Method for preparing high-performance electrolyzed water anode catalyst and extracting lithium element by recycling waste lithium iron phosphate anode powder

By coating nickelides and leaching lithium ions, the problem of insufficient utilization of lithium elements in the recycling of waste lithium iron phosphate positive electrode materials is solved, efficient recycling and improved catalyst performance, reducing environmental pollution and energy consumption, and improving waste phosphoric acid The economic benefits of iron lithium batteries.

CN118970256AActive Publication Date: 2024-11-15SHANGHAI JIAOTONG UNIV

Patent Information

Application Number
CN202411020838.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing methods for recycling waste lithium iron phosphate positive electrode materials for preparing oxygen evolution catalysts mainly focus on directly destroying the lithium iron phosphate structure. The use of strong acid reagents is not environmentally friendly and fails to effectively utilize the lithium elements in it, and the catalytic performance is insufficient.

Method used

By recycling waste lithium iron phosphate positive electrode powder, coating and modifying nickelides, and leaching lithium ions in the oxidizing solvent, an efficient electrolytic anode catalyst is prepared, and lithium elements are extracted at the same time, and low-cost hot water soaking and solvent-thermal method are used to perform the deal with.

Benefits of technology

It has achieved efficient recycling and reuse of lithium, iron and phosphorus elements in waste lithium iron phosphate batteries, significantly improving the oxygen evolution reaction performance of the composite catalyst, and its performance is better than that of commercial Rainey nickel electrocatalysts, reducing environmental pollution and energy consumption. Improved economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970256A_ABST
    Figure CN118970256A_ABST
Patent Text Reader

Abstract

The invention relates to a method for recycling waste lithium iron phosphate positive electrode powder for preparing a high-performance electrolyzed water positive electrode catalyst and extracting lithium element, which comprises the following steps: disassembling a waste lithium iron phosphate battery, stripping a positive electrode piece from a current collector, and grinding; and coating the surface of the obtained lithium iron phosphate powder with a modified nickel compound. The obtained material is soaked in an oxidizing solution, residual lithium in the material is leached out, and composite catalyst powder obtained after lithium removal is collected. The soaking solution containing the lithium ions is settled into lithium salt in a further recrystallization mode, and lithium extraction is achieved. Compared with the prior art, the method has the advantages that efficient lithium iron phosphate recovery and reutilization are realized, the effect of the obtained composite structure catalyst for catalyzing the electrolysis water oxygen evolution reaction is greatly improved compared with that of waste lithium iron phosphate powder, and the performance is superior to that of a commercial Raney nickel electrocatalyst. In addition, compared with a nickel compound coated with lithium directly extracted from the waste lithium iron phosphate powder, the composite structure catalyst has better catalytic performance on oxygen evolution reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium battery recycling, and in particular to a method for recycling waste lithium iron phosphate positive electrode powder for preparing a high-performance water electrolysis anode catalyst and extracting lithium elements. Background Art

[0002] The research on renewable energy and clean energy has attracted much attention. Lithium-ion batteries, as batteries with high energy density and long cycle life, are widely used in electric vehicles and energy storage systems. However, with the gradual popularization and replacement of lithium-ion batteries, the treatment and resource recovery of waste batteries have become increasingly prominent. Therefore, it is urgent to develop an efficient and environmentally friendly method for recycling lithium-phosphorus batteries to solve environmental problems, recycle elemental resources, and achieve efficient utilization of recycled products.

[0003] Due to the high overlap of transition metal elements between lithium batteries and catalysts for oxygen evolution reaction in water electrolysis, it is expected that by recycling waste lithium batteries, the transition metal elements rich in lithium batteries can be extracted and utilized to obtain efficient electrocatalysts. In recent years, the technology of hydrogen production by water electrolysis through renewable electricity (such as wind power and photovoltaics) has developed rapidly this year. This technology can not only solve the intermittent and regional problems of new energy, but also is expected to achieve distributed hydrogen production in the future. However, the overall water electrolysis efficiency is subject to the efficiency of the oxygen evolution reaction at the anode of water electrolysis. The reaction kinetics are slow and efficient catalysts are required to reduce the reaction energy barrier. At present, precious metal catalysts such as iridium dioxide are considered to be efficient oxygen evolution catalysts, but their expensive prices have led to high costs for hydrogen production by water electrolysis. Transition metal catalysts with abundant reserves, low prices and efficient catalytic performance have attracted much attention in recent years. Recycling transition metal compounds in lithium batteries and further preparing electrocatalysts are expected to solve the problems of disposal and recycling of waste batteries and the high cost of water electrolysis at the same time.

[0004] At present, lithium iron phosphate batteries among waste batteries are a common type of battery, occupying a significant share of the lithium-ion battery market, and have been widely used in electric vehicles, energy storage systems and other fields. The positive electrode materials of lithium iron phosphate batteries often contain abundant resources of elements such as iron and phosphorus. Through effective recycling and reuse, the positive electrode materials in waste lithium iron phosphate batteries can be processed to prepare efficient electrolytic water catalysts. For example, CN113355690A discloses a method for large-scale preparation of efficient electrolytic water catalysts using waste lithium ion battery positive electrode materials, and CN111659399A discloses a method for preparing efficient oxygen evolution catalysts using waste lithium iron phosphate positive electrode materials. It opens up new ways for the recycling and reuse of waste lithium iron phosphate batteries, while promoting the innovation and application of electrochemical catalytic materials and the development of clean energy technologies, and contributing to sustainable development and environmental protection.

[0005] Existing research on recycling waste lithium iron phosphate positive electrode materials for the preparation of oxygen evolution catalysts is still mainly concentrated in the following two aspects: First, it focuses on the synthesis of composite structures of waste lithium iron phosphate positive electrode powders (such as the LiFePO4@Ni(OH)2 heterogeneous composite catalyst material disclosed in CN113355690A). However, little attention is paid to the rational utilization of residual lithium in waste lithium iron phosphate positive electrode materials. The high-value element in waste lithium iron phosphate positive electrode materials is mainly lithium, and lithium is generally not used as an active metal site for oxygen evolution reaction. Whether lithium can be pre-extracted from the catalyst structure still lacks corresponding attention. Second, existing research on recycling waste lithium iron phosphate positive electrode materials for the preparation of oxygen evolution catalysts focuses on directly destroying the structure of lithium iron phosphate materials, such as using strong acid reagents to dissolve the transition metal element iron in lithium iron phosphate, and then further inputting the dissolved iron-containing components as raw materials into the synthesis of oxygen evolution catalysts (such as a method disclosed in CN111659399A). However, the above method involves the use of strong acid reagents, which is not environmentally friendly and involves additional steps to destroy the lithium iron phosphate structure.

[0006] Therefore, there is an urgent need for a method that can effectively recover lithium from waste batteries and further enhance the catalytic performance of the composite catalyst for the oxygen evolution reaction. Summary of the invention

[0007] The purpose of the present invention is to provide a method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance electrolytic water anode catalyst and extracting lithium element, by recycling retired lithium iron phosphate battery positive electrode material and coating and modifying nickel oxide, nickel sulfide, nickel selenide, nickel phosphide, or nickel nitride, etc. and further leaching lithium, and at the same time preparing a highly efficient oxygen evolution reaction composite catalyst and extracting element lithium from waste lithium iron phosphate positive electrode. Waste lithium iron phosphate batteries are processed at a lower cost and highly efficient recycling and reuse is achieved.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] The object of the present invention is to provide a method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element, the method comprising the following steps:

[0010] (1) obtaining a positive electrode sheet from a recycled waste lithium iron phosphate power battery, separating a positive electrode material and a current collector in the positive electrode sheet, preparing the obtained positive electrode material into a positive electrode material powder, and recovering retired lithium iron phosphate powder from the obtained positive electrode material powder;

[0011] (2) mixing the retired lithium iron phosphate powder recovered in step (1) with the nickel-coated raw material to react and obtain a composite structure of nickel-coated lithium iron phosphate material;

[0012] ((3) soaking the composite structure of the nickel compound-coated lithium iron phosphate material obtained in step (2) in an oxidizing solvent to dissolve the remaining lithium ions in the composite structure of the nickel compound-coated lithium iron phosphate material, and separating the required water electrolysis oxygen evolution reaction catalyst from the soaking solution; the soaking solution containing lithium ions is further recrystallized to precipitate into lithium salts to extract the lithium element.

[0013] Furthermore, the method comprises the following steps:

[0014] (1) Pretreatment step: dismantle the waste lithium iron phosphate power battery after full discharge after recycling, and use organic solvent to clean the side reaction products and residual lithium salt electrolyte on the surface of the positive electrode to obtain the positive electrode. Separate the positive electrode material and the current collector by hot water immersion or other methods, and dry and grind the obtained positive electrode material into powder. Collect the positive electrode material powder, wash it with organic solvent, and dry it to obtain the retired lithium iron phosphate powder.

[0015] (2) The steps of preparing a nickel-coated retired lithium iron phosphate composite material include mixing the recovered lithium iron phosphate and the coating raw material to react, and after the reaction is completed, obtaining a composite structure of the nickel-coated lithium iron phosphate material.

[0016] (3) Lithium ion recovery step, immersing the obtained composite structure of nickel compound-coated lithium iron phosphate material in an oxidizing solvent, dissolving the remaining lithium ions in the composite structure of nickel compound-coated lithium iron phosphate material, and separating the required electrolytic water oxygen evolution reaction catalyst composite material from the immersion solution. The immersion solution containing lithium ions is further recrystallized to precipitate into lithium salts to extract the lithium element.

[0017] (4) Electrode preparation step: the water electrolysis oxygen evolution reaction catalyst composite material, conductive agent and binder separated in (3) are mixed and evenly dispersed in a solvent to obtain a dispersion liquid, and the dispersion liquid is dropped onto the target electrode to obtain a water electrolysis anode electrode.

[0018] Furthermore, the method comprises the following steps:

[0019] (1) Pretreatment step: dismantle the recycled waste lithium iron phosphate power battery after full discharge, and use dimethyl carbonate, an organic solvent, to clean the side reaction products and residual lithium salt electrolyte on the surface of the positive electrode to obtain a positive electrode. Separate the positive electrode material and the current collector by soaking in hot water, and dry and grind the obtained positive electrode material into powder. After collecting the positive electrode material powder, wash it with an organic solvent such as N-methylpyrrolidone (to remove the binder polyvinylidene fluoride PVDF) and dry it to obtain retired lithium iron phosphate powder.

[0020] (2) Preparation step of nickelide-coated retired lithium iron phosphate composite material, using a one-step hydrothermal / solvothermal method or a two-step method (hydrothermal / solvothermal method plus further high-temperature sulfurization, selenization or phosphating, etc.). The one-step method includes mixing retired lithium iron phosphate and nickelide-coated raw materials (including nickel source or nickel source and anion source) and transferring them to a hydrothermal reactor for reaction, heating to 150-300°C under stirring for 30-360 minutes to prepare a coating layer on the surface of lithium iron phosphate, and after the reaction is completed, collecting the product and washing and drying to obtain a nickelide-coated lithium iron phosphate composite material.

[0021] Optionally, the nickel source includes one or more of nickel acetylacetonate, nickel nitrate, nickel sulfate, nickel chloride, etc., the anion source includes one or more of thiourea, sodium thiosulfate, sulfur powder, selenium powder, selenium oxide, diammonium phosphate, phosphorus powder, sodium hypophosphite, etc., and the dispersion includes one or more of mesitylene, dimethylformamide, benzyl alcohol, diethylene glycol, ethanol, water, etc.

[0022] Optionally, the additives include one or more of hexadecylamine, oleic acid, octylamine, oleylamine, didodecylamine, ethylenediaminetetraacetic acid, urea, etc. The two-step method is mainly used to prepare composite materials of retired lithium iron phosphate coated with nickel sulfide, nickel selenide, nickel phosphide, nickel nitride, etc., which specifically includes: first preparing a lithium iron phosphate precursor coated with nickel hydroxide or nickel oxide by hydrothermal / solvothermal method, and then heat treating the above composite material and one or more anion sources such as selenium powder, sulfur powder, phosphorus powder, sodium hypophosphite, etc. in an inert gas atmosphere (one of argon, nitrogen, etc.). During the heat treatment process, the vacuum degree is controlled to be 0.05-0.01MPa, the heat treatment reaction temperature is 300-500℃, and the heating rate is 1-10℃min -1 The heat preservation time is 30-480 minutes. After cooling, a composite material of nickel sulfide, nickel selenide, nickel phosphide or nickel nitride coated lithium iron phosphate is obtained.

[0023] (3) Lithium ion recovery step: using chemical soaking method, soak the obtained lithium iron phosphate composite material modified with nickel-based compound in an oxidizing solvent (such as potassium ferrocyanide, sodium persulfate or ferric sulfate solution) whose standard electrode potential exceeds the standard electrode potential of lithium iron phosphate, and leaching the remaining lithium ions in the material. After sufficient soaking, centrifuge to separate the solid precipitate in the soaking solution, and further wash and dry the collected solid precipitate to obtain the required composite structure electrolysis water oxygen evolution reaction catalyst composite material. Evaporate and concentrate the soaking solution containing lithium ions to increase the concentration of lithium ions to improve the extraction efficiency of lithium elements, and then add a purifying agent such as sodium hydroxide solution to the solution, adjust the pH value of the solution so that the impurity metal ions such as iron ions in the solution form precipitates in the form of hydroxides, and filter to obtain a purified soaking solution containing lithium ions. The purified soaking solution containing lithium ions is further added with a recrystallization additive to react chemically with the lithium ions in the leaching solution to generate a lithium-containing precipitate that is insoluble in water. Control the reaction conditions (such as temperature, pH value, stirring speed, etc.) to allow the precipitation reaction to proceed fully. After the precipitation is complete, the lithium-containing precipitate is separated from the mother liquor by filtering, washing, drying and other steps to obtain a crystalline product.

[0024] The pure lithium salt is precipitated by recrystallization. Optionally, the crystallization additive includes sodium carbonate, sodium phosphate and sodium hydroxide, and the crystallization product is lithium carbonate, lithium phosphate or lithium hydroxide.

[0025] Furthermore, after step (3), the following steps are also included:

[0026] (4) The prepared water electrolysis oxygen evolution reaction catalyst composite material, conductive agent, and binder are mixed and uniformly dispersed in a solvent to obtain a dispersion liquid, and the dispersion liquid is dropped onto a target electrode to obtain a water electrolysis anode electrode.

[0027] Furthermore, after step (3), the method further comprises the following steps:

[0028] (4) The water electrolysis oxygen evolution reaction catalyst, conductive agent and binder obtained in step (3) are mixed and uniformly dispersed in a solvent to obtain a first dispersion liquid, and the first dispersion liquid is dropped onto a target electrode to obtain a water electrolysis anode electrode.

[0029] Furthermore, in step (4), the mass ratio of the catalyst for oxygen evolution reaction in electrolysis of water to the conductive agent is (1:5)-(5:1).

[0030] Furthermore, in step (4), the first dispersion liquid is a mixture of ethanol, water, a binder (such as Nafion (wt 5%) solution, polytetrafluoroethylene PTFE, etc.), etc.

[0031] Furthermore, in step (4), the solvent is a mixed solvent of water and ethanol.

[0032] Furthermore, in step (4), the volume ratio of water, ethanol and binder is 3:1:(0.2-0.4).

[0033] Furthermore, in step (4), the binder is a 5% by weight Nafion solution or polytetrafluoroethylene (PTFE).

[0034] Furthermore, in step (4), the electrode material of the target electrode is nickel foam, carbon paper and glassy carbon electrode, and the catalyst loading of the electrolytic water oxygen evolution reaction is 40 to 1000 μg cm -2 .

[0035] Furthermore, step (1) specifically includes the following process:

[0036] The waste lithium iron phosphate power battery after recycling is disassembled after being fully discharged, and the side reaction products and residual lithium salt electrolyte on the surface of the positive electrode are cleaned with an organic solvent to obtain a positive electrode plate;

[0037] Separating the positive electrode material and the current collector in the positive electrode sheet by soaking in hot water, drying and grinding the obtained positive electrode material into positive electrode material powder;

[0038] After collecting the positive electrode material powder, the residual binder in the powder is washed with a second organic solvent and dried to obtain retired lithium iron phosphate powder.

[0039] Furthermore, in step (1), the first organic solvent used to clean the side reaction products and residual lithium salt electrolyte on the surface of the positive electrode is one or more organic electrolytes such as dimethyl carbonate.

[0040] Furthermore, the first organic solvent is preferably dimethyl carbonate.

[0041] Furthermore, in step (1), the second organic solvent used to clean the residual binder in the positive electrode material powder is N-methylpyrrolidone or the like.

[0042] Furthermore, the second organic solvent is preferably N-methylpyrrolidone.

[0043] Furthermore, in step (1), the conditions for hot water immersion are: the hot water temperature range is 95-100° C., and the time is 1 to 5 minutes.

[0044] Furthermore, in step (2), the composite structure of the nickelide-coated lithium iron phosphate material includes lithium iron phosphate particles and a coating layer coating the lithium iron phosphate particles, the thickness of the coating layer is within 1 / 5 of the size / diameter of the lithium iron phosphate particles, and the coating layer material is one or more of nickel oxide, nickel hydroxide, nickel sulfide, nickel selenide, nickel phosphide, and nickel nitride.

[0045] Furthermore, in step (2), the composite structure of the nickel compound-coated lithium iron phosphate material is prepared by a one-step hydrothermal / solvothermal method or a two-step method (hydrothermal / solvothermal method plus further high-temperature sulfurization, selenization or phosphating).

[0046] Furthermore, the one-step hydrothermal / solvothermal method comprises the following steps: the one-step hydrothermal / solvothermal method comprises the following steps: dispersing lithium iron phosphate and nickel compound-coated raw materials in a solvent (such as mesitylene) for hydrothermal or solvothermal reaction to obtain a second dispersion, heating the second dispersion to 150-300°C at a heating rate of 1-10°C min -1 , the reaction temperature is 150-300°C, the reaction time is 30-360min, the stirring speed is 200-800rpm, and a composite structure of nickel compound-coated lithium iron phosphate material is obtained.

[0047] Optionally, when synthesizing nickel oxide or nickel hydroxide, in the one-step hydrothermal / solvothermal method, the nickel compound coating raw material includes a nickel source.

[0048] Optionally, when synthesizing nickel sulfide, nickel selenide, nickel phosphide, or nickel nitride, in the one-step hydrothermal / solvothermal method, the nickel compound coating raw material includes a nickel source and an anion source.

[0049] Furthermore, lithium iron phosphate and nickel-coated raw materials (including a nickel source, or a nickel source and an anion source) are dispersed in a hydrothermal / solvothermal solvent used for a hydrothermal or solvothermal reaction. Specifically, if nickel oxide or nickel hydroxide is synthesized, no additional anion source is required; but if nickel sulfide, nickel selenide, nickel phosphide or nickel nitride is synthesized, an anion source needs to be added.

[0050] Furthermore, the nickel source in the one-step hydrothermal / solvothermal method includes one or more of nickel acetylacetonate, nickel nitrate, nickel chloride, nickel acetate, nickel sulfate, and the like.

[0051] Furthermore, the anion source in the one-step hydrothermal / solvothermal method includes one or more of thiourea, sodium thiosulfate, sulfur powder, selenium powder, selenium oxide, diammonium dihydrogen phosphate, phosphorus powder, sodium hypophosphite, etc.

[0052] Furthermore, the one-step hydrothermal / solvothermal method comprises the following steps: dispersing lithium iron phosphate, nickel compound coating raw materials and additives in a solvent (such as mesitylene) for hydrothermal or solvothermal reaction to obtain a second dispersion.

[0053] Furthermore, in the one-step hydrothermal / solvothermal method, optional additives include one or more of hexadecylamine, oleic acid, octylamine, oleylamine, didodecylamine, ethylenediaminetetraacetic acid, urea, etc., which are used to adjust the reaction environment.

[0054] Furthermore, the two-step method comprises the following steps:

[0055] (2-1) dispersing lithium iron phosphate and nickel compound coating raw materials in a hydrothermal / solvothermal solvent to obtain a third dispersion, and preparing a lithium iron phosphate precursor coated with nickel hydroxide or nickel oxide by a hydrothermal / solvothermal method;

[0056] (2-2) The anion source and the lithium iron phosphate precursor are heat-treated in an inert gas atmosphere, and after cooling, a composite structure of the nickel compound-coated lithium iron phosphate material is obtained.

[0057] Furthermore, the hydrothermal / solvothermal solvent includes one or more of mesitylene, dimethylformamide, benzyl alcohol, diethylene glycol, ethanol, water, and the like.

[0058] Furthermore, the nickel compound coating raw material in the two-step method includes a nickel source.

[0059] Furthermore, the nickel source in the two-step method includes one or more of nickel acetylacetonate, nickel nitrate, nickel chloride, nickel acetate, nickel sulfate, and the like.

[0060] Furthermore, the anion source in the two-step method includes one or more of selenium powder, sulfur powder, phosphorus powder, sodium hypophosphite, etc.

[0061] Furthermore, in the two-step method, the mass ratio of the lithium iron phosphate precursor to the anion source is (1:0.1)-(1:2).

[0062] Furthermore, the inert gas in the two-step method includes one of argon, nitrogen and the like.

[0063] Further, the process of step (2-1) is as follows: dispersing additives, lithium iron phosphate and nickel compound coating raw materials in a hydrothermal / solvothermal solvent to obtain a third dispersion, and preparing a lithium iron phosphate precursor coated with nickel hydroxide or nickel oxide by a hydrothermal / solvothermal method. The hydrothermal / solvothermal solvent provides a solvent environment for coating, and the additive provides a pH environment for hydrolysis.

[0064] Furthermore, in step (2-1), the conditions for preparing the lithium iron phosphate precursor coated with nickel hydroxide or nickel oxide by hydrothermal / solvothermal method are as follows: the third dispersion liquid is heated to 150-300°C at a heating rate of 1-10°C min -1 , the reaction temperature is 150-300° C., the reaction time is 30-360 min, and the stirring speed is 200-800 rpm to obtain a lithium iron phosphate precursor coated with nickel hydroxide or nickel oxide.

[0065] Furthermore, in step (2-1), the optional additives include one or more of hexadecylamine, oleic acid, octylamine, oleylamine, didodecylamine, ethylenediaminetetraacetic acid, urea, etc., which are used to adjust the reaction environment.

[0066] Furthermore, during the heat treatment process, the vacuum degree is controlled to be 0.05-0.01 MPa, the heat treatment reaction temperature is 200-500°C, and the heating rate is 1-10°C min -1 , the insulation time is 30-480 minutes.

[0067] Furthermore, in step (3), the optional oxidizing solvent is a solution whose standard electrode potential exceeds the standard electrode potential of lithium iron phosphate, such as potassium ferrocyanide solution. The standard electrode potential, sometimes also called equilibrium electrode potential, reflects the redox ability of a substance.

[0068] Furthermore, in step (3), the recrystallization additive is one or more of carbonates, hydroxides, and sulfates.

[0069] Furthermore, step (3) specifically includes the following steps:

[0070] The composite structure of the nickel compound-coated lithium iron phosphate material is immersed in an oxidizing solvent to dissolve the remaining lithium ions in the composite structure of the nickel compound-coated lithium iron phosphate material, and after sufficient reaction, the desired delithiated water electrolysis oxygen evolution reaction catalyst solid is separated by centrifugation from the immersion solution;

[0071] The collected lithium ion-containing soaking solution is evaporated and concentrated to improve the efficiency of lithium element extraction, and then a purifying agent is added to the solution to adjust the pH value of the solution so that the impure metal ions are precipitated in the form of hydroxide and filtered.

[0072] A recrystallization additive is added to the purified lithium ion-containing soaking solution to precipitate the lithium ions into lithium salts to achieve the extraction of lithium elements. The function of the recrystallization additive is to chemically react with the lithium ions in the solution to generate lithium-containing precipitates that are insoluble in water, and the lithium-containing recrystallized product is obtained after filtration.

[0073] Compared with the prior art, the present invention has the following beneficial effects:

[0074] (1) The present invention provides a new method for recycling battery materials that is simple to operate, low in cost, and has extremely low equipment requirements. It does not require long-term high-temperature pyrometallurgical reactions or the use of large amounts of acid and alkali reagents in hydrometallurgy. In addition, the method of using hot water immersion to separate lithium iron phosphate and current collectors does not produce waste liquid. It is a low-cost, low-energy green recycling method that reduces the pollution of waste lithium iron phosphate batteries to the environment.

[0075] (2) The method provided by the present invention can recycle the lithium, iron and phosphorus elements in the positive electrode lithium iron phosphate, avoid the energy consumption of repeated mining, and save resources. The composite structure catalyst finally obtained has a much better effect of catalyzing the oxygen evolution reaction in water electrolysis than retired lithium iron phosphate powder, and has better performance than commercial Raney nickel electrocatalysts, has more excellent water electrolysis catalytic performance and stability, can effectively improve the efficiency of oxygen evolution reaction, and is easy to operate and mass produce, significantly improving the economic benefits of recycling waste lithium iron phosphate batteries.

[0076] (3) The present invention prepares the catalyst and extracts the lithium element in the same process, thereby achieving high performance of the anode catalyst for water electrolysis and extracting high-value lithium elements from waste lithium iron phosphate batteries, thereby obtaining high-value, high-quality pure lithium compounds. This realizes the comprehensive utilization of resources and the efficient conversion of energy, and has important economic and environmental significance.

[0077] (4) The method provided by the present invention can not only extract the high-value element lithium from the waste lithium iron phosphate positive electrode, but also utilize the leaching effect of lithium from the composite structure of the nickel compound-coated lithium iron phosphate material to significantly enhance the catalytic performance of the composite catalyst for oxygen evolution reaction. The composite catalyst obtained by the method provided by the present invention (compared with the method of directly extracting lithium from the waste lithium iron phosphate positive electrode and then coating it with nickel compound) has significantly improved oxygen evolution catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0078] Figure 1 Transmission electron micrograph of the retired lithium iron phosphate composite material of s-LFP@NiO modified nickel oxide prepared in Example 1 of the present invention, including: (a) TEM image of a single s-LFP@NiO particle, and (b) an enlarged image of the heterojunction structure at the edge of the s-LFP@NiO particle and its lattice fringes.

[0079] Figure 2 These are the SEM spectra and element mapping diagrams of the s-LFP@NiO-PL composite catalyst prepared in Example 1 of the present invention, wherein (a) and (b) are SEM spectra of the s-LFP@NiO-PL composite catalyst at different magnifications, (c) SEM spectrum of the s-LFP@NiO-PL energy spectrum element mapping area, (d) Ni element analysis diagram, (e) Fe element analysis diagram, and (f) P element analysis diagram.

[0080] Figure 3 This is an oxygen evolution reaction performance diagram of the s-LFP@NiO-PL composite catalyst prepared in Example 1 of the present invention loaded on a glassy carbon electrode, the s-LFP catalyst prepared in Comparative Example 1 loaded on a glassy carbon electrode, and the s-FP@NiO composite catalyst prepared in Comparative Example 2 loaded on a glassy carbon electrode after cyclic voltammetry scanning and stabilization.

[0081] Figure 4 It is an oxygen evolution reaction performance diagram of the s-LFP@NiO-PL composite catalyst prepared in Example 1 of the present invention loaded on the nickel foam electrode, the Raney nickel catalyst loaded on the nickel foam electrode, and the blank nickel foam electrode after cyclic voltammetry scanning and stabilization. DETAILED DESCRIPTION

[0082] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments. It should be understood that the accompanying drawings and the following embodiments are only used to illustrate the present invention, rather than to limit the present invention. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0083] Any value in the numerical range disclosed in the present invention is not limited to the precise range or value. These ranges or values ​​should be understood to include values ​​close to these ranges or values. The endpoint values ​​of each range, the endpoint values ​​of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges. These numerical ranges should be deemed to be specifically disclosed in the present invention.

[0084] The preparation methods, materials, structures or composition ratios not explicitly described in this technical solution are deemed to be common technical features disclosed in the prior art.

[0085] The steps without specified conditions will be operated according to the routine. The reagents and instruments used are common and easy to buy products in the market, and the technical terms used are in accordance with the general standards in the field.

[0086] The present invention provides a method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium elements, comprising the following steps: dismantling waste lithium iron phosphate power batteries, stripping the positive electrode plate from the current collector to obtain positive electrode black powder, further grinding the dried positive electrode lithium iron phosphate black powder; coating the surface of the obtained lithium iron phosphate powder with modified nickel compound. The obtained material is immersed in an oxidizing solution to leach the remaining lithium in the material, and the composite catalyst powder after delithiation is collected. The present invention realizes efficient lithium iron phosphate recovery and reuse, and the obtained composite structure catalyst has a significantly improved effect on the oxygen evolution reaction of water electrolysis than the waste lithium iron phosphate powder, and the performance is better than that of the commercial Raney nickel electrocatalyst. In addition, compared with directly extracting lithium from the waste lithium iron phosphate powder and then coating the nickel compound, the composite structure catalyst of the present invention has better catalytic performance for the oxygen evolution reaction.

[0087] The present invention provides a method for simultaneously recovering waste lithium iron phosphate positive electrode materials for preparing composite catalysts on the anode side (oxygen evolution reaction) of electrolyzed water and efficiently extracting residual elemental lithium from waste lithium iron phosphate. The process comprises the following steps: step 1, dismantling waste lithium iron phosphate power batteries, cleaning the side reaction products and lithium salts on the surface of the pole pieces to obtain positive pole pieces, separating them from the current collector, and grinding the obtained dry positive electrode material lithium iron phosphate powder; step 2, coating and modifying the surface of the obtained lithium iron phosphate powder with nickel compounds, including one or more of nickel oxide, nickel hydroxide, nickel sulfide, nickel selenide, nickel phosphide, and nickel nitride, to obtain a lithium iron phosphate composite material coated with modified nickel-based compounds. Step 3, soaking the obtained material in an oxidizing solution, leaching the remaining lithium in the material, further extracting it in the form of lithium salt, and collecting the composite catalyst powder after delithiation at the same time. Step 4, mixing the obtained composite catalyst, conductive agent, and binder uniformly and dispersing them in a solvent to obtain a dispersion, and dripping the dispersion on the target electrode to obtain an electrolyzed water anode electrode. The present invention realizes efficient recovery and reuse of lithium iron phosphate and effective recycling of resources. The obtained composite structure catalyst has a greatly improved effect of catalyzing oxygen evolution reaction in electrolysis of water compared with waste lithium iron phosphate powder, and its performance is better than that of commercial Raney nickel electrocatalyst.

[0088] A method for recycling waste lithium iron phosphate positive electrode material to prepare a composite catalyst for electrolysis of water anode side (oxygen evolution reaction), comprising the following steps:

[0089] First, the waste lithium iron phosphate battery after recycling is fully discharged, disassembled, and the side reaction products on the surface of the positive electrode sheet and the lithium salt electrolyte are cleaned with dimethyl carbonate, and the obtained positive electrode sheet is immersed in hot water at 95-99°C. After 10 seconds, the positive electrode material on the aluminum foil is manually peeled off and collected with a clamp. The polyvinylidene fluoride (PVDF) remaining in the positive electrode material is washed with N-methylpyrrolidone (NMP), and the retired lithium iron phosphate powder (s-LFP) is obtained after drying and grinding. The reason for using hot water immersion is that it can cause the binder PVDF to phase separate and the viscosity to deteriorate. In addition, NMP is also commonly used to dissolve PVDF, thereby separating the active substances on the positive electrode sheet. However, the price of NMP is very expensive, and solvent post-treatment is required, which has negative effects on economic benefits and the environment. In comparison, the method of manual separation after immersion in hot water for 10 seconds has the advantages of shorter time and lower cost, and is more in line with the requirements of waste battery recycling industrialization.

[0090] The nickel compound coating adopts a one-step solvothermal method. 60mg of retired lithium iron phosphate (s-LFP) nanoparticles, 160mg of nickel acetylacetonate and 480mg of hexadecylamine are added to 16mL of mesitylene. After the mixture is ultrasonically treated for 20min, the uniform colloidal suspension obtained is transferred to a 50mL hydrothermal reactor and solvothermally reacted at a temperature of 150-200℃ for 1-4 hours. After the reaction is completed, it is cooled to room temperature, and the turbid liquid is washed with ethanol and water, centrifuged, and the precipitate is collected, and the process is repeated many times. After the collected product is dried in a vacuum oven, a black s-LFP@NiO modified nickel oxide lithium iron phosphate composite material is obtained.

[0091] Furthermore, the remaining lithium ions in the product are recovered by chemical leaching. 20 mg of the obtained s-LFP@NiO modified nickel-based compound lithium iron phosphate composite material is immersed in 50 mL of an oxidizing solvent such as a 0.2 M potassium ferrocyanide solution and allowed to stand for 24 hours for full reaction. Through the redox reaction, the remaining lithium ions in the leached material enter the solution. The precipitated product is washed with water, centrifuged, and repeatedly collected. After drying, the precipitated product is obtained to obtain a black s-LFP@NiO-PL delithiation composite catalyst powder. PL refers to the use of a pre-leaching chemical method to pre-leach the lithium ions in the material to obtain the required electrolytic water oxygen evolution reaction catalyst. The lithium-containing solution obtained by evaporation and concentration makes the concentration of lithium element reach 40 g L -1 To improve the subsequent extraction efficiency of lithium. Then add 2 mol L -1 The pH value of the solution was adjusted to 7-8 by adding sodium hydroxide solution to precipitate the impurity metal ions. After filtering the precipitate, the solution was stirred at 1-5 mL min -1 Saturated sodium carbonate solution is added at a rate of 300 rpm to react with lithium ions to form lithium carbonate precipitate. During the precipitation process, the solution is continuously stirred at a stirring speed of 300 rpm, the solution temperature is maintained at 95°C, and the precipitation process lasts for 2 hours. The obtained lithium carbonate precipitate is filtered, washed and dried, thereby completing the extraction of lithium element.

[0092] Finally, the s-LFP@NiO-PL composite catalyst, conductive agent, and binder are evenly dispersed in a solvent to obtain a dispersion, and the mass ratio of the catalyst to the conductive agent is 1:4-4:1. The dispersion is a mixture of ethanol, water, and Nafion (wt 5%) solution, with a volume ratio of 3:1:0.2-0.4. The dispersion is dripped onto the target electrode, such as nickel foam, carbon paper, and glassy carbon electrode, to obtain a catalyst loading of 40 to 1000 μg cm -2 Anode electrode for water electrolysis.

[0093] The separated waste lithium iron phosphate active material is collected and dried, specifically to remove the binder and other impurities on the collected lithium iron phosphate positive electrode material to reduce the impact of the separation process on the lithium iron phosphate sample. The collected lithium iron phosphate is washed with N-methylpyrrolidone (NMP) and centrifuged at 8000rpm for 8 minutes. After repeating this process three times, the lithium iron phosphate is dried at 80°C in a vacuum environment for 12 hours.

[0094] s-LFP, nickel acetylacetonate, and hexadecylamine were mixed in mesitylene for solvothermal reaction. Specifically, nickel salt was introduced to achieve nickel compound coating; hexadecylamine was used as a surfactant and stabilizer, which could be adsorbed on the surface of nanoparticles to form a protective layer, which helped to control the growth of the coating layer and avoid agglomeration; mesitylene was used as a good dispersant to provide a solvent environment, in order to make nickel acetylacetonate uniformly dispersed in the solution. In detail, the concentration of nickel acetylacetonate was 0.02-0.04 mol L -1 ; Hexadecylamine concentration is 0.12-0.14 mol L -1 ; The liquid-to-solid ratio of the solution to the s-LFP used is 3.5-5 L g -1 The concentration of nickel acetylacetonate is set to control the Ni source to achieve a controllable coating amount. The concentration of hexadecylamine and the solid-liquid ratio of s-LFP to trimethylbenzene solution are set to provide a uniform liquid phase environment to ensure sufficient contact between s-LFP powder and nickel acetylacetonate, so that the solvent thermal reaction can proceed fully.

[0095] The hydrothermal reactor is subjected to solvent thermal reaction at a temperature of 150-200°C for 1-4 hours, with a heating rate of 5-10°C min -1 After the reaction is completed, wait for it to cool to room temperature, take out the turbid liquid in the hydrothermal kettle and wash it with ethanol and water alternately, centrifuge it at 9000rpm for 5 minutes, repeat it 5 times in total, the purpose is to remove the residual organic liquid and residual nickel salt on the surface of s-LFP@NiO. Then the collected black powder is dried at room temperature for 12 hours under vacuum environment to obtain s-LFP@NiO modified nickel oxide lithium iron phosphate composite material.

[0096] In the lithium ion recovery step, the optional oxidizing solvent is a solution whose standard electrode potential exceeds the standard electrode potential of lithium iron phosphate, such as potassium ferrocyanide. Optionally, the recrystallization additive is one or more of carbonates and hydroxides. The purpose of soaking in an oxidizing solvent is to further leach out the residual Li ions in the s-LFP@NiO powder and recover them by recrystallization to improve economic benefits. In addition, the chemical method of leaching lithium from the s-LFP@NiO material can simultaneously enhance the oxygen evolution performance of the composite catalyst, and obtain a high-performance, long-term stable electrolytic water oxygen evolution catalyst.

[0097] Example 1

[0098] This embodiment provides a method for recycling waste lithium iron phosphate positive electrode powder for preparing a high-performance water electrolysis anode catalyst and extracting high-value lithium elements, which is used to illustrate the nickel oxide-coated lithium iron phosphate composite structure nanomaterial prepared by the solvothermal method provided by the present invention, comprising the following steps:

[0099] The cathode strips of the dismantled self-discharged waste lithium iron phosphate batteries were cleaned with dimethyl carbonate, cut into 3cm×7cm sizes, and immersed in 95°C hot water. After 10 seconds, the cathode materials were manually peeled off and collected. The separated cathode materials were collected and the residual PVDF in the cathode materials was washed with N-methylpyrrolidone, and then dried and ground to obtain retired lithium iron phosphate powder (s-LFP).

[0100] 60 mg of retired s-LFP nanoparticles (retired lithium iron phosphate powder (s-LFP)), 160 mg of nickel acetylacetonate and 480 mg of hexadecylamine were added to 16 mL of mesitylene. After ultrasonic treatment for 20 min, the obtained uniform colloidal suspension was transferred to a 50 mL hydrothermal reactor and subjected to solvothermal reaction at 170 °C with a heating rate of 5 °C min -1 , the temperature was kept at 200℃ for 60min, and then the temperature was raised to 200℃, the temperature was kept at 75min, and the stirring speed was 400rpm. Wash with ethanol and water, centrifuge, collect the precipitate product repeatedly, and dry it to obtain a black s-LFP@NiO modified nickel-based compound lithium iron phosphate composite material (i.e., a composite structure of nickel compound coated lithium iron phosphate material), and its heterojunction components are lithium iron phosphate s-LFP and nickel oxide NiO from the center to the outside. 20mg of the prepared s-LFP@NiO composite structure nanomaterial was soaked in 50mL 0.2M potassium ferrocyanide solution and allowed to stand for 24 hours to fully react. Wash with water, centrifuge at 8000rpm, collect the precipitate product repeatedly, and dry it to obtain a black s-LFP@NiO-PL composite catalyst, which was used as a catalyst for electrolytic water oxygen evolution reaction. The s-LFP@NiO-PL composite catalyst obtained above has components of FePO4 and NiO from the center to the outside.

[0101] The lithium-containing solution obtained by evaporation and concentration (the supernatant obtained after centrifugation) was concentrated to a lithium concentration of 40 g L -1 To improve the subsequent extraction efficiency of lithium. Then add 2 mol L -1 The pH value of the solution was adjusted to 7-8 by adding sodium hydroxide solution to precipitate the impurity metal ions. After filtering the precipitate, the solution was stirred at 1-5 mL min -1Saturated sodium carbonate solution is added at a rate of 300 rpm to react with lithium ions to form lithium carbonate precipitate. During the precipitation process, the solution is continuously stirred at a stirring speed of 300 rpm, the solution temperature is maintained at 95°C, and the precipitation process lasts for 2 hours. The obtained lithium carbonate precipitate is filtered, washed and dried, thereby completing the extraction of lithium element.

[0102] Electrode preparation: The obtained s-LFP@NiO-PL composite catalyst, conductive agent Vulcan Carbon (purchased from CABOT, model XC-72), and binder (Nafion (wt 5%)) were uniformly dispersed in a solvent to obtain a dispersion, and the mass ratio of the catalyst to the conductive agent was 4:1. The dispersion was a mixture of ethanol, water, Nafion (wt 5%) and other solutions, and the volume ratio of ethanol, water, and Nafion (wt 5%) was 3:1:0.2. The solid-liquid ratio of the obtained dispersion was 3.75 mg mL -1 Further, the dispersion was dripped onto a surface with an area of ​​0.19625 cm 2 The catalyst loading was 255 μg cm -2 The anode electrode for water electrolysis. Add the dispersion dropwise to a 0.8*1.8cm 2 The catalyst loading was 1388 μg cm -2 Self-supporting anode electrode for water electrolysis.

[0103] Electrochemical performance test: The prepared glassy carbon working electrode loaded with s-LFP@NiO-PL, the counter electrode (platinum sheet) and the HgO / Hg reference electrode were assembled into a three-electrode system, and the assembled three-cell was electrochemically tested using a biologic electrochemical workstation. The voltage applied to the working electrode ranged from 1.1-1.6 V vs. RHE, and the scan rate was 10 mV s -1 , and obtain stable catalytic performance for oxygen evolution reaction in water electrolysis. For nickel foam electrodes with larger specific surface area, a larger scanning range is required, and the voltage range applied to the electrode is 1.0-1.7V vs.RHE, and the scanning speed is 10mV s -1 .

[0104] See also Figure 1 (a) and (b) weigh a certain amount of the s-LFP@NiO modified nickel-based compound lithium iron phosphate composite material sample prepared in Example 1 and observe it under a transmission electron microscope. It can be seen that the s-LFP@NiO modified nickel-based compound lithium iron phosphate composite material obtained after coating has a size of about 200nm and a uniform morphology. The coated shell is about 9nm and is evenly coated on the s-LFP nanoparticles without destroying the overall structure. Figure 1(b) and its illustration show that the components of s-LFP@NiO from the center to the outside are: clear lattice fringes, corresponding to the (200) crystal plane of the core layer LiFePO4, and the outer amorphous NiO shell.

[0105] See also Figure 2 (a), (b), a certain amount of sample s-LFP@NiO-PL prepared in Example 1 was weighed and observed under a scanning electron microscope. It can be seen that the immersion did not destroy the overall structure of the composite structural material s-LFP@NiO-PL, and the morphology and size were well maintained. Figure 2 Evenly distributed Ni, Fe, and P elements can be seen in the element energy spectra (d), (e), and (f) corresponding to the (c) region.

[0106] Comparative Example 1

[0107] The retired dry lithium iron phosphate powder s-LFP was obtained according to the operation steps of Example 1. The s-LFP catalyst was used to prepare a glassy carbon electrode, and the same catalytic performance test and analysis of oxygen evolution by electrolysis of water as in Example 1 were performed.

[0108] Comparative Example 2s-FP@NiO composite catalyst

[0109] This comparative example provides a s-FP@NiO composite catalyst, which is as follows:

[0110] Obtain retired dry lithium iron phosphate powder s-LFP according to the operating steps of Example 1. Soak 100 mg of the obtained s-LFP lithium iron phosphate powder in 50 mL of 0.2 M potassium ferrocyanide solution and let stand for 24 hours for sufficient reaction. Wash with water, centrifuge at a speed of 8000 rpm-10000 rpm, collect the precipitated product repeatedly, and obtain black retired iron phosphate s-FP granular powder after drying. Add 60 mg of retired iron phosphate granular powder (iron phosphate powder (s-FP)), 160 mg of nickel acetylacetonate and 480 mg of hexadecylamine to 16 mL of mesitylene, transfer the obtained uniform colloidal suspension to a 50 mL hydrothermal reactor after ultrasonication for 20 minutes, and carry out solvent thermal reaction at a temperature of 170°C, with a heating rate of 5°C min -1 , the temperature was kept at 200 ° C for 60 minutes, then the temperature was raised to 200 ° C, the temperature was kept at 75 minutes, and the stirring speed was 400 rpm. Washing with ethanol and water, centrifugation, and repeated collection and drying of the precipitated product obtained a black s-FP@NiO modified nickel-based compound iron phosphate composite material, the heterojunction components of which are iron phosphate s-FP and nickel oxide NiO from the center to the outside. It is used as a catalyst for the electrolysis of water and oxygen evolution reaction. The s-FP@NiO catalyst is used to prepare a glassy carbon electrode, and the same electrolysis of water and oxygen evolution catalytic performance test and analysis as in Example 1 are carried out.

[0111] like Figure 3 As shown in the figure, after the above electrochemical oxygen evolution reaction performance test, the electrochemical CV curves of oxygen evolution reaction under voltage of Example 1, Comparative Example 1 and Comparative Example 2 were obtained, wherein the abscissa is voltage and the ordinate is current density. The s-LFP@NiO-PL composite catalyst material prepared in Example 1 of the present invention has a catalytic oxygen evolution reaction current density of 10 mA cm -2 The overpotential required under this condition is about 267mV, and the electrochemical performance is much better than that of the initial material s-LFP. In contrast, the s-FP@NiO composite catalyst in Comparative Example 2 has a current density of 10mAcm -2 The overpotential required is about 327mV, and the performance is obviously inferior to the prepared s-LFP@NiO-PL composite catalyst, which shows that through the method provided by the present invention, not only the high-value element lithium in the waste lithium iron phosphate positive electrode can be extracted, but also the leaching effect of lithium from the composite structure of nickel-coated lithium iron phosphate material can be utilized to significantly enhance the catalytic performance of the composite catalyst for oxygen evolution reaction. Compared with the method of directly extracting lithium from the waste lithium iron phosphate positive electrode and then coating the nickel compound in the comparative example, the method provided by the present invention first recovers the retired lithium iron phosphate battery positive electrode material and coats and modifies nickel oxide, nickel sulfide, nickel selenide, nickel phosphide, or nickel nitride and other nickel compounds, and further leaches lithium, the obtained composite catalyst has a significantly improved oxygen evolution catalytic performance.

[0112] like Figure 4 As shown, the obtained Example 1 is prepared into a porous nickel foam electrode. Nickel foam is the most commonly used self-supporting electrode and is widely used in industrial water electrolysis. Figure 4 As shown in the figure, the nickel foam electrode (s-LEP@NiO-PL / Ni Foam) loaded with 2 mg of s-LFP@NiO-PL composite catalyst has a catalytic oxygen evolution reaction current density of 50 mA cm -2 The required overpotential is 307 mV. In comparison, the Raney nickel catalyst is prepared into a porous nickel foam electrode (Rayne Ni / Ni Foam). The industrially used Raney nickel catalyst (Rayne Ni) has a 35-fold catalyst mass loading (70 mg cm -2 ), a 450 mV overpotential is required to achieve 50 mA cm -2 In addition, the above electrodes all showed catalytic performance that was significantly better than that of blank nickel foam (NiFoam) electrodes.

[0113] In summary, the present invention provides a new method for preparing composite structural materials from waste lithium iron phosphate batteries for use as anode catalysts for electrolysis of water, which is simple to operate, low in cost, and has low equipment requirements. By recycling the positive electrode materials of retired lithium iron phosphate batteries, a lithium iron phosphate composite material modified with nickel-based compounds is prepared by adding nickel acetylacetonate, hexadecylamine, and trimethylbenzene by a solvothermal method to coat nickel oxide on the surface of lithium iron phosphate. The remaining lithium ions in the composite structural material are further leached out by a chemical soaking method to obtain an efficient catalyst for oxygen evolution reaction in electrolysis of water. Waste lithium iron phosphate batteries are treated at a lower cost and are efficiently recycled and reused. Compared with the recycling of traditional battery materials, there is no need for long-term high-temperature reactions of pyrometallurgy and the use of a large amount of acid and alkali reagents in hydrometallurgy. It is a low-cost, low-energy green recycling method that reduces the pollution of waste lithium iron phosphate batteries to the environment. By preparing a catalyst for oxygen evolution reaction in electrolysis of water, the utilization of the recovered lithium iron phosphate is achieved, the energy consumption of repeated mining is avoided, and resources are saved. The composite catalyst finally obtained has more excellent electrolytic water catalysis and stability than commercial Raney nickel electrocatalysts, can effectively improve the efficiency of oxygen evolution reaction, and is easy to operate and mass produce, which significantly improves the economic benefits of recycling waste lithium iron phosphate batteries. The present invention realizes catalyst preparation and lithium element extraction by immersing the obtained material in an oxidizing solution to extract the remaining lithium in the material. The high-value lithium element extracted from the waste lithium iron phosphate battery is converted into high-value, high-quality pure lithium compounds. Lithium is an indispensable and important material in current new energy batteries, and its demand is increasing year by year. Through the application of this technical solution, it is possible to achieve efficient recovery of the available lithium resources still contained in waste batteries, improve resource utilization, and provide more raw material support for the new energy battery industry. This unique method not only improves the economic benefits of waste battery recycling, but also realizes the comprehensive utilization of resources and efficient conversion of energy, which has important economic and environmental significance.

[0114] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element, characterized in that: The method comprises the following steps: (1) obtaining a positive electrode sheet from a recycled waste lithium iron phosphate power battery, separating a positive electrode material and a current collector in the positive electrode sheet, preparing the obtained positive electrode material into a positive electrode material powder, and recovering retired lithium iron phosphate powder from the obtained positive electrode material powder; (2) mixing the retired lithium iron phosphate powder recovered in step (1) with the nickel-coated raw material to react and obtain a composite structure of nickel-coated lithium iron phosphate material; (3) soaking the composite structure of the nickel compound-coated lithium iron phosphate material obtained in step (2) in an oxidizing solvent to dissolve the remaining lithium ions in the composite structure of the nickel compound-coated lithium iron phosphate material, and separating the required electrolytic water oxygen evolution reaction catalyst from the soaking solution; the soaking solution containing lithium ions is further recrystallized to precipitate into lithium salts to extract the lithium element.

2. The method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element according to claim 1, characterized in that: After step (3), the method further comprises the following steps: (4) The water electrolysis oxygen evolution reaction catalyst, conductive agent and binder obtained in step (3) are mixed and uniformly dispersed in a solvent to obtain a first dispersion liquid, and the first dispersion liquid is dropped onto a target electrode to obtain a water electrolysis anode electrode.

3. The method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element according to claim 1, characterized in that: Step (1) specifically includes the following process: Dismantling the recycled waste lithium iron phosphate power battery after full discharge, and using a first organic solvent to clean the side reaction products and residual lithium salt electrolyte on the surface of the positive electrode to obtain a positive electrode; Separating the positive electrode material and the current collector in the positive electrode sheet, and drying and grinding the obtained positive electrode material into positive electrode material powder; After collecting the positive electrode material powder, the residual binder in the powder is washed with a second organic solvent and dried to obtain retired lithium iron phosphate powder.

4. The method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element according to claim 1, characterized in that: In step (2), the composite structure of the nickel compound-coated lithium iron phosphate material includes lithium iron phosphate particles and a coating layer coating the lithium iron phosphate particles, and the thickness of the coating layer is within 1 / 5 of the diameter of the lithium iron phosphate particles; The coating layer material is one or more of nickel oxide, nickel hydroxide, nickel sulfide, nickel selenide, nickel phosphide and nickel nitride.

5. The method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element according to claim 1, characterized in that: In step (2), the composite structure of the nickel compound-coated lithium iron phosphate material is prepared by a one-step hydrothermal / solvothermal method or a two-step method.

6. The method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element according to claim 5, characterized in that: The one-step hydrothermal / solvothermal method comprises the following steps: dispersing lithium iron phosphate and nickel compound coated raw materials in a hydrothermal / solvothermal solvent for hydrothermal or solvothermal reaction to obtain a second dispersion, heating the second dispersion to react, and obtaining a composite structure of nickel compound coated lithium iron phosphate material; The hydrothermal / solvothermal solvent includes one or more of mesitylene, dimethylformamide, benzyl alcohol, diethylene glycol, ethanol, and water; The nickelide coating raw material includes a nickel source; The nickel source includes one or more of nickel acetylacetonate, nickel nitrate, nickel chloride, nickel acetate, and nickel sulfate; Additives are also dispersed in the hydrothermal / solvothermal solvent used for the hydrothermal or solvothermal reaction, and are used to adjust the reaction environment.

7. The method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element according to claim 6, characterized in that: The nickel compound coating raw material also includes an anion source; The anion source includes one or more of thiourea, sodium thiosulfate, sulfur powder, selenium powder, selenium oxide, ammonium dihydrogen phosphate, phosphorus powder, and sodium hypophosphite.

8. The method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element according to claim 5, characterized in that: The two-step method comprises the following steps: (2-1) dispersing lithium iron phosphate and nickel compound coating raw materials in a hydrothermal / solvothermal solvent, and preparing a lithium iron phosphate precursor coated with nickel hydroxide or nickel oxide by a hydrothermal / solvothermal method; (2-2) heat-treating the anion source and the lithium iron phosphate precursor in an inert gas atmosphere, and obtaining a composite structure of the nickel compound-coated lithium iron phosphate material after cooling; In step (2-1), the hydrothermal / solvothermal solvent includes one or more of mesitylene, dimethylformamide, benzyl alcohol, diethylene glycol, ethanol, and water; The nickelide coating raw material includes a nickel source; The nickel source includes one or more of nickel acetylacetonate, nickel nitrate, nickel chloride, nickel acetate, and nickel sulfate; In step (2-2), the anion source includes one or more of selenium powder, sulfur powder, phosphorus powder, and sodium hypophosphite; In step (2-1), an additive is dispersed in the hydrothermal / solvothermal solvent used for the hydrothermal or solvothermal reaction, and the additive is used to adjust the reaction environment.

9. The method for recycling waste lithium iron phosphate positive electrode powder for preparing high-performance water electrolysis anode catalyst and extracting lithium element according to claim 1, characterized in that: In step (3), the oxidizing solvent is a solution having a standard electrode potential exceeding the standard electrode potential of lithium iron phosphate; Step (3) specifically includes the following steps: The composite structure of the nickel compound-coated lithium iron phosphate material is immersed in an oxidizing solvent to dissolve the remaining lithium ions in the composite structure of the nickel compound-coated lithium iron phosphate material, and after the reaction, the desired delithiated water electrolysis oxygen evolution reaction catalyst solid is separated from the immersion solution by centrifugation; The collected lithium ion-containing soaking solution is evaporated and concentrated to improve the efficiency of lithium element extraction, and then a purifying agent is added to the solution to adjust the pH value of the solution, so that the impure metal ions are precipitated in the form of hydroxide precipitation and filtered to obtain a purified lithium ion-containing soaking solution; A recrystallization additive is added to the purified lithium ion-containing soaking solution to precipitate the lithium ions into lithium salts, thereby achieving the extraction of lithium elements.

Citation Information

Patent Citations

  • Method for preparing efficient oxygen evolution catalyst from lithium iron phosphate cathode material of waste lithium ion battery

    CN111659399A

  • Method for large-scale preparation of efficient electrolyzed water catalyst by using positive electrode material of waste lithium ion batteries

    CN113355690A

  • Method for preparing iron-based carbon / foamed nickel composite catalyst based on waste lithium iron phosphate electrode material

    CN116005191A

  • Method for preparing electrocatalyst by utilizing positive electrode material of waste lithium ion battery

    CN116565366A

  • Doped lithium iron phosphate encapsulated in ligand, and preparation method therefor and use thereof

    US20240222626A1

Cited By

  • Recycling method of lithium ion battery electrode plate

    CN120015990A

  • A method for recycling lithium-ion battery electrode sheets

    CN120015990B

  • Method for rapidly repairing waste lithium iron phosphate

    CN120364669A