, and the dissolution amount of Mn and Mn-doped elements is reduced after cycling, and the high temperature stability, high temperature cycle performance and rate performance are improved. In addition, the raw material source is wide, the cost is low, the process is simple, and it is conducive to industrialization.
[0328] In some embodiments, the positive electrode active material may adopt other positive electrode active materials for batteries that are well known in the art. As an example, other positive electrode active materials may also include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0329] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0330] In some embodiments, the positive electrode film layer may further include a conductive agent, for example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0331] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0332] [Negative electrode]
[0333] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0334] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0335] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0336] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0337] In some embodiments, the negative electrode film layer may further include a binder. As an example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0338] In some embodiments, the negative electrode film layer may further include a conductive agent. As an example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0339] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0340] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0341] [Isolation film]
[0342] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0343] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0344] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0345] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0346] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0347] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.
[0348] In some embodiments, reference Figure 2 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0349] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.
[0350] Figure 3 4 is an example of a battery module. Figure 3 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.
[0351] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0352] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0353] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and 5 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0354] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0355] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.
[0356] Figure 6The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.
[0357] [Example]
[0358] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0359] Wherein, the first solvent is selected from the following solvents:
[0360]
[0361] The first additive is selected from the following compounds:
[0362]
[0363] I. Battery Preparation
[0364] Embodiment 1:
[0365] Step 1: Preparation of positive electrode active materials
[0366] Step S1: Preparation of Fe, Co, V and S co-doped manganese oxalate
[0367] 689.6g of manganese carbonate, 455.27g of ferrous carbonate, 4.65g of cobalt sulfate, and 4.87g of vanadium dichloride were added to a mixer and mixed thoroughly for 6h. The obtained mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added, heated to 80°C, and stirred at a speed of 500rpm for 6h, mixed evenly, until the reaction was terminated and no bubbles were generated, to obtain a Fe, Co, and V co-doped manganese oxalate suspension. The suspension was then filtered, dried at 120°C, and sand-milled to obtain manganese oxalate particles with a particle size of 100nm.
[0368] Step S2: Preparation of inner core Li 0.997 Mn 0.60 Fe 0.393 V 0.004 Co 0.003 P 0.997 S 0.003 O4
[0369] Take 1793.1g of manganese oxalate prepared in (1), 368.3g of lithium carbonate, 1146.6g of ammonium dihydrogen phosphate and 4.9g of dilute sulfuric acid, add them to 20L of deionized water, stir them thoroughly, and evenly mix and react at 80°C for 10h to obtain a slurry. The slurry is transferred to a spray drying device for spray drying and granulation, and dried at a temperature of 250°C to obtain a powder. In a protective atmosphere (90% nitrogen and 10% hydrogen), the powder is sintered in a roller kiln at 700°C for 4h to obtain the above-mentioned core material.
[0370] Step S3: Preparation of the first coating layer suspension
[0371] To prepare Li2FeP2O7 solution, 7.4 g lithium carbonate, 11.6 g ferrous carbonate, 23.0 g ammonium dihydrogen phosphate and 12.6 g oxalic acid dihydrate were dissolved in 500 mL deionized water, the pH was controlled to 5, and then stirred and reacted at room temperature for 2 h to obtain a solution, and then the solution was heated to 80 ° C and maintained at this temperature for 4 h to obtain a first coating layer suspension.
[0372] Step S4: Coating of the first coating layer
[0373] The doped 1571.9 g lithium manganese phosphate core material obtained in step S2 was added to the first coating layer suspension (coating material content was 15.7 g) obtained in step S3, and the mixture was stirred and mixed for 6 h. After mixing evenly, the mixture was transferred to a 120° C. oven and dried for 6 h, and then sintered at 650° C. for 6 h to obtain the pyrophosphate-coated material.
[0374] Step S5: Preparation of the second coating layer suspension
[0375] 3.7 g of lithium carbonate, 11.6 g of ferrous carbonate, 11.5 g of ammonium dihydrogen phosphate and 12.6 g of oxalic acid dihydrate were dissolved in 1500 mL of deionized water, and then stirred and reacted for 6 hours to obtain a solution, and then the solution was heated to 120° C. and maintained at this temperature for 6 hours to obtain a second coating layer suspension.
[0376] Step S6: Coating of the second coating layer
[0377] 1586.8 g of the pyrophosphate-coated material obtained in step S4 was added to the second coating layer suspension (coating material content was 47.1 g) obtained in step S5, and the mixture was stirred and mixed for 6 hours. After mixing evenly, the mixture was transferred to a 120°C oven and dried for 6 hours, and then sintered at 700°C for 8 hours to obtain a two-layer coated material.
[0378] Step S7: Preparation of the third coating layer aqueous solution
[0379] 37.3 g of sucrose was dissolved in 500 g of deionized water, and then stirred and fully dissolved to obtain a sucrose aqueous solution.
[0380] Step S8: Coating of the third coating layer
[0381] 1633.9 g of the two-layer coated material obtained in step S6 was added to the sucrose solution obtained in step S7, and stirred and mixed together for 6 hours. After mixing evenly, it was transferred to a 150°C oven for drying for 6 hours, and then sintered at 700°C for 10 hours to obtain a three-layer coated material.
[0382] Step 2: Preparation of positive electrode
[0383] The three-layer coated positive electrode active material, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) prepared above were added to N-methylpyrrolidone (NMP) at a weight ratio of 97.0:1.2:1.8, and stirred to mix evenly to obtain positive electrode slurry. Then, the positive electrode slurry was heated to 0.280 g / 1540.25 mm 2 It is evenly coated on aluminum foil, dried, cold pressed and cut to obtain the positive electrode sheet.
[0384] Step 3: Preparation of negative electrode
[0385] The negative electrode active material artificial graphite, hard carbon, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) were dissolved in solvent deionized water at a weight ratio of 90:5:2:2:1, and stirred and mixed to prepare the negative electrode slurry. The negative electrode slurry was evenly coated on the negative electrode current collector copper foil at 0.117g / 1540.25mm2, and the negative electrode sheet was obtained after drying, cold pressing, and slitting.
[0386] Step 4: Preparation of electrolyte
[0387] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), solvent 1 was used as the first solvent, a mixed solution of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) in a volume ratio of 3 / 7 was used as the second solvent, additive 1 was used as the first additive, and LiPF6 was used as the lithium salt. The first solvent, the second solvent, the first additive and the lithium salt constituted an electrolyte, the mass ratio of the first solvent to the second solvent was 1:1, and based on the total mass of the electrolyte, the mass content of the first additive was 3%, and the mass content of the lithium salt was 12.5%.
[0388] Step 5: Preparation of isolation membrane
[0389] A commercially available PP-PE copolymer microporous film (from Zhuogao Electronic Technology Co., Ltd., Model 20) with a thickness of 20 μm and an average pore size of 80 nm was used.
[0390] Step 6: Preparation of the full battery
[0391] The positive electrode sheet, separator, and negative electrode sheet obtained above are stacked in order, with the separator placed between the positive and negative electrodes to play a role of isolation, and then wound to obtain a bare cell. The bare cell is placed in an outer package, injected with the above electrolyte and packaged to obtain a full battery (hereinafter also referred to as "full battery").
[0392] [Preparation of button cell]
[0393] The positive electrode active material, polyvinylidene fluoride (PVDF) and acetylene black prepared above were added to N-methylpyrrolidone (NMP) at a weight ratio of 90:5:5, and stirred in a drying room to form a slurry. The slurry was coated on aluminum foil, dried, and cold pressed to form a positive electrode sheet. The coating amount was 0.2g / cm2 and the compaction density was 2.0g / cm3.
[0394] A lithium sheet is used as the negative electrode, solvent 1 is used as the first solvent, a mixed solution of ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1 is used as the second solvent, additive 1 is used as the first additive, and LiPF6 is used as the lithium salt. The first solvent, the second solvent, the first additive and the lithium salt form an electrolyte, the mass ratio of the first solvent to the second solvent is 1:1, and the mass content of the first additive is 3% and the mass content of the lithium salt is 1 mol / L based on the total mass of the electrolyte. Together with the positive electrode sheet prepared above, it is assembled into a button battery (hereinafter also referred to as "button battery") in a button box.
[0395] Examples 2 to 27 and Comparative Examples 1 to 19
[0396] The positive electrode active materials and batteries in Examples 2 to 27 and Comparative Examples 1 to 19 were prepared in a manner similar to Example 1. The differences in the preparation of the positive electrode active materials are shown in Tables 1-6, wherein Comparative Examples 1-2, 4-10 and 12 were not coated with the first layer, and therefore did not have steps S3 and S4; Comparative Example 1-11 was not coated with the second layer, and therefore did not have steps S5-S6.
[0397] Note: In all embodiments and comparative examples of the present application, if not specified, the first coating layer material and / or the second coating layer material used are assumed to be crystalline.
[0398] Table 1: Raw materials for preparation of kernel
[0399]
[0400]
[0401]
[0402]
[0403]
[0404] Table 2: Preparation of the first coating layer suspension (step S3)
[0405]
[0406] Table 3: Coating of the first coating layer (step S4)
[0407]
[0408]
[0409] Table 4: Preparation of the second coating layer suspension (step S5)
[0410]
[0411] Table 5: Coating of the second coating layer (step S6)
[0412]
[0413]
[0414] Table 6: Coating of the third coating layer (step S8)
[0415]
[0416]
[0417]
[0418] Examples 30-42: Investigation of other coating materials
[0419] Examples 30-42 were carried out in a manner similar to that of Example 1, except for the differences shown in Tables 7-9 below.
[0420] Table 7: Investigation of the first coating layer material
[0421]
[0422] Table 8: Investigation of the second coating layer material
[0423] serial number Second coating material Preparation of the second coating layer suspension Embodiment 37 <![CDATA[Cu3(PO4)2]]> 48.0g copper sulfate; 23.0g ammonium dihydrogen phosphate; 37.8g oxalic acid dihydrate Embodiment 38 <![CDATA[Zn3(PO4)2]]> 37.6g zinc carbonate; 23.0g ammonium dihydrogen phosphate; 37.8g oxalic acid dihydrate Embodiment 39 <![CDATA[Ti3(PO4)4]]> 72.0g titanium sulfate; 46.0g ammonium dihydrogen phosphate; 75.6g oxalic acid dihydrate Embodiment 40 <![CDATA[Ag3PO4]]> 50.9g silver nitrate; 11.5g ammonium dihydrogen phosphate; 18.9g oxalic acid dihydrate Embodiment 41 <![CDATA[Zr3(PO4)4]]> 85.0g zirconium sulfate; 46.0g ammonium dihydrogen phosphate; 37.8g oxalic acid dihydrate Embodiment 42 <![CDATA[AlPO4]]> 13.3g aluminum chloride; 11.5g ammonium dihydrogen phosphate; 18.9g oxalic acid dihydrate
[0424] II. Performance Evaluation
[0425] 1. Lattice change rate test method:
[0426] Under a constant temperature of 25°C, the positive electrode active material sample was placed in an XRD (model: Bruker D8Discover), and the sample was tested at 1° / min. The test data was sorted and analyzed, and the lattice constants a0, b0, c0 and v0 were calculated with reference to the standard PDF card (a0, b0 and c0 represent the lengths of each aspect of the unit cell, and v0 represents the unit cell volume, which can be directly obtained through the XRD refinement results).
[0427] The positive electrode active material sample is prepared into a button battery by using the button battery preparation method in the above embodiment, and the button battery is charged at a small rate of 0.05C until the current is reduced to 0.01C. Then the positive electrode plate in the button battery is taken out and immersed in dimethyl carbonate (DMC) for 8 hours. Then it is dried, powdered, and particles with a particle size of less than 500nm are screened out. Take a sample and calculate its unit cell volume v1 in the same way as the above test of the fresh sample, and (v0-v1) / v0×100% is shown in the table as the lattice change rate (unit cell volume change rate) before and after complete lithium deintercalation.
[0428] 2. Li / Mn antisite defect concentration
[0429] The XRD results tested in the "lattice change rate measurement method" are compared with the PDF (Powder Diffraction File) card of the standard crystal to obtain the Li / Mn antisite defect concentration. Specifically, the XRD results tested in the "lattice change rate measurement method" are imported into the General Structural Analysis System (GSAS) software to automatically obtain the refinement results, which include the occupancy of different atoms, and the Li / Mn antisite defect concentration is obtained by reading the refinement results.
[0430] 3. Compacted density
[0431] Take 5g of the above-prepared positive electrode active material powder and put it in a special compaction mold (American CARVER mold, model 13mm), and then put the mold on the compaction density instrument. Apply a pressure of 3T, read the thickness of the powder under pressure on the device (thickness after pressure relief), and calculate the compaction density through ρ=m / v, where the area value used is the standard small picture area of 1540.25mm2.
[0432] 4.3C charging constant current ratio
[0433] At a constant temperature of 25°C, let the fresh full batteries prepared in the above embodiments and comparative examples stand for 5 minutes, and discharge to 2.5V at 1 / 3C. Let stand for 5 minutes, charge to 4.3V at 1 / 3C, and then charge at a constant voltage at 4.3V until the current is less than or equal to 0.05mA. Let stand for 5 minutes, and record the charging capacity at this time as C0. Discharge to 2.5V at 1 / 3C, let stand for 5 minutes, and then charge to 4.3V at 3C, let stand for 5 minutes, and record the charging capacity at this time as C1. The 3C charging constant current ratio is C1 / C0×100%.
[0434] The higher the 3C charging constant current ratio, the better the rate performance of the secondary battery.
[0435] 5. Transition metal Mn (and Mn-doped Fe) dissolution test
[0436] After cycling at 45°C until the capacity decays to 80%, the full batteries prepared in the above embodiments and comparative examples are discharged at a rate of 0.1C to a cut-off voltage of 2.0V. The battery is then disassembled, the negative electrode plate is taken out, 30 discs of unit area (1540.25 mm2) are randomly taken from the negative electrode plate, and the inductively coupled plasma emission spectrum (ICP) is tested using Agilent ICP-OES730. The amount of Fe (if the Mn position of the positive electrode active material is doped with Fe) and Mn is calculated based on the ICP results, thereby calculating the amount of Mn (and Fe doped at the Mn position) dissolved after cycling. The test standard is based on EPA-6010D-2014.
[0437] 6. Surface oxygen valence state
[0438] Take 5g of the above-prepared positive electrode active material sample and prepare it into a buckle battery according to the buckle battery preparation method described in the above embodiment. The buckle battery is charged at a small rate of 0.05C until the current is reduced to 0.01C. Then take out the positive electrode plate in the buckle battery and soak it in DMC for 8 hours. Then dry it, scrape the powder, and screen out the particles with a particle size of less than 500nm. The obtained particles are measured with an electron energy loss spectrum (EELS, the instrument model used is Talos F200S) to obtain the energy loss near-edge structure (ELNES), which reflects the state density and energy level distribution of the element. According to the state density and energy level distribution, the number of occupied electrons is calculated by integrating the valence band state density data, thereby inferring the valence state of the surface oxygen after charging.
[0439] 7. Measurement of manganese and phosphorus in positive electrode active materials
[0440] 5 g of the positive electrode active material prepared above was dissolved in 100 ml of reverse aqua regia (concentrated hydrochloric acid: concentrated nitric acid = 1:3) (concentrated hydrochloric acid concentration ~37%, concentrated nitric acid concentration ~65%), the content of each element in the solution was tested by ICP, and then the content of manganese or phosphorus was measured and converted (the amount of manganese or phosphorus / the amount of positive electrode active material*100%) to obtain its weight ratio.
[0441] 8. Measurement method of initial gram capacity of button cell
[0442] At 2.5-4.3V, the button cells prepared in the above embodiments and comparative examples were charged to 4.3V at 0.1C, then charged at a constant voltage at 4.3V until the current was less than or equal to 0.05mA, allowed to stand for 5 minutes, and then discharged to 2.0V at 0.1C. The discharge capacity at this time was the initial gram capacity, recorded as D0.
[0443] 9. Full battery cell expansion test at 60°C for 30 days:
[0444] The full batteries prepared in the above-mentioned embodiments and comparative examples were stored at 100% state of charge (SOC) at 60°C. The open circuit voltage (OCV) and AC internal resistance (IMP) of the battery cells were measured before, during and after storage to monitor the SOC, and the volume of the battery cells was measured. The full battery was taken out after every 48 hours of storage, and the open circuit voltage (OCV) and internal resistance (IMP) were tested after standing for 1 hour. The volume of the battery cells was measured by the water displacement method after cooling to room temperature. The water displacement method is to first use a balance that automatically converts units using dial data to measure the gravity F1 of the battery cell alone, and then completely place the battery cell in deionized water (density is known to be 1g / cm 3 ), measure the gravity F2 of the battery cell at this time, and the buoyancy Fbuoyancy of the battery cell is F1-F2, and then according to the Archimedean principle, Fbuoyancy = ρ×g×V 排 , the cell volume V = (F1-F2) / (ρ×g) is calculated.
[0445] From the OCV and IMP test results, the batteries of all embodiments maintained a SOC of more than 99% throughout the experiment until the end of storage.
[0446] After 30 days of storage, the cell volume was measured, and the percentage increase in the cell volume after storage relative to the cell volume before storage was calculated.
[0447] 10. Full battery cycle performance test at 45°C
[0448] At a constant temperature of 45°C, charge at 1C to 4.3V at 2.5-4.3V, then charge at a constant voltage at 4.3V to a current ≤ 0.05mA, let stand for 5 minutes, then discharge at 1C to 2.5V, and record the capacity as Dn (n = 0, 1, 2, ...). Repeat the above process until the capacity fades to 80%, and record the number of repetitions at this time, which is the number of cycles corresponding to 80% capacity retention at 45°C.
[0449] 11. Crystal plane spacing and angle test
[0450] Take 1g of each positive electrode active material powder prepared above into a 50mL test tube, and inject 10mL of 75% alcohol by mass into the test tube, then stir and disperse it for 30 minutes, then use a clean disposable plastic pipette to take an appropriate amount of the above solution and drop it on a 300-mesh copper grid. At this time, some powder will remain on the copper grid. Transfer the copper grid and the sample to the TEM (Talos F200s G2) sample chamber for testing, and obtain the original TEM test image, and save the original image format (xx.dm3).
[0451] The original image obtained by the above TEM test was opened in the DigitalMicrograph software, and Fourier transform was performed (automatically completed by the software after clicking the operation) to obtain the diffraction pattern. The distance from the diffraction spot to the center position in the diffraction pattern was measured to obtain the crystal plane spacing, and the angle was calculated according to the Bragg equation.
[0452] By comparing the obtained crystal plane spacing and corresponding angle data with their standard values, different materials in the coating layer can be identified.
[0453] 12. Coating thickness test
[0454] The thickness test of the coating layer is mainly carried out by cutting a thin slice of about 100nm thickness from the middle of a single particle of the positive electrode active material prepared above by FIB, and then performing TEM test on the thin slice to obtain the original TEM test image and save the original image format (xx.dm3).
[0455] The original image obtained from the above TEM test was opened in the DigitalMicrograph software, and the coating layer was identified through the lattice spacing and angle information, and the thickness of the coating layer was measured.
[0456] The thickness of the selected particles was measured at three locations and the average value was taken.
[0457] 13. Determination of the molar ratio of SP2 and SP3 in the third coating carbon
[0458] This test is performed by Raman spectroscopy. By separating the peaks of the energy spectrum of the Raman test, Id / Ig is obtained, where Id is the peak intensity of the carbon in the SP3 form and Ig is the peak intensity of the carbon in the SP2 form, thereby confirming the molar ratio of the two.
[0459] The performance test results of all embodiments and comparative examples are shown in the table below.
[0460] Table 9: Powder properties of positive electrode active materials in Examples 1-29 and Comparative Examples 1-17 and battery properties of the prepared batteries
[0461]
[0462]
[0463]
[0464] As can be seen from Table 9, compared with the comparative example, the embodiment achieves a smaller lattice change rate, a smaller Li / Mn antisite defect concentration, a larger compaction density, a surface oxygen valence state closer to -2, less Mn and Fe dissolution after cycling, and better battery performance, such as better high-temperature storage performance and high-temperature cycling performance.
[0465] Table 10: Thickness of each layer of the positive electrode active materials prepared in Examples 1-14 and Comparative Examples 3-4 and 12 and the weight ratio of manganese element to phosphorus element
[0466]
[0467]
[0468] It can be seen from Table 10 that by doping the manganese and phosphorus sites of lithium manganese iron phosphate (containing 35% manganese and about 20% phosphorus) and three-layer coating, the manganese content and the weight content ratio of manganese to phosphorus in the positive electrode active material are significantly reduced; in addition, comparing Examples 1-14 with Comparative Examples 3, 4 and 12, combined with Table 9, it can be seen that the reduction of manganese and phosphorus in the positive electrode active material will lead to a reduction in the dissolution of ferromanganese and an improvement in the battery performance of the secondary battery prepared therefrom.
[0469] Table 11: Powder properties of positive electrode active materials in Examples 30-42 and battery properties of the prepared batteries
[0470]
[0471]
[0472] It can be seen from Table 11 that the use of the first coating layer and the second coating layer containing other elements within the scope of the present application also obtains a positive electrode active material with good performance and achieves good battery performance results.
[0473] The first solvent, the second solvent and the first additive in the electrolyte of Example 4 are replaced with the corresponding substances and contents in Table 12 in turn to form the corresponding batteries of Examples 43 to 71. Among them, the content W1% and the content W2% add up to 100%, and the content W3% of the first additive is based on the electrolyte measurement.
[0474] Table 12
[0475]
[0476]
[0477] According to the above test method, the initial gram capacity (mAh / g) of 0.1C charge, the constant current ratio of 3C charge (%), the number of cycles of 80% capacity retention rate at 45℃, and the expansion rate of the battery cell (%) after 30 days of storage at 60℃ were tested, and the test results are recorded in Table 13.
[0478] Table 13
[0479]
[0480]
[0481] Moreover, the electrolyte in the full battery of the above-mentioned Examples 1 to 29 is replaced by: the organic solvent ethylene carbonate (EC) / ethyl methyl carbonate (EMC) is mixed evenly in a volume ratio of 3 / 7, 12.5 wt% (based on the weight of the ethylene carbonate / ethyl methyl carbonate solvent) LiPF6 is added and dissolved in the above-mentioned organic solvent, and stirred evenly to obtain an electrolyte; the electrolyte of the button battery is replaced by: a solution of 1 mol / L LiPF6 in ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1 is used as the electrolyte. The Mn and Fe dissolution amount (ppm) after the cycle, 0.1C button capacity (mAh / g) (mAh / g), 3C charging constant current ratio (%), 45°C capacity retention rate 80% cycle number, 60°C storage battery expansion rate (%) of the button batteries or full batteries formed in Comparative Examples 18 to 46 are tested according to the above method, and the test results are recorded in Table 14.
[0482] Table 14
[0483]
[0484]
[0485] According to the comparison between Table 9 and Table 14, it can be seen that the electrolyte composition of the present application can further improve the rate performance and cycle performance of the secondary battery.
[0486] Based on the electrolyte of Example 4, a second additive is further added, and the type of the additive and the content of the additive in the electrolyte are indicated in Table 15. The above method is used to test the initial gram capacity (mAh / g), 3C charging constant current ratio (%), 45°C capacity retention rate 80% cycle number, 60°C storage battery expansion rate (%), and the test results are recorded in Table 15.
[0487] Table 15
[0488]
[0489]
[0490]
[0491] It can be seen from the comparison between the data in Table 15 and the data in Example 4 that the cycle performance can be further improved when the second additive is used.
[0492] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A secondary battery, include: It includes a positive electrode plate and a non-aqueous electrolyte, wherein: The positive electrode sheet includes a positive electrode active material having a core-shell structure, wherein the positive electrode active material includes a core and a shell covering the core. The chemical formula of the core is Li 1+x Mn 1-y A y P 1-z R z O 4 , wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, z is any value in the range of 0.001-0.100, the A comprises one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be one or more elements selected from Fe, Ti, V, Ni, Co and Mg, the R comprises one or more elements selected from B, Si, N and S, and optionally, the R comprises an element selected from B, Si, N and S; the values of the x, y and z satisfy the following conditions: keep the entire core electrically neutral; The shell includes a first coating layer coating the inner core; The first coating layer includes crystalline pyrophosphate LiaMP 2 O 7 and / or Mb(P 2 O 7 ) c , wherein 0≤a≤2, 1≤b≤4, 1≤c≤6, and the values of a, b and c satisfy the following conditions: 2 O 7 or Mb(P 2 O 7 ) c Maintaining electrical neutrality, the crystalline pyrophosphate LiaMP 2 O 7 and Mb(P 2 O 7 ) c Each of the M's independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al; The non-aqueous electrolyte includes an organic solvent, the organic solvent includes a first solvent, and the first solvent includes one or more of the compounds shown in Formula 1. R 1 and R 2 are independently one of C1-C10 alkyl and C1-C10 haloalkyl. 1 and R 2 are independently one of methyl, ethyl, propyl, butyl, pentyl, hexyl, fluoromethyl, fluoroethyl, fluoropropyl, fluorobutyl, fluoropentyl, and fluorohexyl, and further optionally R 1 and R 2 are independently one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl and fluoropropyl; The surface oxygen valence state of the core-shell structured positive electrode active material is less than -1.
90.
2. The secondary battery according to claim 1, in, The shell further includes a second covering layer covering the first covering layer.
3. The secondary battery according to claim 2, It is characterized in that The second coating layer includes crystalline phosphate XPO 4 , wherein the element comprises one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb or Al.
4. The secondary battery according to claim 2 or 3, in, The shell further includes a third coating layer coating the second coating layer.
5. The secondary battery according to claim 4, in, The third coating layer includes carbon.
6. The secondary battery according to any one of claims 1 to 5, in, The first solvent comprises at least one of the following compounds: Optionally, the first solvent comprises at least one of the following compounds:
7. The secondary battery according to any one of claims 1 to 5, in, Based on the total mass of the organic solvent, the mass percentage of the first solvent is w1, and the range of w1 is 20% to 80%; optionally, the range of w1 is 30% to 75%; Optionally, the organic solvent also includes a second solvent, and the second solvent includes one or more of the group consisting of linear carbonates and cyclic carbonates; further optionally, based on the total mass of the organic solvent, the mass percentage of the second solvent is w2, and the range of w2 is 20% to 70%; optionally, the range of w2 is 25% to 70%.
8. The secondary battery according to any one of claims 1 to 7, in, The non-aqueous electrolyte further includes a first additive, wherein the first additive includes one or more selected from the group consisting of sultone and cyclic sulfate.
9. The secondary battery according to claim 8, in, The sultone comprises at least one of the compounds shown in Formula 2, p means 1, 2 or 3, R 11 represents one of a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, and a C1-C12 haloalkoxy group; optionally, R 11 represents one of a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, and a C1-C3 haloalkoxy group; the alkoxy group may be a chain alkoxy group or a cyclic alkoxy group, the cyclic alkoxy group may share a carbon atom with the parent ring of the sultone, and the cyclic alkoxy group may have 4, 5 or 6 carbon atoms; Each R 12 Each independently represents a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, or a 4- to 7-membered sultone group; optionally, each R 12 Each independently represents one of a hydrogen atom, a halogen atom, a C1-C3 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, and a 5- to 6-membered sultone group; optionally, the sultone group shares a carbon atom with the parent ring of the sultone group, and optionally, the sultone group is a 5-membered ring; R 11 and R 12 The carbon atoms to which they are attached may form a 5- to 10-membered cycloalkyl group; R 13 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a C2-C6 ester group, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C2-C12 alkenyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, a C6-C20 aryl group or a benzyl group; optionally, R 13 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a C2-C3 ester group, a C1-C3 alkyl group, a C1-C3 haloalkyl group, a C2-C6 alkenyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C6-C10 aryl group or a benzyl group; and / or, The cyclic sulfate comprises at least one of the compounds shown in Formula 3, q means 1, 2 or 3, R 14 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C2-C12 alkenyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, a C2-C6 ester group, and a 4- to 7-membered cyclic sulfate group; optionally, R 14 represents one of a hydrogen atom, a halogen atom, a carbonyl group, a double bond, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C2-C3 ester group, and a 4- to 5-membered cyclic sulfate group; optionally, the cyclic sulfate group and the cyclic sulfate ester share a carbon atom; Each R 15 Each independently represents a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a C1-C12 haloalkyl group, a C1-C12 alkoxy group, a C1-C12 haloalkoxy group, or a C6-C20 aryl group; optionally, each R 15 Each independently represents one of a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, and a C6-C10 aryl group; or R 14 and R 15 Together with the carbon atoms to which they are linked, they form a 4- to 7-membered cyclic sulfate group. 14 and R 15 Together with the carbon atoms to which they are linked, they form a 5-membered cyclic sulfate group; Optionally, the sultone comprises at least one of the following compounds: Optionally, the cyclic sulfate comprises at least one of the following compounds: Further optionally, the sultone comprises at least one of the following compounds: Further optionally, the cyclic sulfate comprises at least one of the following compounds:
10. The secondary battery according to claim 8 or 9, in, Based on the total mass of the non-aqueous electrolyte, the content of the first additive is W3, and 0.01%≤W3≤20%, optionally 0.1%≤W3≤10%, and further optionally 0.3%≤W3≤5%.
11. The secondary battery according to any one of claims 1 to 9, in, The non-aqueous electrolyte also includes a second additive, which includes one or more of the group consisting of sulfite compounds, disulfonic acid compounds, nitrile compounds, aromatic compounds, phosphazene compounds, cyclic acid anhydride compounds, phosphite compounds, phosphate compounds, and borate compounds.
12. The secondary battery according to claim 11, in, Based on the total mass of the non-aqueous electrolyte, the content of the second additive is W4, and 0.01%≤W4≤20%, optionally 0.05%≤W4≤5%, and further optionally 0.1%≤W4≤3%.
13. The secondary battery according to any one of claims 1 to 12, in, Based on the weight of the inner core, the coating amount of the first coating layer is C1 weight %, C1 being greater than 0 and less than or equal to 6, and optionally greater than 0 and less than or equal to 5.5, and more optionally greater than 0 and less than or equal to 2.
14. The secondary battery according to any one of claims 2 to 13, in, Based on the weight of the inner core, the coating amount of the second coating layer is C2 weight %, wherein C2 is greater than 0 and less than or equal to 6, and may be greater than 0 and less than or equal to 5.5, and may be more preferably 2-4.
15. The secondary battery according to any one of claims 4 to 15, in, Based on the weight of the inner core, the coating amount of the third coating layer is C3 weight %, wherein C3 is greater than 0 and less than or equal to 6, and may be greater than 0 and less than or equal to 5.5, and may be further greater than 0 and less than or equal to 2.
16. The secondary battery according to any one of claims 1 to 15, in, The interplanar spacing of the crystalline pyrophosphate in the first coating layer ranges from 0.293 to 0.470 nm, and the angle of the crystal orientation (111) ranges from 18.00° to 32.00°.
17. The secondary battery according to any one of claims 2 to 16, in, The interplanar spacing of the crystalline phosphate in the second coating layer is in the range of 0.244-0.425 nm, and the angle of the crystal orientation (111) is in the range of 20.00°-37.00°.
18. The secondary battery according to any one of claims 1 to 17, in, In the kernel, the ratio of y to 1-y is from 1:10 to 1:1, optionally from 1:4 to 1:1; and / or In the kernel, the ratio of z to 1-z is 1:9 to 1:999, and optionally 1:499 to 1:
249.
19. The secondary battery according to any one of claims 4 to 18, in, The carbon in the third coating layer is a mixture of SP2 carbon and SP3 carbon. Optionally, the molar ratio of the SP2 carbon to the SP3 carbon is any value in the range of 0.1-10, and can be any value in the range of 2.0-3.
0.
20. The secondary battery according to any one of claims 1 to 19, in, The thickness of the first coating layer is 1-10 nm.
21. The secondary battery according to any one of claims 2 to 20, in, The thickness of the second coating layer is 2-15 nm.
22. The secondary battery according to any one of claims 4 to 21, in, The thickness of the third coating layer is 2-25 nm.
23. The secondary battery according to any one of claims 1 to 22, in, Based on the weight of the positive electrode active material, The manganese content is in the range of 10 wt% to 35 wt%, optionally in the range of 15 wt% to 30 wt%, and more preferably in the range of 17 wt% to 20 wt%; The phosphorus content is in the range of 12 wt% to 25 wt%, and can be in the range of 15 wt% to 20 wt%. Optionally, the weight ratio of manganese element to phosphorus element ranges from 0.90 to 1.25, and optionally ranges from 0.95 to 1.
20.
24. The secondary battery according to any one of claims 1 to 23, in, The lattice change rate of the positive electrode active material with a core-shell structure before and after complete lithium deintercalation is less than 4%, optionally less than 3.8%, and more optionally 2.0-3.8%.
25. The secondary battery according to any one of claims 1 to 24, in, The Li / Mn antisite defect concentration of the core-shell structured positive electrode active material is less than 4%, optionally less than 2.2%, and more optionally 1.5-2.2%.
26. The secondary battery according to any one of claims 1 to 25, in, The surface oxygen valence state of the positive electrode active material having a core-shell structure is -1.90 to -1.
98.
27. A battery module comprising a secondary battery, in, The secondary battery is the secondary battery according to any one of claims 1 to 26.
28. A battery pack comprising a battery module, wherein the battery module is the battery module according to claim 27.
29. An electrical device comprising a secondary battery or a battery module or a battery pack, in, The secondary battery is selected from the secondary battery of any one of claims 1 to 26, the battery module is the battery module of claim 27, or the battery pack is the battery pack of claim 28.
Citation Information
Patent Citations
Cathode active material, cathode and non-aqueous secondary battery
CN103069624A
Composite material containing lithium manganese ferric phosphate with core-shell structure and preparation method thereof
CN110416525A
Preparation method of coated lithium manganate positive electrode material and positive electrode material thereof
CN111180702A
Secondary battery, battery module, battery pack, and electric device
CN116830314A