Method for producing aromatic dicarboxylic acid bis (hydroxyalkyl) ester and method for producing regenerated aromatic polyester

Through the depolymerization and polycondensation method in the presence of manganese catalysts and alkali metals, the coloring and heat resistance problems in the regeneration of aromatic polyesters are solved, and high-quality regenerated aromatic polyester production is achieved, which is suitable for a variety of materials applications.

CN118973998APending Publication Date: 2024-11-15TEIJIN FRONTIER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032094.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to suppress coloring and maintain heat resistance when the aromatic polyester is depolymerized and regenerated, especially when the isophthalic acid sulfonic acid component is included, resulting in a decrease in the molecular weight, melting point and crystallinity of the regenerated polymer. , and the by-products increase and the heat resistance is poor.

Method used

Depolymerization and repolymerization of aromatic dicarboxylic acid bis(hydroxyalkyl) ester in the presence of a catalyst is carried out using a manganese catalyst, and purified by cooling and crystallization in alkylene glycol and water washing, followed by alkali metal and/ Or polycondensation is carried out in the presence of alkaline earth metal, and the amount of catalyst used is controlled between 20 and 500 mmol%, and catalysts such as manganese acetate and antimony trioxide are preferably used.

Benefits of technology

It effectively inhibits the coloring of regenerated aromatic polyester, maintains the same heat resistance as the original product, improves the hue and physical stability of the polymer, and is suitable for fibers, films and resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005068020930000151
    Figure BDA0005068020930000151
  • Figure BDA0005068020930000161
    Figure BDA0005068020930000161
  • Figure BDA0005068020930000171
    Figure BDA0005068020930000171
Patent Text Reader

Abstract

Provided is a method for producing an aromatic dicarboxylic acid bis (hydroxyalkyl) ester in which a polyester is depolymerized in the presence of a catalyst, the method being characterized in that the catalyst is a manganese-based catalyst, the amount of the catalyst used relative to the polyester being 20-500 mmol%, and the amount of the catalyst used relative to the polyester being 20-500 mmol%. Also provided are: a method for producing an aromatic dicarboxylic acid bis (hydroxyalkyl) ester by depolymerizing a polyester by the production method; and a method for producing a polyester polymer by re-polymerizing the aromatic dicarboxylic acid bis (hydroxyalkyl) ester as a starting material. The present invention relates to a method for producing a polyester polymer having little coloration as the original product (a substance produced by polymerizing a monomer without depolymerization), and an intermediate thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester by depolymerizing polyester and a method for producing an aromatic polyester using the same. More specifically, the present invention relates to a method for producing a recycled aromatic polyester by depolymerizing an aromatic polyester contained in polyester scraps, product recycling products, etc. containing the aromatic polyester and repolymerizing the depolymerized aromatic polyester to obtain the recycled aromatic polyester. Background Art

[0002] Aromatic polyesters, such as polyethylene terephthalate, are widely used as fibers, films, and resin molded products due to their excellent properties. In these manufacturing processes and processing processes, unused polyester raw materials, fibers, films, and other shaped scraps or scraps are generated. In addition, fibers, films, and resin molded products used as polyester products are discarded after use or in an unused state, but such waste has the problem of deteriorating the environment.

[0003] As a method for recycling these process scraps, scraps, unused raw materials or product waste, there are material recycling, chemical recycling and thermal recycling. Among chemical recycling, the monomer in the form of ester-bonded aromatic dicarboxylic acid 1 molecule and diol 2 molecules, or the intermediate product further depolymerized to ester-bonded oligomers is used again. Chemical recycling is an excellent method because it can produce recycled aromatic polyester by direct polycondensation reaction, which requires less energy.

[0004] As an example of such a method, there is a method of depolymerizing polyethylene terephthalate in ethylene glycol to obtain bis(2-hydroxyethyl)terephthalate, and polycondensing the bis(2-hydroxyethyl)terephthalate to obtain a regenerated aromatic polyester.

[0005] However, the regenerated aromatic polyester polymer thus obtained has the problem of coloration. Furthermore, in order to improve the dyeability of polyester fibers, there are aromatic polyesters containing isophthalic acid sulfonic acid metal salts such as sodium isophthalic acid sulfonate, isophthalic acid tetraalkyl sulfonate, and the like. In the case where an isophthalic acid sulfonic acid component such as tetraalkylammonium salt of isophthalic acid sulfonate or isophthalic acid sulfonic acid tetraalkylammonium salt is used as the dicarboxylic acid component, the regenerated aromatic polyester obtained by simply depolymerizing and then repolymerizing has problems such as coloration, lowering of molecular weight (intrinsic viscosity), melting point and crystallinity, and increasing of by-products (such as diethylene glycol), resulting in poor heat resistance.

[0006] Among them, in Patent Document 1, as a coloring main substance removal step, attempts are made to perform an adsorption treatment in which the coloring main substance is brought into contact with an adsorbent, a decomposition treatment in which the coloring main substance is decomposed with a decomposer, a reduction treatment in which the coloring main substance is reduced with a reducing agent, etc. However, although the coloring main substance such as a dye that is obviously mixed into the polymer is removed to some extent, a method for producing a polyester polymer in which coloring is suppressed as in conventionally produced polyester polymers has not yet been obtained.

[0007] Patent Document 1: Japanese Patent Application Publication No. 2008-88096 Summary of the invention

[0008] The present invention has been accomplished in view of the above background. The object of the present invention is, first, to provide a method for producing an aromatic polyester polymer and an intermediate thereof in which coloration is suppressed as in the case of an original product (a product produced by polymerizing monomers without depolymerization) in a method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester by depolymerizing a polyester and a method for producing a polyester polymer therefrom.

[0009] The present invention aims to provide a method for producing a regenerated aromatic polyester by depolymerizing an aromatic polyester contained in polyester fiber scraps, recycled polyester products, etc., and then repolymerizing the aromatic polyester to obtain the regenerated aromatic polyester, and a method for producing a regenerated aromatic polyester having heat resistance as good as that of the original aromatic polyester. In particular, a method for producing a regenerated aromatic polyester having heat resistance as good as that of the original aromatic polyester even when the aromatic polyester contains an isophthalic acid sulfonic acid component as a dicarboxylic acid component.

[0010] That is, the first invention of the present invention is a method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester, characterized in that it is a method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester by depolymerizing a polyester in the presence of a catalyst, the catalyst being a manganese-based catalyst, and the amount of the catalyst used being 20 to 500 mmol% relative to the polyester.

[0011] The method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester of the present invention is a method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester by depolymerizing a polyester in the presence of a catalyst, wherein the catalyst is a manganese-based catalyst and the amount of the catalyst used is 20 to 500 mmol% based on the polyester.

[0012] The polyester contains polyalkylene terephthalate as a main component, and the polyalkylene terephthalate is any one of polyethylene terephthalate, polypropylene terephthalate, and polybutylene terephthalate.

[0013] In addition, it is preferred that the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is bis(hydroxyalkyl) benzene dicarboxylate, or that the manganese-based catalyst is manganese acetate. It is preferred that the catalyst be used in the form of a solution preliminarily dissolved in an alkylene glycol, and after depolymerization, the temperature is lowered in the alkylene glycol to perform crystallization, and after the crystallization, the solution is washed with water.

[0014] The first invention of the present invention also includes a method for producing a polyester resin, characterized in that the aromatic dicarboxylic acid bis(hydroxyalkyl) ester obtained by any of the above-mentioned production methods is repolymerized, and includes a polyester resin obtained by the production method.

[0015] The present invention adopts a method for producing a regenerated aromatic polyester as a preferred embodiment, characterized in that the method comprises depolymerizing a polyester containing an aromatic polyester and then polycondensing the components obtained by depolymerization to obtain a regenerated aromatic polyester, wherein the depolymerization is carried out by depolymerizing the polyester in the presence of a catalyst to obtain an aromatic dicarboxylic acid bis(hydroxyalkyl) ester, and the catalyst used for the depolymerization is a manganese-based catalyst, and the amount of the catalyst used is 20 to 500 mmol% relative to the polyester.

[0016] In this preferred embodiment, it is more preferred to purify the aromatic dicarboxylic acid bis(hydroxyalkyl) ester after depolymerization and before polycondensation.

[0017] Furthermore, it is particularly preferred that the polycondensation is carried out by polycondensing the purified aromatic dicarboxylic acid bis(hydroxyalkyl) ester in the presence of an alkali metal and / or an alkaline earth metal.

[0018] In addition, the present invention is a method for producing a regenerated aromatic polyester, characterized in that the polyester containing the aromatic polyester is depolymerized and then the depolymerized components are polycondensed to obtain the regenerated aromatic polyester, wherein the polyester containing the aromatic polyester is depolymerized in an alkylene glycol to obtain an aromatic dicarboxylic acid bis(hydroxyalkyl) ester, the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is purified, and the purified aromatic dicarboxylic acid bis(hydroxyalkyl) ester is polycondensed in the presence of an alkali metal and / or an alkaline earth metal to obtain the regenerated aromatic polyester. This is the second invention of the present invention, which will be described in detail later.

[0019] According to the present invention, first, in a method for producing a bis(hydroxyalkyl) aromatic dicarboxylate by depolymerizing a polyester and a method for producing a polyester polymer therefrom, a method for producing a polyester polymer and an intermediate thereof in which coloring is suppressed as with an original product (a product produced by polymerizing monomers without depolymerization).

[0020] According to the present invention, secondly, a method for producing a recycled aromatic polyester can be provided, wherein the recycled aromatic polyester is obtained by depolymerizing the aromatic polyester contained in polyester fiber scraps, recycled polyester products, etc., and then polymerizing the recycled aromatic polyester again, and a method for producing a recycled aromatic polyester having heat resistance as good as that of the original aromatic polyester can be provided. In particular, a method for producing a recycled aromatic polyester having heat resistance as good as that of the original aromatic polyester can be provided even when the aromatic polyester contains an isophthalic acid sulfonic acid component as a dicarboxylic acid component. DETAILED DESCRIPTION

[0021] [First invention]

[0022] Hereinafter, the first aspect of the present invention will be described in detail.

[0023] The present invention is a method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester by depolymerizing a polyester in the presence of a catalyst. Here, polyester refers to a polycondensate synthesized by forming an ester bond by dehydration condensation of a polycarboxylic acid and a polyol. Alternatively, polyester refers to a polymer having an ester bond. The polyester is preferably a semi-aromatic polyester.

[0024] As the polycarboxylic acid constituting such a polyester, a dicarboxylic acid or an ester-forming derivative thereof is preferably used, and specific examples thereof include terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, bis(p-carboxyphenyl)methane, anthracene dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 5-tetrabutyl Aromatic dicarboxylic acids such as isophthalic acid and sodium 5-sulfoisophthalic acid. In addition, aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, malonic acid, glutaric acid, and dimer acid, and alicyclic dicarboxylic acids such as 1,3-cyclohexanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid can be mentioned. In addition, ester-forming derivatives of the above dicarboxylic acids can also be used.

[0025] Among them, as the polycarboxylic acid constituting the polyester used in the present invention, it is more preferred to mainly use terephthalic acid and 2,6-naphthalene dicarboxylic acid. In addition, mainly using terephthalic acid can be applied to the case where an isophthalic acid component is used as a copolymerization component, and more specifically, it can be applied to the case where isophthalic acid or 5-sodium sulfoisophthalic acid is copolymerized to form a polyester.

[0026] In addition, as the polyol constituting the other component of the polyester, it is preferred to use a diol or an ester-forming derivative thereof, and specific examples include aliphatic diols having 2 to 20 carbon atoms, namely ethylene glycol, 1,3-propanediol, propylene glycol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, decamethylene glycol, cyclohexanedimethanol, cyclohexanediol, dimer diol, and the like.

[0027] Alternatively, as the polyol, a long-chain diol having a molecular weight of 200 to 100,000 may be used, namely polyethylene glycol, polypropylene glycol, polypropylene glycol, polytetramethylene glycol, etc. In addition, an aromatic dihydroxy compound may be used, namely 4,4'-dihydroxybiphenyl, hydroquinone, tert-butylhydroquinone, bisphenol A, bisphenol S, bisphenol F, etc. In addition, ester-forming derivatives of these polyols and diols are also preferably used.

[0028] Among them, ethylene glycol (hereinafter, sometimes referred to as EG), 1,3-propylene glycol, and 1,4-butanediol are preferably used as the alcohol constituting the polyester used in the present invention.

[0029] In the present invention, a polyester composed of a combination of a polycarboxylic acid and a polyol as described above can be used as a starting material, but the polyester is preferably a semi-aromatic polyester, and more preferably a polyalkylene terephthalate. In particular, the polyalkylene terephthalate is particularly preferably any one of polyethylene terephthalate, polypropylene terephthalate, and polybutylene terephthalate.

[0030] Furthermore, in the method for producing the aromatic dicarboxylic acid bis(hydroxyalkyl) ester of the present invention, the polyester as described above is depolymerized in the presence of a catalyst. However, in the present invention, it is important to select a manganese-based catalyst as the catalyst.

[0031] As the manganese catalyst, for example, fatty acid salts, carbonates, sulfates, phosphates, oxides, hydroxides, halides, alkoxides, etc. of manganese (Mn) can be exemplified, and a combination of one or more of them is also preferred. In the present invention, manganese oxide and manganese acetate can be used in particular, and manganese acetate is particularly preferably used.

[0032] In addition, the catalyst used is preferably used in the form of a solution dissolved in an alkylene glycol in advance. As the alkylene glycol (hereinafter, sometimes referred to as AG), the same diol component as that forming the skeleton structure of the polyester of the above-mentioned starting material can be used. In addition, a diol can also be used, which constitutes the polyester obtained as the final product obtained by repolymerizing the aromatic dicarboxylic acid bis (hydroxyalkyl) ester obtained by the production method of the present invention.

[0033] As the alkylene glycol that forms or can form the backbone structure of the polyester, for example, when the polyester is polyethylene terephthalate (PET), ethylene glycol (EG) can be exemplified, when it is polypropylene terephthalate, 1,3-propylene glycol (trimethylene glycol, C3G) can be exemplified, and when it is polybutylene terephthalate, 1,4-butanediol (C4G) can be exemplified. In addition, as the alkylene glycol, a mixture of the above alkylene glycols can also be preferably used according to the purpose.

[0034] Although the reason is not clear, the effect of the present invention is significantly shown only when a manganese-based catalyst is selected from a plurality of catalysts. It should be noted that the effect of the present invention is particularly significant when no other coloring matter is contained, compared to the depolymerization of recycled polyester containing other coloring matter. For example, the depolymerized polyester often gradually changes color due to long-term storage, but the depolymerized polyester obtained by the production method of the present invention has significantly less color change.

[0035] In addition, in the production method of the present invention, the amount of the catalyst used must be 20 to 500 mmol%, more preferably 30 to 300 mmol, and particularly preferably 50 to 150 mmol% relative to the polyester. Here, mol% represents the ratio of the number of catalyst molecules to the constituent units of the polyester, and mmol% is 1000 times that. In the case of other conventional catalysts, sufficient depolymerization is not performed at such a low addition amount, but by using a manganese-based catalyst, it can be suppressed to a low usage amount. If the catalyst usage is less than this range, the catalyst activity is insufficient, and if it is too much, the effect of suppressing discoloration is reduced.

[0036] The method for producing the aromatic dicarboxylic acid bis(hydroxyalkyl) ester of the present invention comprises depolymerizing the above polyester in the presence of a manganese-based catalyst, wherein the amount of the catalyst used at that time must be 20 to 500 mmol% based on the polyester.

[0037] Furthermore, in the production method of the present invention, after depolymerization using the above-mentioned catalyst, it is preferred to cool down in the alkylene glycol and perform crystallization. As the cooling condition during crystallization, it is preferred to cool down from a temperature of 60°C or more to 25°C or less, and more preferably to cool to 15°C or less. Furthermore, after crystallization, solid-liquid separation is preferably performed, and the alkylene glycol content in the cake after solid-liquid separation is preferably 100% by mass or less. Furthermore, it is preferred to adjust the alkylene glycol content to 55% by mass or less, or in the range of 1 to 30% by mass, and particularly preferably in the range of 5 to 25% by mass. In addition, the amount of alkylene glycol used in the initial depolymerization is preferably 2 to 20 times the amount of the polyester of the raw material, and more preferably 3 to 10 times the amount used. By using such a large amount of alkylene glycol during depolymerization, the amount of depolymerization catalyst and other foreign matter mixed in the production method of the present invention can be further reduced by performing crystallization and solid-liquid separation.

[0038] Since the manganese catalyst used in the present invention is used in a small amount, the amount of the catalyst can be further reduced in the treatment in the alkylene glycol. In addition, when manganese acetate is used as a catalyst, the solubility in the alkylene glycol is high, and the amount of the catalyst remaining in the subsequent steps can be more effectively reduced.

[0039] Furthermore, in the production method of the present invention, it is preferred that the cake after depolymerization is washed with water or with an alkylene glycol after the crystallization as described above. Furthermore, it is preferred that the cleaning liquid is sprayed while being treated with a suction filter. By performing these treatments, the depolymerization catalyst dissolved in the alkylene glycol, other coloring substances, etc. are washed away, and a more purified aromatic dicarboxylic acid bis(hydroxyalkyl) ester can be obtained. As a solution for washing, a solution with low viscosity is preferably used, and water is preferably used from this point of view. As the amount of the cleaning liquid, it is preferably 1 to 100 times the weight of the cake, and more preferably 1.5 to 10 times the weight. As the liquid temperature during washing, it is preferably in the range of 0 to 40°C. If the temperature is too high, the cake itself is easily dissolved and the yield is reduced. Thereafter, by drying with a vacuum dryer or the like, an aromatic dicarboxylic acid bis(hydroxyalkyl) ester can be obtained. It should be noted that when the alkylene glycol used in the production method of the present invention is the same as the diol component of the polyester resin after repolymerization, it is also a preferred method for producing polyester to directly repolymerize without drying.

[0040] As the bis(hydroxyalkyl) aromatic dicarboxylate obtained by the production method of the present invention, it depends on the types of polyester and alkylene glycol used, but when polyester (polyalkylene terephthalate) mainly using terephthalic acid as a polycarboxylic acid is used as a raw material, it is preferable to use a method for producing bis(hydroxyalkyl) terephthalate (hereinafter, BHAT; also referred to as bishydroxyalkyl terephthalate). More specifically, when C3G (1,3-propylene glycol (trimethylene glycol)) is used as an alkylene glycol, BHPT (bishydroxypropyl terephthalate) is produced, and when C4G (1,4-butanediol) is used, BHBT (bishydroxybutyl terephthalate) is produced. In particular, when polyethylene terephthalate composed of terephthalic acid and ethylene glycol is mainly used as a component constituting the polyester, bis(hydroxyethyl) terephthalate (BHET; bishydroxyethyl terephthalate) can be produced.

[0041] Furthermore, the bis(hydroxyalkyl) aromatic dicarboxylate obtained by the production method of the present invention can be repolymerized by a known method to become a polyester resin having an excellent hue and being less prone to coloration.

[0042] That is, another method for producing a polyester resin of the present invention is a method for producing by repolymerizing the aromatic dicarboxylic acid bis(hydroxyalkyl) ester obtained by the above-mentioned production method. Furthermore, another polyester resin of the present invention is obtained by the production method of the polyester resin.

[0043] As a catalyst for the repolymerization to obtain the polyester resin, a known catalyst such as Sb, Ge or titanium can be used, and antimony trioxide is particularly preferred. The alkylene glycol etc. produced by the reaction during the repolymerization preferably flows out of the reactor while undergoing a polycondensation reaction. The amount of the catalyst used is preferably in the range of 10 to 1000 ppm relative to the weight of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester used.

[0044] Furthermore, in the method for producing the polyester resin of the present invention, after polycondensation using a catalyst, a conventionally known phosphorus stabilizer is preferably used. The amount of the phosphorus stabilizer used is preferably in the range of 1 to 100 ppm relative to the weight of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester used.

[0045] The polyester resin obtained in this way is different from the case where magnesium hydroxide, sodium hydroxide, etc., which are commonly used in the past, are used as depolymerization catalysts, and becomes a resin with less discoloration such as yellowing. This is a degree that can be visually confirmed at the stage of the aromatic dicarboxylic acid bis (hydroxyalkyl) ester obtained on the way, but after repolymerization into a resin, when the hue L*, a*, and b* values ​​are measured with a colorimeter, it is particularly significant that the polyester produced under the conditions of the present invention is -3 or less, and more preferably only -3.5 or less, while the values ​​of substances produced by other catalysts are higher than this, and some of them have positive values ​​(yellow tint). Although the reason is not certain, it is believed that the manganese-based catalyst can be depolymerized at a low concentration, and not only is it difficult to generate coloring by-products, but it is also easy to dissociate from the aromatic dicarboxylic acid bis (hydroxyalkyl) ester even in the subsequent crystallization process, and it is extremely difficult to remain as an impurity, which is effective.

[0046] Furthermore, the obtained polyester resin can be suitably used in applications such as fibers, films, and resins.

[0047] [Second invention]

[0048] Next, the second invention of the present invention is described in detail. The second invention of the present invention is a method for producing a regenerated aromatic polyester, characterized in that the polyester containing the aromatic polyester is depolymerized and then the depolymerized components are polycondensed to obtain the regenerated aromatic polyester, wherein the polyester containing the aromatic polyester is depolymerized in an alkylene glycol to obtain an aromatic dicarboxylic acid bis(hydroxyalkyl) ester, the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is purified, and the purified aromatic dicarboxylic acid bis(hydroxyalkyl) ester is polycondensed in the presence of an alkali metal and / or an alkaline earth metal to obtain the regenerated aromatic polyester.

[0049] Hereinafter, the second invention and preferred embodiments thereof will be described in detail.

[0050] [Polyester]

[0051] In the second invention of the present invention, the polyester used as the raw material for obtaining the regenerated aromatic polyester is a polyester recovered from a polyester excipient (hereinafter referred to as "recycled polyester"), and the recycled polyester containing the aromatic polyester is used. The polyester excipient may be a fiber, a film, a sheet, or a product formed into other forms.

[0052] When the recycled polyester is in the form of fiber, it may be in the form of a fiber processed product. When it is in the form of a film or sheet, it may be in the form of a tray or a bag. As another form, a bottle may be exemplified.

[0053] The recycled polyester may be polyester recovered from scraps and unqualified products generated in the manufacturing process. The scraps and unqualified products may include, for example, raw material pellets that do not meet the required level, unnecessary materials during molding or processing, cut pieces, scraps, transitional products generated during brand change, trial products, defective products, or cut products thereof.

[0054] In a preferred embodiment of the second invention of the present invention, polyester fiber scraps are used as the recycled polyester. In the recycled polyester, the polyester fiber scraps preferably account for 50% by mass or more, more preferably 51% by mass or more, and further preferably 70% by mass or more.

[0055] The polyester fiber scraps are recycled as scraps in the manufacturing process, processing process, circulation, etc. before they appear on the market as fiber products or fiber processed products, and the fiber products or fiber processed products recycled after they appear on the market are eligible. The fiber processed products may be used or unused, or they may be discarded.

[0056] The polyester fiber scraps may be composed of polyester fibers, and may also include natural fibers such as cotton, wool, and silk, chemical fibers derived from natural materials such as rayon, cuprammonium, acetate, and lyocell, and synthetic fibers other than polyester fibers such as polyamide fibers, acrylic fibers, and urethane fibers.

[0057] The polyester fiber scraps may be colored, or may be cationically dyeable polyester fibers dyed with cation dyes having excellent color development and vividness. The cationically dyeable polyester fibers are composed of aromatic polyesters copolymerized with aromatic dicarboxylic acids having sulfonate groups as substituents on aromatic rings to which cation dyes can be ionically bonded.

[0058] [Aromatic polyester]

[0059] The aromatic polyester is a polymer obtained by polycondensing an aromatic dicarboxylic acid component and a diol component. The aromatic polyester may be a homopolymer, a copolymer, or a mixture thereof.

[0060] Examples of the aromatic dicarboxylic acid component constituting the aromatic polyester include terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, bis(p-carboxyphenyl)methane, anthracene dicarboxylic acid, and 4,4′-diphenyl ether dicarboxylic acid. Preferred are terephthalic acid and 2,6-naphthalene dicarboxylic acid, and particularly preferred is terephthalic acid.

[0061] In addition to the above aromatic dicarboxylic acid components, 5-sodium sulfoisophthalate, 5-tetrabutyl sulfoisophthalate, An aromatic dicarboxylic acid having a sulfonate group as a substituent on an aromatic ring, such as 5-tetrabutylammonium isophthalate.

[0062] As the diol component constituting the aromatic polyester, an aliphatic diol or an alicyclic diol having 2 to 20 carbon atoms can be used. Specifically, ethylene glycol, 1,3-propylene glycol, propylene glycol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, decamethylene glycol, cyclohexanedimethanol, cyclohexanediol, and dimer glycol can be exemplified, and ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,4-cyclohexanedimethanol are preferred.

[0063] As the aromatic polyester, polyalkylene terephthalate using terephthalic acid as the dicarboxylic acid component and alkylene glycol as the glycol is preferred. In this case, ethylene glycol, 1,3-propylene glycol, and 1,4-butylene glycol are preferred as the aromatic polyester. Polyethylene terephthalate, polypropylene terephthalate, and polybutylene terephthalate are preferred as the aromatic polyester. These aromatic polyesters may also be copolymers.

[0064] The copolymerized aromatic polyester containing an aromatic dicarboxylic acid having a sulfonate group has good dyeability with a cationic dye, and therefore this component is often contained in the aromatic polyester of the fiber.

[0065] In the second invention of the present invention, the aromatic polyester may be a copolyester containing an isophthalic acid component having a sulfonate group, especially a metal sulfonate group, as a dicarboxylic acid component. As the isophthalic acid having a metal sulfonate group, sodium 5-sulfoisophthalate can be exemplified. In this case, the aromatic dicarboxylic acid bis(hydroxyalkyl) ester obtained by depolymerization described later becomes sodium bis(2-hydroxyethyl) 5-sulfoisophthalate.

[0066] The copolymerization amount of the isophthalic acid sulfonate component in the aromatic polyester is 0.5 to 15 mol %, preferably 1 to 10 mol %, based on the total dicarboxylic acid components.

[0067] According to the second aspect of the present invention, even when a copolymerized aromatic polyester obtained by copolymerizing an isophthalic acid sulfonate component is mixed into an aromatic polyester serving as a raw material for depolymerization, a regenerated aromatic polyester having high heat resistance can be obtained.

[0068] As a preferred example of the aromatic polyester of the second invention object of the present invention, the main dicarboxylic acid component is terephthalic acid, the auxiliary dicarboxylic acid component includes sodium 5-sulfoisophthalic acid, and the diol component is ethylene glycol. Here, "mainly" means that the diol component accounts for 80 mol% or more, preferably 90 mol% or more, based on the total dicarboxylic acid component.

[0069] [Depolymerization]

[0070] In the second aspect of the present invention, the aromatic polyester is depolymerized in an alkylene glycol. The depolymerization reaction is carried out in the presence of a catalyst, and as the catalyst, a manganese-based catalyst or a zinc-based catalyst is preferably used, and a manganese-based catalyst is particularly preferably used.

[0071] Examples of the manganese-based catalyst include fatty acid salts, carbonates, sulfates, phosphates, oxides (manganese oxide), hydroxides, halides, and alkoxides of manganese. Examples of the fatty acid salt of manganese include manganese acetate.

[0072] As the manganese catalyst, manganese oxide and manganese acetate are preferably used from the viewpoint of the color of the polymer after repolymerization, and manganese acetate is particularly preferably used. These can be used alone or in combination of multiple types. The catalyst is preliminarily dissolved or suspended in an alkylene glycol and used in the form of a solution or suspension.

[0073] When manganese acetate is used as a catalyst, its solubility in alkylene glycol is high, and the amount of residual catalyst can be reduced. The amount of alkylene glycol used in the depolymerization reaction is preferably 2 to 20 times the mass of the aromatic polyester, and more preferably 3 to 10 times the mass. By using alkylene glycol within this range, the amount of catalyst and other foreign matter mixed in can be reduced, so it is preferred.

[0074] The amount of the manganese catalyst used in the depolymerization reaction is preferably 20 to 500 mmol, more preferably 30 to 300 mmol, and particularly preferably 50 to 150 mmol, relative to the total dicarboxylic acid components constituting the aromatic polyester. When the manganese catalyst is not used, sufficient depolymerization cannot be performed with such a low concentration of the catalyst added. When the amount of the catalyst used is less than 20 mmol%, the catalyst activity is insufficient and is not preferred, and when it exceeds 500 mmol%, the effect of suppressing discoloration becomes less and is not preferred.

[0075] The depolymerization reaction temperature is, for example, 180 to 250° C., preferably 185 to 210° C., the time is, for example, 0.5 to 10 hours, preferably 1 to 4 hours, and the pressure can be normal pressure, for example, 760 to 2000 mmHg.

[0076] [Alkylene glycol]

[0077] As the alkylene glycol, the same diol component as that constituting the above aromatic polyester is used, or preferably the same diol component as that constituting the regenerated aromatic polyester obtained by the production method according to the second aspect of the present invention is used.

[0078] That is, in accordance with the aromatic polyester or the regenerated aromatic polyester, the following are preferably used as the alkylene glycol.

[0079] When the aromatic polyester and / or regenerated aromatic polyester is polyethylene terephthalate, ethylene glycol is preferably used as the alkylene glycol.

[0080] When the aromatic polyester and / or regenerated aromatic polyester is polytrimethylene terephthalate, it is preferred to use 1,3-propylene glycol (trimethylene glycol) as the alkylene glycol.

[0081] When the aromatic polyester and / or regenerated aromatic polyester is polybutylene terephthalate, 1,4-butanediol is preferably used as the alkylene glycol.

[0082] In either case, the alkylene glycol may be a mixture of alkylene glycols constituting the aromatic polyester and / or the regenerated aromatic polyester.

[0083] [purification]

[0084] In the second aspect of the present invention, it is important to purify the aromatic dicarboxylic acid bis(hydroxyalkyl) ester obtained by depolymerizing the aromatic polyester.

[0085] The purification of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is preferably performed by crystallization of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester in an alkylene glycol solution.

[0086] The crystallization is preferably carried out by cooling the solution obtained by depolymerizing the aromatic polyester from a temperature of 60° C. or higher to a temperature of 25° C. or lower, more preferably to a temperature of 15° C. or lower.

[0087] The solid of the crystallized aromatic dicarboxylic acid bis(hydroxyalkyl) ester is separated from the liquid solution by cooling. The solid of the crystallized aromatic dicarboxylic acid bis(hydroxyalkyl) ester is called "cake". After being separated from the liquid, the cake is subjected to polycondensation reaction.

[0088] As one embodiment of the second invention of the present invention, the aromatic polyester is an aromatic polyester containing an isophthalic acid component having a metal sulfonate group as a copolymer component, that is, an embodiment of an aromatic polyester having terephthalic acid as a main dicarboxylic acid component, sodium 5-sulfoisophthalate as an auxiliary dicarboxylic acid component, and ethylene glycol as a diol component. In this case, when depolymerized, the main depolymerized product is bis(2-hydroxyethyl)terephthalate, the auxiliary depolymerized product is sodium bis(2-hydroxyethyl)5-sulfoisophthalate, and the obtained depolymerized product is a mixture of these. When purified, bis(2-hydroxyethyl)terephthalate (sometimes referred to as bis-2-hydroxyethyl terephthalate or BHET) is crystallized as a cake, while the associated depolymerized product, bis(2-hydroxyethyl)isophthalate-5-sodium sulfonate (also referred to as BHESI), is present in a liquid state without crystallization. Therefore, by solid-liquid separation, the crystallized BHET can be obtained in a solid state and separated from the non-crystallized liquid BHESI, so that only BHET can be extracted with high purity.

[0089] Therefore, in the second invention of the present invention, even if the aromatic polyester contains an isophthalic acid component having a metal sulfonate group as a copolymer component, it is possible to produce a regenerated aromatic polyester having excellent heat resistance by depolymerizing it, separating the copolymer component, and polycondensing it again. In this case, the amount of the isophthalic acid component having a metal sulfonate group contained in the aromatic polyester is, for example, 2 mol% or less, preferably 0.5 mol% or less, based on the amount of all dicarboxylic acid components in the aromatic polyester.

[0090] [Cleaning]

[0091] The cake of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is preferably washed. That is, it is preferably washed after the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is crystallized.

[0092] The cake is preferably washed using water or alkylene glycol as a washing liquid. The washing liquid is preferably a washing liquid with low viscosity, and from this viewpoint, water is preferably used. The washing is preferably carried out by spraying the washing liquid onto the cake while treating it with a suction filter.

[0093] By washing, the depolymerization catalyst dissolved in the alkylene glycol solution after depolymerization and the coloring substances contained in the aromatic polyester subjected to depolymerization are washed away, and a highly pure aromatic dicarboxylic acid bis(hydroxyalkyl) ester can be obtained.

[0094] The amount of the washing liquid used for washing is preferably 1 to 100 times the mass of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester cake, and more preferably 1.5 to 10 times the mass. The temperature of the washing liquid is preferably 0 to 40° C. If the temperature exceeds 40° C., the cake itself is easily dissolved, and the yield is reduced, so it is not suitable.

[0095] After washing, the cake is dried to obtain a high-purity aromatic dicarboxylic acid bis(hydroxyalkyl) ester having no sulfonic group. Drying can be performed using, for example, a vacuum dryer.

[0096] When an alkylene glycol is used as the cleaning liquid and the alkylene glycol used is the same as the diol component of the regenerated aromatic polyester, the polyester may be subjected to polycondensation without being dried.

[0097] A preferred embodiment is one in which the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is washed, dried, and then subjected to polycondensation reaction.

[0098] [Polycondensation]

[0099] In order to obtain a regenerated aromatic polyester from an aromatic dicarboxylic acid bis(hydroxyalkyl)ester, a polycondensation reaction is performed. The polycondensation reaction is performed using a polymerization catalyst in the presence of an alkali metal and / or an alkaline earth metal. The polycondensation reaction itself can be performed using a polymerization catalyst conventionally used in the art and in a method conventionally used in the art. The polycondensation reaction is preferably performed while distilling the alkylene glycol produced during the polycondensation reaction out of the reaction vessel.

[0100] Examples of the polymerization catalyst include antimony-based, germanium-based, and titanium-based catalysts, and antimony-based catalysts are preferred. As the antimony-based catalyst, for example, antimony trioxide is used. The amount of the polymerization catalyst used is preferably 10 to 1000 ppm relative to the mass of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester.

[0101] When subjected to the polycondensation reaction, the alkylene glycol content of the cake of the purified aromatic dicarboxylic acid bis(hydroxyalkyl) ester is preferably 100% by mass or less, more preferably 55% by mass or less, further preferably 30% by mass or less, and particularly preferably 25% by mass or less, based on the mass of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester.

[0102] The polycondensation reaction is carried out at a temperature of, for example, 230 to 330° C., preferably 250 to 310° C., for example, 240 minutes or less, preferably 180 minutes or less, and under reduced pressure, for example, 100 Pa or less, preferably 50 Pa or less.

[0103] [Alkali metal and / or alkaline earth metal]

[0104] Examples of the alkali metal include lithium, sodium, potassium, rubidium and cesium, and sodium and potassium are preferably used.

[0105] Examples of the alkaline earth metal include calcium, barium, beryllium and magnesium, and calcium and magnesium are preferably used.

[0106] As the alkali metal and / or alkaline earth metal, sodium is particularly preferred.

[0107] From the viewpoint of the hue of the polymer after repolymerization, the amount of the alkali metal and / or alkaline earth metal used is preferably 5 to 1000 ppm, more preferably 10 to 500 ppm, based on the mass of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester.

[0108] The alkali metal and / or alkaline earth metal are preferably used in the form of their respective salts. That is, they are preferably used in the form of alkali metal salts and / or alkaline earth metal salts.

[0109] Examples of the acid component constituting the alkali metal salt and / or alkaline earth metal salt include propionic acid, acetic acid, oxalic acid, formic acid, carbonic acid and the like, and acetic acid is preferably used.

[0110] As the alkali metal salt and / or alkaline earth metal salt, lithium acetate, sodium acetate, potassium acetate, calcium acetate, barium acetate, and magnesium acetate are preferably used, and sodium acetate is more preferably used.

[0111] [Stabilizer]

[0112] During the polycondensation reaction, it is preferred to add a phosphorus stabilizer. The phosphorus stabilizer may be a known phosphorus stabilizer, and the amount thereof is, for example, 1 to 100 ppm relative to the mass of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester. Examples of the phosphorus stabilizer include phosphorous acid, orthophosphoric acid, trimethyl phosphate, triethyl phosphate, triphenyl phosphate, diethyl phenylphosphonate, dimethyl (2-hydroxyethyl)phosphonate and / or phenylphosphonic acid, preferably orthophosphoric acid, trimethyl phosphate, triethyl phosphate and triphenyl phosphate.

[0113] Example

[0114] Hereinafter, the present invention will be described in more detail by way of examples. It should be noted that each value in the examples was obtained by the following measuring methods.

[0115] In describing the amount of catalyst added, "mol %" of the catalyst relative to the polyester means the ratio of the number of catalyst molecules relative to the constituent units of the polyester.

[0116] (1) Measurement method

[0117] 1) Hue (L*a*b*)

[0118] The measurement was performed by the following method. A polymer (5 g) was pressed between two metal plates to form a plate, and then the sample was heated at 140°C for 2 hours to crystallize. The sample was subjected to measurement using a measuring device ("ZE-6000" manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS Z8781-4:2013 to measure the hue L*, a*, and b* values.

[0119] 2) Metal content

[0120] The amounts of various metal elements in the polymer were measured by heating and melting the polymer to form a disk, and using a fluorescent X-ray measuring device "ZSXPrimus II" manufactured by RIGAKU Co., Ltd. to measure the amount of metal corresponding to the catalyst used. "ND" in the table means below the detection limit (below 5 ppm).

[0121] 3) Intrinsic viscosity number (IV)

[0122] After 0.6 g of the polyester was dissolved in 50 cc of o-chlorophenol by heating, the solution was cooled once and the viscosity of the solution was measured at 35° C. using an Ubbelohde viscometer and calculated using a separately prepared calibration curve.

[0123] 4) Glass transition temperature (Tg), melting point (Tm), crystallization temperature (Tc)

[0124] 10 mg of the sample was cut and filled in an aluminum pan, and the melting point was measured using a "DSC device Q10" manufactured by TA Instruments-Waters LLC. As the measurement conditions, the temperature was first temporarily raised from 25°C to 300°C at a heating rate of 20°C / min, and then rapidly cooled. Then, the quenched sample was heated from 25°C to 300°C at 20°C / min to determine the crystalline melting point.

[0125] 5) Content of 5-Sodium Sulfonisophthalate

[0126] The sample was formed into a plate, and the sulfur content derived from the sulfonic acid group was measured using a fluorescent X-ray apparatus "ZSXPrimus II" manufactured by RIGAKU Co., Ltd. to calculate the content of 5-sodium sulfoisophthalate. "ND" in the table means below the detection limit (5 ppm or less).

[0127] 6) Diethylene glycol (DEG) content

[0128] The polyester was decomposed using hydrazine hydrate, and the content of diethylene glycol in the decomposition product was measured using gas chromatography ("HP6850" manufactured by Hewlett-Packard Company).

[0129] (2) Polyester resin

[0130] As the polyester resin to be depolymerized, polyethylene terephthalate (PET) pellets which are generally available were obtained. The physical properties and color tone of the polyester resin are as shown in Table 1.

[0131] In Examples 1 to 3 and Comparative Examples 1 to 12, the polyethylene terephthalate (PET) pellets were used as the polyester resin for depolymerization.

[0132] [Table 1]

[0133]

[0134] [Example 1]

[0135] 1500 parts by mass of ethylene glycol (EG) and 0.38 parts by mass of manganese acetate as a depolymerization catalyst (100 mmol% relative to the polyester) were placed in a 2 L separable flask with respect to 300 parts by mass of the polyester resin, and the mixture was sealed with nitrogen. At this time, manganese acetate was previously dissolved in EG and then placed. The polyester resin used was an uncolored polyethylene terephthalate resin, and contained 297 ppm of Sb as a polymerization catalyst.

[0136] Thereafter, the separable flask containing the sample was heated and stirred at an internal temperature of 220°C by an electric heating jacket, and a depolymerization treatment was performed for 4 hours at normal pressure. The depolymerized BHET (bis(hydroxyethyl)benzenedicarboxylate) solution was colorless and transparent, and no coloring was observed. Furthermore, the depolymerized solution was filtered with a 200 μm mesh to remove the solid components remaining inside, and then slowly cooled to 70°C, stirred and cooled while cooling with a temperature drop of 70°C → 40°C for a time of 0 → 10 minutes, a temperature drop of 40°C → 30°C for a time of 10 → 60 minutes, and a temperature drop of 30°C → 15°C for a time of 60 → 180 minutes. Thereafter, stirring was performed for 60 minutes at an internal temperature of 15°C, and the internal temperature was lowered to allow BHET crystals to precipitate (a total of 4 hours), thereby obtaining a BHET / EG slurry.

[0137] BHET / EG slurry was squeezed by a filter press manufactured by Nippon Filtration Device Co., Ltd. to separate BHET from EG by solid-liquid separation. The separated BHET contained 35% by mass of EG relative to the weight of the cake recovered after the filter press. For the cake after the EG separation, 2 times the weight of 25°C pure water was sprayed while water washing was performed with a suction filter. For the BHET after the solid-liquid separation was completed, a vacuum dryer was then used to dry it at 50°C for 8 hours to obtain dried BHET. The obtained BHET was white and no foreign matter was seen to be mixed in.

[0138] Thereafter, 254 parts by mass of the obtained dry BHET and 0.007 parts by mass of a phosphorus stabilizer were placed in a reaction vessel at normal pressure under a nitrogen atmosphere together with 0.07 parts by mass of antimony trioxide as a repolymerization catalyst. Next, the temperature in the reactor was set to 285° C., and the pressure was reduced in stages under normal pressure for 10 minutes, 4 kPa for 10 minutes, and 0.4 kPa for 40 minutes, while distilling the ethylene glycol and the like produced by the reaction out of the reactor, a polycondensation reaction was performed.

[0139] Tables 2 and 3 show the quality of the polyethylene terephthalate finally produced.

[0140] [Table 2]

[0141]

[0142] [Table 3]

[0143]

[0144] [Example 2]

[0145] The same treatment was carried out except that the depolymerization catalyst used in Example 1 was replaced with manganese oxide instead of manganese acetate, and the BHET obtained by depolymerization and the repolymerized polyethylene terephthalate resin were collected. At this time, the BHET solution after depolymerization was colorless and transparent, and no coloring was observed. The quality is shown in Tables 2 and 3.

[0146] [Example 3]

[0147] The same treatment was performed except that the amount of manganese acetate used in Example 1 was changed from 0.38 parts by mass (100 mmol% relative to polyester) to 0.30 parts by mass (80 mmol% relative to polyester). Although some undissolved matter was observed in the BHET solution after depolymerization, the BHET obtained by depolymerization and the repolymerized polyethylene terephthalate resin could be collected. The quality is also shown in Tables 2 and 3.

[0148] It should be noted that, when the same treatment as in Example 1 was carried out except that the amount of manganese acetate added was further reduced to 0.038 parts by mass (10 mmol% relative to the polyester), depolymerization did not proceed sufficiently, and a large amount of undecomposed polyester remained in the flask. The amount of BHET obtained was small, and repolymerization could not be performed.

[0149] [Comparative Examples 1 to 4]

[0150] The same treatment was carried out except that the manganese acetate used in Example 1 as the depolymerization catalyst was replaced with calcium acetate (Comparative Example 1), magnesium acetate (Comparative Example 2), cerium acetate (Comparative Example 3), and cobalt acetate (Comparative Example 4), respectively, to collect the BHET obtained by depolymerization and the repolymerized polyethylene terephthalate resin. When calcium acetate (Comparative Example 1) and magnesium acetate (Comparative Example 2) were used, more undecomposed products were observed after depolymerization. In addition, the BHET solutions after depolymerization obtained in Comparative Examples 1 to 4 were different from those in the examples, and coloration was observed. In addition, although the physical properties such as the melting point of the polyester finally obtained were the same as those in the examples, coloration was observed in the same way as the BHET in the intermediate stage. In addition, the metal content derived from each catalyst component showed a higher residual metal amount than manganese. The quality is shown in Tables 2 and 3.

[0151] [Comparative Example 5]

[0152] The depolymerization catalyst was replaced with tetrabutoxytitanium instead of manganese acetate used in Example 1. In addition, since this catalyst is also a polymerization catalyst, 0.07 g of antimony trioxide as a polymerization catalyst was not added. The same treatment was carried out, and the BHET obtained by depolymerization and the repolymerized polyethylene terephthalate resin were collected. The obtained BHET solution after depolymerization was obviously colored. Although the amount of antimony in the polyester resin finally obtained was suppressed, the residual metal amount of titanium was higher than that of manganese, and the coloring of BHET and the resin could not be suppressed. The quality is shown in Tables 2 and 3.

[0153] [Comparative Example 6]

[0154] The same treatment was carried out except that sodium hydroxide was used as the depolymerization catalyst instead of manganese acetate used in Example 1. However, depolymerization did not proceed sufficiently, and a large amount of undecomposed polyester remained in the flask. The amount of BHET was small, and repolymerization could not proceed.

[0155] [Comparative Examples 7 to 9]

[0156] The same treatment was carried out except that the depolymerization catalyst was replaced with sodium hydroxide (Comparative Example 7), sodium carbonate (Comparative Example 8), and sodium acetate (Comparative Example 9) as in Comparative Example 6, instead of manganese acetate used in Example 1, and the amount added was changed from 0.38 parts by mass in Example 1 to 9.0 parts by mass, and the BHET obtained by depolymerization and the repolymerized polyethylene terephthalate resin were collected. The obtained BHET solution after depolymerization was colored. However, the result was that the residual metal component in the repolymerized polyester was more than that in the example, and coloration was also observed. The quality is shown in Tables 2 and 3.

[0157] [Comparative Example 10]

[0158] The same treatment was carried out except that potassium carbonate was used as the depolymerization catalyst instead of manganese acetate used in Example 1. However, depolymerization did not proceed sufficiently, and a large amount of undecomposed polyester remained in the flask. The amount of BHET was small, and repolymerization could not proceed.

[0159] [Comparative Examples 11 and 12]

[0160] The same treatment was carried out except that the depolymerization catalyst was replaced with potassium carbonate (Comparative Example 11) and potassium acetate (Comparative Example 12) as in Comparative Example 10, and the amount added was changed from 0.38 parts by mass in Example 1 to 9.0 parts by mass. The BHET obtained by depolymerization and the repolymerized polyethylene terephthalate resin were collected. The obtained BHET solution after depolymerization was colored. However, the result showed that the residual metal component in the repolymerized polyester was more than that in the example, and coloration was also observed. The quality is shown in Tables 2 and 3.

[0161] [Reference example]

[0162] Hereinafter, the production of the copolyaromatic polyester and the aromatic polyester used in Example 21, Example 22, Reference Example 21 and Comparative Example 21 will be described with reference to Reference Examples 1 to 3.

[0163] [Reference Example 1] (Production of 5-Sodium Sulfonyl Isophthalate Copolymerized Aromatic Polyester 1)

[0164] In a reaction vessel under a nitrogen atmosphere and at normal pressure, 191.3 parts by mass of dimethyl terephthalate (DMT), 124.2 parts by mass of ethylene glycol (EG), and 4.4 parts by mass of sodium dimethyl 5-sulfonate produced by Takemoto Oil & Fats Co., Ltd. were added, and 0.07 parts by mass of manganese acetate and 0.22 parts by mass of sodium acetate were added as catalysts. The reaction temperature was set to 240° C., and an ester exchange reaction was carried out while removing methanol.

[0165] Next, 0.07 parts by mass of antimony trioxide and 0.03 parts by mass of orthophosphoric acid were added to the reactants after the transesterification reaction. The temperature in the reaction vessel was set to 285°C, and the pressure was reduced in stages under normal pressure for 10 minutes, 4 kPa for 10 minutes, and 0.4 kPa for 40 minutes, respectively, while the ethylene glycol produced by the reaction was distilled out of the reaction vessel, and the polycondensation reaction was carried out. Blockage of the distillation section by oligomers did not occur. Table 4 shows the quality of the generated copolyaromatic polyester.

[0166] [Reference Example 2] (Production of 5-Sodium Sulfonyl Isophthalate Copolymerized Aromatic Polyester 2)

[0167] In Reference Example 1, except that dimethyl terephthalate (DMT) was changed to 185.7 parts by mass and dimethyl 5-sodium sulfonate was changed to 13.0 parts by mass, the same conditions as in Reference Example 1 were carried out to obtain a copolymerized aromatic polyester. Table 4 shows the quality.

[0168] [Reference Example 3] (Production of aromatic polyester)

[0169] In a reaction vessel under nitrogen atmosphere and normal pressure, 194.2 parts by mass of dimethyl terephthalate (DMT), 124.2 parts by mass of ethylene glycol (EG), and 0.07 parts by mass of manganese acetate were added, and the reaction temperature was set to 240° C. while distilling off methanol, while carrying out an ester exchange reaction.

[0170] Next, 0.07 parts by mass of antimony trioxide and 0.03 parts by mass of orthophosphoric acid were added to the reactants after the transesterification reaction. The temperature in the reaction vessel was set to 285°C, and the pressure was reduced in stages under normal pressure for 10 minutes, 4 kPa for 10 minutes, and 0.4 kPa for 40 minutes, respectively, while the ethylene glycol produced by the reaction was distilled out of the reaction vessel, and the polycondensation reaction was carried out. Blockage of the distillation section by oligomers did not occur. Table 4 shows the quality of the generated aromatic polyester.

[0171] [Example 21]

[0172] To 300 parts by mass of the copolyaromatic polyester obtained in Reference Example 1, 1500 parts by mass of ethylene glycol (EG) and 0.38 parts by mass of manganese acetate (100 mmol% relative to the total dicarboxylic acid components of the copolyaromatic polyester) were charged in a 2 L separable flask.

[0173] At this time, manganese acetate was dissolved in EG in advance and used as a solution. Thereafter, a depolymerization reaction was carried out at 202° C. for 4 hours while stirring under nitrogen sealing to obtain a depolymerized sample.

[0174] The obtained depolymerized sample was slowly cooled to 70°C, and then the internal temperature was lowered while stirring and cooling in a 15°C thermostatic bath to precipitate crystals of bis-2-hydroxyethyl terephthalate (BHET), thereby obtaining a BHET / EG slurry.

[0175] The BHET / EG slurry was squeezed with a filter press manufactured by Nippon Filtration Devices Co., Ltd. to separate the solid and liquid of BHET and EG to obtain a BHET cake. The BHET contained 34% by mass of EG based on the weight of the cake recovered after the filtration.

[0176] The BHET cake after the EG separation was washed with water using a suction filter while spraying pure water twice its mass. The BHET cake after the solid-liquid separation was dried in a vacuum dryer at 50°C for 8 hours to obtain a depolymerized sample 1.

[0177] Thereafter, 254 parts by mass of the depolymerized sample 1, 0.07 parts by mass of antimony trioxide, 0.005 parts by mass of orthophosphoric acid, and 0.22 parts by mass of sodium acetate were placed in a reaction container under a nitrogen atmosphere and at normal pressure.

[0178] Next, the temperature in the reaction vessel was set to 285° C., and the pressure was reduced stepwise under conditions of normal pressure for 10 minutes, 4 kPa for 10 minutes, and 0.4 kPa for 40 minutes, respectively, while ethylene glycol and the like produced by the reaction were distilled out of the reaction vessel, a polycondensation reaction was carried out to obtain a regenerated aromatic polyester.

[0179] The IV and melting point of the regenerated aromatic polyester are higher than those of the raw material aromatic polyester despite the depolymerization and polycondensation. The regenerated aromatic polyester is white and high quality. Table 5 shows its quality.

[0180] [Example 22]

[0181] A depolymerization reaction was carried out in the same manner as in Example 21, except that the copolyaromatic polyester of Reference Example 1 used in Example 21 was changed to the copolyaromatic polyester of Reference Example 2, thereby obtaining a depolymerized sample 2.

[0182] In a reaction container under a nitrogen atmosphere and at normal pressure, 254 parts by mass of the depolymerized sample 2, 0.07 parts by mass of antimony trioxide, 0.005 parts by mass of orthophosphoric acid, and 0.22 parts by mass of sodium acetate were placed.

[0183] Next, the temperature in the reaction vessel was set to 285° C., and the pressure was reduced stepwise under conditions of normal pressure for 10 minutes, 4 kPa for 10 minutes, and 0.4 kPa for 40 minutes, respectively, while ethylene glycol and the like produced by the reaction were distilled out of the reaction vessel, a polycondensation reaction was carried out to obtain a regenerated aromatic polyester.

[0184] The obtained regenerated aromatic polyester has higher IV and melting point than the raw material aromatic polyester despite being depolymerized and polycondensed, and is white, high-quality regenerated aromatic polyester. Table 5 shows its quality.

[0185] [Reference Example 21]

[0186] 300 parts by mass of the copolyaromatic polyester obtained in Reference Example 1, 1500 parts by mass of ethylene glycol (EG) and 0.38 parts by mass of manganese acetate were placed in a 2 L separable flask, and a depolymerization reaction was carried out at 202° C. for 4 hours while stirring under nitrogen blanketing to obtain a depolymerized sample.

[0187] In a reaction container under nitrogen atmosphere and normal pressure, 508 parts by mass of the depolymerized sample obtained above, 0.07 parts by mass of antimony trioxide, 0.005 parts by mass of orthophosphoric acid and 0.22 parts by mass of sodium acetate were added.

[0188] Next, the temperature in the reaction vessel was set to 285° C., and the pressure was reduced stepwise under conditions of normal pressure for 10 minutes, 4 kPa for 10 minutes, and 0.4 kPa for 40 minutes, respectively, while ethylene glycol and the like produced by the reaction were distilled out of the reaction vessel, a polycondensation reaction was carried out to obtain a regenerated aromatic polyester.

[0189] The obtained regenerated aromatic polyester had a large residual content of sodium sulfoisophthalate, and its IV value and melting point were inferior to those of Examples 21 and 22. Table 5 shows the quality.

[0190] [Comparative Example 21]

[0191] In a reaction container under a nitrogen atmosphere and at normal pressure, 254 parts by mass of the depolymerized sample 2 obtained in Example 22, 0.07 parts by mass of antimony trioxide, and 0.005 parts by mass of orthophosphoric acid were placed.

[0192] Next, the temperature in the reaction vessel was set to 285° C., and the pressure was reduced stepwise under conditions of normal pressure for 10 minutes, 4 kPa for 10 minutes, and 0.4 kPa for 40 minutes, respectively, while ethylene glycol and the like produced by the reaction were distilled out of the reaction vessel, a polycondensation reaction was carried out to obtain a regenerated aromatic polyester.

[0193] The obtained regenerated aromatic polyester had a low melting point although the content of 5-sodium sulfoisophthalate was small. Table 5 shows the quality.

[0194] [Table 4]

[0195]

[0196] [Table 5]

[0197]

[0198] Possibility of Industrial Application

[0199] The regenerated aromatic polyester obtained by depolymerizing and repolymerizing the aromatic polyester component contained in the aromatic dicarboxylic acid bis(hydroxyalkyl) ester obtained by the production method of the present invention, the aromatic polyester obtained by using the aromatic dicarboxylic acid bis(hydroxyalkyl) ester as at least one raw material, and the aromatic polyester component contained in polyester scraps, product recycling products, etc. has less yellow tint and excellent hue, and the deterioration of physical properties due to the presence of copolymer components before depolymerization can be suppressed. Therefore, it can be preferably used as a material for fibers, films, and resins, for example.

Claims

1. A method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester, characterized in that: The invention relates to a method for producing a bis(hydroxyalkyl) aromatic dicarboxylate, wherein polyester is depolymerized in the presence of a catalyst. The catalyst is a manganese catalyst and the amount of the catalyst used is 20 to 500 mmol% based on the polyester.

2. The method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester according to claim 1, wherein Polyester is composed mainly of polyalkylene terephthalate.

3. The method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester according to claim 2, wherein: The polyalkylene terephthalate is any one of polyethylene terephthalate, polypropylene terephthalate, and polybutylene terephthalate.

4. The method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester according to claim 1, wherein The aromatic dicarboxylic acid bis(hydroxyalkyl) ester is bis(hydroxyalkyl) benzene dicarboxylic acid ester.

5. The method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester according to claim 1, wherein The manganese-based catalyst is manganese acetate.

6. The method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester according to claim 1, wherein The catalyst is used in the form of a solution predissolved in an alkylene glycol.

7. The method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester according to claim 1, wherein After depolymerization, the temperature is lowered in alkylene glycol to perform crystallization.

8. The method for producing an aromatic dicarboxylic acid bis(hydroxyalkyl) ester according to claim 7, wherein: After crystallization, the product is washed with water.

9. A method for producing a polyester resin, characterized in that: The aromatic dicarboxylic acid bis(hydroxyalkyl) ester obtained by the production method according to any one of claims 1 to 8 is repolymerized.

10. A polyester resin obtained by the method for producing a polyester resin according to claim 9.

11. A method for producing a regenerated aromatic polyester, characterized in that: A method for producing a regenerated aromatic polyester, comprising depolymerizing a polyester containing an aromatic polyester and then polycondensing the depolymerized components to obtain a regenerated aromatic polyester. The depolymerization is carried out by depolymerizing the polyester to form an aromatic dicarboxylic acid bis(hydroxyalkyl) ester in the presence of a catalyst. The catalyst used for the depolymerization is a manganese-based catalyst. The amount of the catalyst used is 20 to 500 mmol% relative to the polyester.

12. The method for producing a regenerated aromatic polyester according to claim 11, wherein: The aromatic dicarboxylic acid bis(hydroxyalkyl) ester is purified after depolymerization and before polycondensation.

13. The method for producing a regenerated aromatic polyester according to claim 12, wherein: The polycondensation is carried out by polycondensing the purified aromatic dicarboxylic acid bis(hydroxyalkyl) ester in the presence of an alkali metal and / or an alkaline earth metal.

14. A method for producing a regenerated aromatic polyester, characterized in that: The invention relates to a method for producing a regenerated aromatic polyester, wherein a polyester containing an aromatic polyester is depolymerized and then a component obtained by depolymerization is polycondensed to obtain a regenerated aromatic polyester, wherein the polyester containing an aromatic polyester is depolymerized in an alkylene glycol to obtain an aromatic dicarboxylic acid bis(hydroxyalkyl) ester, the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is purified, and the purified aromatic dicarboxylic acid bis(hydroxyalkyl) ester is polycondensed in the presence of an alkali metal and / or an alkaline earth metal to obtain the regenerated aromatic polyester.

15. The manufacturing method according to claim 14, wherein: The polyester is recycled polyester.

16. The manufacturing method according to claim 14, wherein: The purification of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester is carried out by crystallization from an alkylene glycol solution of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester.

17. The manufacturing method according to claim 16, wherein: After the crystallization of the aromatic dicarboxylic acid bis(hydroxyalkyl) ester, washing is performed.

18. The manufacturing method according to claim 17, wherein: Washing is carried out using water or alkylene glycol.

19. The manufacturing method according to claim 16, wherein: The crystallization is performed by cooling the solution obtained by depolymerization reaction of the aromatic polyester from a temperature of 60° C. or higher to a temperature of 25° C. or lower.

20. The manufacturing method according to claim 17, wherein: After washing the aromatic dicarboxylic acid bis(hydroxyalkyl) ester, the mixture is dried and then subjected to polycondensation reaction.

21. A regenerated aromatic polyester obtained by the production method according to claim 14.

22. The manufacturing method according to claim 14, wherein: The purified aromatic dicarboxylic acid bis(hydroxyalkyl) ester has an alkylene glycol content of 100% by mass or less and is subjected to polycondensation in this state.