Cosmetic
By using composite particles in solid powder cosmetics, combining inorganic nucleating agents and metal soaps, the problem of insufficient adhesion and final effect after application is solved, and excellent coating effect and sense of use is achieved. It is suitable for many A kind of cosmetics.
Patent Information
- Application Number
- CN202380032290.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-06
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, solid powder cosmetics have shortcomings in their adhesion, final effect and sense of use after application, especially the application effect of the skin, lips, eyelashes, etc. has not been recorded and guided in detail.
Cosmetics containing composite particles are used, where the composite particles are composed of inorganic nucleating agents and metal soaps, specifically including glass particles and insoluble sulfate particles. By controlling the internal introduction rate, particle size distribution and component ratio of composite particles, the coating is improved. afterwards and final effect.
In addition to good coating and spreadability during application, it also has excellent adhesion and final effect after application, and has a good sense of use, which is suitable for a variety of cosmetics types.
Smart Images

Figure BDA0005069326860000251 
Figure BDA0005069326860000281 
Figure BDA0005069326860000291
Abstract
Description
Technical Field
[0001] The present disclosure relates to cosmetics. Background Art
[0002] Patent Document 1 discloses a solid powder cosmetic using a metal soap, wherein the metal soap is a metal soap that can impart high dispersibility or coating properties to the powder and can improve the anti-coagulation property, fluidity, or touch of the powder.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. WO2016 / 132967 Summary of the invention
[0006] Problems to be solved by the invention
[0007] Patent Document 1 discloses that metal soap particles containing specific inorganic particles and metal soap exhibit good ductility, but there is no description or suggestion of the adhesion after application to the skin, lips, eyelashes, etc., which are important characteristics of cosmetics. In addition, Patent Document 1 does not describe or suggest the important characteristics of formability, handling, and adhesion resistance, etc., such as solid powder cosmetics represented by powder foundation.
[0008] The object of the present disclosure is to provide a novel cosmetic material which is excellent in not only spreadability during application but also adhesion after application and / or final effect after application and has a good feeling during use.
[0009] Means for solving problems
[0010] This disclosure includes the following methods:
[0011] [Item 1]
[0012] A cosmetic comprising composite particles, wherein:
[0013] The composite particles contain an inorganic nucleating agent and a metal soap,
[0014] The inorganic nucleating agent is at least one selected from glass particles and insoluble sulfate particles.
[0015] The metal soap is a salt of a fatty acid and at least one selected from calcium and magnesium.
[0016] [Item 2]
[0017] The cosmetic according to item 1, wherein
[0018] The amount of the inorganic nucleating agent in the composite particles is 0.1 wt % or more and 30 wt % or less.
[0019] [Item 3]
[0020] The cosmetic according to item 1 or 2, wherein
[0021] The internal introduction rate A represented by the following formula (1) is 25% or more,
[0022] Internal introduction rate A = 100-(X / X') × 100 (1)
[0023] [In formula (1),
[0024] X is the surface content of the inorganic nucleating agent in the composite particles,
[0025] X' is the total content of the inorganic nucleating agent in the composite particles,
[0026] X and X' are the average values obtained by performing elemental analysis at three locations within a 15 μm square range on the composite particles before and after homogenization by SEM / EDX at an accelerating voltage of 10 kV and a height of 15 mm].
[0027] [Item 4]
[0028] The cosmetic according to any one of items 1 to 3, wherein
[0029] The particle size summary value B expressed by the following formula (2) is 3 or less,
[0030] Particle size summary value B-(D90-D10) / D50···(2)
[0031] [In formula (2),
[0032] D10 is the 10% cumulative diameter (μm) of the composite particles on a volume basis,
[0033] D50 is the 50% cumulative diameter (μm) of the composite particles on a volume basis.
[0034] D90 is the 90% cumulative diameter (μm) on a volume basis of the composite particles.
[0035] [Item 5]
[0036] The cosmetic according to any one of items 1 to 4, wherein
[0037] The glass particles are silicate glass particles.
[0038] [Item 6]
[0039] The cosmetic according to any one of items 1 to 5, wherein
[0040] The inorganic nucleating agent is at least one selected from borosilicate glass particles and barium sulfate particles.
[0041] [Item 7]
[0042] The cosmetic according to any one of items 1 to 6, wherein
[0043] The fatty acid has 8 or more and 22 or less carbon atoms.
[0044] [Item 8]
[0045] The solid powder cosmetic according to any one of items 1 to 7, wherein
[0046] The amount of the composite particles in the cosmetic is 1% by weight or more and 75% by weight or less.
[0047] [Item 9]
[0048] The cosmetic according to any one of items 1 to 8, wherein
[0049] The cosmetic further comprises an oily component,
[0050] The amount of the oily component in the cosmetic is 0.1% by weight or more and 20% by weight or less.
[0051] [Item 10]
[0052] The cosmetic according to any one of items 1 to 9, wherein
[0053] The cosmetic further comprises spherical particles,
[0054] The 50% cumulative value of the spherical particles on a volume basis is 1 μm or more and 30 μm or less,
[0055] The amount of the spherical particles in the cosmetic is 1% by weight or more.
[0056] [Item 11]
[0057] The cosmetic according to any one of Items 1 to 10, which is a solid powder cosmetic.
[0058] Effects of the Invention
[0059] According to the present disclosure, it is possible to provide a novel cosmetic material which is excellent in not only spreadability during application but also adhesion and final effect after application and has a good feeling during use. DETAILED DESCRIPTION
[0060] <Cosmetics>
[0061] The cosmetic disclosed herein contains at least composite particles.
[0062] 〔Composite particles〕
[0063] The composite particles of the present disclosure include an inorganic nucleating agent and a metal soap.
[0064] [Inorganic nucleating agent]
[0065] The inorganic nucleating agent is an inorganic particle that can function as a nucleus when the composite particles are generated. The inorganic nucleating agent may be at least one selected from glass particles and sparingly soluble sulfate particles.
[0066] The glass particles may be various glass particles with an amorphous three-dimensional mesh-like inorganic oxide structure as the main component. For example, preferably, the glass particles are composed of one or more oxides of elements selected from Si, B, Al, Ba, Ca, Mg, Li, Na, K, Zn, Sr, Sn, Zr, Sb, Bi, Te, Pb, W, Ti, Y and Ag. As preferred examples of the components of the glass particles, glass particles containing at least one selected from SiO2, B2O3, Al2O3, BaO, CaO, MgO, ZnO, SrO, ZrO2, Bi2O3, PbO, Y2O3, TeO2, WO3, TiO2, R2O (R represents an alkali metal such as Na, K, Li) can be cited. As an example of glass particles that can be used, silicate glass containing SiO2 and metal components as the main components is preferred. Borosilicate glass containing components such as boron oxide (B2O3) is particularly preferred. Specific examples of glass particles include silicate glass, borosilicate glass, soda-lime glass, soda glass, fused quartz glass, alkali-free glass, aluminosilicate glass, boroaluminosilicate glass, aluminosilicate glass, lithium aluminosilicate glass, alkali-barium glass, lead glass, bismuth-based glass, etc. These can be used alone or in combination of two or more. In one embodiment, borosilicate (Ca / Al) can be used as the glass particles.
[0067] A sparingly soluble sulfate is a sulfate that is sparingly soluble in water. The water solubility (20°C) of the sparingly soluble sulfate can be 1g / 100mlL or less, 0.5g / 100mlL or less, 0.1g / 100mlL or less, 0.05g / 100mlL or less, 0.01g / 100mlL or less, preferably 0.1g / 100mL or less. As specific examples of sparingly soluble sulfates, anhydrous or hydrates of barium sulfate, calcium sulfate, lead sulfate, silver sulfate, strontium sulfate, etc. can be cited. These can be used alone or in combination of two or more. In one embodiment, barium sulfate can also be used as the sparingly soluble sulfate.
[0068] The 50% cumulative diameter (D50) of the volume basis of the inorganic nucleating agent can be 0.1 μm or more, 1 μm or more, 3 μm or more, 5 μm or more, 10 μm or more, 20 μm or more, or 30 μm or more, preferably 1 μm or more, more preferably 3 μm or more, and further preferably 5 μm or more. The 50% cumulative diameter (D50) of the volume basis of the inorganic nucleating agent can be 100 μm or less, 75 μm or less, 50 μm or less, 20 μm or less, 10 μm or less, or 5 μm or less, preferably 50 μm or less, and more preferably 20 μm or less. By being within the above range, while having the function of serving as a crystal nucleus, the internal introduction rate A described later can also be increased, the particle size of the obtained composite particles can be finer, and the particle shape can be uniform. It should be noted that the particle size distribution of the inorganic nucleating agent can be unimodal or multimodal, for example, unimodal.
[0069] In the present disclosure, particle diameters such as 50% cumulative diameter (D50) can be measured by laser diffraction. Laser diffraction is a method of obtaining the particle diameter using scattered light obtained by irradiating a laser to the particle. In the present disclosure, the particle diameter can be measured by a wet method in which a sample is directly put into the particle while circulating a dispersion medium such as an organic solvent such as ethanol or isopropanol. As a measuring device, for example, Microtrac MT-3000 manufactured by Nikkiso Co., Ltd. can be used.
[0070] (Amount of inorganic nucleating agent)
[0071] The amount of the inorganic nucleating agent in the composite particles may be 0.1% by weight or more, 0.5% by weight or more, 1% by weight or more, 3% by weight or more, 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, or 30% by weight or more, preferably 5% by weight or more, more preferably 10% by weight or more, and further preferably 15% by weight or more. The amount of the inorganic nucleating agent in the composite particles may be 60% by weight or less, 50% by weight or less, 40% by weight or less, 35% by weight or less, 30% by weight or less, 25% by weight or less, 22.5% by weight or less, 20% by weight or less, 17.5% by weight or less, 15% by weight or less, 12.5% by weight or less, or 10% by weight or less, preferably 50% by weight or less, more preferably 45% by weight or less, and further preferably 40% by weight or less. By making the amount of the inorganic nucleating agent within the above range, the internal introduction rate A can be increased, the particle size of the obtained composite particles can be made fine, and the particle shape can be made uniform, so that the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic can be well exerted.
[0072] [Metallic Soap]
[0073] The metal soap may be a metal soap which is a salt of a fatty acid and at least one selected from calcium and magnesium. The metal soap may be a layer which covers at least a part of the inorganic nucleating agent.
[0074] The metal soap can be any kind of saturated fatty acid salt and unsaturated fatty acid salt, and can also be any kind of straight chain and branched chain. In addition, the fatty acid structure can also contain functional groups such as hydroxyl, aldehyde, epoxy group. As metal soap, for example, caproate, heptanoate, caprylate, caprate, laurate, myristate, palmitate, stearate, arachidate, and behenate can be cited. These can be used alone, or two or more can be used in combination. In one embodiment, at least one selected from myristate, laurate, palmitate, and stearate can also be used as the metal soap.
[0075] The salt in the metal soap is calcium or magnesium, and either one of them may be used or both may be used in combination.
[0076] The carbon number of the fatty acid in the metal soap may be 6 or more, 8 or more, 10 or more, 12 or more, 14 or more, or 16 or more, preferably 8 or more, and more preferably 12 or more. The carbon number of the fatty acid in the metal soap may be 26 or less, 24 or less, 22 or less, 20 or less, 18 or less, 16 or less, or 14 or less, preferably 22 or less, and more preferably 20 or less. When the carbon number of the fatty acid in the metal soap is within the above range, the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic can be well exerted.
[0077] (Amount of Metal Soap)
[0078] The amount of metal soap in the composite particles can be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, or 99% by weight or more, or 99.9% by weight or more, preferably 50% by weight or more, more preferably 55% by weight or more, and further preferably 60% by weight or more. The amount of metal soap in the composite particles can be 99.9% by weight or less, 95% by weight or less, 90% by weight or less, 85% by weight or less, 80% by weight or less, 75% by weight or less, 70% by weight or less, or 65% by weight or less, preferably 95% by weight or less, 90% by weight or less, or 85% by weight or less. By making the amount of metal soap within the above range, the internal introduction rate A can be increased, the particle size of the obtained composite particles can be made fine, and the particle shape can be made uniform, so that the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic material can be well exerted.
[0079] [Other ingredients]
[0080] The composite particles may contain other components other than the above, within the range that the effects disclosed in the present application are not lost. Examples of other components include inorganic particle components other than the above, metal soap components other than the above, and various other additive components.
[0081] [Characteristics of composite particles]
[0082] The internal introduction rate A, the particle size summary value B, the degree of agglomeration C, the loose packing density D, and the average circularity E of the composite particles described below may have values in specific ranges described below.
[0083] (A internal introduction rate)
[0084] The composite particles disclosed herein contain an inorganic nucleating agent and a metal soap, and the inorganic nucleating agent is introduced into the interior of the composite particles. The composite particles preferably have an internal introduction rate A within a specific range shown below. The internal introduction rate A is an indicator indicating the degree to which the inorganic nucleating agent is biased toward the interior of the composite particles. Specifically, the internal introduction rate A is obtained from the following formula (1).
[0085] Internal introduction rate A = 100-(X / X') × 100 (1)
[0086] [Wherein,
[0087] X is the surface content of the inorganic nucleating agent in the composite particles,
[0088] X' is the total content of the inorganic nucleating agent in the composite particles,
[0089] X and X' are the average values obtained by performing elemental analysis at three locations within a 15 μm square range on the composite particles before and after homogenization by SEM / EDX at an accelerating voltage of 10 kV and a height of 15 mm].
[0090] In the composite particles disclosed herein, the internal introduction rate A may be 25% or more, 30% or more, 40% or more, 50% or more, or 60% or more, preferably 40% or more, more preferably 50% or more, and further preferably 60% or more. By making the internal introduction rate A within the above range, the proportion of the inorganic nucleating agent that contributes to the crystal shape and powder properties of the composite particles generated during the double decomposition reaction becomes high, thereby making it easy to obtain the desired particle size summary value B, cohesion C, and average roundness E.
[0091] Although the elements contained in the composite particles can be quantified by scanning electron microscopy / energy dispersive X-ray spectroscopy (SEM / EDX), the inorganic nucleating agent introduced into the interior of the composite particles cannot be detected by SEM / EDX. Therefore, the more the inorganic nucleating agent is concentrated in the interior of the composite particles, the smaller the calculated value of the inorganic nucleating agent content in the composite particles is compared with the case where the inorganic nucleating agent is homogenized. In other words, the more the inorganic nucleating agent is concentrated in the interior of the composite particles, the smaller the surface content X is compared with the overall content X', and the greater the internal introduction rate.
[0092] Homogenization may be performed by crushing the composite particles. As in the preparation of powder samples such as EDX and IR, the crushing should be performed as finely as possible and in a manner that the overall content of the inorganic nucleating agent in the composite particles is as close to the true value as possible. For example, the composite particles may be crushed until they pass through a 325-mesh filter. The crushing method is not particularly limited, and for example, a crushing method using a mortar or various grinding devices may be used.
[0093] (B granularity summary value)
[0094] The composite particles used in the present disclosure preferably have a particle size summary value B in a specific range shown below. The particle size summary value B is an indicator of the deviation of the particle size. By making the particle size summary value B within a specific range and having a specific particle size distribution, it is possible to make the coating more uniform when used for powders, thereby making it easier to more stably exert the effects of the present disclosure. Specifically, the particle size summary value B is obtained from the following formula (2).
[0095] Particle size summary value B = (D90-D10) / D50 (2)
[0096] D10: 10% cumulative diameter of composite particles based on volume (μm)
[0097] D50: 50% cumulative diameter of composite particles based on volume (μm)
[0098] D90: 90% cumulative diameter of composite particles based on volume (μm)
[0099] The particle size summary value B may be 0.1 or more, 0.6 or more, 0.8 or more, 1 or more, 1.2 or more, 1.4 or more, preferably 0.8 or more, and more preferably 1 or more. The particle size summary value B may be 3 or less, 2.7 or less, 2.5 or less, 2.2 or less, 2 or less, 1.8 or less, 1.3 or less, 1 or less, or 0.8 or less, preferably 2.5 or less, and more preferably 2.2 or less. By making the particle size summary value B within the above range, the deviation of the particle size of the composite particles is small, and the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic material can be well exerted.
[0100] The 50% cumulative diameter (D50) of the composite particles on a volume basis can be 1 μm or more, 3 μm or more, 5 μm or more, 10 μm or more, 30 μm or more, 50 μm or more, 75 μm or more, 100 μm or more, preferably 1 μm or more. The 50% cumulative diameter (D50) of the composite particles on a volume basis can be 150 μm or less, 125 μm or less, 100 μm or less, 75 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less, 15 μm or less, or 10 μm or less, preferably 30 μm or less. By being within the above range, the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic can be well exerted. The particle size summary value B can be calculated from the particle size (cumulative diameter) measured by the laser diffraction method. The particle size distribution of the composite particles can be unimodal or multimodal, for example, unimodal.
[0101] (C cohesion)
[0102] The composite particles used in the present invention preferably have a cohesion degree C in a specific range as shown below. It is an index indicating the ease of disintegration of the composite particles. The particles on the sieve are vibrated without applying a load, and the degree of fine disintegration is quantified based on the residues on the sieves with different apertures. The cohesion degree C is measured by a powder tester when placed in an environment of 80°C for 10 minutes, and is obtained by the following formula (3).
[0103] Agglomeration degree C = [(mass of composite particles remaining on a sieve with a mesh size of 350 μm) / 2] × 100 × (1 / 1) + [(mass of composite particles remaining on a sieve with a mesh size of 250 μm) / 2] × 100 × (3 / 5) + [(mass of composite particles remaining on a sieve with a mesh size of 150 μm) / 2] × 100 × (1 / 5)] ... (3) Formula
[0104] The cohesion degree C may be 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, 5% or more, or 10% or more, preferably 2% or more. The cohesion degree C may be 50% or less, 40% or less, 30% or less, 25% or less, 20% or less, 15% or less, or 10% or less, preferably 25% or less, more preferably 15% or less. By being within the above range, the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic can be well exerted.
[0105] The degree of aggregation C of the composite particles measured by the powder tester used here is a value obtained by the following measurement method. That is, for example, the following steps (a) to (f) are sequentially performed using a powder tester (manufactured by Hosokawa Micron Co., Ltd., PT-N model).
[0106] (a) The composite particles to be measured are left to stand in a thermostat set at 80°C for 10 minutes.
[0107] (b) On the vibration table of the powder tester, sieves with mesh sizes of 350 μm, 250 μm, and 150 μm are placed in order from the top.
[0108] (c) Then, 2.0 g of the composite particles after the step (a) were evenly placed on a sieve with a mesh size of 350 μm.
[0109] (d) The sieve was vibrated at an amplitude of 1 mm for 105 seconds.
[0110] (e) The mass of the composite particles remaining in each sieve is measured.
[0111] (f) The masses obtained in the above step (e) are multiplied by weights of 1 / 1, 3 / 5 and 1 / 5, respectively, and the sum is calculated using the above formula (3) to obtain a percentage value, which is used as the degree of aggregation C (%).
[0112] The steps (a) to (f) were repeated 5 or more times, and the average value was used as the measured value.
[0113] It should be noted that the adjustment of the cohesion degree C can be performed by reacting the fatty acid alkali metal salt with the raw material calcium salt or the raw material magnesium salt under mild conditions and preventing the cohesion between the composite particles in the slurry obtained by the reaction. That is, for example, it can be performed by reacting at a mild temperature to a degree that does not reduce the reaction rate of the fatty acid alkali metal salt and the raw material calcium salt or the raw material magnesium salt, and shortening the aging time. By appropriately adjusting these factors during the reaction, the cohesion degree C can be adjusted to the range specified in the present disclosure.
[0114] (D loose bulk density)
[0115] The composite particles used in the present disclosure preferably have a loose bulk density D in the specific range shown below. This makes it easier to obtain high dispersibility and more stably exert the effects of the present disclosure. The loose bulk density D is obtained by the following formula (4).
[0116] Loose bulk density D = mass of the cup containing the sample (g) / volume of the cup (cc) ... (4)
[0117] The loose bulk density D may be 0.08 or more, 0.1 or more, 0.12 or more, 0.135 or more, or 0.15 or more, preferably 0.12 or more, and more preferably 0.135 or more. The loose bulk density D may be 0.25 or less, 0.22 or less, 0.20 or less, 0.18 or less, or 0.16 or less, preferably 0.2 or less, and more preferably 0.18 or less. By being within the above range, high dispersibility can be obtained, and the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic material can be well exerted.
[0118] The loose bulk density D is a value obtained by the following measurement method. First, for example, using a powder tester (manufactured by Hosokawa Micron Co., Ltd., PT-N model), a sieve with a mesh size of 710 μm is set on a vibration table, 250 cc of a sample is added thereto, and the sample is vibrated for 30 seconds, and the fallen sample is collected in a measurement cup set below the sieve. After scraping off the excess composite particles on the cup using the attached scraper, the mass of the cup containing the sample is measured. It should be noted that in the present disclosure, this operation and measurement are repeated 5 times, and the average value is used as the measured value of the bulk density D. The PT-N model automatically displays the measured value.
[0119] (E average roundness)
[0120] The composite particles used in the present disclosure preferably have an average roundness E (hereinafter also referred to as "average roundness E") of a group of particles having a specific range of 10% to 90% particle sizes as shown below. The average roundness E in the present disclosure is an index indicating the degree of concavity and convexity of the particle shape of the composite particles. The closer the surface shape of the composite particles is to a circle, the closer it is to 1, and the more complex the surface shape of the particles, the smaller the average roundness E. By making the composite particles have an average roundness E in a specific range, the dispersibility and coating properties can be further improved, and it is easy to more stably show the effects of the present disclosure. The average roundness E is used as a simple method for quantitatively expressing the shape of the composite particles, and can be defined as follows. First, using a flow particle image analyzer (e.g., a flow particle image analyzer "FPIA-3000" manufactured by Sysmex Corporation), particles in the range of 0.5 to 200 μm equivalent to a circle diameter are measured, and the roundness (ai) of each particle measured here is obtained by the following formula (5).
[0121] Circularity (ai) = (circumference of a circle having the same area as the projection image of a particle) / (circumference of the projection image of a particle) (5)
[0122] The "FPIA-3000" flow particle image analyzer measuring device that can be used in the present disclosure uses the following calculation method: the roundness of each particle is calculated, and the obtained roundness is divided into 61 levels with the roundness of the particle 0.4 to 1.0, and the average roundness is calculated using the center and frequency of the dividing points.
[0123] In the present disclosure, the average roundness E of the group of particles with a particle size of 10% to 90% is the value obtained by dividing the sum of the roundnesses of particles in the range of 10% to 90% of the particle size from the small particle size side of the particle size distribution among all the particles measured by the above-mentioned measuring device by the number of particles.
[0124] The average roundness E can be 0.7 or more, 0.75 or more, 0.8 or more, 0.85 or more, 0.9 or more, or 0.95 or more, preferably 0.75 or more, or more preferably 0.85 or more. The average roundness E can be 1 or less, 0.95 or less, 0.9 or less, 0.85 or less, or 0.8 or less, preferably 0.95 or less, or more preferably 0.9 or less. If the average roundness E is within the above range, the dispersibility and coating properties can be further improved, and the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic can be well exerted.
[0125] The specific measurement of the average circularity E is as follows. Prepare 30 ml of ion exchange water from which solid impurities have been removed in advance in a container, add a surfactant as a dispersant as needed, preferably polyoxyethylene nonylphenyl ether (manufactured by NOF Corporation, trade name: -NONION NS-210), and then add 20 mg of the measurement sample to make it uniformly dispersed. As a dispersing means, for example, a device with a 5 mm diameter titanium alloy end as an oscillator is used in an ultrasonic disperser UH-50 (manufactured by SMT, 20kHz / 50W), and perform a dispersion treatment for 5 minutes to make the dispersion concentration reach 3,000 / ml to 20,000 / ml to prepare a dispersion for measurement. At this time, it is performed while appropriately cooling the dispersion so that the temperature of the dispersion for measurement does not reach 40°C or above. Then, the flow particle image analyzer "FPIA-3000" is used for measurement, and the obtained data is processed to obtain the average circularity E.
[0126] It should be noted that the adjustment of the average circularity E can be carried out by reacting the fatty acid alkali metal salt with the raw material calcium salt or the raw material magnesium salt under mild conditions and preventing the particle shape of the composite particles in the slurry obtained by the reaction from being uneven. That is, for example, it can be carried out in the following manner: reacting at a mild temperature that does not reduce the reaction rate of the fatty acid alkali metal salt and the raw material calcium salt or the raw material magnesium salt, slowing down the dripping speed when the aqueous solution containing the metal salt is dripped into the aqueous solution containing the fatty acid alkali metal salt, and adding the above-mentioned polyalkylene glycol ether to stabilize the slurry. By appropriately adjusting these factors during the reaction, the average circularity E can be adjusted to the range specified in the present disclosure. Furthermore, it is more preferred that after dispersing the inorganic nucleating agent to the fatty acid alkali metal salt aqueous solution in the adjusted aqueous solution containing the fatty acid alkali metal salt, an aqueous solution containing the raw material calcium salt or the raw material magnesium salt is added, or both are added in another reaction tank. After dispersing the crystal nucleating agent in an aqueous solution containing fatty acid alkali metal salt, when it reacts with an aqueous solution containing raw calcium salt or raw magnesium salt, composite particles are generated with the crystal nucleating agent as the nucleus, so the particle shape grows uniformly and high roundness is easily obtained.
[0127] [Amount of composite particles]
[0128] The amount of the composite particles can be 1% by weight or more, 3% by weight or more, 5% by weight or more, 10% by weight or more, 20% by weight or more, 30% by weight or more, 40% by weight or more, 50% by weight or more, 60% by weight or more, or 70% by weight or more in the cosmetic. The amount of the composite particles can be 75% by weight or less, 65% by weight or less, 55% by weight or less, 45% by weight or less, 35% by weight or less, 25% by weight or less, or 15% by weight or less in the cosmetic. By being within the above range, the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic can be well exerted. The amount of the composite particles can also be appropriately changed according to the type of the cosmetic.
[0129] [Method for producing composite particles]
[0130] The composite particles disclosed herein can be produced by reacting a fatty acid alkali metal salt with a raw material calcium salt or a raw material magnesium salt by double decomposition in the presence of an inorganic nucleating agent.
[0131] The fatty acid alkali metal salt is a salt of the fatty acid constituting the metal soap described above and an alkali metal (sodium, potassium, etc.).
[0132] The fatty acid alkali metal salt used in the present disclosure can be obtained by reacting a fatty acid with an alkaline compound at a temperature generally above the melting point of the fatty acid and at a temperature to which the fatty acid will not decompose, preferably below 100°C, more preferably 50 to 100°C, further preferably 60 to 95°C, and particularly preferably 70 to 95°C. Alkaline compounds that serve as raw materials for fatty acid alkali metal salts include hydroxides of alkali metals (sodium, potassium, etc.), and amines such as ammonia, monoethanolamine, diethanolamine, and triethanolamine. From the point of view of high solubility in water when forming fatty acid alkali metal salts, hydroxides of alkali metals such as sodium and potassium (e.g., sodium hydroxide and potassium hydroxide) are preferred. These alkaline compounds may be used alone or in combination of two or more.
[0133] As the raw material calcium salt or raw material magnesium salt, it is preferred to select a salt with high water solubility, for example, a water solubility (20° C.) of 10 g / 100 mL or more, 30 g / 100 mL or more, 50 g / 100 mL or more, or 70 g / 100 mL or more, and examples thereof include: chlorides, sulfates, nitrates, etc. of calcium or magnesium such as calcium chloride, magnesium chloride, magnesium sulfate, calcium nitrate, and magnesium nitrate. If the water solubility is high, it can react with the fatty acid alkali metal salt at a high concentration, which is preferred from the viewpoint of productivity.
[0134] The reaction of the fatty acid alkali metal salt with the raw material calcium salt or the raw material magnesium salt can be carried out, for example, by preparing an aqueous solution of the raw material calcium salt or the raw material magnesium salt and an aqueous solution of the fatty acid alkali metal salt separately and then mixing them. For example, the reaction can be carried out by adding the raw material calcium salt or the raw material magnesium salt aqueous solution to the aqueous solution of the fatty acid alkali metal salt, or by adding both in another reaction tank.
[0135] When mixing the aqueous solution of fatty acid alkali metal salt and the aqueous solution of raw material calcium salt or raw material magnesium salt, for example, if the aqueous solution of raw material calcium salt or raw material magnesium salt is added to the aqueous solution of fatty acid alkali metal salt at one time, there is a possibility that the shape of the obtained composite particles is uneven and the particle size distribution becomes wide. Therefore, in the present disclosure, it is preferred that the aqueous solution of raw material calcium salt or raw material magnesium salt is slowly added dropwise to the aqueous solution of fatty acid alkali metal salt at an appropriate speed.
[0136] In the above reaction, it is more preferred that the inorganic nucleating agent is dispersed in the prepared aqueous solution of the fatty acid alkali metal salt and then the aqueous solution of the raw material calcium salt or raw material magnesium salt is added, or both are added in a separate reaction tank.
[0137] The inorganic nucleating agent acts as a nucleus to promote the growth of composite particles and has the effect of miniaturizing or homogenizing the crystal size. By adding the inorganic nucleating agent to the aqueous solution of the fatty acid alkali metal salt, the fatty acid alkali metal salt is evenly dispersed, and when reacting with the aqueous solution of the raw material calcium salt or raw material magnesium salt, the inorganic nucleating agent acts as a nucleating agent when the composite particles are crystallized, and the particle shape becomes uniform with the nucleating agent as the starting point, and the particle size distribution of the composite particles becomes sharp.
[0138] The amount of the inorganic nucleating agent added relative to the total amount of the fatty acid alkali metal salt and the inorganic nucleating agent may be 0.1% by weight or more, 0.5% by weight or more, 1% by weight or more, 3% by weight or more, 5% by weight or more, 10% by weight or more, or 15% by weight or more, preferably 0.5% by weight or more, and more preferably 1% by weight or more. The amount of the inorganic nucleating agent added relative to the total amount of the fatty acid alkali metal salt and the inorganic nucleating agent may be 30% by weight or less, 25% by weight or less, 22.5% by weight or less, 20% by weight or less, 17.5% by weight or less, 15% by weight or less, 12.5% by weight or less, or 10% by weight or less, preferably 25% by weight or less, and more preferably 20% by weight or less. By making the addition amount of the inorganic nucleating agent within the above-mentioned range, the internal introduction rate A can be increased, the particle size of the obtained composite particles can be made fine, the particle shape can be made uniform, and the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic can be well exerted.
[0139] The concentration of the fatty acid alkali metal salt in the reaction aqueous solution may be 1% by weight or more, 5% by weight or more, 10% by weight or more, or 15% by weight or more, preferably 5% by weight or more. The concentration of the fatty acid alkali metal salt in the reaction aqueous solution may be 50% by weight or less, 40% by weight or less, 30% by weight or less, 20% by weight or less, or 10% by weight or less, preferably 15% by weight or less. By being within the above range, a more uniform reaction can be performed while maintaining a high productivity of the composite particles, so it is preferred.
[0140] The concentration of the raw calcium salt or raw magnesium salt in the raw calcium salt or raw magnesium salt aqueous solution may be 10% by weight or more, 20% by weight or more, or 30% by weight or more. The concentration of the raw calcium salt or raw magnesium salt in the raw calcium salt or raw magnesium salt aqueous solution may be 60% by weight or less, 50% by weight or less, 40% by weight or less, or 30% by weight or less. The above range is preferred from the viewpoint of the productivity of the composite particles and the handleability of the fatty acid alkali metal salt aqueous solution or the obtained composite particle slurry.
[0141] Considering the solubility of the fatty acid alkali metal salt, the reaction of the fatty acid alkali metal salt with the raw material calcium salt or raw material magnesium salt is carried out under the reaction temperature conditions generally carried out by those skilled in the art. The reaction temperature may be above 20°C, above 40°C, above 60°C, or above 80°C, preferably above 60°C. The reaction temperature may be below the boiling point, for example, below 120°C, below 110°C, below 100°C, below 90°C, below 80°C, or below 70°C, preferably below 100°C. By being within the above range, a good reaction rate can be achieved.
[0142] During the reaction of the fatty acid alkali metal salt with the raw material calcium salt or the raw material magnesium salt, a surfactant may be present for the purpose of stabilizing the composite particle slurry and improving the productivity of the composite particles. As a surfactant, a nonionic surfactant is preferably used, such as a polyalkylene glycol ether, especially a triblock ether having a structure (EO-PO-EO) in which an oxypropylene block (PO) is clamped by an oxyethylene block (EO). The content of the surfactant can be 0.01% by weight or more, 0.1% by weight or more, 0.3% by weight or more, 0.5% by weight or more, or 1% by weight or more relative to the fatty acid alkali metal salt. The content of the surfactant can be less than 5% by weight, less than 3% by weight, less than 1% by weight, less than 0.5% by weight, or less than 0.1% by weight relative to the fatty acid alkali metal salt.
[0143] It should be noted that the surfactant may be present in the reaction system before the reaction of the basic compound and the fatty acid, or may be present in the reaction system before the reaction of the fatty acid alkali metal salt and the raw material calcium salt or raw material magnesium salt.
[0144] The composite particle slurry can be obtained by the above method. The composite particle slurry is subjected to solvent separation directly or by a centrifugal dehydrator, a filter press, a vacuum rotary filter, etc., and washed as needed, and after removing the salt containing calcium or magnesium as a by-product, it is dried with a rotary dryer, an airflow drying device, a ventilated dryer, a spray dryer, a fluidized bed drying device, etc. The drying method can be any type of continuous or batch type, or under normal pressure or vacuum. Furthermore, the dried composite particles are crushed as needed. The crushing method is not particularly limited, for example, a crushing method based on a pin grinder, an airflow grinder, an atomizer, etc. can be adopted. The crushed composite particles are classified. That is, classification is performed using a multi-stage screen device that applies vibration for screening, and the particle size distribution is adjusted. In this way, the composite particles disclosed in the present invention can be obtained.
[0145] 〔Oily ingredients〕
[0146] The cosmetic material disclosed herein may contain an oily component. The oily component may be a liquid oil, a paste oil or a solid oil, preferably a liquid oil or a paste oil. It should be noted that the oily component does not include the composite particles disclosed herein.
[0147] The oily component may be any oily component used in ordinary cosmetics. Examples of the oily component include straight-chain or branched hydrocarbon oils such as liquid paraffin, light isoparaffin, liquid isoparaffin, vaseline, polybutene, polyisobutene, hydrogenated polyisobutene, hydrogenated polydecene, squalane, and squalene; vegetable oils such as avocado oil, macadamia oil, olive oil, rapeseed oil, sesame oil, wheat germ oil, linseed oil, cottonseed oil, soybean oil, palm oil, coconut oil, castor oil, jojoba oil, sunflower seed oil, camellia oil, and corn oil; animal oils such as lanolin, liquid lanolin, whale oil, and cod liver oil; isopropyl myristate, octyl dodecyl myristate, isopropyl isostearate, isononyl isononanoate, butyl stearate, oleyl oleate, isononanoate Isostearyl myristate, Octyldodecyl ricinoleate, Octyl hydroxystearate, Ethylhexyl palmitate, Cetyl ethylhexanoate, Octyl methoxycinnamate, Tocopheryl acetate, Propylene carbonate, Propylene glycol dicaprylate, Neopentyl glycol dicaprate, Neopentyl glycol diethylhexanoate, Propylene glycol diisostearate, Monomyristyl monoisostearate, Propylene glycol di(caprylic acid / caprylic acid) esters, Tri(caprylic acid / capric acid) esters, Tri-2-ethylhexanoin, Triisostearate, Trimethylolpropane tri-2-ethylhexanoate, Trimethylolpropane triisostearate, Pentaerythrityl tetraoctanoate, Pentaerythrityl tetraethylhexanoate, Polyglyceryl-6 octaoctanoate, Di-trimethylolpropane (isostearate / sebacic acid) Ester oligomers, dipentaerythritol tripolyhydroxystearate, di(phytosteryl / octyldodecyl) lauroyl glutamate, di(phytosteryl / behenyl / octyldodecyl) lauroyl glutamate, trehalose isostearate, ethylhexyl hydroxystearate, phytosteryl fatty acid esters, cholesterol fatty acid esters, polyglycerol fatty acid esters, pentaerythritol fatty acid esters, trilanolin fatty acid glyceryl, branched or hydroxylated fatty acid cholesterol esters, dipentaerythritol fatty acid esters (hexahydroxystearate dipentaerythritol, etc.), hydrogenated castor oil isostearate, hydrogenated castor oil monohydroxystearate, tri(caprylic / capric / myristic / stearic)glyceryl, hydrogenated castor oil dimer linoleate, dimer linoleic acid (phytosteryl / isostearyl) Ester oils such as esters such as octyldodecanol, myristyl alcohol, stearyl alcohol, behenyl alcohol, and isostearyl alcohol; fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, isostearic acid, and soft lanolin fatty acid; silicone oils such as diphenyl dimethicone, dimethyl polysiloxane, methyl cyclopolysiloxane, methylphenyl polysiloxane, methyl hydrogen polysiloxane, higher alcohol modified organopolysiloxane, tris(trimethylsiloxy)methylsilane, and trimethyl pentaphenyl trisiloxane; fluorine oils such as fluoropolyether and perfluoroalkyl ether silicone; waxes such as beeswax, candelilla wax, carnauba wax, and jojoba wax. These can be used alone or in combination of two or more.
[0148] [Amount of oily ingredients]
[0149] The amount of the oily component in the cosmetic can be 0.1% by weight or more, 0.5% by weight or more, 1% by weight or more, 3% by weight or more, 5% by weight or more, or 10% by weight or more. The amount of the composite particles in the cosmetic can be 20% by weight or less, 15% by weight or less, 10% by weight or less, 5% by weight or less, or 3% by weight or less. By being within the above range, the effects of the present disclosure such as spreadability, adhesion, final effect, and formability can be well exerted in the cosmetic having the oily component.
[0150] 〔Spherical particles〕
[0151] The cosmetic material disclosed herein may contain spherical particles. The spherical particles may be inorganic particles or organic particles, preferably silicon dioxide particles or silicone particles. The spherical inorganic particles or spherical organic particles are suitable for solid powder cosmetic materials (e.g., powder foundation).
[0152] As examples of spherical particles, there can be mentioned: spherical inorganic particles such as spherical silica, spherical calcium carbonate, spherical aluminum oxide, spherical titanium dioxide, and spherical zirconium oxide; spherical cellulose, spherical silicone particles (e.g., (vinyl dimethyl siloxane / methyl siloxane silsesquioxane) cross-linked polymers, etc.), spherical silk powder, spherical nylon particles, spherical acrylic particles, spherical polyethylene particles, spherical polypropylene particles, spherical polystyrene particles, spherical nylon particles, spherical carbamate particles, spherical starch particles and other spherical organic particles. These can be used alone or in combination of two or more. In addition, the spherical particles can also be used after hydrophilization or hydrophobization.
[0153] The 50% cumulative diameter (D50) of the spherical particles under the volume basis can be 1 μm or more, 3 μm or more, 5 μm or more, 10 μm or more, 30 μm or more, 50 μm or more, 75 μm or more, or 100 μm or more. The 50% cumulative diameter (D50) of the spherical particles under the volume basis can be 150 μm or less, 125 μm or less, 100 μm or less, 75 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less, 15 μm or less, or 10 μm or less, preferably 30 μm or less. By being within the above range, the effects of the present disclosure such as the spreadability, adhesion, final effect, and formability of the cosmetic can be well exerted. The 50% cumulative diameter (D50) can be measured by laser diffraction. The particle size distribution of the spherical particles can be unimodal or multimodal, for example, unimodal.
[0154] [Amount of spherical particles]
[0155] The amount of the spherical particles in the cosmetic can be 1% by weight or more, 3% by weight or more, 5% by weight or more, 10% by weight or more, 15% by weight or more, or 20% by weight or more. The amount of the spherical particles in the cosmetic can be 50% by weight or less, 40% by weight or less, 30% by weight or less, 20% by weight or less, or 10% by weight or less. By being within the above range, in the cosmetic, the effects of the present disclosure such as spreadability, adhesion, final effect, and formability can be well exerted.
[0156] [Other ingredients]
[0157] Furthermore, the cosmetics of the present disclosure may also contain ingredients generally used in cosmetics as other ingredients within the scope of not losing the effects of the present disclosure, such as surfactants, extender pigments, colorants, UV inhibitors, oil-soluble gelling agents (organically modified clay minerals), water-soluble polymers, resins, antiperspirants, moisturizers, antibacterial preservatives, fragrances, salts, antioxidants, pH adjusters, chelating agents, cooling agents, anti-inflammatory agents, skin beautifying ingredients (whitening agents, cell activators, rough skin improvers, blood circulation promoters, skin astringents, anti-seborrheic agents, etc.), vitamins, amino acids, etc. These may be used alone or in combination of two or more.
[0158] Examples of the surfactant include anionic, cationic, nonionic, or amphoteric surfactants, including silicone-based or hydrocarbon-based surfactants, and these may be used alone or in combination of two or more.
[0159] Examples of extender pigments include mica, synthetic mica, sericite, synthetic sericite, talc, kaolin, silicon carbide, silicate, barium sulfate, hydroxyapatite, bentonite, montmorillonite, aluminum oxide, silicon dioxide, magnesium oxide, zirconium oxide, magnesium carbonate, calcium carbonate, chromium oxide, aluminum hydroxide, magnesium hydroxide, boron nitride, hydroxyapatite, aluminum oxide, lauroyl lysine, metal soap powder, etc. These may be used alone or in combination of two or more.
[0160] Examples of colorants include: inorganic white pigments such as titanium oxide and zinc oxide, inorganic colored pigments such as yellow iron oxide, red iron oxide, black iron oxide, carbon black, ultramarine, Prussian blue, Prussian blue titanium oxide, black titanium oxide, chromium oxide, chromium hydroxide, and titanium / titanium oxide sintered products; organic pigments such as Red No. 201, Red No. 202, Red No. 226, Yellow No. 401, and Blue No. 404; lake pigments such as Red No. 104, Red No. 230, Yellow No. 4, Yellow No. 5, and Blue No. 1; and colorants obtained by coating organic pigments with polymers such as polymethacrylates. In addition, examples of pearlescent pigments include titanium mica, red iron oxide-coated (titanium oxide / aluminum hydroxide) mixtures, red iron oxide-coated mica, bismuth oxychloride, titanium oxide-coated bismuth oxychloride, titanium oxide-coated titanium mica, organic pigment-coated titanium mica, silicate / titanium-treated mica, titanium oxide-coated talc, silicon dioxide / red iron oxide-treated aluminum, inorganic powders such as titanium oxide-coated glass powder, resin-coated plate-shaped aluminum powder, titanium oxide / yellow iron oxide / red iron oxide / lauryl methacrylate / dimethacrylate EG copolymer mixtures, etc. These can be used alone or in combination of two or more.
[0161] Examples of anti-ultraviolet agents include ultraviolet absorbers such as ethylhexyl methoxycinnamate, octocrylene, dimethicodiethylbenzalmalonate, polysilicone-15, tert-butyl methoxydibenzoylmethane, ethylhexyl triazone, diethylaminohydroxybenzoyl hexyl benzoate, bis-ethylhexyloxyphenol methoxyphenyl triazine, benzophenone-3, methylene bisbenzotriazolyl tetramethylbutylphenol, phenylbenzimidazole sulfonic acid, homosalate, and ethylhexyl salicylate; and microparticles of metal oxides such as microparticles of titanium oxide, microparticles of zinc oxide, microparticles of iron oxide, and microparticles of cerium oxide. These may be used alone or in combination of two or more.
[0162] As the example of oil-soluble gelling agent, can enumerate: metal soaps such as aluminum stearate, magnesium stearate, zinc myristate, amino acid derivatives such as N-lauroyl-L-glutamic acid dibutylamide, dextrin fatty acid esters such as dextrin palmitate, dextrin stearate, dextrin 2-ethylhexanoic acid palmitate, sucrose fatty acid esters such as sucrose palmitate, sucrose stearate, oligofructose fatty acid esters such as oligofructose stearate, oligofructose 2-ethylhexanoate, benzylidene sorbitol, benzylidene sorbitol, benzylidene sorbitol, dimethyl benzyl dodecyl ammonium montmorillonite clay, organic modified clay minerals such as dimethyl di (octadecyl) ammonium montmorillonite clay, etc. These can be used alone, or two or more can be used in combination. These can be used alone, or two or more can be used in combination.
[0163] Examples of water-soluble polymers include carboxyvinyl polymers, ammonium polyacrylate, sodium polyacrylate, sodium acrylate / alkyl acrylate / sodium methacrylate / alkyl methacrylate copolymers, carrageenan, pectin, mannan, curdlan, chondroitin sulfate, starch, glycogen, gum arabic, sodium hyaluronate, tragacanth, xanthan gum, sulfated mucopolysaccharide, hydroxyethyl guar gum, carboxymethyl guar gum, guar gum, dextran, keratan sulfate, locust bean gum, succinylglucan, chitin, chitosan, carboxymethyl chitin, agar, etc. These can be used alone or in combination of two or more.
[0164] Examples of the antiperspirant include one or more antiperspirants selected from aluminum chlorohydrate, aluminum chloride, aluminum sesquichlorohydrate, zirconium hydroxychloride, aluminum zirconium hydroxychloride, aluminum zirconium glycinate complex, etc. These may be used alone or in combination of two or more.
[0165] Examples of the moisturizing agent include, for example, glycerin, sorbitol, propylene glycol, dipropylene glycol, 1,3-butylene glycol, pentylene glycol, glucose, xylitol, maltitol, polyethylene glycol, hyaluronic acid, chondroitin sulfate, pyrrolidone carboxylate, polyoxyethylene methyl glucoside, polyoxypropylene methyl glucoside, etc. One or more moisturizing agents can be used alone or in combination of two or more.
[0166] Examples of antimicrobial preservatives include alkyl p-hydroxybenzoates, benzoic acid, sodium benzoate, sorbic acid, potassium sorbate, phenoxyethanol, etc., and antimicrobial agents include benzoic acid, salicylic acid, carbolic acid, sorbic acid, alkyl p-hydroxybenzoates, parachloro-meta-cresol, hexachlorophene, benzalkonium chloride, chlorhexidine hydrochloride, trichlorocarbamide, photosensitizer, phenoxyethanol, etc. These can be used alone or in combination of two or more.
[0167] Examples of salts include inorganic salts, organic acid salts, amine salts, and amino acid salts. Inorganic salts include sodium salts, potassium salts, magnesium salts, calcium salts, aluminum salts, zirconium salts, and zinc salts of inorganic acids such as hydrochloric acid, sulfuric acid, carbonic acid, and nitric acid; organic acid salts include salts of organic acids such as acetic acid, dehydroacetic acid, citric acid, malic acid, succinic acid, ascorbic acid, and stearic acid; amine salts and amino acid salts include salts of amines such as triethanolamine and salts of amino acids such as glutamic acid. In addition, salts of hyaluronic acid, chondroitin sulfate, aluminum zirconium complexes of glycine, and neutralized salts of acids and bases used in cosmetic prescriptions can also be used. These can be used alone or in combination of two or more.
[0168] As the above-mentioned antioxidant, tocopherol, butylated hydroxyanisole, dibutyl hydroxytoluene, phytic acid, etc. can be mentioned, as the pH adjusting agent, lactic acid, citric acid, glycolic acid, succinic acid, tartaric acid, dl-malic acid, potassium carbonate, sodium bicarbonate, ammonium bicarbonate, etc. can be mentioned, as the chelating agent, alanine, sodium edetate, sodium polyphosphate, sodium metaphosphate, phosphoric acid, etc. can be mentioned, as the cooling agent, L-menthol, camphor, etc. can be mentioned, as the anti-inflammatory agent, allantoin, glycyrrhizic acid and its salt, glycyrrhetinic acid and glycyrrhetinic acid stearyl ester, tranexamic acid, azulene, etc. can be mentioned. These can be used alone or in combination of two or more.
[0169] As skin beautifying ingredients, for example, whitening agents such as placenta extract, arbutin, glutathione, and saxifrage extract, cell activators such as royal jelly, photosensitizer, cholesterol derivatives, and calf blood extract, skin roughness improving agents, nonanoic acid vanillamide, nicotinate benzyl ester, nicotinate β-butoxyethyl ester, capsaicin, gingerol, cantharide tincture, ichthyol, caffeine, tannic acid, α-borneol, nicotinate tocopherol, inositol nicotinate, cycloamycin, cinnarizine, tolazoline, acetylcholine, verapamil, cepharanthin, γ-oryzanol and other blood circulation promoters, skin astringents such as zinc oxide and tannic acid, anti-seborrheic agents such as sulfur and dimethylthiothrene (thianthol), etc. These can be used alone or in combination of two or more.
[0170] Examples of the vitamins include vitamin A oil, retinol, retinyl acetate, retinyl palmitate and other vitamin A compounds, riboflavin, riboflavin butyrate, flavin adenine nucleotide and other vitamin B2 compounds, pyridoxine hydrochloride, pyridoxine dioctanoate, pyridoxine tripalmitate and other vitamin B6 compounds, vitamin B12 and its derivatives, vitamin B15 and its derivatives and other vitamin B15 compounds, L-ascorbic acid, L-ascorbic acid dipalmitate, L-ascorbic acid-2 -Sodium sulfate, vitamin C such as dipotassium L-ascorbyl phosphate, vitamin D such as ergocalciferol and cholecalciferol, vitamin E such as α-tocopherol, β-tocopherol, γ-tocopherol, dl-α-tocopherol acetate, dl-α-tocopherol nicotinate, dl-α-tocopherol succinate, vitamin H, vitamin P, nicotinic acid, benzyl nicotinate, nicotinamide and other nicotinic acids, calcium pantothenate, D-panthenol, panthenyl ethyl ether, acetyl panthenyl ethyl ether and other pantothenic acids, biotin, etc. These can be used alone or in combination of two or more.
[0171] As amino acids, for example, glycine, valine, leucine, isoleucine, serine, threonine, phenylalanine, arginine, lysine, aspartic acid, glutamic acid, cystine, cysteine, methionine, tryptophan, etc. can be mentioned; as nucleic acids, deoxyribonucleic acid, etc. can be mentioned; as hormones, estradiol, ethinyl estradiol, etc. can be mentioned. These can be used alone or in combination of two or more.
[0172] <Method for producing cosmetics>
[0173] The manufacturing method of the cosmetic disclosed herein is not particularly limited, and known manufacturing methods can be used. For example, a method of uniformly dispersing the raw materials by heating as required and stirring as required can be cited. As required, high dispersion machines such as a roller mill, a high pressure homogenizer, a bead mill, and a microfluidizer can also be used. The cosmetic can be a shaped material, and the shaping can be dry shaping or wet shaping.
[0174] <Uses of cosmetics>
[0175] As the use of the cosmetics disclosed in the present invention, it is possible to cite: skin care cosmetics such as lotions, creams, makeup removers, facial masks, massage agents, beauty serums, beauty oils, cleansers, hand creams, lipsticks, wrinkle-covering creams, body powders, essences, and shaving agents; color cosmetics such as powder foundations, liquid foundations, primers, eye shadows, concealers, white powders, lipsticks, and mascara; hair cosmetics such as shampoos, conditioners, hair masks, scalp creams, and fixatives; antiperspirants such as deodorants; UV protection cosmetics such as sunscreen oils, sunscreen lotions, and sunscreens. The cosmetics disclosed in the present invention have good spreadability, adhesion, final effect, and formability, and are also suitable for use as liquid or paste cosmetics, and are particularly suitable for use as solid powder cosmetics. Solid powder cosmetics are cosmetics with powder as the main component, and can be formed materials (e.g., dry forming or wet forming).
[0176] According to the present disclosure, a novel cosmetic material can be provided that is excellent in adhesion and / or final effect after coating, and has a good feeling of use, in addition to the spreadability during coating. According to the present disclosure, preferably, a novel cosmetic material can be further provided that is excellent in formability, adhesion resistance, handling and / or final effect, and has a good feeling of use.
[0177] Although the embodiments have been described above, various changes may be made to the embodiments and details without departing from the spirit and scope of the invention.
[0178] Example
[0179] Although the present disclosure is described in detail below with reference to examples, the present disclosure is not limited to these examples.
[0180] <Synthesis of Composite Particles>
[0181] [Synthesis example 1]
[0182] Add 200g of myristic acid (NAA-142 manufactured by NOF Corporation) and 2119g of water to a 3L separable flask and heat to 80°C. Then, add 73.6g of 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 43.5g of borosilicate glass (Ca / Al) (FTD008FY manufactured by Nippon Sheet Glass Co., Ltd.) with an average particle size of 8.2μm and stir for 1 hour. Then, while maintaining at 80°C, add 145.5g of 35% by mass calcium chloride aqueous solution to the fatty acid alkali metal salt aqueous solution over 30 minutes. After the addition is completed, maintain stirring at 80°C for 30 minutes to mature. Add 1500g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered with a suction filter, washed twice with 1000 g of water, and the filter cake obtained was dried with a micron dryer, crushed and classified to obtain myristic acid calcium salt particles having borosilicate glass (Ca / Al) as a nucleating agent.
[0183] [Synthesis example 2]
[0184] Add 200g of lauric acid (NAA-122 manufactured by NOF Corporation) and 2136g of water to a 3L separable flask and heat to 80°C. Then, add 84.0g of 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 44.0g of borosilicate glass (Ca / Al) (FTD008FY manufactured by Nippon Sheet Glass Co., Ltd.) with an average particle size of 8.2μm and stir for 1 hour. Then, while maintaining at 80°C, add 166.2g of 35% by mass calcium chloride aqueous solution to the aqueous solution of fatty acid alkali metal salt over 30 minutes. After the addition is completed, stir at 80°C for 30 minutes to mature. Add 1500g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered with a suction filter, washed twice with 1000 g of water, and the obtained filter cake was dried with a micron dryer, crushed and classified to obtain lauric acid calcium salt particles having borosilicate glass (Ca / Al) as a nucleating agent.
[0185] [Synthesis example 3]
[0186] Add 200g of palmitic acid (NAA-160 manufactured by NOF Corporation) and 2106g of water to a 3L separable flask and heat to 80°C. Next, add 65.6g of a 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 43.1g of borosilicate glass (Ca / Al) (FTD008FY manufactured by Nippon Sheet Glass Co., Ltd.) with an average particle size of 8.2μm and stir for 1 hour. Then, while maintaining at 80°C, add 129.8g of a 35% by mass calcium chloride aqueous solution to the fatty acid alkali metal salt aqueous solution over 30 minutes. After the addition is completed, stir at 80°C for 30 minutes to mature. Add 1500g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered with a suction filter, washed twice with 1000 g of water, and the filter cake obtained was dried with a micron dryer, crushed and classified to obtain palmitic acid calcium salt particles having borosilicate glass (Ca / Al) as a nucleating agent.
[0187] [Synthesis example 4]
[0188] Add 200g of stearic acid (NAA-180 manufactured by NOF Corporation) and 2095g of water to a 3L separable flask and heat to 80°C. Then, add 59.1g of 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 42.8g of borosilicate glass (Ca / Al) (FTD008FY manufactured by Nippon Sheet Glass Co., Ltd.) with an average particle size of 8.2μm and stir for 1 hour. Then, while maintaining at 80°C, add 116.8g of 35% by mass calcium chloride aqueous solution to the fatty acid alkali metal salt aqueous solution over 30 minutes. After the addition is completed, stir at 80°C for 30 minutes to mature. Add 1500g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered with a suction filter, washed twice with 1000 g of water, and the filter cake obtained was dried with a micron dryer, crushed and classified to obtain calcium stearate particles having borosilicate glass (Ca / Al) as a nucleating agent.
[0189] [Synthesis Example 5]
[0190] Add 200 g of myristic acid (NAA-142 manufactured by NOF Corporation) and 2119 g of water to a 3L separable flask and heat to 80°C. Next, add 73.6 g of a 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 43.5 g of barium sulfate (plate-shaped barium sulfate H manufactured by Sakai Chemical Industry Co., Ltd.) with an average particle size of 8.1 μm and stir for 1 hour. Then, while maintaining at 80°C, add 145.5 g of a 35% by mass calcium chloride aqueous solution to the fatty acid alkali metal salt aqueous solution over 30 minutes. After the addition is completed, maintain stirring at 80°C for 30 minutes to mature. Add 1500 g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered with a suction filter, washed twice with 1000 g of water, and the obtained filter cake was dried with a micron dryer, crushed and classified to obtain myristic acid calcium salt particles having barium sulfate as a nucleating agent.
[0191] [Synthesis Example 6]
[0192] Add 200 g of myristic acid (NAA-142 manufactured by NOF Corporation) and 2119 g of water to a 3L separable flask, and heat to 80°C. Next, add 73.6 g of a 48% by mass sodium hydroxide aqueous solution, stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salts. Add 42.1 g of borosilicate glass (Ca / Al) (FTD008FY manufactured by Nippon Sheet Glass Co., Ltd.) with an average particle size of 8.2 μm, and stir for 1 hour. Then, while maintaining at 80°C, add 124.9 g of a 35% by mass magnesium chloride aqueous solution to the aqueous solution of fatty acid alkali metal salts over 30 minutes. After the addition is completed, maintain stirring at 80°C for 30 minutes to mature. Add 1500 g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered with a suction filter, washed twice with 1000 g of water, and the obtained filter cake was dried with a micron dryer, crushed and classified to obtain myristic acid magnesium salt particles having borosilicate glass (Ca / Al) as a nucleating agent.
[0193] [Synthesis Example 7]
[0194] Add 200g of myristic acid (NAA-142 manufactured by NOF Corporation) and 2119g of water to a 3L separable flask and heat to 80°C. Next, add 73.6g of a 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 42.1g of barium sulfate (plate-shaped barium sulfate H manufactured by Sakai Chemical Industry Co., Ltd.) with an average particle size of 8.1μm and stir for 1 hour. Then, while maintaining at 80°C, add 124.9g of a 35% by mass magnesium chloride aqueous solution to the aqueous solution of fatty acid alkali metal salt over 30 minutes. After the addition is completed, stir at 80°C for 30 minutes to mature. Add 1500g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered with a suction filter, washed twice with 1000 g of water, and the obtained filter cake was dried with a micron dryer, crushed and classified to obtain myristic acid magnesium salt particles having barium sulfate as a nucleating agent.
[0195] [Synthesis example 8]
[0196] Add 200g of myristic acid (NAA-142 manufactured by NOF Corporation) and 2119g of water to a 3L separable flask and heat to 80°C. Then, add 73.6g of 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 43.5g of talc (JA-46R manufactured by Asada Flour Milling Co., Ltd.) with an average particle size of 11.2μm and stir for 1 hour. Then, while maintaining at 80°C, add 145.5g of 35% by mass calcium chloride aqueous solution to the aqueous solution of fatty acid alkali metal salt over 30 minutes. After the addition is completed, stir at 80°C for 30 minutes to mature. Add 1500g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered with a suction filter, washed twice with 1000 g of water, and the obtained filter cake was dried with a micron dryer, crushed and classified to obtain myristic acid calcium salt particles having talc as a nucleating agent.
[0197] [Synthesis Example 9]
[0198] Add 200 g of myristic acid (NAA-142 manufactured by NOF Corporation) and 2119 g of water to a 3L separable flask and heat to 80°C. Next, add 73.6 g of a 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 43.5 g of boron nitride (SHP-5 manufactured by Mizushima Iron & Steel Co., Ltd.) with an average particle size of 25.4 μm and stir for 1 hour. Then, while maintaining at 80°C, add 145.5 g of a 35% by mass calcium chloride aqueous solution to the aqueous solution of fatty acid alkali metal salt over 30 minutes. After the addition is completed, maintain stirring at 80°C for 30 minutes to mature. Add 1500 g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered by a vacuum machine and washed twice with 1000 g of water. The filter cake was dried, crushed and classified by a micron dryer to obtain myristic acid calcium salt particles having boron nitride as a nucleating agent.
[0199] [Synthesis Example 10]
[0200] Add 200g of myristic acid (NAA-142 manufactured by NOF Corporation) and 2119g of water to a 3L separable flask and heat to 80°C. Then, add 73.6g of 48% by mass sodium hydroxide aqueous solution and stir at the same temperature (80°C) for 1 hour to obtain an aqueous solution of fatty acid alkali metal salt. Add 45.8g of borosilicate glass (Ca / Al) (FTD008FY manufactured by Nippon Sheet Glass Co., Ltd.) with an average particle size of 8.2μm and stir for 1 hour. Then, while maintaining at 80°C, add 178.7g of 35% by mass zinc chloride aqueous solution to the aqueous solution of fatty acid alkali metal salt over 30 minutes. After the addition is completed, maintain stirring at 80°C for 30 minutes to mature. Add 1500g of water to the obtained fatty acid calcium salt aqueous solution slurry and cool to below 65°C. Then, the mixture was filtered by a vacuum machine, washed twice with 1000 g of water, and the filter cake obtained was dried, crushed and classified by a micron dryer to obtain myristic acid zinc salt particles having borosilicate glass (Ca / Al) as a nucleating agent.
[0201] <Measurement of Physical Properties of Composite Particles>
[0202] The physical properties of the composite particles obtained in the above-mentioned Synthesis Examples 1 to 10 were measured by the following methods.
[0203] 〔Internal introduction rate A〕
[0204] The internal introduction rate A is described in the main text of the specification and is obtained by the following formula.
[0205] Internal introduction rate A = 100-(X / X') × 100 (1)
[0206] [Wherein,
[0207] X is the surface content of the inorganic nucleating agent in the composite particles,
[0208] X' is the total content of the inorganic nucleating agent in the composite particles,
[0209] X and X' are the average values obtained by performing elemental analysis at three locations within a 15 μm square range on the composite particles before and after homogenization by SEM / EDX at an accelerating voltage of 10 kV and a height of 15 mm].
[0210] In addition, homogenization was performed by grinding|pulverizing with a mortar.
[0211] [D10, D50, and D90]
[0212] D10 (10% cumulative diameter on a volume basis), D50 (50% cumulative diameter on a volume basis), and D90 (90% cumulative diameter on a volume basis) were measured using Microtrac MT-3000 manufactured by Nikkiso Co., Ltd.
[0213] 〔Granularity Summary Value B〕
[0214] The particle size summary value B is described in the main text of the specification and is obtained by the following formula.
[0215] Particle size summary value B = (D90-D10) / D50
[0216] [Table 1]
[0217]
[0218] <Powder foundation>
[0219] The ingredients described in Tables 2-1 and 2-2 were uniformly mixed in a manner to achieve the content (weight %) described in Tables 2-1 and 2-2, and filled and formed in a middle plate to obtain a powder foundation as a solid powder cosmetic. In addition, the ingredients described in Table 2-3 were uniformly mixed in a manner to achieve the content (weight %) described in Table 2-3, and a slurry was made by uniformly dispersing it with ethanol and filled in a middle plate, and a powder foundation as a solid powder cosmetic was obtained by a wet molding method. The performance of the powder foundation was evaluated by the following method. The results are shown in Table 2.
[0220] 〔Formability of powder foundation〕
[0221] The formability of powder foundation was compared in the following manner: after the cosmetic material was prepared, it was placed in a specified powder box container and dropped vertically from a height of 50 cm onto a plywood with a thickness of 2 cm. The average number of drops (n=3) until any one of breakage, chipping, and cracking occurred was compared.
[0222] [Evaluation criteria]
[0223] ◎: 4 times or more
[0224] ○: 3 or more times but less than 4 times
[0225] △: 2.0 times or more and less than 3.0 times
[0226] ×: Unable to form, or less than 2 times
[0227] 〔Anti-adhesion of powder foundation〕
[0228] The sticking of the powder foundation was evaluated by rubbing the surface of the powder foundation with a prescribed puff 40 times after the preparation of the cosmetic material, and 7 professional judges performed the following 4-level evaluation, and compared the average evaluation: 4 points: no sticking, 3 points: a little sticking, but it can be taken with a puff without any problem, 2 points: sticking and it is difficult to take with a puff, which has problems in usability, and 1 point: sticking and it cannot be taken with a puff at all.
[0229] [Evaluation criteria]
[0230] ◎: 3.5 or above to 4.0
[0231] ○: 2.5 or more and less than 3.5
[0232] △: 1.5 or more and less than 2.5
[0233] ×: 1.0 or more and less than 1.5
[0234] [How to use a powder puff for powder foundation]
[0235] Regarding the application of the powder foundation with a powder puff, after preparing the cosmetic material, 10 professional judges used a specified powder puff to perform the following 4-level evaluation, and compared them by the average evaluation: 4 points: very good application, 3 points: good application, 2 points: slightly poor application, 1 point: poor application.
[0236] [Evaluation criteria]
[0237] ◎: 3.5 or above to 4.0
[0238] ○: 2.5 or more and less than 3.5
[0239] △: 1.5 or more and less than 2.5
[0240] ×: 1.0 or more and less than 1.5
[0241] [Spreadability of powder foundation]
[0242] Regarding the spreadability of the powder foundation during application, after the preparation of the cosmetic material, 7 professional judges conducted the following 4-level evaluation, and compared the average evaluation: 4 points: very good spreadability, 3 points: good spreadability, 2 points: slightly poor spreadability, 1 point: poor spreadability.
[0243] [Evaluation criteria]
[0244] ◎: 3.5 or above to 4.0
[0245] ○: 2.5 or more and less than 3.5
[0246] △: 1.5 or more and less than 2.5
[0247] ×: 1.0 or more and less than 1.5
[0248] [The feeling of close fit when applying powder foundation]
[0249] Regarding the close feeling of the powder foundation when applied, after the cosmetic material was prepared, 7 professional judges performed the following 4-level evaluation, and compared by the average evaluation: 4 points: very good close feeling, 3 points: good close feeling, 2 points: slightly poor close feeling, 1 point: poor close feeling.
[0250] [Evaluation criteria]
[0251] ◎: 3.5 or above to 4.0
[0252] O: 2.5 or more and less than 3.5
[0253] △: 1.5 or more and less than 2.5
[0254] ×: 1.0 or more and less than 1.5
[0255] [The final effect after applying powder foundation]
[0256] Regarding the final effect after application of the powder foundation, after the cosmetic material was prepared, 7 professional judges performed the following 4-level evaluation, and compared by the average evaluation: 4 points: the final effect is very good, 3 points: the final effect is good, 2 points: the final effect is slightly poor, and 1 point: the final effect is poor.
[0257] [Evaluation criteria]
[0258] ◎: 3.5 or above to 4.0
[0259] O: 2.5 or more and less than 3.5
[0260] △: 1.5 or more and less than 2.5
[0261] ×: 1.0 or more and less than 1.5
[0262] [Table 2-1]
[0263] Powder foundation-1
[0264]
[0265] [Table 2-2]
[0266] Powder foundation-2
[0267]
[0268] [Table 2-3]
[0269]
[0270] <Liquid Foundation>
[0271] The components listed in Table 3 were uniformly mixed to give the contents (weight %) listed in Table 3 to obtain a liquid foundation as a water-in-oil emulsified cosmetic. Evaluation was performed in the same manner as for the powder foundation. The results are shown in Table 3.
[0272] [Table 3]
[0273] Liquid Foundation
[0274]
[0275] <Eyeshadow>
[0276] The components having the display names shown in Table 4 were uniformly mixed so as to have the contents (weight %) shown in Table 4, and filled and molded in a middle pan to obtain an eye shadow as a solid powder cosmetic.
[0277] [Table 4]
[0278] Eyeshadow
[0279]
[0280] The obtained eye shadow exhibited sufficient moldability and good handling using a predetermined eye shadow stick, and was excellent in spreadability, adhesion, and final effect during application.
[0281] <White powder>
[0282] The components having the display names described in Table 5 were uniformly mixed so as to have the contents (weight %) described in Table 5, thereby obtaining white powder.
[0283] [Table 5]
[0284] White powder
[0285]
[0286] The obtained white powder is excellent in spreadability during application, adhesion, and final effect.
[0287] <Mascara>
[0288] The components having the display names described in Table 6 were uniformly mixed so as to have the contents (% by weight) described in Table 6, thereby obtaining a mascara.
[0289] [Table 6]
[0290] Mascara
[0291]
[0292] The obtained mascara was excellent in the effects of improving the adhesion and volume of eyelashes.
[0293] <Lipstick>
[0294] The components having the display names described in Table 7 were uniformly mixed so as to have the contents (weight %) described in Table 7, thereby obtaining a lipstick.
[0295] [Table 7]
[0296] Lipstick
[0297]
[0298] The obtained lipstick was excellent in spreadability during application, fit to lips, and final effect.
[0299] <Skin Care Lotion>
[0300] The components having the display names described in Table 8 were uniformly mixed so as to have the contents (weight %) described in Table 8, thereby obtaining a skin care lotion.
[0301] [Table 8]
[0302] Skin care lotion
[0303]
[0304] The obtained skin care lotion is excellent in spreadability during application, smoothness after application, and final effect after application.
[0305] <Shake-to-fit sunscreen>
[0306] The components having the display names described in Table 9 were uniformly mixed so as to achieve the contents (weight %) described in Table 9 to obtain a shake-type sunscreen.
[0307] [Table 9]
[0308] Shake-to-dry sunscreen
[0309]
[0310] The obtained shake-type sunscreen is excellent in spreadability during application, smoothness after application, and final effect after application.
[0311] <Sunscreen>
[0312] The components having the display names described in Table 10 were uniformly mixed so as to have the contents (weight %) described in Table 10, thereby obtaining a sunscreen.
[0313] [Table 10]
[0314] Sunscreen
[0315]
[0316] The obtained sunscreen was excellent in spreadability during application, smoothness after application, and final effect after application.
Claims
1. A cosmetic comprising composite particles, wherein: The composite particles contain an inorganic nucleating agent and a metal soap, The inorganic nucleating agent is at least one selected from glass particles and insoluble sulfate particles. The metal soap is a salt of a fatty acid and at least one selected from calcium and magnesium.
2. The cosmetic according to claim 1, wherein The amount of the inorganic nucleating agent in the composite particles is 0.1 wt % or more and 30 wt % or less.
3. The cosmetic according to claim 1 or 2, wherein The internal introduction rate A represented by the following formula (1) is 25% or more, Internal introduction rate A = 100 - (X / X') × 100 (1) Formula (1) In the formula, X is the surface content of the inorganic nucleating agent in the composite particles, X' is the total content of the inorganic nucleating agent in the composite particles, X and X' are average values obtained by performing elemental analysis at three locations within a 15 μm square range on the composite particles before and after homogenization by SEM / EDX at an accelerating voltage of 10 kV and a height of 15 mm.
4. The cosmetic according to any one of claims 1 to 3, wherein The particle size summary value B expressed by the following formula (2) is 3 or less, Particle size summary value B = (D90-D10) / D50 (2) Formula (2) In the formula, D10 is the 10% cumulative diameter of the composite particle on a volume basis, D50 is the 50% cumulative diameter of the composite particle on a volume basis, D90 is the 90% cumulative diameter of the composite particles on a volume basis, The unit of the cumulative diameter is μm.
5. The cosmetic according to any one of claims 1 to 4, wherein The glass particles are silicate glass particles.
6. The cosmetic according to any one of claims 1 to 5, wherein The inorganic nucleating agent is at least one selected from borosilicate glass particles and barium sulfate particles.
7. The cosmetic according to any one of claims 1 to 6, wherein The fatty acid has 8 or more and 22 or less carbon atoms.
8. The cosmetic according to any one of claims 1 to 7, wherein The amount of the composite particles in the cosmetic is 1% by weight or more and 75% by weight or less.
9. The cosmetic according to any one of claims 1 to 8, wherein The cosmetic further comprises an oily component, The amount of the oily component in the cosmetic is 0.1% by weight or more and 20% by weight or less.
10. The cosmetic according to any one of claims 1 to 9, wherein The cosmetic further comprises spherical particles, The 50% cumulative value of the spherical particles on a volume basis is 1 μm or more and 30 μm or less, The amount of the spherical particles in the cosmetic is 1% by weight or more. 11 . The cosmetic according to claim 1 , which is a solid powder cosmetic.
Citation Information
Patent Citations
Metal soap and manufacturing method therefor
WO2016132967A1