Sodium ion halide solid electrolyte material and preparation method and application thereof
By replacing chloride ions into borohydride ions and oxygen ions in sodium ion halide electrolytes and introducing Ga elements, the problems of low conductivity and poor mechanical properties of solid electrolyte materials are solved, and high energy density and cycling stability are achieved The improvement is suitable for all solid sodium ion batteries.
Patent Information
- Application Number
- CN202411038352.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
In the existing sodium ion solid-state battery technology, the solid electrolyte material has low ionic conductivity and poor mechanical properties, making it difficult to be compatible with high-voltage positive electrodes and sodium metal negative electrodes, resulting in insufficient battery energy density and cycle stability.
By replacing the chloride ions in the sodium ion halide electrolyte with borohydride ions and oxygen ions, and using the synergistic effect of dual ion doping, the sodium ion transport kinetics are optimized, the room temperature ion conductivity of the solid electrolyte is improved, and Ga is introduced. Elements are used to optimize Na+ migration paths to improve the mechanical properties of the material.
It significantly improves the room temperature ionic conductivity and mechanical properties of sodium ion solid electrolytes, enhances the interface contact stability with the electrode material, improves the energy density and cyclic stability of the battery, and reduces the risk of thermal runaway.
Smart Images

Figure CN118970153A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion solid-state batteries, and in particular to a sodium ion halide solid-state electrolyte material and a preparation method and application thereof. Background Art
[0002] Among various electrochemical energy storage technologies, lithium-ion batteries have become the mainstream technology route for existing electrochemical energy storage due to their advantages such as high energy density, good cycle stability, and low self-discharge rate. However, lithium resources are insufficient and unevenly distributed, making it difficult to support the sustainable development of lithium-ion battery technology. In contrast, sodium resources are abundant and low in cost, so sodium-ion batteries have good application prospects in the field of energy storage technology.
[0003] The organic electrolyte used in traditional sodium-ion batteries is flammable and volatile. When the battery is overcharged, short-circuited or subjected to external impact, it is easy to catch fire, explode and cause serious safety accidents. Using solid electrolytes to replace organic electrolytes and developing all-solid-state sodium-ion batteries can effectively improve battery safety performance and reduce the risk of thermal runaway. At the same time, solid electrolytes are expected to be compatible with high-voltage positive electrodes and sodium metal negative electrodes, significantly improving battery energy density.
[0004] Solid-state batteries have attracted extensive attention from relevant practitioners due to their high energy density and good safety performance. How to improve the ionic conductivity of solid-state electrolytes while maintaining their interfacial contact with electrode materials and chemical / electrochemical compatibility and stability is one of the core difficulties in the development of solid-state batteries. Solid-state electrolytes can be divided into organic polymer electrolytes and inorganic solid electrolytes based on their chemical properties. Organic polymer electrolytes are easy to deform and can form close interfacial contact with electrode materials without applying large stacking pressure, but their ion transport properties are usually poor. The ionic conductivity of inorganic solid electrolytes is usually high, but their poor mechanical properties result in the need to apply large stacking pressures (up to several to hundreds of MPa) during the assembly of solid-state batteries, making them difficult to apply in practice.
[0005] Therefore, the development of a new solid electrolyte material that has both good ion transport properties and excellent mechanical properties is of great significance for the development of high-performance solid-state sodium-ion batteries. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the existing sodium ion solid-state battery technology and provide a sodium ion halide solid electrolyte material with high ionic conductivity, good mechanical properties and excellent oxidation resistance, as well as a preparation method and application thereof.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] In a first aspect, the present invention provides a sodium ion halide solid electrolyte material, wherein the sodium ion halide solid electrolyte has a chemical formula of NaACl 4-x-2y (BH4) x O y , wherein A is at least one of Al, Ga, Sc, Y, In, Yb, Er, Ho, La, and Sm, 0.1≤x≤1.0, and 0.1≤y≤1.0.
[0009] The present invention partially replaces the chloride ions in the electrolyte tetrachlorometallic salt (NaACl4) with borohydride ions and oxygen ions, synergistically utilizes the rotation behavior of borohydride ion polyanions and the lattice structure disorder caused by double anion mixed doping to promote the diffusion of sodium ions, optimizes the sodium ion transport kinetics, and achieves a significant improvement in the room temperature ionic conductivity of the solid electrolyte; doping with borohydride ions or oxygen ions alone can also improve the ionic conductivity of the material, but the effect is significantly inferior to the synergistic interaction of double ion doping provided by the present invention.
[0010] In addition, the doping amount of borohydride ions and oxygen ions in the electrolyte material has a great influence on the conductivity performance: within the range of x and y in the above chemical formula, when the doping amount is moderate, the material conductivity is high; when the doping amount is higher than this range, that is, more chloride ions are replaced, the material lattice structure is prone to collapse, and NaCl impurities will be generated, causing the material ion conductivity to decrease rapidly.
[0011] In addition, the sodium ion halide solid electrolyte material provided by the present invention has good oxidation resistance, is compatible with common high-voltage positive electrode materials, ensures its structural integrity during the battery cycle and the chemical / electrochemical stability of its interface with the positive electrode material, and achieves a significant improvement in the battery energy density and cycle stability.
[0012] Preferably, A is Al or Ga.
[0013] Preferably, 0.1≤x≤0.3, 0.6≤y≤0.8.
[0014] As one preferred solution, the sodium ion halide solid electrolyte material is NaAlCl 4-x-2y (BH4) x O y , 0.1≤x≤0.3, 0.6≤y≤0.8;
[0015] More preferably, the sodium ion halide solid electrolyte material is NaAlCl 4-x-2y (BH4) x O y , 0.1≤x≤0.3, y=0.7;
[0016] As one preferred solution, the sodium ion halide solid electrolyte material is NaAl a Ga b Cl 4-x-2y (BH4) x O y , and 0.1≤x≤0.3, 0.6≤y≤0.8, 0.8≤a≤0.9, 0.1≤b≤0.2, a+b=1.
[0017] The introduction of cations with larger ionic radius will cause changes in the crystal structure or lattice parameters. This structural change can broaden the ion transport channel and facilitate Na + Therefore, the introduction of an appropriate amount of Ga element on the basis of A being Al can optimize the Na + migration path, reducing the ion transition barrier and further improving the ionic conductivity of the material.
[0018] Preferably, the room temperature conductivity of the sodium ion halide solid electrolyte material is ≥ 0.3 mS·cm -1 .
[0019] Preferably, the room temperature conductivity of the sodium ion halide solid electrolyte material is 0.3 mS·cm -1 、0.35mS·cm -1 、0.36mS·cm -1 、0.38mS·cm -1 、0.4mS·cm -1 、0.44mS·cm -1 、0.45mS·cm -1 、0.5mS·cm -1 、0.55mS·cm -1 、0.56mS·cm -1 、0.6mS·cm -1 、0.65mS·cm -1 、0.7mS·cm -1 、0.71mS·cm -1 、0.75mS·cm -1 、0.8mS·cm -1 、0.85mS·cm -1 、0.9mS·cm -1 、1mS·cm -1 The range value of one or both of them.
[0020] Preferably, the oxidation potential of the sodium ion halide solid electrolyte material is 4-5V.
[0021] In a second aspect, the present invention provides a method for preparing the above-mentioned sodium ion halide solid electrolyte material, wherein the preparation method is selected from any one of (a) to (c):
[0022] (a) mixing the raw materials in a stoichiometric ratio and then ball milling to obtain the sodium ion halide solid electrolyte material;
[0023] (b) mixing the raw materials in a stoichiometric ratio and then heating and melting them under a protective atmosphere to obtain the sodium ion halide solid electrolyte material;
[0024] (c) mixing the raw materials in a stoichiometric ratio, ball milling the raw materials, and then sintering the raw materials to obtain the sodium ion halide solid electrolyte material;
[0025] The preparation raw materials include ACl z and NaBH4, and also includes at least one of NaOH, Na2O, and A2O3.
[0026] Further preferably, in the preparation methods (a) and (c), the preparation raw materials include ACl z , NaBH4, and also includes NaOH or Na2O; in the preparation method (b), the preparation raw materials include ACl z , NaBH4 and A2O3.
[0027] Preferably, the raw materials are ground and premixed under an inert atmosphere before ball milling.
[0028] Preferably, in the preparation methods (a) and (c), the ball-to-material ratio of the ball mill is (40-85):1, the ball mill speed is 350-650rpm, and the ball milling time is 1-200 hours; in the preparation method (b), the heating and melting temperature is 120-500°C, and the insulation time is 0.5-20 hours; in the preparation method (c), the sintering temperature is 150-600°C, and the insulation time is 1-100 hours. Preferably, the preparation method of the sodium ion halide solid electrolyte material of the present invention is the preparation method (a).
[0029] More preferably, the ball-to-material ratio of the ball mill is (75-85):1, the rotation speed of the ball mill is 450-650 rpm, and the ball milling time is 10-20 h.
[0030] The sodium ion halide solid electrolyte material prepared under the ball milling conditions has high room temperature conductivity.
[0031] The sodium ion halide solid electrolyte material prepared by the present invention is in a clay-like state, has strong deformability, can achieve close electrode / electrolyte interface contact, reduces interface resistance, and improves battery rate performance.
[0032] In a third aspect, the present invention provides an application of the above-mentioned sodium ion halide solid electrolyte material in a secondary battery; preferably, the secondary battery is an all-solid-state sodium ion battery.
[0033] The all-solid-state sodium battery prepared and assembled using the above-mentioned sodium ion halide solid electrolyte material has the characteristics of good safety, high charge and discharge specific capacity, and excellent cycle stability.
[0034] Preferably, the secondary battery comprises a positive electrode layer, a negative electrode layer, a buffer layer and an electrolyte layer, and the sodium ion halide solid electrolyte material exists in at least one of the positive electrode layer, the negative electrode layer, the buffer layer and the electrolyte layer.
[0035] Further preferably, the secondary battery can be further used in large-scale energy storage equipment for solar power generation, wind power generation, smart grid peak regulation, distributed power stations, backup power supplies or communication base stations.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] The improvement of the ionic conductivity of the sodium ion halide solid electrolyte material provided by the present invention is due to the synergistic effect of the rotation behavior of the borohydride ion polyanion and the double ion doping to improve the lattice disorder. The existing technology is mainly single ion doping or multi-ion doping without polyanion rotation behavior, which can only improve the lattice disorder of the material, so its effect is significantly inferior to the doping strategy used in the present invention; in addition, the sodium ion halide solid electrolyte material provided by the present invention retains the good oxidation resistance of the halide electrolyte and can be compatible with common high-voltage positive electrode materials; in addition, the sodium ion halide solid electrolyte material provided by the present invention has excellent mechanical properties, that is, different from traditional powdered or ceramic solid electrolyte materials, it can be clay-like at room temperature, so it can form a close solid-solid interface contact with the electrode material without applying a large stacking pressure, which is conducive to solving the difficult problem of poor physical contact between the electrode and the electrolyte interface in the existing solid-state battery technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The sodium ion halide solid electrolyte material NaAlCl of Example 1 2.7 (BH4) 0.1 O 0.6 XRD spectrum of
[0039] Figure 2 The sodium ion halide solid electrolyte material NaAlCl of Example 1 2.7 (BH4) 0.1 O 0.6 AC impedance spectrum of
[0040] Figure 3Example 2 Sodium ion halide solid electrolyte material NaAlCl 2.6 (BH4) 0.2 O 0.6 XRD spectrum of
[0041] Figure 4 Example 2 Sodium ion halide solid electrolyte material NaAlCl 2.6 (BH4) 0.2 O 0.6 AC impedance spectrum of
[0042] Figure 5 Example 3 Sodium ion halide solid electrolyte material NaAlCl 2.5 (BH4) 0.3 O 0.6 XRD spectrum of
[0043] Figure 6 Example 3 Sodium ion halide solid electrolyte material NaAlCl 2.5 (BH4) 0.3 O 0.6 AC impedance spectrum of
[0044] Figure 7 Example 9 Sodium ion halide solid electrolyte material NaAl 0.9 Ga 0.1 Cl 2.4 (BH4) 0.2 O 0.7 XRD spectrum of
[0045] Figure 8 Example 9 Sodium ion halide solid electrolyte material NaAl 0.9 Ga 0.1 Cl 2.4 (BH4) 0.2 O 0.7 AC impedance spectrum of
[0046] Fig. 9 Example 10 Sodium ion halide solid electrolyte material NaAl 0.8 Ga 0.2 Cl 2.4 (BH4) 0.2 O 0.7 XRD spectrum of
[0047] Fig.10 Example 10 Sodium ion halide solid electrolyte material NaAl 0.8 Ga 0.2 Cl 2.4 (BH4) 0.2 O 0.7 AC impedance spectrum of
[0048] Fig.11 The electrolyte material of Comparative Example 1 is NaAlCl 2.8 O 0.6 XRD spectrum of
[0049] Fig.12 The electrolyte material of Comparative Example 1 is NaAlCl 2.8 O 0.6 AC impedance spectrum of
[0050] Fig.13 XRD spectrum of electrolyte material NaAlCl4 of comparative example 2;
[0051] Fig.14 This is the AC impedance spectrum of the electrolyte material NaAlCl4 in comparative example 2. DETAILED DESCRIPTION
[0052] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific examples. The test methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0053] Example 1
[0054] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAlCl 2.7 (BH4) 0.1 O 0.6 .
[0055] The NaAlCl 2.7 (BH4) 0.1 O 0.6 The preparation method is:
[0056] (1) In a glove box filled with argon, NaCl, AlCl3, NaBH4 and NaOH in a molar ratio of 3:10:1:6 were pre-mixed in a mortar and ground to obtain a mixture;
[0057] (2) The mixture was poured into a ball mill with a ball-to-material ratio of 80:1, and then the ball mill was sealed and taken out of the glove box for ball milling. The ball milling speed was 500 rpm and the ball milling time was 14 h. The ball material was separated by molecular sieve in the glove box to obtain the sodium ion halide solid electrolyte material NaAlCl 2.7 (BH4) 0.1 O 0.6 .
[0058] Figure 1 is the NaAlCl of Example 12.7 (BH4) 0.1 O 0.6 XRD spectrum of solid electrolyte material. It can be seen from the figure that NaAlCl 2.7 (BH4) 0.1 O 0.6 The diffraction peaks of the solid electrolyte material are mainly those of NaAlCl4 and NaCl. However, it was observed in the experiment that with the extension of ball milling time, the diffraction peak of NaAlCl4 gradually weakened, while the diffraction peak of NaCl gradually strengthened.
[0059] The linear sweep voltammetry (LSV) method was used to measure the sodium ion halide solid electrolyte material NaAlCl using a biologic electrochemical workstation. 2.7 (BH4) 0.1 O 0.6 The oxidation resistance potential is 4.3V.
[0060] Example 2
[0061] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAlCl 2.6 (BH4) 0.2 O 0.6 .
[0062] The NaAlCl 2.6 (BH4) 0.2 O 0.6 The preparation method of the present invention is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3, NaBH4 and NaOH in a molar ratio of 1:5:1:3 are ground and premixed in a mortar to obtain a mixture. The sodium ion halide solid electrolyte material NaAlCl is prepared. 2.6 (BH4) 0.2 O 0.6 .
[0063] Figure 3 is the NaAlCl of Example 2 2.6 (BH4) 0.2 O 0.6 XRD spectrum of solid electrolyte material. It can be seen from the figure that NaAlCl 2.6 (BH4) 0.2 O 0.6 The diffraction peaks of the solid electrolyte material are mainly the diffraction peaks of NaAlCl4 and NaCl. Similarly, with the extension of ball milling time, the diffraction peak of NaAlCl4 gradually weakens, while the diffraction peak of NaCl gradually strengthens; while in Comparative Example 1, the more the double anion replaces the chloride ion, the easier it is for the chloride ion to combine with the sodium cation to generate the NaCl impurity.
[0064] Example 3
[0065] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAlCl 2.5 (BH4) 0.3 O 0.6 .
[0066] The NaAlCl 2.5 (BH4) 0.3 O 0.6 The preparation method of the present invention is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3, NaBH4 and NaOH in a molar ratio of 1:10:3:6 are ground and premixed in a mortar to obtain a mixture. The sodium ion halide solid electrolyte material NaAlCl is prepared. 2.5 (BH4) 0.3 O 0.6 .
[0067] Figure 5 is the NaAlCl of Example 3 2.5 (BH4) 0.3 O 0.6 XRD spectrum of solid electrolyte material. It can be seen from the figure that NaAlCl 2.5 (BH4) 0.3 O 0.6 The diffraction peaks of the solid electrolyte material are mainly those of NaAlCl4 and NaCl. As the number of chloride ions replaced by borohydride ions and oxygen ions increases, the diffraction peak of NaCl becomes stronger.
[0068] Example 4
[0069] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAlCl 2.5 (BH4) 0.1 O 0.7 .
[0070] The NaAlCl 2.5 (BH4) 0.1 O 0.7 The preparation method of the present invention is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3, NaBH4 and NaOH in a molar ratio of 2:10:1:7 are ground and premixed in a mortar to obtain a mixture. The sodium ion halide solid electrolyte material NaAlCl is prepared. 2.5 (BH4) 0.1 O 0.7 .
[0071] Example 5
[0072] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAlCl 2.4 (BH4) 0.2 O 0.7 .
[0073] The NaAlCl 2.4 (BH4) 0.2 O 0.7 The preparation method of the present invention is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3, NaBH4 and NaOH in a molar ratio of 1:10:2:7 are ground and premixed in a mortar to obtain a mixture. The sodium ion halide solid electrolyte material NaAlCl is prepared. 2.4 (BH4) 0.2 O 0.7 .
[0074] Example 6
[0075] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAlCl 2.3 (BH4) 0.3 O 0.7 .
[0076] The NaAlCl 2.3 (BH4) 0.3 O 0.7 The preparation method of the present invention is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and AlCl3, NaBH4 and NaOH with a molar ratio of 10:3:7 are ground and premixed in a mortar to obtain a mixture. The sodium ion halide solid electrolyte material NaAlCl is prepared. 2.3 (BH4) 0.3 O 0.7 .
[0077] Example 7
[0078] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAlCl 2.3 (BH4) 0.1 O 0.8 .
[0079] The NaAlCl 2.3 (BH4) 0.1 O 0.8The preparation method of the present invention is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3, NaBH4 and NaOH in a molar ratio of 1:10:1:8 are ground and premixed in a mortar to obtain a mixture. The sodium ion halide solid electrolyte material NaAlCl is prepared. 2.3 (BH4) 0.1 O 0.8 .
[0080] Example 8
[0081] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAlCl 2.2 (BH4) 0.2 O 0.8 .
[0082] The NaAlCl 2.2 (BH4) 0.2 O 0.8 The preparation method of the present invention is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and AlCl3, NaBH4 and NaOH with a molar ratio of 5:1:4 are ground and premixed in a mortar to obtain a mixture. The sodium ion halide solid electrolyte material NaAlCl is prepared. 2.2 (BH4) 0.2 O 0.8 .
[0083] Example 9
[0084] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAl 0.9 Ga 0.1 Cl 2.4 (BH4) 0.2 O 0.7 .
[0085] The NaAl 0.9 Ga 0.1 Cl 2.4 (BH4) 0.2 O 0.7 The preparation method is:
[0086] (1) In a glove box filled with argon, NaCl, AlCl3, GaCl3, NaBH4 and NaOH in a molar ratio of 1:9:1:2:7 were pre-mixed by grinding in a mortar to obtain a mixture;
[0087] (2) The mixture was poured into a ball mill with a ball-to-material ratio of 80:1, and then the ball mill was sealed and taken out of the glove box for ball milling. The ball milling speed was 500 rpm and the ball milling time was 14 h. The ball material was separated by molecular sieve in the glove box to obtain the sodium ion halide solid electrolyte material NaAl 0.9 Ga 0.1 Cl 2.4 (BH4) 0.2 O 0.7 .
[0088] Figure 7 is the NaAl of Example 9 0.9 Ga 0.1 Cl 2.4 (BH4) 0.2 O 0.7 XRD spectra of solid electrolyte materials.
[0089] Example 10
[0090] An embodiment of the sodium ion halide solid electrolyte material of the present invention has a chemical formula of NaAl 0.8 Ga 0.2 Cl 2.4 (BH4) 0.2 O 0.7 .
[0091] The NaAl 0.8 Ga 0.2 Cl 2.4 (BH4) 0.2 O 0.7 The preparation method of is different from that of Example 9 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3, GaCl3, NaBH4 and NaOH in a molar ratio of 1:8:2:2:7 are ground and premixed in a mortar to obtain a mixture. The sodium ion halide solid electrolyte material NaAl is prepared. 0.8 Ga 0.2 Cl 2.4 (BH4) 0.2 O 0.7 .
[0092] Fig. 9 is the NaAl of Example 10 0.8 Ga 0.2 Cl 2.4 (BH4) 0.2 O 0.7 XRD spectra of solid electrolyte materials.
[0093] Comparative Example 1
[0094] Solid electrolyte material NaAlCl 2.8O 0.6 , and its preparation method is as follows:
[0095] (1) In a glove box filled with argon, NaCl, AlCl3, and NaBH4 in a molar ratio of 2:5:3 were ground and premixed in a mortar to obtain a mixture;
[0096] (2) The mixture was poured into a ball mill, which was then sealed and taken out of a glove box for ball milling. The ball milling speed was 500 rpm and the ball milling time was 12 h (the ion conductivity of the ball milled material was the highest after 12 h). After the ball milling was completed, the ball material was separated with a molecular sieve in the glove box to obtain a solid electrolyte material NaAlCl 2.8 O 0.6 .
[0097] Fig.11 For the NaAlCl in Comparative Example 1 2.8 O 0.6 XRD spectrum of solid electrolyte material. It can be seen from the figure that NaAlCl 2.8 O 0.6 The diffraction peaks are mainly those of NaAlCl4 and NaCl.
[0098] Comparative Example 2
[0099] The preparation method of the solid electrolyte material NaAlCl4 is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl and AlCl3 with a molar ratio of 1:1 are ground and premixed in a mortar to obtain a mixture.
[0100] Fig.13 This is the XRD spectrum of the NaAlCl4 solid electrolyte material in Comparative Example 2.
[0101] Comparative Example 3
[0102] Solid electrolyte material NaAlCl 3.9 (BH4) 0.1 The preparation method thereof is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3 and NaBH4 in a molar ratio of 9:10:1 are ground and premixed in a mortar to obtain a mixture.
[0103] Comparative Example 4
[0104] Solid electrolyte material NaAlCl 3.8 (BH4) 0.2 The preparation method thereof is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3 and NaBH4 in a molar ratio of 4:5:1 are ground and premixed in a mortar to obtain a mixture.
[0105] Comparative Example 5
[0106] Solid electrolyte material NaAlCl 3.7 (BH4) 0.3 The preparation method thereof is different from that of Example 1 only in that: in step (1), the raw materials are adjusted, and NaCl, AlCl3 and NaBH4 in a molar ratio of 7:10:3 are ground and premixed in a mortar to obtain a mixture.
[0107] Comparative Example 6
[0108] Solid electrolyte material NaAlCl 1.6 (BH4) 0.2 O 1.1 , and its preparation method is as follows:
[0109] (1) In a glove box filled with argon, AlCl 3 , NaBH 4 , and NaOH in a molar ratio of 10:2:11 were ground and premixed in a mortar to obtain a mixture;
[0110] (2) The mixture was poured into a ball mill, which was then sealed and taken out of the glove box for ball milling. The ball milling speed was 500 rpm and the ball milling time was 14 h. After the ball milling was completed, the ball material was separated by molecular sieve in the glove box to obtain the solid electrolyte material NaAlCl 1.6 (BH4) 0.2 O 1.1 .
[0111] Comparative Example 7
[0112] Solid electrolyte material NaAlCl 1.5 (BH4) 1.1 O 0.7 , and its preparation method is as follows:
[0113] (1) In a glove box filled with argon, AlCl 3 , NaBH 4 , and NaOH in a molar ratio of 10:11:7 were ground and premixed in a mortar to obtain a mixture;
[0114] (2) The mixture was poured into a ball mill, which was then sealed and taken out of the glove box for ball milling. The ball milling speed was 500 rpm and the ball milling time was 12 h. After the ball milling was completed, the ball material was separated by molecular sieve in the glove box to obtain the solid electrolyte material NaAlCl 2.5 (BH4) 1.1 O 0.7 .
[0115] Effect Example 1
[0116] In order to explore the ionic conductivity of the sodium ion halide solid electrolyte material provided by the present invention, the solid electrolyte materials of the embodiments and comparative examples were subjected to AC impedance tests, and the AC impedance was performed on a Biologic electrochemical workstation, and the ionic conductivity was calculated according to the obtained AC impedance spectrum and the formula: σ = L / R; wherein σ is the ionic conductivity (S / cm), L is the thickness of the electrolyte membrane (cm), R is the measured impedance (Ω), and S is the area of the electrolyte membrane (cm 2 ).
[0117] Figure 2 , Figure 4 , Figure 6 , Figure 8 , Fig.10 The AC impedance spectra of the sodium ion halide solid electrolyte materials in Examples 1, 2, 3, 9, and 10 of the present invention are respectively calculated. 2.7 (BH4) 0.1 O 0.6 The conductivity is 0.31mS·cm -1 , NaAlCl 2.6 (BH4) 0.2 O 0.6 The electrical conductivity is 0.36mS·cm -1 , NaAlCl 2.5 (BH4) 0.3 O 0.6 The conductivity is 0.35mS·cm -1 , NaAl 0.9 Ga 0.1 Cl 2.4 (BH4) 0.2 O 0.7 The conductivity is 0.80mS·cm -1 , NaAl 0.8 Ga 0.2 Cl 2.4 (BH4) 0.2 O 0.7 The electrical conductivity is 0.71 mS·cm -1 .
[0118] Fig.12 , 14 The AC impedance spectra of the solid electrolyte materials of Comparative Examples 1 and 2 are respectively, and the NaAlCl 2.8 O 0.6 The conductivity of NaAlCl4 is 0.10mS·cm -1 , 0.012mS·cm -1 .
[0119] The calculation data results of the ionic conductivity of the materials in the embodiments and comparative examples are summarized in Table 1. It can be seen from Table 1 that:
[0120] (1) From the comparison between Examples 1-7 and Comparative Examples 1, 3-5, it can be seen that the dual anion doping effect of borohydride ions and oxygen ions used in the present invention is significantly better than that of Comparative Example 1 doped with single oxygen ions or Comparative Examples 3-5 doped with single borohydride ions, with a conductivity of 0.31 mS·cm -1 above.
[0121] (2) It can be seen from Examples 1-8 and Comparative Examples 6 and 7 that within the scope of the present invention, as the amount of dual ion doping gradually increases, the amorphization can be enhanced by changing the local structure of the solid electrolyte, optimizing the sodium ion transmission path, and significantly improving its ionic conductivity; however, when the amount of borohydride ion and oxygen ion doping increases, more chloride ions are replaced, NaCl impurities are generated, and the amorphization degree of the solid electrolyte may be weakened, and its ionic conductivity is reduced. In Comparative Examples 6 and 7, the doping amounts of oxygen ions and borohydride ions are increased to be higher than the scope of the present invention, and their ionic conductivity is significantly reduced.
[0122] (3) In Example 5, when A is a single metal element Al, the sodium ion halide solid electrolyte material of the present invention conforms to the chemical formula NaAlCl 2.4 (BH4) 0.2 O 0.7 The ionic conductivity of -1 ; Based on metal A, a certain amount of metal Ga is introduced, and the chemical formula conforms to NaAl 0.9 Ga 0.1 Cl 2.4 (BH4) 0.2 O 0.7 、NaAl 0.8 Ga 0.2 Cl 2.4 (BH4) 0.2 O 0.7 When the ionic conductivity is increased to 0.8 mS·cm -1 The introduction of cations with different radii will lead to changes in its crystal structure or lattice parameters. This structural change can expand the ion transport channel, making Na + The carriers can migrate more easily in the lattice, thus achieving higher ionic conductivity. A certain amount of Ga is further doped on the basis of Al to optimize the Na + The migration path is shortened and the migration activation energy is reduced, so that the ionic conductivity of the solid electrolyte is significantly improved.
[0123] Table 1 Calculation data results of ionic conductivity of materials in Example and Comparative Example
[0124]
[0125]
[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A sodium ion halide solid electrolyte material, characterized in that: The sodium ion halide solid electrolyte material has a general chemical formula of NaACl 4-x-2y (BH4) x O y , wherein A is at least one of Al, Ga, Sc, Y, In, Yb, Er, Ho, La, and Sm, 0.1≤x≤1.0, and 0.1≤y≤1.
0.
2. The sodium ion halide solid electrolyte material according to claim 1, characterized in that The A is at least one of Al and Ga.
3. The sodium ion halide solid electrolyte according to claim 1, wherein the sodium ion halide solid electrolyte material is in a crystalline state, an inorganic glass state, or a glass-ceramic phase.
4. The sodium ion halide solid electrolyte material according to claim 1, characterized in that Said 0.1≤x≤0.3, 0.6≤y≤0.
8.
5. The sodium ion halide solid electrolyte material according to claim 1, characterized in that: The room temperature conductivity of the sodium ion halide solid electrolyte material is ≥0.3 mS·cm -1 Preferably, the room temperature conductivity of the sodium ion halide solid electrolyte material is 0.3-1.0 mS·cm -1 .
6. The sodium ion halide solid electrolyte material according to claim 1, characterized in that: The sodium ion halide solid electrolyte material has an oxidation resistance potential of 4-5V.
7. The method for preparing the sodium ion halide solid electrolyte material according to any one of claims 1 to 6, characterized in that: The preparation method is selected from any one of (a) to (c): (a) mixing the raw materials in a stoichiometric ratio and then ball milling them to obtain the sodium ion halide solid electrolyte material; (b) mixing the raw materials in a stoichiometric ratio and then heating and melting them under a protective atmosphere to obtain the sodium ion halide solid electrolyte material; (c) mixing the raw materials in a stoichiometric ratio, ball milling them, and then sintering them to obtain the sodium ion halide solid electrolyte material; The preparation raw materials include ACl z and NaBH4, and also includes at least one of NaOH, Na2O, and A2O3.
8. The method for preparing the sodium ion halide solid electrolyte material according to claim 7, characterized in that: In the preparation methods (a) and (c), the ball-to-material ratio of the ball mill is (40-85):1, the rotation speed of the ball mill is 350-650 rpm, and the ball milling time is 1-200 hours; in the preparation method (b), the heating and melting temperature is 120-500°C, and the insulation time is 0.5-20 hours; in the preparation method (c), the sintering temperature is 150-600°C, and the insulation time is 1-100 hours.
9. Use of the sodium ion halide solid electrolyte material according to any one of claims 1 to 6 in a secondary battery; preferably, the secondary battery is an all-solid-state sodium ion battery.
10. The use of the sodium ion halide solid electrolyte material in a secondary battery according to claim 9, characterized in that: The secondary battery includes a positive electrode layer, a negative electrode layer, a buffer layer and an electrolyte layer, and the sodium ion halide solid electrolyte material exists in at least one of the positive electrode layer, the negative electrode layer, the buffer layer and the electrolyte layer.
Citation Information
Patent Citations
Solid electrolyte, preparation method thereof and all-solid-state battery
CN112768754A
Solid-state ion conductor and preparation method thereof, positive electrode, negative electrode, negative electrode for lithium secondary battery, and electrochemical battery
CN114976000A
Sodium ion halide solid electrolyte and preparation method and application thereof
CN119315094A
Solid electrolyte material and molded body thereof
JP2020064832A
Constructing method of impermeable purifying layer and impermeable purifying layer of the method