Preparation method of perovskite layer, coating equipment and perovskite solar cell
By using nitrogen and amine gas or liquid gases or liquids to slow down crystallization during the coating process of perovskite solar cells, and combined with infrared irradiation, the problem of preferential crystallization on the surface of perovskite film is solved, and the uniformity of the perovskite layer is improved and photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202411028103.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
During the coating process of perovskite solar cells, the preferential crystallization of the perovskite film surface leads to uneven crystallization, affecting the photoelectric conversion efficiency.
By setting a wind knife in the backward direction of the coating device, airflow containing nitrogen and amine gases or liquids is blown out, the crystallization speed of the perovskite liquid film surface is delayed, the surface is prevented from crystallizing first, and infrared irradiation is used after the coating is completed. Promote uniform crystallization.
The uniform crystallization of the perovskite layer is achieved, and the photoelectric conversion efficiency and layer quality of the perovskite solar cells are improved.
Smart Images

Figure CN118973353A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells and the technical field of photovoltaic device manufacturing, and in particular to a method for preparing a perovskite layer, a coating device, a perovskite solar cell, a photovoltaic module and a photovoltaic system. Background Art
[0002] The coating method is a method for preparing a perovskite layer. The coating method refers to applying a precursor solution on a substrate and using an air knife to blow air to volatilize the solvent in the precursor solution. The obtained perovskite film is crystallized to form a perovskite layer.
[0003] However, during the coating process, after the solvent evaporates, the surface of the perovskite film will crystallize preferentially, forming a situation where crystallization occurs from the surface to the bottom; this will cause the perovskite film to be layered up and down, with uneven crystallization and holes at the bottom, affecting the photoelectric conversion efficiency of the perovskite solar cell. Summary of the invention
[0004] The embodiments of the present application provide a method for preparing a perovskite layer, a coating device, a perovskite solar cell, a photovoltaic module, and a photovoltaic system to solve or alleviate one or more technical problems in the prior art.
[0005] As a first aspect of an embodiment of the present application, an embodiment of the present application provides a method for preparing a perovskite layer, comprising:
[0006] Using a coating device to coat a perovskite precursor solution toward a target substrate to form a perovskite liquid film on the target substrate;
[0007] The wind knife is located on the side of the coating device that is opposite to the coating direction; the wind knife is used to blow out an airflow, and the airflow flows to the surface of the perovskite liquid film. The airflow includes a first component that takes away the solvent in the perovskite liquid film, and a second component that slows down the crystallization speed of the surface of the perovskite liquid film.
[0008] In one embodiment, the first component includes nitrogen; the second component includes: amine gas or amine liquid.
[0009] In one embodiment, the second component includes one or more of butylamine solution, phenylethylamine solution, amine gas or amine mixed gas.
[0010] In one embodiment, an air knife is used to blow out an air flow, and the air flow flows toward the surface of the perovskite liquid film, which includes:
[0011] In the case where the second component is an amine gas, the gas of the first component is mixed with the amine gas to obtain a mixed gas, so that the air knife blows out a flow of the mixed gas; or
[0012] When the second component is an amine liquid, the gas of the first component is passed through the amine solution, so that the air knife blows out a first component gas flow containing the amine solution.
[0013] In one embodiment, when the second component is an amine gas, the wind knife includes: a first wind knife and a second wind knife; the wind knife is used to blow out an airflow, and the airflow flows to the surface of the perovskite liquid film, including:
[0014] The first air knife blows out a first airflow, the first airflow includes a first component; the first airflow flows toward the surface of the perovskite liquid film;
[0015] The second air knife blows out a second airflow, which includes a second component; the second airflow flows toward the surface of the perovskite liquid film.
[0016] In one embodiment, the mass ratio of the first component to the second component is 10:1 to 2:1.
[0017] In one embodiment, it further includes:
[0018] An infrared irradiation device is used to emit infrared light to irradiate the surface of the perovskite liquid film. The infrared irradiation device is located on the side of the wind knife that is not facing the coating direction. The distance between the infrared irradiation device and the wind knife is adapted to the size of the target substrate along the coating direction.
[0019] As a second aspect of the embodiment of the present application, the embodiment of the present application further provides a coating device for implementing the preparation method of any implementation aspect of the above-mentioned embodiment, and the coating device includes:
[0020] A conveying device, the conveying device includes a conveyor belt; the conveying device is used to convey the target substrate from the input end of the conveyor belt to the output end of the conveyor belt;
[0021] A coating device is mounted above the conveyor belt, and is used to coat the perovskite precursor solution on the target substrate;
[0022] The wind knife is located on one side of the coating device close to the output end. The wind knife is used to blow out airflow, and the airflow flows to the surface of the perovskite liquid film; the airflow includes a first component that takes away the solvent in the perovskite liquid film, and a second component that delays the crystallization speed of the surface of the perovskite liquid film.
[0023] In one embodiment, the coating device further includes: an infrared irradiation device, which is disposed on a side of the air knife close to the output end.
[0024] As a third aspect of the embodiments of the present application, the embodiments of the present application further provide a perovskite solar cell, comprising a perovskite layer, wherein the perovskite layer is prepared by the preparation method of any implementation aspect of the above embodiments.
[0025] As a fourth aspect of the embodiments of the present application, the embodiments of the present application further provide a photovoltaic module, including: at least one battery string, the battery string including at least two perovskite solar cells according to any of the implementation aspects of the above embodiments.
[0026] As a fifth aspect of the embodiments of the present application, the embodiments of the present application further provide a photovoltaic system, comprising a photovoltaic component according to any one of the implementation aspects of the above embodiments.
[0027] The embodiment of the present application adopts the above-mentioned technical solution. By introducing an airflow including a second component that delays the crystallization rate of the surface of the perovskite liquid film into the surface of the perovskite liquid film, the airflow blowing toward the surface of the perovskite liquid film can delay the crystallization of the surface of the liquid film, so that when the entire perovskite liquid film is coated, the entire perovskite liquid film is uniformly crystallized, thereby improving the quality of the perovskite layer.
[0028] The above summary is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present application will be readily apparent by reference to the accompanying drawings and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0030] Figure 1 A schematic flow chart of a method for preparing a perovskite layer according to an embodiment of the present application is shown.
[0031] Figure 2 A schematic flow chart of a method for preparing a perovskite layer according to another embodiment of the present application is shown.
[0032] Figure 3 A schematic structural diagram of a coating device according to an embodiment of the present application is shown. DETAILED DESCRIPTION
[0033] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0034] Perovskite solar cells are solar cells that use perovskite-type organic metal halide semiconductors as light-absorbing materials and belong to the third generation of solar cells. Due to their light weight, low cost, and high conversion efficiency, they have become an important development direction of photovoltaic cell technology in the future.
[0035] Perovskite solar cells include a perovskite layer made from a perovskite precursor solution. The perovskite precursor solution is applied to a target substrate to obtain a perovskite liquid film, and an air flow is blown in by a wind knife to cause the solvent to evaporate, so that the perovskite liquid film nucleates and crystallizes. However, in the existing method, the perovskite precursor solution has not yet been applied to the target substrate, and the surface of the previously applied perovskite liquid film has begun to crystallize, so that the perovskite liquid film crystallizes from the surface to the bottom, resulting in uneven crystal phases, which affects the photoelectric conversion efficiency of the perovskite solar cell.
[0036] Based on this, an embodiment of the present application provides a method for preparing a perovskite layer to solve the surface preferential crystallization of the perovskite liquid film and a series of problems caused by the surface preferential crystallization.
[0037] Figure 1 A schematic diagram of a process for preparing a perovskite layer according to an embodiment of the present application is shown. Figure 1 As shown, the preparation method comprises:
[0038] S210, using a coating device to coat a perovskite precursor solution toward a target substrate to form a perovskite liquid film on the target substrate.
[0039] The coating device includes a device using a doctor blade coating, a slit coating, a dip coating, a spin coating, a roller coating, and an ultrasonic spray coating.
[0040] The coating device is used to coat the perovskite precursor solution on the target substrate. It is understood that the coating device can also adopt various devices known to ordinary technicians in this field now and in the future, which will not be described in detail here.
[0041] In the embodiment of the present application, the perovskite precursor solution can be any solution that can be used to prepare a perovskite layer by a coating method, and there is no limitation on this.
[0042] The target substrate may be a substrate for preparing a perovskite layer according to the requirements for preparing a perovskite solar cell. For example, to prepare a single-junction perovskite solar cell, the target substrate may be a substrate including a conductive glass substrate, and an electron transport layer / hole transport layer is deposited on the conductive glass substrate. A perovskite layer is prepared on the target substrate, and then a hole transport layer / electron transport layer and an electrode layer are deposited on the perovskite layer to obtain a perovskite solar cell.
[0043] In some other examples, the target substrate may be a plate that does not belong to the layer structure in the perovskite solar cell, for example, a glass plate. A perovskite precursor solution is coated on the glass plate to obtain a perovskite thin film layer. An electron transport layer is then deposited on one side of the perovskite thin film layer, a hole transport layer is deposited on the other side, and the remaining layers are then deposited to obtain a perovskite solar cell.
[0044] The coating device coats the perovskite precursor solution toward the target substrate. The coating device may be filled with the perovskite precursor solution, and then the perovskite precursor solution is coated on the target substrate by coating.
[0045] The coating device coats the perovskite precursor solution toward the target substrate, and the coating device may move relative to the target substrate so that the coating device coats the perovskite precursor solution on the target substrate at a certain speed. The coating device may move, or the target substrate may move.
[0046] S220, the wind knife is located on the side of the coating device that is opposite to the coating direction; the wind knife is used to blow out an airflow, and the airflow flows to the surface of the perovskite liquid film; the airflow includes a first component that takes away the solvent in the perovskite liquid film, and a second component that delays the crystallization speed of the surface of the perovskite liquid film.
[0047] The target substrate moves relative to the coating device. Before coating begins, the target substrate includes a first end close to the coating device and a second end away from the coating device, and the second end is opposite to the first end. During coating, coating starts from the first end and gradually moves until coating to the second end of the target substrate. The coating direction can be a direction from the first end of the target substrate toward the second end of the target substrate.
[0048] Before starting coating, the target substrate is located on the side of the coating device facing the coating direction, so that the coating device moves relative to the target substrate in the coating direction until the first end of the target substrate is located at the coating position of the coating device, and the coating device starts to coat the perovskite precursor solution on the target substrate.
[0049] The wind knife is located on the side of the coating device facing away from the coating direction, so that the first end of the target substrate moves toward the wind knife after being coated with the perovskite precursor solution by the coating device, so that the airflow blown by the wind knife can act on the surface of the coated perovskite liquid film.
[0050] On the target substrate, during the process of coating the perovskite liquid film, the coating device coats from the first end to the second end of the target substrate, and the wind knife starts to blow air from the first end of the target substrate until it blows to the second end of the target substrate. The wind knife can be started synchronously when the coating device is started, so as to blow air toward the perovskite liquid film in time when the target substrate passes by.
[0051] In an embodiment of the present application, the air flow blown out by the wind knife includes at least two components. The first component is a component that can take away the solvent in the perovskite liquid film, such as nitrogen, or other gases that can take away the solvent in the perovskite liquid film; the second component is a component that can slow down the crystallization rate of the surface of the perovskite liquid film. By slowing down the crystallization rate of the surface of the perovskite liquid film, it can be avoided that the surface of the perovskite liquid film begins to crystallize before the coating is completed, resulting in uneven crystallization.
[0052] In the embodiment of the present application, an air flow is blown toward the surface of the perovskite liquid film by a wind knife. When the solvent component of the perovskite liquid film is dried, a second component that delays the crystallization rate of the surface of the perovskite liquid film is blown in at the same time. By adding the second component in a suitable ratio, it can be ensured that before the coating is completed, the surface of the perovskite liquid film does not preferentially crystallize, so that the perovskite liquid film can be uniformly crystallized under a preset environment, thereby improving the quality of the obtained perovskite layer and the photoelectric conversion efficiency of the perovskite solar cell.
[0053] In one embodiment, the first component includes nitrogen; the second component includes: amine gas or amine liquid.
[0054] Nitrogen is used to remove the solvent components in the perovskite liquid film.
[0055] The first component may also be various substances known to ordinary technicians in the field now and in the future that can remove the solvent in the perovskite liquid film.
[0056] The amines in the amine gas or amine liquid can slow down the crystallization rate of the surface of the perovskite liquid film. The amines in the amine gas or amine liquid can dissolve the perovskite precursor solution and slow down its film formation and crystallization. When the amine gas or amine liquid contacts the surface of the perovskite liquid film, the surface crystallization of the perovskite liquid film can be slowed down.
[0057] The embodiment of the present application uses nitrogen and amine gas or amine liquid to prevent the surface of the perovskite liquid film from preferentially crystallizing during the coating process, resulting in uneven crystallization of the perovskite layer. Therefore, on this basis, a thicker perovskite layer can be prepared based on this solution without uneven crystallization.
[0058] In one embodiment, the second component includes one or more of butylamine solution, phenylethylamine solution, amine gas or amine mixed gas.
[0059] In an embodiment of the present application, the second component can be mixed with the gas of the first component in the form of gas or liquid, so that the airflow blown out by the wind knife includes the second component, and the second component contacts the surface of the perovskite liquid film, which can achieve the effect of slowing down the crystallization rate of the surface of the perovskite liquid film.
[0060] In one embodiment, before step S220, it includes: when the second component is amine gas, mixing the gas of the first component with the amine gas to obtain a mixed gas, so that the air knife blows out a flow of the mixed gas; or, when the second component is an amine liquid, passing the gas of the first component through an amine solution, so that the air knife blows out a flow of the first component dissolved in the amine solution.
[0061] In the embodiment of the present application, a wind knife is used to blow out a gas flow including a mixture of a first component and a second component. When the second component is a gas, the gases of the two components are first mixed in a preset ratio and then blown out in the form of a mixed gas. When the second component is a liquid, the gas of the first component flows through the second component, so that the amine solution can be dissolved in the gas of the first component, and the blown gas flow also includes the second component. After the amine in the second component contacts the perovskite liquid film, it can dissolve the lead and the like in the perovskite material and slow down its crystallization rate.
[0062] In one embodiment, when the second component is an amine gas, the wind knife includes: a first wind knife and a second wind knife; step S220 of "using the wind knife to blow out the airflow, and the airflow flows to the surface of the perovskite liquid film" may include:
[0063] The first air knife blows out a first airflow, the first airflow includes a first component; the first airflow flows toward the surface of the perovskite liquid film;
[0064] The second air knife blows out a second airflow, which includes a second component; the second airflow flows toward the surface of the perovskite liquid film.
[0065] In the embodiment of the present application, when the second component is an amine gas, two air knives can be used to blow airflows of different components to the surface of the perovskite liquid film. By using two air knives, the flow rate of the first air knife or the proportion of the first component in the first airflow can be adjusted based on the volatilization of the solvent; the flow rate of the second air knife or the proportion of the second component in the second airflow can be adjusted based on the components of the perovskite precursor solution. Through the two air knives, the amount of the two components can be adjusted based on the actual situation, quickly and accurately meet the needs, and improve the preparation efficiency of the perovskite layer.
[0066] In one embodiment, the mass ratio of the first component to the second component is 10:1 to 2:1.
[0067] The mass ratio of the first component to the second component can be determined according to the composition of the perovskite precursor solution, the size of the target substrate, the thickness of the coated perovskite layer, etc.
[0068] For example, based on the composition of the perovskite precursor solution, the flow rate of the first component and the flow rate of the second component can be determined respectively; then, based on the two flow rates, the proportion of each component is determined, and the gas flow including the first component and the second component is output according to the proportion.
[0069] In one embodiment, Figure 2 As shown, the method for preparing the perovskite layer may further include:
[0070] S230, using an infrared irradiation device to emit infrared light to irradiate the surface of the perovskite liquid film, the infrared irradiation device is located on the side of the wind knife that is not facing the coating direction. The distance between the infrared irradiation device and the wind knife is adapted to the size of the target substrate along the coating direction.
[0071] The infrared irradiation device emits infrared light to irradiate the surface of the perovskite liquid film, which can promote the crystallization of the perovskite liquid film and improve the efficiency of the perovskite liquid film crystallization. Based on the requirements of film crystallization, the relevant parameters of the infrared irradiation device are set.
[0072] The following specific examples further illustrate the present application, but should not be construed as limiting the present application. Without departing from the spirit and substance of the present application, modifications or replacements made to the methods, steps or conditions of the present application are within the scope of the present application.
[0073] First, a plurality of target substrates are prepared by the same method as described below. The preparation process of the target substrates includes:
[0074] S01, provides bright conductive glass.
[0075] The transparent conductive glass uses FTO (Fluorine-doped Tin Oxide Glass).
[0076] S02, depositing a hole transport layer on the transparent conductive glass.
[0077] A hole transport layer with a thickness of 15 nm was formed on the upper surface of the transparent conductive glass by magnetron sputtering.
[0078] Secondly, the perovskite precursor solution is coated on multiple target substrates by slit coating, and the following treatments are performed simultaneously to obtain the perovskite layer. The perovskite precursor solution is obtained by dissolving methylammonium in dimethyl sulfoxide.
[0079] [Example 1]
[0080] After the amine gas is mixed with nitrogen, it is blown onto the surface of the perovskite liquid film from the air knife. The mass ratio of the amine gas to the nitrogen gas is 1:5.
[0081] [Example 2]
[0082] Nitrogen is passed into the butylamine solution and then blown to the surface of the perovskite liquid film through an air knife.
[0083] [Comparative Example 1]
[0084] The nitrogen gas is introduced into the wind and blown to the surface of the perovskite liquid film through a wind knife.
[0085] Finally, the obtained perovskite layer is treated as follows:
[0086] S11, evaporate 25nm C on the upper surface of the perovskite layer 60 (
[60] Fullerene, carbon 60) as the first electron transport layer;
[0087] S12, on the upper surface of the first electron transport layer, a layer of tin dioxide (SnO2) is deposited by atomic layer deposition as a second electron transport layer with a thickness of 20 nm.
[0088] Based on the above steps, perovskite solar cells corresponding to Example 1, Example 2 and Comparative Example 1 were prepared.
[0089] The performance of the three perovskite solar cells prepared was tested to obtain the open circuit voltage Voc, short circuit current density Jsc, fill factor FF, and photoelectric conversion efficiency PCE of the corresponding battery devices. The test results are shown in Table 1.
[0090] Table 1. Performance test results of perovskite solar cells of Examples 1-2 and Comparative Example 1
[0091]
[0092] The data in Table 1 show that the short-circuit current density, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cells prepared by the methods of Example 1 and Example 2 are significantly improved.
[0093] The present application also provides a coating device for implementing the preparation method of any of the above embodiments, such as Figure 3 As shown, the coating equipment includes: a conveying device (a conveyor belt 200 is shown for simplicity), a coating device 300 and an air knife 400.
[0094] The conveying device includes a conveyor belt 200, which is used to convey the target substrate 100 from the input end of the conveyor belt 200 to the output end of the conveyor belt 200. The target substrate 100 is conveyed from the input end of the conveyor belt 200 toward the coating device 300, the air knife 400, etc.
[0095] The coating device 300 is mounted above the conveyor belt 200, and is used to coat the perovskite precursor solution on the target substrate 100. When the conveyor belt 200 transports the target substrate 100 to the bottom of the coating device 300, the coating device 300 coats the perovskite precursor solution. As the target substrate 100 moves, the coating device 300 coats the perovskite precursor solution from the first end of the target substrate 100 to the second end of the target substrate 100. The coating direction is as follows: Figure 3 Direction indicated by the arrow.
[0096] The air knife 400 is located on one side of the coating device 300 close to the output end. The air knife 400 blows out an airflow, and the airflow flows to the surface of the perovskite liquid film; the airflow includes a first component that takes away the solvent in the perovskite liquid film, and a second component that delays the crystallization speed of the surface of the perovskite liquid film. The target substrate 100 continues to move toward the output end to the bottom of the air knife 400, and the airflow blown by the air knife 400 can act on the surface of the perovskite liquid film on the target substrate 100 to promote the volatilization of the solvent and delay the crystallization of the surface of the perovskite liquid film.
[0097] In the embodiment of the present application, an airflow including a second component that slows down the crystallization rate of the surface of the perovskite liquid film is introduced into the surface of the perovskite liquid film. The airflow blowing toward the surface of the perovskite liquid film can slow down the crystallization of the surface of the liquid film, so that when the entire perovskite liquid film is coated, the entire perovskite liquid film is uniformly crystallized, thereby improving the quality of the perovskite layer.
[0098] In one embodiment, the coating device further includes: an infrared irradiation device 500 , which is disposed on a side of the wind knife 400 close to the output end.
[0099] The target substrate 100 continues to move from under the wind knife 400. The target substrate 100 has been coated with a layer of perovskite liquid film. When it moves to the infrared irradiation device 500, the perovskite liquid film can be irradiated by infrared light to promote film formation and crystallization. The infrared irradiation area of the infrared irradiation device 500 can match the size of the target substrate 100, so that when the target substrate 100 moves to under the infrared irradiation device 500, the perovskite liquid film on the target substrate 100 can be simultaneously affected by infrared and form a film and crystallize.
[0100] In one example, when the target substrate 100 moves to a predetermined position, the infrared irradiation device 500 is activated to irradiate infrared light. The predetermined position may be a position when the target substrate 100 is completely located below the infrared irradiation device 500 .
[0101] Other components of the coating device of the above embodiment may adopt various technical solutions known to ordinary technicians in this field now and in the future, and will not be described in detail here.
[0102] The embodiment of the present application also provides a perovskite solar cell, including a perovskite layer, wherein the perovskite layer is prepared by the preparation method of any implementation aspect of the above embodiment.
[0103] The perovskite solar cell may include a single-junction perovskite solar cell or a stacked perovskite solar cell. The perovskite solar cell may be any cell that requires a perovskite layer, wherein the perovskite layer is prepared by the preparation method provided in the embodiment of the present application, so that the perovskite solar cell has better photoelectric conversion efficiency.
[0104] Other structures of the perovskite solar cell in the above-mentioned embodiment may adopt various technical solutions known to ordinary technicians in this field now and in the future, and will not be described in detail here.
[0105] The present application also provides a photovoltaic module, including: at least one battery string, the battery string including at least two perovskite solar cells according to any of the above embodiments. Adjacent perovskite solar cells can be connected together by serial welding.
[0106] The present application also provides a photovoltaic system, including a photovoltaic module of any of the above embodiments. The advantages of the above photovoltaic modules are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic modules. For example, multiple photovoltaic modules may form multiple photovoltaic arrays. The photovoltaic array is connected to a junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.
[0107] In the description of this specification, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0108] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0109] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or a communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0110] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0111] The disclosure above provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described above. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numerals and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed.
[0112] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a perovskite layer, It is characterized in that include: Using a coating device to coat a perovskite precursor solution toward a target substrate to form a perovskite liquid film on the target substrate; The wind knife is located on the side of the coating device that is opposite to the coating direction; the wind knife is used to blow out an airflow, and the airflow flows to the surface of the perovskite liquid film; the airflow includes a first component that takes away the solvent in the perovskite liquid film, and a second component that slows down the crystallization speed of the surface of the perovskite liquid film.
2. The preparation method according to claim 1, It is characterized in that The first component includes nitrogen; the second component includes amine gas or amine liquid.
3. The preparation method according to claim 2, It is characterized in that The second component includes one or more of butylamine solution, phenylethylamine solution, amine gas or amine mixed gas.
4. The preparation method according to claim 2, It is characterized in that The air knife is used to blow out the air flow, and the air flow flows to the surface of the perovskite liquid film. Previously, it included: In the case where the second component is an amine gas, the gas of the first component is mixed with the amine gas to obtain a mixed gas, so that the air knife blows out a flow of the mixed gas; or When the second component is an amine liquid, the gas of the first component is passed through the amine solution, so that the air knife blows out a first component gas flow containing the amine solution.
5. The preparation method according to claim 2, It is characterized in that When the second component is an amine gas, the wind knife includes: a first wind knife and a second wind knife; the wind knife is used to blow out an airflow, and the airflow flows to the surface of the perovskite liquid film, including: The first air knife blows out a first airflow, the first airflow includes a first component, and the first airflow flows toward the surface of the perovskite liquid film; The second air knife blows out a second airflow, the second airflow includes a second component, and the second airflow flows toward the surface of the perovskite liquid film.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The mass ratio of the first component to the second component is 10:1 to 2:
1.
7. The preparation method according to any one of claims 1 to 5, It is characterized in that Also includes: An infrared irradiation device is used to emit infrared light to irradiate the surface of the perovskite liquid film. The infrared irradiation device is located on the side of the wind knife that is not facing the coating direction. The distance between the infrared irradiation device and the wind knife is adapted to the size of the target substrate along the coating direction.
8. A coating device, It is characterized in that For implementing the preparation method according to any one of claims 1 to 7, the coating device comprises: A conveying device, the conveying device includes a conveyor belt; the conveying device is used to convey the target substrate from the input end of the conveyor belt to the output end of the conveyor belt; A coating device is mounted above the conveyor belt, and is used to coat the perovskite precursor solution on the target substrate; The wind knife is located on one side of the coating device close to the output end. The wind knife is used to blow out airflow, and the airflow flows to the surface of the perovskite liquid film; the airflow includes a first component that takes away the solvent in the perovskite liquid film, and a second component that delays the crystallization speed of the surface of the perovskite liquid film.
9. The coating device according to claim 8, It is characterized in that Also includes: The infrared irradiation device is arranged on one side of the wind knife close to the output end.
10. A perovskite solar cell, It is characterized in that The invention comprises a perovskite layer, wherein the perovskite layer is prepared by the preparation method according to any one of claims 1 to 7.
11. A photovoltaic module, It is characterized in that The invention comprises: at least one battery string, wherein the battery string comprises at least two perovskite solar cells as claimed in claim 10.
12. A photovoltaic system, It is characterized in that Comprising the photovoltaic module as claimed in claim 11.