Halide solid electrolyte and preparation method thereof
LixLayZr2Cl24 type halide solid electrolyte prepared by adjusting components and mechanical ball milling methods solves the problems of low thermal stability and improving the performance of solid electrolyte materials in traditional lithium-ion batteries, and realizes high-performance and low-cost halide solid electrolytes, which is suitable for the industry Chemical production.
Patent Information
- Application Number
- CN202411270975.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional lithium-ion batteries are due to the problems of low thermal stability and flammable and explosiveness, and there is still room for improvement in cost and performance of existing solid electrolyte materials, especially halide solid electrolytes, which have ionic conductivity and stability in a wider range of applications. The problem of sexual inadequacy.
The halide solid electrolyte of the type LixLayZr2Cl24 was prepared by adjusting the components from the oxide Li7La3Zr2O12, and the halide solid electrolyte material with excellent ionic conductivity and high oxidation stability was prepared by mechanical ball milling under the protection of inert gas.
Halogen solid electrolyte with good ionic conductivity and wide electrochemical windows at room temperature is achieved, reducing resource costs and having the prospect of suitable for large-scale production and industrialization.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state lithium batteries, and in particular relates to a halide solid electrolyte and a preparation method thereof. Background Art
[0002] As global energy shortages and environmental pollution become increasingly serious, it has become an inevitable trend to use clean, sustainable, and renewable energy to replace traditional, non-renewable fossil fuels. Traditional lithium-ion batteries are prone to fire and explosion due to their low thermal stability and easy-to-trigger ignition point, while solid electrolytes stand out in the battery field due to their safety, stability, low cost, and long cycle life, triggering intensive exploration and continuous innovation in this field in the scientific research community in recent years.
[0003] Halide solid electrolytes have become a research hotspot due to their excellent ionic conductivity and good stability to the positive electrode. In order to better promote the development of solid electrolytes, it is urgent to develop new halide solid electrolyte materials with excellent performance. Summary of the invention
[0004] The purpose of the present invention is to provide a halide solid electrolyte and a preparation method thereof, from the oxide Li7La3Zr2O 12 The halide solid electrolyte prepared by adjusting the components based on the (LLZO) and resource cost has excellent ionic conductivity, high oxidation stability potential and low resource cost, and has good prospects in industrial production.
[0005] The present invention provides a halide solid electrolyte, the chemical formula of which is Li x La y Zr2Cl 24 , where x=1-13, y=1-5.
[0006] Li x La y Zr2Cl 24 When 3≤y≤5, the diffraction peak is single phase and the structure is UCl3 type; when 1≤y<3, it is double phase and the second crystal phase is LiCl.
[0007] In order not to change the original configuration, x and y must satisfy: x+3y=16, 1≤y≤5, 1≤x≤13.
[0008] The halide electrolyte material includes Li 13 LaZr2Cl 24 , Li 10 La2Zr2Cl 24 、Li7La3Zr2Cl 24 、Li4La4Zr2Cl 24、LiLa5Zr2Cl 24 .
[0009] The ion conductivity of the halide solid electrolyte material is ≥0.46×10 -4 S cm -1 .
[0010] The invention provides a method for preparing a halide solid electrolyte. Under the protection of an inert gas, corresponding masses of LiCl, LaCl3 and ZrCl4 raw materials are weighed according to the atomic ratio of the halide solid electrolyte, and the raw materials are uniformly ground and then mechanically ball-milled to obtain a halide electrolyte. The ball-to-material mass ratio of the mechanical ball milling is 10-60:1; the ball milling time is 4-40 h; and the ball milling speed is 500 rpm-1100 rpm.
[0011] In summary, the present invention provides a new halide solid electrolyte material, which has good ionic conductivity at room temperature, a wide electrochemical window, low cost of required materials, a simple preparation process, can meet large-scale production requirements, and has good prospects for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The X-ray diffraction analysis spectrum of the halide solid electrolyte material obtained in the embodiment; Figure 2 ion conductivity and activation energy curve of the halide solid electrolyte material prepared in the embodiment; Figure 3 This is the LSV curve of the halide solid electrolyte prepared in Example 4. DETAILED DESCRIPTION
[0013] The present invention will be further described below in conjunction with specific implementation modes.
[0014] The raw materials used in the present invention include commercially available anhydrous LiCl, LaCl3, and ZrCl4 products, with a purity of ≥99.9%.
[0015] Example 1: Li 13 LaZr2Cl 24 In an argon-filled glove box, accurately weigh 0.437 g of anhydrous LiCl, 0.1941 g of anhydrous LaCl3 and 0.3689 g of anhydrous ZrCl4, grind and mix them, and then mechanically mill the resulting product, which is Li 13 LaZr2Cl 24 Materials, mechanical ball milling ball-to-material mass ratio is 10:1; ball milling time is 6 h; ball milling speed is 1000 rpm.
[0016] Example 2: Li 10 La2Zr2Cl24 In an argon-filled glove box, accurately weigh 0.3075 g of anhydrous LiCl, 0.3551 g of anhydrous LaCl3 and 0.3374 g of anhydrous ZrCl4, grind and mix them, and then mechanically mill the resulting product, which is Li 10 La2Zr2Cl 24 Materials, mechanical ball milling ball-to-material mass ratio is 60:1; ball milling time is 20 h; ball milling speed is 500 rpm.
[0017] Example 3: Li7La3Zr2Cl 24 In an argon-filled glove box, accurately weigh 0.1983 g of anhydrous LiCl, 0.4908 g of anhydrous LaCl3 and 0.3109 g of anhydrous ZrCl4, grind and mix them, and then mechanically mill the resulting product, which is Li7La3Zr2Cl 24 The material mass ratio of mechanical ball milling was 20:1; the ball milling time was 16 h; and the ball milling speed was 600 rpm.
[0018] Example 4: Li4La4Zr2Cl 24 In an argon-filled glove box, accurately weigh 0.105 g of anhydrous LiCl, 0.6067 g of anhydrous LaCl3 and 0.2883 g of anhydrous ZrCl4, grind and mix them, and then mechanically mill the resulting product, which is Li4La4Zr2Cl 24 The material mass ratio of mechanical ball milling was 10:1; the ball milling time was 20 h; and the ball milling speed was 700 rpm.
[0019] Example 5: LiLa5Zr2Cl 24 In an argon-filled glove box, accurately weigh 0.0245 g of anhydrous LiCl, 0.7068 g of anhydrous LaCl3 and 0.2687 g of anhydrous ZrCl4, grind and mix them, and then mechanically mill the resulting product, which is LiLa5Zr2Cl 24 Materials, mechanical ball milling ball-to-material mass ratio is 20:1; ball milling time is 30 h; ball milling speed is 500 rpm.
[0020] Figure 1 3 is the X-ray diffraction analysis spectrum of the halide solid electrolyte material prepared in the examples; the diffraction peak of the second phase LiCl appears near 30° in Examples 1 and 2, marked with *, and the diffraction peaks of the other examples are consistent with the LaCl3 standard card and belong to the UCl3 configuration.
[0021] The following tests were performed on the halide solid electrolyte of the above embodiment: 1) Lithium ion conductivity test Test method: Take 200 mg of the sample of the above embodiment in a glove box and press it into a sheet in a mold with a diameter of 13 mm. Stick indium sheets on both sides of the sheet as ion blocking electrodes. The impedance is tested by electrochemical impedance spectroscopy (EIS), and the lithium ion conductivity σ=d / (RS) is finally obtained by the formula, where σ is the lithium ion conductivity, d is the thickness of the electrolyte sheet, R is the impedance, and S is the contact area between the blocking electrode and the electrolyte sheet.
[0022] 2) Linear sweep voltammetry (LSV) test The electrochemical oxidation stability potential was measured by linear voltammetry. The cell configuration was: blocking electrode / electrolyte-carbon mixture / electrolyte / Li6PS5Cl / lithium. The scan rate was 1mV / s and the voltage range was from open circuit voltage to 5V. LSV testing only involved Li4La4Zr2Cl 24 Halide solid electrolyte.
[0023] Figure 2 ion conductivity and activation energy curves of the halide solid electrolyte materials prepared in the examples; Example 4 has the highest ion conductivity and the lowest activation energy.
[0024] Figure 3 This is the LSV curve of the halide solid electrolyte prepared in Example 4. Through the local enlarged schematic diagram of the LSV curve, it is found that Li self-oxidation occurs near 0.34V, and the curve is stable from this position to 5V, which proves that the example has excellent stability within the test range.
[0025] The ionic conductivity and activation energy results of Examples 1 to 5 are recorded in Table 1.
[0026] As can be seen from the above table, Example 4 (Li4La4Zr2Cl 24 ) has the highest ionic conductivity and the lowest activation energy. Reasonable control of the range of y / 2 and the amount of x is more conducive to the improvement of the performance of this material. Combined with the high oxidation stability of this embodiment within the test range of LSV, it is shown that the method of this application has industrial prospects.
Claims
1. A halide solid electrolyte, Features: Its chemical formula is Li x La y Zr 2 Cl 24 , x=1-13, y=1-5.
2. The halide solid electrolyte according to claim 1, Features: Li x La y Zr 2 Cl 24 When 3≤y≤5, the diffraction peak is single phase and the structure is UCl 3 Type; when 1≤y<3, it is a dual phase, and the second crystal phase is LiCl.
3. The method for preparing the halide solid electrolyte according to claim 1, Features: Under the protection of inert gas, weigh the corresponding mass of LiCl and LaCl according to the atomic ratio of the halide solid electrolyte. 3 、ZrCl 4 The raw materials are ground uniformly and then mechanically ball-milled to obtain a halide electrolyte.
4. The method for preparing the halide electrolyte according to claim 3, Features: The ball-to-material mass ratio of mechanical ball milling is 10-60:1; the ball milling time is 4-40 h; and the ball milling speed is 500 rpm-1100 rpm.
5. The halide solid electrolyte according to any one of claims 1 to 4, Features: The ion conductivity of the halide solid electrolyte is ≥ 0.46×10 -4 S cm -1 .