Fast curing aqueous coating composition and method for coating substrates using the same
By using a waterborne coating composition of three polyurethane resins and a crosslinking agent, the problem of long curing time of waterborne coatings at room temperature is solved, achieving rapid curing and high adhesion coatings suitable for safe and efficient coating of plastic substrates.
Patent Information
- Application Number
- CN202380032383.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-06
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-15
AI Technical Summary
Existing water-based coating compositions have excessively long curing times at room temperature, resulting in uneven coatings that are easily peeled off, making it difficult to meet the requirements for rapid processing and safety of plastic substrates such as toys.
The waterborne coating composition, containing three different polyurethane resins and crosslinking agents, ensures extremely fast curing at room temperature while providing excellent adhesion and optical properties, suitable for a variety of manual and automatic application methods.
It achieves rapid curing in less than 1 minute at room temperature, forming a highly adhesive coating on plastic substrates that resists mechanical stress and environmental influences, avoids peeling and splitting, and is suitable for a variety of application methods.
Smart Images

Figure BDA0005069815810000101 
Figure BDA0005069815810000111 
Figure BDA0005069815810000321
Abstract
Description
[0001] The present invention relates to an aqueous coating composition comprising three different aqueous dispersions, each aqueous dispersion comprising a different polyurethane resin, and a crosslinking agent. Despite the presence of a large amount of water in the aqueous coating compositions of the present invention, they produce a fast curing time at room temperature, thereby allowing the coating of substrates that require the use of fast curing aqueous coating compositions to comply with safety and environmental standards and requirements in production processes. In addition, the present invention relates to a method for coating a substrate using the coating composition of the present invention and a coating produced by the method of the present invention. Finally, the present invention relates to a substrate with a coating produced by the method of the present invention. Background Art
[0002] Children's toys have a history dating back to ancient times. Plastic toys are usually produced by injecting molten polymer or plastic pellets into a mold cavity with the desired shape. In order to obtain a colored toy, a pigment can be incorporated into the polymer melt before introduction into the mold cavity. After cooling, the solid toy or parts of the toy are removed and optionally further hardened. In the case of toys made of different parts, the parts are assembled to obtain the toy.
[0003] Although the use of pigments in the polymer melt or the use of colored pellets allows colored toys or toy parts to be obtained, the injection molding process results in toys and toy parts having a single uniform color and does not allow the production of toys and toy parts with specific areas dyed with at least one different color, such as plastic animal toys that resemble real animals.
[0004] In order to achieve flexible coloring of toys and toy parts, coating compositions are used to coat toys and toy parts after their production to provide the desired appearance. These coating compositions are applied to the toys and toy parts obtained after injection molding to obtain the desired appearance.
[0005] Regardless of the type of coating used on a toy article, it remains extremely important that such coatings are safe for children. Safety requirements have been evolving over the years as safety concerns have grown. Generally speaking, safety requirements dictate that any material composition used in a toy be odorless, non-irritating to the skin or eyes, etc., and non-toxic if ingested. Additional requirements are expected for compositions used to coat or paint toy articles, as they must be non-stripping, requiring the coating or painting to adhere firmly to the toy article to avoid flaking or peeling and possible consumption by child users. And in addition, the coating should be able to withstand the physical impacts that occur during toy use, so as to maintain the appearance of the coated surface. And most importantly, the coating or coating composition must avoid the use of undesirable volatile organic solvents, as the residual presence of the solvent in the coating may be dangerous due to the toxic effects of certain aromatic and chlorinated hydrocarbon solvents.
[0006] Especially in the manufacture of toys, when it comes to applying coating compositions to injection-molded parts, the degree of automation is very low and many manual processes, such as the application of coatings, are still used. For this reason, it is crucial to use coating compositions that allow short curing times at room temperature in order to ensure fast processing of (partially) painted toys and toy parts without damaging or soiling the formed coating. Due to the fast evaporation of organic solvents at room temperature, such fast curing times are currently mostly ensured by using solvent-based coating compositions.
[0007] In view of the environmental, health and safety issues in the use of organic solvents, toy paint or toy coating compositions containing less controversial solvents such as water are desirable. However, water evaporates relatively slowly over long periods of time at room temperature, resulting in uneven and unstable coatings, making these coatings susceptible to usage factors that produce peeling and splitting along with other negative consequences. In addition, the use of elevated temperatures to accelerate the curing of waterborne coating compositions is not feasible because the plastics of the toys or toy parts tend to deform and melt at these elevated temperatures, resulting in damage or at least a negative impact on the appearance of the coated toys or toy parts.
[0008] Therefore, there is a need for aqueous coating compositions with short curing times, especially at room temperature, to allow rapid processing of coated plastic parts. The coating composition should have good application characteristics despite large amounts of water and should not flow even after application at high film thicknesses to avoid negative effects on the appearance of the coated substrate. The resulting coating should have excellent adhesion to various substrates, particularly plastic substrates, to avoid peeling or splitting during use of the coated substrate, and have sufficient hiding power to avoid re-coating of the substrate.
[0009] Purpose
[0010] Therefore, the object of the present invention is to provide a kind of water-based coating composition, it has excellent curing time at room temperature, and produces the coating that shows excellent adhesion to various substrates, particularly plastic substrates and good optical properties.Although the curing time is short, the coating formed should not be peeled off or split during mechanical stress, and environmental influences such as solvents and UV irradiation have high resistance.In addition, the water-based coating composition should be suitable for various manual and automatic application methods, and even if applied with high wet film thickness, it should not cause the formation of sagging.
[0011] Technical Solutions
[0012] The above objects are achieved by the subject matter claimed in the claims and also by preferred embodiments of the subject matter described in the following description.
[0013] Therefore, a first subject of the present invention is an aqueous coating composition comprising:
[0014] (a) at least one aqueous dispersion D1 comprising a first polyurethane resin P1 having a glass transition temperature (Tg) of less than or equal to -30°C as determined in accordance with DIN EN ISO 11357-2-2020-08,
[0015] (b) at least one aqueous dispersion D2 comprising a second polyurethane resin P2 different from the first polyurethane resin P1, said second polyurethane resin P2 having a 100% modulus of at least 1 MPa as determined according to DIN 53504:2017-03,
[0016] (c) at least one aqueous dispersion D3 comprising a third polyurethane resin P3 different from the first polyurethane resin P1 and the second polyurethane resin P2, said third polyurethane resin P3 having a glass transition temperature (Tg) less than or equal to -40°C as determined according to DIN EN ISO 11357-2-2020-08, and
[0017] (d) at least one cross-linking agent.
[0018] The aqueous coating composition specified above is also referred to hereinafter as the aqueous coating composition of the invention and is accordingly a subject of the present invention.Preferred embodiments of the aqueous coating composition of the invention are evident from the following description and also from the dependent claims.
[0019] According to the prior art, it is unexpected and unforeseeable for a skilled worker that the purpose on which the present invention is based can be achieved by an aqueous coating composition comprising three different polyurethane resins P1 to P3 and at least one crosslinking agent. When applied with a wet film thickness of up to 60 μm, the aqueous coating composition produces an extremely fast curing time of less than 1 minute at room temperature. The resulting coating shows excellent adhesion to various plastic substrates such as PVC (polyvinyl chloride), TPE (thermoplastic elastomer), TPU (thermoplastic polyurethane), eTPU (expanded and expandable thermoplastic polyurethane), PA (polyamide) and PU (polyurethane) and natural substrates such as wood. Although the curing time is short, the formed coating does not peel off, split or change its color during mechanical stress or when exposed to other environmental influences (such as solvents and UV irradiation). In addition, the aqueous coating composition is suitable for various manual application methods such as dipping and brushing and automatic application methods such as spraying, and does not cause the formation of sagging even if applied with high wet film thickness. Furthermore, the aqueous coating compositions produce coatings having good optical properties, such as good hiding power, thereby avoiding the need to re-coat the substrate in order to achieve the desired optical appearance.
[0020] Another subject of the present invention is a process for producing a coating (C) on a substrate (S), said process comprising the step of applying the aqueous coating composition of the invention to the substrate (S) and the step of curing the applied coating composition.
[0021] A further subject of the present invention is a coating produced by the process according to the invention.
[0022] A final subject of the present invention is a substrate (S) provided with a coating (C) according to the invention. DETAILED DESCRIPTION
[0023] definition:
[0024] First, some terms used in the context of the present invention will be explained.
[0025] As used herein, unless otherwise indicated, the grammatical articles "a", "an", and "the" are intended to include "at least one" or "one or more", even though "at least one" or "one or more" are explicitly used in certain instances. Thus, these articles are used in this specification to refer to one or more than one (i.e., "at least one") of the grammatical objects of the article. By way of example and not limitation, "a component" means one or more components, and thus, potentially, more than one component is contemplated and may be employed or used in the implementation of the described embodiments. Further, use of a singular noun includes the plural, and use of a plural noun includes the singular, unless the context of the usage requires otherwise.
[0026] In this description of the invention, for convenience, "polymer" and "resin" are used interchangeably to encompass resins, oligomers and polymers.
[0027] In the context of the present invention and according to DIN EN ISO 4618:2007-03, "binders" are non-volatile components of coating compositions that are free of pigments and fillers. However, in the following, this expression is mainly used with respect to specific physically and / or chemically curable polymers, examples being polyurethanes, polyesters, polyethers, polyureas, polyacrylates, polysiloxanes and / or copolymers of said polymers. The non-volatile fraction can be determined according to DIN EN ISO 3251:2018-07 using a starting weight of 1.0 g at 130° C. for 60 min.
[0028] As used herein, the term "aqueous coating composition" refers to a coating composition comprising a water fraction of at least 20 wt.%, preferably at least 25 wt.%, very preferably at least 30 wt.%, in each case based on the total weight of the coating composition. The water fraction is preferably 25 to 60 wt.%, more particularly 30 to 70 wt.%, very preferably 30 to 60 wt.%, in each case based on the total weight of the coating composition. In contrast, the term "solvent-based coating composition" refers to a coating composition comprising an organic solvent fraction of at least 20 wt.%, preferably at least 25 wt.%, very preferably at least 45 wt.%, in each case based on the total weight of the coating composition. The organic solvent fraction is preferably 40 to 70 wt.%, more particularly 45 to 65 wt.%, very preferably 50 to 60 wt.%, in each case based on the total weight of the coating composition.
[0029] "Room temperature" refers to a temperature of 15°C to 25°C.
[0030] As used herein, the term "drying" an applied coating composition refers to evaporating the solvent from the applied coating composition. Drying can be performed at ambient temperature or by using elevated temperatures. However, drying does not produce a ready-to-use coating film, i.e., a cured coating film as described below, because the coating film remains soft or tacky after drying.
[0031] Accordingly, "curing" an applied coating composition or a coating film resulting from drying an applied coating composition refers to converting such a composition or film into a ready-to-use state, i.e., into a state in which the substrate provided with the corresponding coating can be transported, stored and used as intended. More particularly, a cured coating is no longer soft or tacky, but has been adjusted to a solid coating which does not undergo any further significant changes in its properties, such as hardness or adhesion to the substrate, even when further exposed to curing conditions. Curing can be carried out at higher temperatures and / or for longer periods of time than used for drying the applied coating composition.
[0032] The measurement methods to be used in the context of the present invention for determining certain characteristic variables can be found in the Examples section. Unless otherwise explicitly indicated, these measurement methods are to be used to determine the corresponding characteristic variables. In the context of the present invention, when an official standard is cited without any indication of the official effective date, it is implied that the standard version in force on the date of submission is cited, or the latest effective version is cited at that point in time when no effective version exists.
[0033] Unless expressly stated otherwise, all film thicknesses reported in the context of the present invention are to be understood as dry film thicknesses. It is therefore in each case the cured film thickness. Thus, where it is reported that a coating material is applied at a certain film thickness, this means that the coating material is applied in such a way that after curing the stated film thickness results.
[0034] All temperatures stated in the context of the present invention are to be understood as the temperature of the chamber in which the substrate or coated substrate is located. Therefore, this does not mean that it is required that the substrate itself has the temperature in question.
[0035] Aqueous coating composition of the present invention
[0036] Aqueous dispersion D1 comprising a first polyurethane resin P1:
[0037] As a first mandatory component, the aqueous coating composition of the present invention comprises at least one aqueous dispersion D1, which comprises a first polyurethane resin P1. The first polyurethane resin P1 has a glass transition temperature (hereinafter also indicated as Tg) of less than or equal to -30°C. The glass transition temperature can be determined by DSC according to DIN EN ISO 11357-2-2020-08. The aqueous dispersion D1, especially the preferred embodiment of the aqueous dispersion D1 as outlined below, is used in combination with aqueous dispersions D2 and D3 to ensure extremely fast curing times of the aqueous coating composition of the present invention at room temperature, while producing excellent adhesion to various plastic substrates as well as excellent optical properties and resistance to environmental influences.
[0038] In a preferred embodiment, the first polyurethane resin P1 has a glass transition temperature (Tg) of -30°C to -50°C, preferably -35°C to -45°C, very preferably -38°C to -42°C.
[0039] The first polyurethane resin P1 is preferably an anionic polyurethane resin. The term "anionic polyurethane resin" refers to a polyurethane resin containing anionic groups and / or groups (potential anionic groups) that can be converted into anionic groups, for example, by neutralization with a suitable base. The anionic group can provide hydrophilic stability or increased dispersibility in an aqueous medium. Suitable anionic groups or potential anionic groups include, for example, carboxylic acid, sulfonic acid and / or phosphonic acid groups or carboxylate, sulfonate and / or phosphonate groups. Preferably, the anionic polyurethane resin contains carboxylic acid or carboxylate groups. Anionic modification can be introduced into the polyurethane resin by a monomer containing anionic groups or potential anionic groups and at least one group reactive to isocyanate groups (preferably at least one hydroxyl group). The anionic polyurethane resin P1 can be neutralized with a suitable neutralizing agent such as inorganic and organic bases (including amino alcohols).
[0040] Particularly preferably, the first polyurethane resin P1 is an aliphatic polyester-based polyurethane resin. The term "polyester-based polyurethane resin" refers to a polyurethane resin comprising polyester units (i.e., units comprising at least two ester groups). Preferably, the polyester-based polyurethane resin comprises polyester units as a main component, i.e., the polyester-based polyurethane resin is obtained by reacting at least one polyester polyol with a polyisocyanate compound. The polyester polyol can be obtained, for example, by reacting at least one polyol (such as a diol) with at least one acid (such as a polycarboxylic acid), as described below.
[0041] The first polyurethane resin P1 preferably has an acid number of 5 to 100 mg KOH / g solid, preferably 10 to 50 mg KOH / g solid, very preferably 15 to 30 mg KOH / g solid. The acid number can be determined by titration as described in DIN EN ISO 2114:2002-06 (procedure A). The introduction of acid functionality allows the water dispersibility of the first polyurethane resin P1 to be improved, so that the resin can be stably introduced into aqueous coating compositions without the use of organic solvents.
[0042] In an embodiment, the first polyurethane resin P1 has a hydroxyl number of 1 to 150 mg KOH / g solid, preferably 2 to 100 mg KOH / solid, more preferably 5 to 70 mg KOH / g solid, very preferably 10 to 25 mg KOH / g solid. The hydroxyl number can be determined by titration as described in DIN EN ISO 2114:2002-06 (procedure A). Therefore, the first polyurethane resin P1 is preferably hydroxy-functional and can be cured using commonly known polyisocyanate crosslinkers.
[0043] The first polyurethane resin P1 has a number average molecular weight M n The number average molecular weight M is preferably 750 to 2,000,000 g / mol, preferably 1,000 to 1,000,000, more preferably 2,000 to 500,000, very preferably 5,000 to 10,000 g / mol. n It can be determined, for example, using GPC with polystyrene as an internal standard.
[0044] The first polyurethane resin P1 is preferably obtained by reacting an NCO-functional prepolymer with at least one polyol, as described, for example, in publication DE 199 21 457 A1. The term "NCO-functional" refers to compounds containing free NCO groups or compounds containing at least one blocked NCO group which is blocked by a blocking agent known in the art and can be deblocked, for example using heat, to produce free NCO groups. The term "polyol" refers to compounds containing at least two hydroxyl groups.
[0045] The reaction of the NCO functional prepolymer with at least one polyol can be carried out in the presence of conventional and known organic solvents. In this case, the amount of the organic solvent can vary within a wide range and should be sufficient to form a prepolymer solution with a suitable viscosity. In general, based on the solid content, up to 70 wt.%, preferably 5 to 50 wt.%, and more preferably less than 20 wt.% of solvent is used. Thus, for example, based on the solid content, the reaction can be very particularly preferably carried out at a solvent content of 10-15 wt.%. The reaction of the components can optionally be carried out in the presence of a catalyst such as an organotin compound and / or a tertiary amine. The organic solvent is removed after the formation of the first polyurethane resin P1 as described later to obtain an aqueous dispersion D1.
[0046] Suitable weight ratios between the active hydrogens of the polyol and the NCO groups of the NCO-functional prepolymer include 2:1 to 1:2, preferably 1.1:1 to 1:1.1.
[0047] At least one polyol is used as a modifier or chain extender. In this case, the modifier is preferably added in an amount such that there is chain extension and thus increases the molecular weight. Examples of polyols that can be used are trimethylolpropane, 1,3,4-butanetriol, glycerol, erythritol, meso-erythritol, arabitol, adonitol, etc. It is preferred to use aliphatic monomer polyols, and more preferably aliphatic monomer polyols containing at least three hydroxyls. "Aliphatic polyol" refers to a polyol that is not aromatic. Aliphatic polyols can be saturated or unsaturated and can contain heteroatoms (e.g., oxygen, nitrogen, sulfur). Heteroatoms can be present in bridging groups (such as ether linkages, ester linkages, urea linkages) and / or can be present in functional groups containing heteroatoms (e.g., hydroxyl, amine groups, etc.). "Monomeric" refers to a compound that is not formed by reacting at least two monomer compounds with each other, i.e., a compound that is not a polymer. Particularly preferably, the polyol is trimethylolpropane.
[0048] The NCO-functional prepolymer is preferably obtained by reacting:
[0049] at least one aliphatic polyester polyol having an OH number of 40 to 100 mg KOH / g solid and a number average molecular weight Mn of 1,000 to 3,000 g / mol,
[0050] at least one compound comprising at least one acid group and at least one group capable of reacting with an NCO group,
[0051] at least one polyol having an average molecular weight Mw of 60 to 400 g / mol, and
[0052] • At least one polyisocyanate.
[0053] The reaction can be carried out in an organic solvent that is unreactive toward isocyanates at temperatures up to 150° C., preferably 50 to 130° C. A suitable weight ratio of NCO groups to OH groups is between 2.0:1.0 and >1.0:1.0, preferably between 1.4:1 and 1.1:1.
[0054] In order to obtain highly flexible NCO prepolymers, preference is given to using a high fraction of predominantly linear polyester polyols having preferably an OH value of 30 to 150 mg KOH / g. Up to 97 wt.% of the total polyester polyols can be composed of a number-average molecular weight M n The present invention relates to a saturated polyester diol having a content of 400 to 5,000 g / mol and a saturated and unsaturated polyester composition. Suitable polyester diols can be prepared by esterification of organic dicarboxylic acids or their anhydrides with organic diols, or can be derived from hydroxycarboxylic acids or lactones. Particularly preferably, aliphatic polyester polyols, in particular aliphatic linear polyester polyols, are obtained by reacting dimerized fatty acids with aromatic dicarboxylic acids and diols. Dimerized fatty acids (also called dimerized fatty acids or dimer acids for a long time) are usually and especially in the context of the present invention a mixture prepared by oligomerization of unsaturated fatty acids. For example, dimerized fatty acids can be prepared by catalytic dimerization of unsaturated vegetable fatty acids, wherein the starting materials used are more particularly unsaturated C 12 To C 22 Fatty acids. The linkage is mainly according to the Diels-Alder type, and depending on the number and position of double bonds in the fatty acids used to prepare the dimerized fatty acids, the product is a mixture of mainly dimerized products, which have cycloaliphatic, linear aliphatic, branched aliphatic and C6 aromatic hydrocarbon groups between the carboxyl groups. Depending on the mechanism and / or the optional subsequent hydrogenation, the aliphatic groups can be saturated or unsaturated, and the fraction of aromatic groups can also vary. The group between the carboxylic acid groups then contains, for example, 24 to 44 carbon atoms. For the preparation, preferably fatty acids with 18 carbon atoms are used, and the dimerized product thus has 36 carbon atoms. The groups connecting the carboxyl groups of the dimerized fatty acids preferably do not have unsaturated bonds and aromatic hydrocarbon groups. The preferred dimerized fatty acids are those obtained by using C 18 Fatty acids such as linolenic acid, linoleic acid and / or oleic acid are obtained as dimerized fatty acids as starting materials.
[0055] In addition to polyester polyols, at least one compound comprising at least one acid group and at least one group capable of reacting with the NCO groups of the NCO functional prepolymer is used. Such compounds include alkanoic acids having 3 to 8 carbon atoms and 2 hydroxyl groups. These compounds preferably account for 3 to 100 wt.%, preferably 5 to 50 wt.%, of the entire polyol component in the NCO functional prepolymer. A particularly preferred compound is dimethylol propionic acid. Based on the solid of the NCO functional prepolymer, the amount of ionizable carboxyl groups that can be obtained in the form of salts by carboxyl neutralization is at least 0.4 wt.%, preferably at least 0.7 wt.%. The dihydroxyalkanoic acid in the unneutralized prepolymer is preferably used in an amount that produces the above-mentioned acid value.
[0056] Average molecular weight M w The polyol having a molecular weight of 60 to 400 g / mol is preferably selected from aliphatic polyols having 3 to 10 carbon atoms and 2 hydroxyl groups. The polyol preferably does not contain carboxyl, sulfonic acid and / or phosphonic acid groups and is preferably selected from diols of formula (1):
[0057]
[0058] wherein R1 and R2 each represent the same or different radicals and are alkyl, aryl or cycloaliphatic radicals having 1 to 18 carbon atoms. Particularly preferred diols of formula (1) are diols in which R1 and R2 are each methyl (i.e. neopentyl glycol). The diols of formula (1) are conventionally used in amounts of 0.1 to 15 wt. %, preferably 0.5 to 5 wt. %, in each case based on the total weight of the components used to prepare the NCO-functional prepolymer.
[0059] Typical polyfunctional isocyanates for preparing NCO functional prepolymers are aliphatic, cycloaliphatic and / or aromatic polyisocyanates, particularly cycloaliphatic polyisocyanates, having at least two isocyanate groups per molecule. Isomers or isomer mixtures of preferred organic diisocyanates. Due to the high stability of (cyclo)aliphatic diisocyanates to ultraviolet rays, (cyclo)aliphatic diisocyanates produce products with almost no yellowing tendency. The polyisocyanate component for forming NCO functional prepolymers can also contain a certain fraction of polyisocyanates with higher functionality, provided that this does not cause any gelling. Established triisocyanates are products formed by trimerization or oligomerization of diisocyanates or by reacting diisocyanates with polyfunctional compounds containing OH or NH groups. The average functionality 10 can be optionally reduced by adding monoisocyanates.
[0060] Examples of polyisocyanates that can be used are phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, bisphenylene diisocyanate, naphthylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, cyclobutane diisocyanate, cyclopentylene diisocyanate, cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, dicyclohexylmethane diisocyanate, ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, propylene diisocyanate, ethylethylene diisocyanate and trimethylhexane diisocyanate.
[0061] In order to produce high-solids, anionically stable aqueous dispersions D1, diisocyanates of the general formula (2) are used in particular
[0062]
[0063] wherein X is a divalent cyclic and optionally aromatic hydrocarbon radical, preferably optionally halogen-, methyl- or methoxy-substituted dicyclohexylmethyl, naphthylene, diphenylene or 1,2-, 1,3- or 1,4-phenylene, more preferably dicyclohexylmethyl. A diisocyanate of formula (2) which is particularly preferably used in the context of the present invention is 4,4′-methylenedicyclohexyl diisocyanate (also known as H 12 MDI).
[0064] The NCO functional prepolymer contains at least 0.5 wt. % isocyanate groups, preferably at least 1 wt. % isocyanate groups, based on solids. The upper limit is 15 wt. %, preferably 10 wt. %, more preferably 5 wt. % isocyanate groups.
[0065] Particularly preferably, the NCO prepolymer is obtainable by the reaction of:
[0066] I. 55 to 70 wt.% based on the total weight of compounds (I) to (IV) of at least one compound having an OH value of 40 to 100 mg KOH / g solid and a number average molecular weight M of 1,000 to 3,000 g / mol n Polyester polyols, in particular polyester polyols prepared by reacting dimer fatty acids with aromatic dicarboxylic acids and diols,
[0067] II. 3 to 7 wt. %, based on the total weight of compounds (I) to (IV), of at least one alkanoic acid having 3 to 8 carbon atoms and also two hydroxyl groups on the alpha carbon atom, in particular dimethylolpropionic acid,
[0068] III. 0.5 to 3 wt.% of at least one polyol of formula (1) based on the total weight of compounds (I) to (IV), wherein R1 = R2 = methyl, and
[0069] IV. 25 to 30 wt. %, based on the total weight of compounds (I) to (IV), of at least one diisocyanate of the formula (2) in which X=dicyclohexylmethyl.
[0070] The organic solvent used to synthesize the polyurethane resin P1 is preferably removed under reduced pressure after the addition of water to obtain an aqueous dispersion D1. The anionically stabilized polyurethane resin P1 is preferably neutralized with a base, preferably an organic base, more particularly N,N'-dimethylethanolamine, the base being added in an amount such that a degree of neutralization of 50% to 100%, preferably 60% to 80%, is achieved. As a result of the addition of the base, the dispersion has a pH of 7 to 8.
[0071] In order to promote the dispersion of the partially neutralized anionically stabilized polyurethane resin P1 in water, an alkylene glycol, preferably with an average molar mass M n In addition to the alkylene glycol, the aqueous dispersion D1 preferably contains only water and the first polyurethane resin P1, that is, the first aqueous dispersion D1 preferably does not contain organic solvents (that is, the total amount of organic solvents in the dispersion D1 is less than 1% by weight based on the total weight of the dispersion D1).
[0072] The aqueous dispersion D1 preferably has an average particle size (z-average), determined by photon correlation spectroscopy, of 30 to 200 nm, preferably of 40 to 100 nm, very preferably of 45 to 60 nm.
[0073] The aqueous dispersion D1 preferably comprises the first polyurethane resin P1 in a total amount of 10 to 60% by weight, preferably 15 to 50% by weight, more preferably 20 to 40% by weight, very preferably 25 to 35% by weight, in each case based on the total weight of the aqueous dispersion D1. The use of high-solids aqueous dispersions which have a low viscosity despite their high solids content is preferred with regard to achieving extremely fast curing times of the aqueous coating composition at room temperature.
[0074] In an embodiment, the aqueous coating composition comprises aqueous dispersion D1 in a total amount of 5 to 60% by weight, preferably 10 to 50% by weight, very preferably 15 to 25% by weight, in each case based on the total weight of the aqueous coating composition. The above amounts of aqueous dispersion D1 in combination with aqueous dispersions D2 and D3 ensure extremely fast curing times of the aqueous coating composition of the invention at room temperature, while producing excellent adhesion to various plastic substrates as well as excellent optical properties and high resistance to environmental influences such as solvents, abrasion and UV radiation.
[0075] Aqueous dispersion D2 comprising a second polyurethane resin P2:
[0076] As a second mandatory ingredient, the aqueous coating composition comprises an aqueous dispersion D2 containing a second polyurethane resin P2. The second polyurethane resin P2 is different from the first polyurethane resin P1 described in detail above and has a 100% modulus of at least 1 MPa as determined according to DIN53504:2017-03. The term "modulus" refers to the force at a specific elongation value and is usually expressed in pounds per square inch (psi) or megapascals (MPa). The term "100% modulus" refers to the modulus at 100% elongation. The use of aqueous dispersion D2 in combination with aqueous dispersions D1 and D3 ensures extremely fast curing times of the aqueous coating composition of the present invention at room temperature, while producing excellent adhesion to various plastic substrates as well as excellent optical properties and resistance to environmental influences.
[0077] According to a preferred embodiment, the second polyurethane resin P2 has a 100% modulus as determined according to DIN 53504:2017-03 of 1 to 6 MPa, preferably 1 to 4 MPa, very preferably 1.4 to 1.9 MPa.
[0078] The second polyurethane resin P2 preferably has a tensile strength, as determined in accordance with DIN 53504:2017-03, of 10 to 50 MPa, preferably of 15 to 40 MPa, very preferably of 22 to 28 MPa.
[0079] Suitable second polyurethane resins P2 include polyurethane resins having an elongation at break of 400% to 1,500%, preferably 600% to 900%, very preferably 720% to 780%, as determined in accordance with DIN 53504:2017-03.
[0080] In an embodiment, the second polyurethane resin P2 has a melting range of 150° C. to 300° C., preferably 190° C. to 230° C. “Melting range” refers to the temperature span from the point at which crystals first begin to liquefy to the point at which the entire sample is liquid. The melting range is preferably determined using a Kofler heating stage.
[0081] The 100% modulus, tensile strength, elongation at break and melting range of the polyurethane resin P2 can be measured by using the polymer (using 2% The results were determined by measuring approximately 0.1 mm transparent films of Gel ALA (thickened by OMG Borchers).
[0082] The second polyurethane resin P2 is preferably an anionic polyurethane resin. The anionic resin may be neutralized with an organic base such as those described above to facilitate dispersion in water.
[0083] The second polyurethane resin P2 is preferably an aliphatic polycarbonate-polyether-based polyurethane resin. The term "polycarbonate-polyether-based polyurethane resin" refers to a polyurethane resin comprising a polycarbonate unit and a polyether unit. A polycarbonate unit is a unit comprising at least two carbonate groups in its structure. Such groups can be formed, for example, by the polycondensation of a diol with a carbonate precursor such as phosgene. A polyether unit is a unit comprising at least two ether groups and can be formed, for example, by the catalytic polymerization of an epoxide. The use of anionic polycarbonate-polyether-based polyurethane resins produces higher water dispersibility, and therefore allows the polyurethane resin P2 to be incorporated into an aqueous dispersion without the need for the additional use of undesirable organic solvents. Suitable aqueous dispersions include commercial anionic aliphatic polycarbonate-polyester-based polyurethane dispersion Impranil DLV / 1 available from Covestro Deutschland AG, Germany.
[0084] The aqueous dispersion D2 preferably comprises the second polyurethane resin P2 in a total amount of 10 to 70% by weight, preferably 15 to 60% by weight, more preferably 25 to 50% by weight, very preferably 35 to 45% by weight, in each case based on the total weight of the aqueous dispersion D2. The use of high-solids aqueous dispersions which have a low viscosity despite their high solids content is preferred with regard to achieving extremely fast curing times of the aqueous coating composition at room temperature.
[0085] In an embodiment, the aqueous coating composition comprises aqueous dispersion D2 in a total amount of 5 to 60% by weight, preferably 10 to 50% by weight, very preferably 20 to 35% by weight, in each case based on the total weight of the aqueous coating composition. The use of the above amounts of dispersion D2 in combination with aqueous dispersions D1 and D3 ensures extremely fast curing times of the aqueous coating composition of the invention at room temperature, while producing excellent adhesion to various plastic substrates as well as excellent optical properties and high resistance to environmental influences such as solvents, abrasion and UV radiation.
[0086] Aqueous dispersion D3 comprising a third polyurethane resin P3:
[0087] As a third mandatory ingredient, the aqueous coating composition comprises an aqueous dispersion D3 containing a third polyurethane resin P3. The third polyurethane resin P3 is different from the first polyurethane resin P1 and the second polyurethane resin P2 described in detail above and has a glass transition temperature (Tg) of less than or equal to -40°C. The use of aqueous dispersion D3 in combination with aqueous dispersions D1 and D2 ensures extremely fast curing times of the aqueous coating composition of the invention at room temperature, while producing excellent adhesion to various plastic substrates as well as excellent optical properties and resistance to environmental influences.
[0088] Preferred third polyurethane resins P3 have a glass transition temperature (Tg) of -40°C to -80°C, preferably -40°C to -60°C, very preferably -42°C to -55°C.
[0089] The third polyurethane resin P3 is preferably an anionic polyurethane resin. The anionic resin can be neutralized with an organic base such as the organic base previously described above to promote the dispersion of the polyurethane resin in water. Particularly preferably, the third polyurethane resin P3 is an aliphatic polycarbonate-polyester-based polyurethane resin. The term "polycarbonate-polyester-based polyurethane resin" refers to a polyurethane resin comprising polycarbonate units as well as polyester units. The polycarbonate unit is a unit comprising at least two carbonate groups in its structure. Such groups can be formed, for example, by the condensation polymerization of a diol with a carbonate precursor such as phosgene. The polyester unit is a unit comprising at least two ester groups and can be formed, for example, by the reaction of a polyol such as a diol with a polycarboxylic acid such as a dicarboxylic acid. The use of an anionic polycarbonate-polyester-based polyurethane resin produces higher water dispersibility and therefore allows the polyurethane resin P3 to be incorporated into an aqueous dispersion without the need for the additional use of undesirable organic solvents.
[0090] In an embodiment, the aqueous dispersion D3 has an average particle size (z-average) determined according to photon correlation spectroscopy of 20 to 200 nm, preferably 30 to 100 nm, very preferably 40 to 80 nm. Suitable aqueous dispersions include the commercial anionic aliphatic polycarbonate-polyether-based polyurethane dispersion Bayhydrol UH 2648 / 1 available from Covestro, Germany.
[0091] The aqueous dispersion D3 comprises the third polyurethane resin P3 in a total amount of 10 to 60% by weight, preferably 20 to 50% by weight, very preferably 30 to 40% by weight, based in each case on the total weight of the aqueous dispersion D3. With regard to achieving extremely fast curing times of the aqueous coating composition at room temperature, the use of high-solids aqueous dispersions which have a low viscosity despite their high solids content is preferred.
[0092] In an embodiment, the aqueous coating composition comprises aqueous dispersion D3 in a total amount of 1 to 40% by weight, preferably 5 to 30% by weight, very preferably 8 to 20% by weight, in each case based on the total weight of the aqueous coating composition. The use of the above amounts of dispersion D3 in combination with aqueous dispersions D1 and D2 ensures extremely fast curing times of the aqueous coating composition of the invention at room temperature, while producing excellent adhesion to various plastic substrates as well as excellent optical properties and high resistance to environmental influences such as solvents, abrasion and UV radiation.
[0093] Cross-linking agent:
[0094] As a fourth mandatory ingredient, the aqueous coating composition comprises at least one crosslinking agent. "Crosslinking agent" refers to a compound, in particular an organic compound, containing reactive functional groups complementary to the reactive functional groups present in the first polyurethane resin P1 and / or the second polyurethane resin P2 and / or the third polyurethane resin P3. The crosslinking of the polyurethane resins P1 to P3 with at least one crosslinking agent produces a cured coating having high adhesion to various plastic substrates, thereby avoiding the peeling and splitting of the cured coating from the plastic substrate during use. In addition, crosslinking prevents the release of substances such as pigments from the formed coating, thereby avoiding negative health effects caused by the released substances.
[0095] The crosslinking agent is preferably selected from amino resins, unblocked polyisocyanates, at least partially blocked polyisocyanates, polycarbodiimides and mixtures thereof. Unblocked polyisocyanates refer to polyisocyanates containing free NCO groups, while the term "blocked polyisocyanates" refers to polyisocyanates containing at least one NCO group blocked by a blocking agent commonly used in the prior art. The unblocking of the NCO groups can be promoted, for example, by heating the coating composition, for example, during the curing process.
[0096] Particularly preferably, at least one crosslinking agent is selected from unblocked polyisocyanates. Unblocked polyisocyanates are preferably selected from hexamethylene diisocyanate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, tetramethylhexane diisocyanate, isophorone diisocyanate (IPDI), 2-isocyanatopropylcyclohexyl isocyanate, dicyclohexylmethane 2,4'-diisocyanate, dicyclohexyl-methane 4,4'-diisocyanate, 1,4- or 1,3-bis(isocyanato-methyl)cyclohexane, 1,4- or 1,3- or 1,2-diisocyanato-cyclohexane, and 2,4- or 2,6-diisocyanato-1-methyl-cyclohexane, dimers, trimers and tetramers thereof, and also mixtures of these polyisocyanates. Particularly preferably, the polyisocyanate comprises an aliphatic and / or cycloaliphatic, very preferably an aliphatic polyisocyanate. As diisocyanate main component used as the above oligomer, more particularly the above trimer or tetramer, very preferably hexamethylene diisocyanate and / or isophorone diisocyanate, and especially preferably only hexamethylene diisocyanate.
[0097] In this context, it is particularly preferred if the polyisocyanates have an NCO group functionality of more than 2.4 to 5, preferably 2.6 to 4, more preferably 2.8 to 3.6.
[0098] Particular preference is given in the context of the present invention to using polyisocyanates which comprise at least one isocyanurate ring or at least one iminooxadiazinedione ring.
[0099] It may be preferred if at least two polyisocyanates different from one another are used as crosslinkers, wherein the first polyisocyanate contains at least one isocyanurate ring and the second polyisocyanate contains at least one iminooxadiazinedione ring. The use of such a crosslinker mixture results in high adhesion of the cured coating on various plastic substrates, thereby avoiding peeling and splitting of the cured coating during use of the coated substrate.
[0100] In one embodiment, the aqueous coating composition comprises at least one crosslinking agent in a total amount of 1 wt.% to 40 wt.% solids, preferably 2 to 30 wt.% solids, more particularly 6 to 12 wt.% or 15 to 25 wt.% solids, in each case based on the total weight of the aqueous coating composition. The use of said amounts results in sufficient crosslinking of the coating during curing, thereby allowing excellent adhesion of the cured coating on various plastic substrates and good abrasion resistance to be obtained.
[0101] Depending on the specific crosslinker present in the composition of the invention, the composition of the invention is configured as a one-component system or can be obtained by mixing two (two-component system) or more (multi-component system) components. In thermochemically curable one-component systems, the components to be crosslinked, in other words the polyurethane resins P1 to P3 and optionally further binders and crosslinkers, are present together with one another, in other words as a single component. A condition for this is that the components to be crosslinked react effectively with one another only at relatively high temperatures of more than 100° C., for example in order to prevent premature, at least proportional, thermochemical curing. Such combinations can be exemplified by hydroxy-functional polyesters and / or polyurethanes with melamine resins and / or blocked polyisocyanates as crosslinkers.
[0102] In thermochemically curable two-component or multi-component systems, the components to be crosslinked, in other words, the polyurethane resins P1 to P3 and optionally further binders and crosslinkers, are present in at least two components independently of one another and are not combined until shortly before application. This form is selected when the components to be crosslinked react effectively with one another even at ambient temperature or at slightly elevated temperatures of, for example, 40° C. to 90° C. Such a combination can be exemplified by hydroxyl-functional polyesters and / or polyurethanes and / or poly(meth)acrylates and free polyisocyanates as crosslinkers. According to a preferred embodiment of the present invention, the aqueous coating composition is formulated as a two-component or multi-component aqueous coating composition and is prepared by mixing a base component comprising an aqueous dispersion D1 to D3 and optionally further ingredients mentioned below with a hardener component comprising a crosslinker dissolved in at least one solvent and optionally a base color component. In the context of the present invention, a "hardener component" is a material comprising at least one crosslinking component that is capable of reacting with chemical functional groups present in the polyurethane resins P1 to P3 of the base component and optionally further polymers. The components may be mixed prior to application using commonly known mixing methods.
[0103] In the case of compositions of the invention obtainable by mixing two components, the weight ratio of the base component comprising the aqueous dispersions D1 to D3 and optionally the further ingredients listed below to the hardener component comprising at least one crosslinking agent is preferably 100: 1 to 100: 50, more preferably 100: 2 to 100: 30, more particularly 100: 3 to 100: 7. The use of the above mixing ratios ensures sufficient crosslinking of the aqueous coating composition upon curing and provides high adhesion to the plastic substrate surface.
[0104] Additional Ingredients:
[0105] In addition to the mandatory ingredients mentioned above, the aqueous coating composition may further comprise additional ingredients. Suitable additional ingredients include at least polymers different from the polyurethane resins P1 to P3, colorants and / or effect pigments, matting agents, thickeners, dispersants, leveling agents, pH regulators, defoamers, biocides, UV absorbers, crosslinking catalysts and mixtures thereof.
[0106] Examples of the additional polymer include additional polyurethane resins other than the polyurethane resins P1 to P3.
[0107] Aqueous coating composition of the present invention can further comprise at least one coloring agent and / or effect pigment, to realize colored coating. Coloring agent and / or effect pigment can be introduced in the aqueous coating composition by mixing aqueous dispersion D1 to D3 and alternatively other composition with at least one color base component.Term " color base component " means the colorant composition with the color of precise measurement definition at this.Use at least one color base component to allow to realize colored coating with high color accuracy, i.e. the color of gained coating matches with the color expected by using corresponding color base component.In addition, high color diversity is possible, because color base component exists with multiple colors, and described color base component can be mixed with each other to obtain other tone.
[0108] The at least one color base component comprises at least one effect pigment and / or at least one coloring pigment.
[0109] Effect pigments are pigments which are able to produce decorative effects in the coating and additionally, but not exclusively, coloring effects. Effect pigments are particularly used in particular for flake-shaped structures. Preferred effect pigments are, for example, flake-shaped metal effect pigments, such as flake-shaped aluminum pigments, gold bronze, oxidized bronze and / or iron oxide-aluminum pigments, pearlescent pigments and / or metal oxide-mica pigments, and / or other effect pigments, such as flake-shaped graphite, flake-shaped iron oxide, multilayer effect pigments consisting of PVD films and / or liquid crystal polymer pigments. Particularly preferred are flake-shaped metal effect pigments, more particularly flake-shaped aluminum pigments and / or coated metal oxide-mica pigments and / or borosilicates coated with metal oxides.
[0110] Examples of inorganic coloring pigments are white pigments such as titanium dioxide, black pigments such as carbon black, iron manganese black or spinel black, colored pigments such as ultramarine green, ultramarine blue or manganese blue, ultramarine violet or manganese violet, iron oxide red, molybdenum chrome red or ultramarine red, iron oxide brown, mixed brown, spinel and corundum phases, or iron oxide yellow or bismuth vanadate yellow. Examples of suitable organic coloring pigments are monoazo pigments, disazo pigments, anthraquinone pigments, benzimidazole pigments, quinacridone pigments, quinoline yellow pigments, pyrrolopyrrole diketopyrrole pigments, dioxazine pigments, indanthrone pigments, isoindoline pigments, isoindoline ketone pigments, azomethine pigments, thioindigo pigments, metal complex pigments, perinone pigments, perylene pigments, phthalocyanine pigments or aniline black.
[0111] The at least one effect pigment and / or the at least one coloring pigment is preferably present in a total amount of 0.5 to 70 wt. %, based on the total weight of the color base component.
[0112] The color base component can also include at least one adhesive. This adhesive is used for the stable dispersion of the pigment and ensures the high intensity of the color and the high color uniformity of the color base component in this way. Suitable adhesives include polyurethane polymers, more particularly anionically stable polyurethane polymers, such as anionic first polyurethane resins P1. Using polyurethane resins P1 and / or P2 and / or P3 such as first polyurethane resins P1 in the color base component avoids incompatibility when the color base component is mixed with other components of the aqueous coating composition. At least one adhesive, more particularly the aforementioned anionically stable polyurethane resins P1 preferably exist in an amount of 10 to 80wt% based on the gross weight of the color base component.
[0113] The color base component may also contain at least one solvent. Solvents that may be used are water, commonly known organic solvents and mixtures thereof. It is particularly preferred to use a mixture of water and butanediol and / or methyl ethyl ketone.
[0114] Preferred color base components each comprise - based on their total weight -
[0115] 0.5 to 70 wt. % of at least one effect pigment and / or at least one coloring pigment,
[0116] 10 to 80 wt.% of at least one binder selected from the group of polyurethane polymers, amino resin polymers, polyacrylate polymers, polyester polymers and mixtures thereof, more particularly the anionically stabilized polyurethane resin P1 described above, and
[0117] At least one organic solvent.
[0118] It is particularly preferred that the color base component does not contain a large amount of organic solvents, that is, it is a low-VOC color base component with a VOC of less than 250 g / L. Suitable low-VOC color base components for use in the present invention include the color base components disclosed in the published applications WO 2021 / 018595 A1 and WO 2021 / 018594 A1.
[0119] Suitable matting agents are, for example, silicon dioxide adjusted to the particle size required for the respective coating. Alternatively, urea-formaldehyde condensates or mixtures based on polyamide-12 can also be used.
[0120] Suitable thickeners include inorganic thickeners and / or organic thickeners. Examples of inorganic thickeners are those from the group of layered silicates, such as lithium aluminum magnesium silicate. Organic thickeners are preferably selected from (meth)acrylic acid-(meth)acrylate copolymer thickeners (e.g. commercial product AS1130 (BASF SE) and polyurethane thickeners (e.g. commercial products from BASF SE) PU 1250). (Meth)acrylic acid-(meth)acrylate copolymer thickeners are those which, together with acrylic acid and / or methacrylic acid, also contain in copolymerized form one or more esters of acrylic acid (i.e., acrylates) and / or one or more esters of methacrylic acid (i.e., methacrylates). A common feature of (meth)acrylic acid-(meth)acrylate copolymer thickeners is that they exhibit a strong increase in viscosity in alkaline media, in other words at pH levels >7, more particularly >7.5, by forming salts of acrylic acid and / or methacrylic acid, in other words, by forming carboxylate groups. If (meth)acrylic acid esters formed from (meth)acrylic acid and C1-C6 alkanols are used, the product is an essentially non-associative (meth)acrylic acid-(meth)acrylate copolymer thickener, such as, for example, Rheovis AS1130, as described above. Essentially non-associative (meth)acrylic acid-(meth)acrylate copolymer thickeners are also referred to in the literature as ASE thickeners (“alkali soluble / swellable emulsions” or dispersions). However, what can also be used as (meth)acrylic acid-(meth)acrylate copolymer thickeners are those known as HASE thickeners ("hydrophobically modified anionic soluble emulsions" or dispersions). These are obtained by using those with a larger number of carbon atoms, such as, for example, 7 to 30 or 8 to 20 carbon atoms, as alkanols instead of C1-C6 alkanols or in addition to C1-C6 alkanols. HASE thickeners have a substantially associative thickening effect. Due to their thickening properties, the (meth)acrylic acid-(meth)acrylate copolymer thickeners that can be used are not suitable as binder resins and therefore do not belong to the physically, thermally or thermally and photochemically curable binders identified as binders, and therefore they are clearly different from the poly(meth)acrylate-based binders that can be used in the base coating material composition of the present invention. Polyurethane thickeners are associative thickeners identified in the literature as HEURs ("hydrophobically modified ethylene oxide urethane rheology modifiers"). Chemically, these are nonionic, branched or unbranched block copolymers consisting of polyethylene oxide chains (sometimes also polypropylene oxide chains), which are interconnected via urethane bonds and carry terminal long-chain alkyl or alkylene groups having 8 to 30 carbon atoms. Typical alkyl groups are, for example, dodecyl or stearyl; typical alkenyl groups are, for example, oleyl; typical aryl groups are phenyl groups; and typical alkylated aryl groups are, for example, nonylphenyl groups. Due to their thickening properties and structure, polyurethane thickeners are not suitable as physical, thermal or both thermally and physically curable binder resins. Therefore, they are clearly different from the polyurethanes that can be used as binders in the base coating material composition of the present invention.
[0121] The at least one additive is preferably present in a total amount of 0 wt.% to 10 wt.%, based on the total weight of the aqueous coating composition.
[0122] Characteristics of the waterborne coating composition of the present invention:
[0123] The aqueous coating composition preferably has a high solids content to reduce the curing time required to obtain a fully cured coating at room temperature. Preferred solids contents include 10 to 70 wt.%, preferably 20 to 65 wt.%, especially 35 to 55 wt.%, in each case based on the total weight of the aqueous coating composition.
[0124] Despite the high solids content, the aqueous coating composition preferably has a low viscosity to allow the aqueous coating composition to be applied using commonly known application methods. Preferably, the aqueous coating composition has a viscosity of 10 to 1,000 mPa*s, preferably 40 to 600 mPa*s, in particular 100 to 250 mPa*s as determined according to DIN EN ISO 3219-1994-10.
[0125] The aqueous coating composition preferably contains 10 to 100 g / L, preferably 10 to 60 g / L of VOC. The VOC value is defined as follows: VOC (g / L) = (total weight of volatile components (g) - total weight of water (g)) / (volume of coating agent (L) - volume of water (L)). Volatile components are compounds having a vapor pressure greater than 10 Pascals at processing temperature, in particular at 20°C (see the 31st BImSchV and the corresponding VOC directive and the VOC regulations of the EU). In addition, volatile components should be understood as organic compounds having an initial boiling point less than or equal to 250°C at a standard pressure of 101.3 kPa (see Directive 2004 / 42 / EC of the European Parliament and the Council). Due to the low amount of organic solvents, the aqueous coating composition of the present invention meets the strict safety requirements associated with toys, making the aqueous coating composition particularly suitable for the coating of toys and toy parts.
[0126] Method for preparing waterborne coating composition of the present invention:
[0127] The aqueous coating composition of the invention can be prepared by introducing all ingredients into corresponding containers and mixing these ingredients using generally known mixing equipment. If the aqueous coating composition is a 2K coating composition as described above, a base component comprising the aqueous dispersions D1 to D3 and optionally the aforementioned further ingredients and a hardener component comprising at least one crosslinker are prepared separately and mixed shortly before application to the substrate.
[0128] According to a preferred embodiment, the aqueous coating composition is a 3K composition and is prepared by mixing a base component comprising aqueous dispersions D1 to D3 and optionally the additional ingredients listed above with at least one base color component and a hardener component. Suitable weight ratios of the base component to the color base component to the hardener component include 100:1:1 to 1:100:50 or 80:80:2 to 20:80:20 or 60:60:4 to 40:40:10. In case more than one color base component is used, the above weight ratios refer to the sum of all color base components used during the production of the aqueous coating composition of the present invention.
[0129] The mixing of the components can be carried out manually, wherein an appropriate amount of the base component is introduced into a container and mixed with a corresponding amount of the base color component and the hardener component. The order in which the components are introduced into the container can also be changed, so that, for example, the base component and the base color component are introduced into the container and mixed with a corresponding amount of the hardener component. However, the mixing of two or more components can also be carried out automatically by an automatic mixing system. Such an automatic mixing system can include a mixing unit, more particularly a static mixer, and at least three devices for supplying a base component containing a polyurethane resin, a color base component and a hardener component containing a crosslinking agent, more particularly a gear pump and / or a pressure valve. In the case of manual mixing and in the case of supplying the components for automatic mixing, the individual components preferably each have a temperature of 15°C to 70°C, more preferably 15°C to 40°C, more particularly 20°C to 30°C.
[0130] Coating method of the present invention
[0131] According to the method of the present invention, a coating layer (C) is produced on a substrate (S) by applying the aqueous coating composition of the present invention to the substrate (S) and curing the applied coating composition to form a coating layer (C).
[0132] The substrate can be selected from a metal substrate, a plastic substrate, a substrate comprising metal and plastic components, wood or paper. Particularly preferably, the substrate is selected from a plastic substrate.
[0133] Suitable plastic substrates include (i) thermoplastics, such as polyolefins, thermoplastic polyurethanes (TPU), thermoplastic rubbers (TPE), poly(meth)acrylates (PA), polystyrenes, polyvinyl chlorides (PVC), polyamides, polyurethanes, polycarbonates, polylactic acid (PLA), saturated polyesters like PET (polyethylene terephthalate), ethylene-propylene-diene (EPDM), acrylonitrile-styrene-butadiene (ABS), vinyl polymers selected from halogenated polymers other than PVC, (ii) thermosetting plastics, such as phenolic resins, epoxy resins, unsaturated polyester resins, resins with furan groups, resins with urea groups, melamine resins, polyurethane resins (PU), (iii) mixtures of the above thermoplastics and thermosetting plastics, (iv) fiber-reinforced polymers or composite materials derived from the above thermoplastics or thermosetting plastics. Particularly preferably, the substrate is a thermoplastic rubber substrate, such as a molded thermoplastic toy or a part thereof.
[0134] Applying the aqueous coating composition of the present invention to a substrate:
[0135] In the first step of the inventive method, water-based coating composition of the present invention is applied to substrate, particularly applied to at least a portion of substrate surface. At least a portion of water-based coating composition being applied to substrate surface should be understood as follows: applying the water-based coating composition discussed makes the film produced by the composition be arranged on at least a portion of substrate surface, but does not necessarily need to directly contact with the surface of substrate. For example, between the surface of film and substrate, other coatings can be arranged. Preferably, in the first step, water-based coating composition of the present invention is directly applied to at least a portion of substrate surface, which means that the film produced by applying the water-based coating composition of the present invention directly contacts with the surface of substrate.
[0136] The aqueous coating composition of the present invention can be applied by methods known to the skilled person for applying liquid coating materials, such as, for example, by dipping, scraping, spraying, rolling, brushing, etc. Preferably, a spraying application method is used, such as, for example, compressed air spraying (pneumatic application), airless spraying, high-speed rotation, electrostatic spray application (ESTA), optionally in combination with thermal spraying application such as hot air (thermal spraying) or brushing. Very particularly preferably, the radiation-curable coating composition of the present invention is applied by pneumatic spraying or brushing.
[0137] Despite the aqueous nature of the coating composition of the present invention, the coating composition can be applied at high wet film thicknesses without forming undesirable runs that lead to an undesirable optical appearance. In addition, the high wet film thickness allows good hiding power of the cured coating to be achieved, thereby avoiding repainting of the coated substrate in order to avoid the color of the underlying substrate still being visible through the cured coating.
[0138] Curing of the applied waterborne coating composition:
[0139] In the second step of the method of the present invention, the applied aqueous coating composition is cured. The aqueous coating composition has a very short curing time at room temperature. Preferably, when applied to the substrate (S) with a wet thickness of up to 60 μm, the aqueous coating composition forms a cured coating at a temperature of 18° C. to 25° C. in less than 1 minute, preferably in 10 to 40 seconds. These short curing times allow, for example, extremely rapid further processing of the coated substrate by applying another coating on the part of the substrate that has not yet been coated with the coating. Therefore, the short curing time of the aqueous coating composition of the present invention at room temperature allows an extremely efficient coating process for plastic substrates.
[0140] In one example, the applied aqueous coating composition is cured for a duration of less than 3 minutes, in particular 10 seconds to 2 minutes, at a temperature of 18° C. to 40° C., preferably 18° C. to 25° C. Such a curing time may be preferred if the aqueous coating composition is applied at a wet film thickness of up to 60 μm.
[0141] In another example, the applied coating composition is cured for a duration of 10 to 50 minutes, in particular 10 to 35 minutes, at a temperature of 18° C. to 40° C., preferably 18° C. to 25° C. Such a curing time may be preferred if the aqueous coating composition is applied at a wet film thickness of more than 60 μm, for example by brushing, in order to achieve a high hiding power of the resulting coating.
[0142] The dry film thickness of the cured coating obtained after curing may vary widely and depends mainly on the surface roughness and / or geometry of the substrate. It may range, for example, from 5 to 200 μm, preferably from 5 to 80 μm.
[0143] Additional steps:
[0144] Method of the present invention may further comprise the step of applying other coating compositions such as the aqueous coating compositions of the present invention that do not comprise any pigment, i.e., clear coating compositions, to the cured coating. Other aqueous coating compositions may be applied and cured as previously described. If a specific optical appearance such as high gloss or matte finish of a coated substrate should be achieved, applying other aqueous coating compositions of the present invention may be beneficial.
[0145] What has been said about the aqueous coating composition of the invention applies mutatis mutandis to the further preferred embodiments of the method of the invention.
[0146] The coating of the present invention
[0147] After the process of the present invention is completed, the product is the coating of the present invention. The coating of the present invention exhibits high adhesion to various plastic substrates such as molded TPE and PVC toys and toy parts, thereby preventing the coating from splitting and peeling during use of the substrate.
[0148] What has been said with regard to the aqueous coating composition of the invention and the method of the invention applies mutatis mutandis to the further preferred embodiments of the coating of the invention.
[0149] Coated substrate of the present invention
[0150] The last subject of the present invention is a substrate (S) with a coating (C) according to the invention. The coating according to the invention can be produced according to the method according to the invention described above and shows high adhesion to the underlying substrate without the use of a primer layer. Since the aqueous coating compositions used to prepare the coatings according to the invention contain only small amounts of organic solvents and allow extremely fast curing times at room temperature, they are particularly suitable for plastic substrates such as molded TPE and PVC toys and parts thereof, where strict safety regulations apply to the components used.
[0151] What has been said with regard to the aqueous coating composition of the invention, the process of the invention and the coating of the invention applies mutatis mutandis to further preferred embodiments of the coated substrate of the invention.
[0152] The present invention is particularly described by the following clauses:
[0153] 1. A water-based coating composition, comprising:
[0154] (a) at least one aqueous dispersion D1 comprising a first polyurethane resin P1 having a glass transition temperature (Tg) of less than or equal to -30°C as determined in accordance with DIN EN ISO 11357-2-2020-08,
[0155] (b) at least one aqueous dispersion D2 comprising a second polyurethane resin P2 different from the first polyurethane resin P1, said second polyurethane resin P2 having a 100% modulus of at least 1 MPa as determined according to DIN 53504:2017-03,
[0156] (c) at least one aqueous dispersion D3 comprising a third polyurethane resin P3 different from the first polyurethane resin P1 and the second polyurethane resin P2, said third polyurethane resin P3 having a glass transition temperature (Tg) less than or equal to -40°C as determined according to DIN EN ISO 11357-2-2020-08, and
[0157] (d) at least one cross-linking agent.
[0158] 2. The aqueous coating composition according to clause 1, wherein the first polyurethane resin P1 has a glass transition temperature (Tg) of -30°C to -50°C, preferably -35°C to -45°C, very preferably -38°C to -42°C.
[0159] 3. The aqueous coating composition according to clause 1 or 2, wherein the first polyurethane resin P1 is an anionic polyurethane resin.
[0160] 4. The aqueous coating composition according to any one of clauses 1 to 3, wherein the first polyurethane resin P1 is an aliphatic polyester-based polyurethane resin.
[0161] 5. The aqueous coating composition according to any one of clauses 1 to 4, wherein the first polyurethane resin P1 has an acid value of 5 to 100 mg KOH / g solid, preferably 10 to 50 mg KOH / g solid, very preferably 15 to 30 mg KOH / g solid.
[0162] 6. The aqueous coating composition according to any one of clauses 1 to 5, wherein the first polyurethane resin P1 has a hydroxyl value of 1 to 150 mg KOH / g solid, preferably 2 to 100 mg KOH / solid, more preferably 5 to 70 mg KOH / g solid, very preferably 10 to 25 mg KOH / g solid.
[0163] 7. The aqueous coating composition according to any one of clauses 1 to 6, wherein the first polyurethane resin P1 has a number average molecular weight M n It is 750 to 2,000,000 g / mol, preferably 1,000 to 1,000,000, more preferably 2,000 to 500,000, very preferably 5,000 to 10,000 g / mol.
[0164] 8. The aqueous coating composition according to any one of clauses 1 to 7, wherein the first polyurethane resin P1 is obtained by reacting an NCO-functional prepolymer with at least one polyol.
[0165] 9. The aqueous coating composition of clause 8, wherein the equivalent ratio between the active hydrogens of the polyol and the NCO groups of the NCO-functional prepolymer is 2:1 to 1:2, preferably 1.1:1 to 1:1.1.
[0166] 10. The aqueous coating composition of clause 8 or 9, wherein the polyol is an aliphatic monomeric polyol, preferably an aliphatic monomeric polyol containing at least three hydroxyl groups, in particular trimethylolpropane.
[0167] 11. The aqueous coating composition of any one of clauses 8 to 10, wherein the NCO functional prepolymer is obtained by reacting:
[0168] at least one having an OH value of 40 to 100 mg KOH / g solid and a number average molecular weight M of 1,000 to 3,000 g / mol n Aliphatic polyester polyols,
[0169] - at least one compound comprising at least one acid group and at least one group capable of reacting with an NCO group,
[0170] - at least one average molecular weight M w A polyol of 60 to 400 g / mol, and
[0171] - at least one polyisocyanate.
[0172] 12. The aqueous coating composition according to Item 11, wherein the aliphatic polyester polyol is obtained by reacting a dimerized fatty acid with an aromatic dicarboxylic acid and a diol.
[0173] 13. An aqueous coating composition according to clause 11 or 12, wherein the at least one compound comprising at least one acid group and at least one group capable of reacting with an NCO group is chosen from alkanoic acids having 3 to 8 carbon atoms and 2 hydroxyl groups, in particular from dimethylolpropionic acid.
[0174] 14. An aqueous coating composition as described in any one of clauses 11 to 13, wherein the at least one average molecular weight M w The polyol having an amount of 60 to 400 g / mol is an aliphatic polyol having 3 to 10 carbon atoms and 2 hydroxyl groups, in particular neopentyl glycol.
[0175] 15. The aqueous coating composition according to any one of clauses 11 to 14, wherein the polyisocyanate is selected from aliphatic, cycloaliphatic, araliphatic and / or aromatic polyisocyanates, in particular from cycloaliphatic polyisocyanates.
[0176] 16. The aqueous coating composition according to any of clauses 1 to 15, wherein the aqueous dispersion D1 has an average particle size (z-average) determined according to photon correlation spectroscopy of 30 to 200 nm, preferably 40 to 100 nm, very preferably 45 to 60 nm.
[0177] 17. The aqueous coating composition according to any of clauses 1 to 16, wherein the aqueous dispersion D1 comprises the first polyurethane resin P1 in a total amount of 10 to 60% by weight, preferably 15 to 50% by weight, more preferably 20 to 40% by weight, very preferably 25 to 35% by weight, in each case based on the total weight of the aqueous dispersion D1.
[0178] 18. The aqueous coating composition according to any of clauses 1 to 17, wherein the aqueous coating composition comprises the aqueous dispersion D1 in a total amount of 5 to 60% by weight, preferably 10 to 50% by weight, very preferably 15 to 25% by weight, in each case based on the total weight of the aqueous coating composition.
[0179] 19. An aqueous coating composition according to any of clauses 1 to 18, wherein the second polyurethane resin P2 has a 100% modulus as determined according to DIN 53504:2017-03 of 1 to 6 MPa, preferably 1 to 4 MPa, very preferably 1.4 to 1.9 MPa.
[0180] 20. The aqueous coating composition of any one of clauses 1 to 19, wherein the second polyurethane resin P2 has a tensile strength as determined according to DIN 53504:2017-03 of 10 to 50 MPa, preferably 15 to 40 MPa, very preferably 22 to 28 MPa.
[0181] 21. The aqueous coating composition of any of clauses 1 to 20, wherein the second polyurethane resin P2 has an elongation at break as determined according to DIN 53504:2017-03 of 400% to 1,500%, preferably 600% to 900%, very preferably 720% to 780%.
[0182] 22. The aqueous coating composition according to any one of clauses 1 to 21, wherein the second polyurethane resin P2 has a melting range of 150°C to 300°C, preferably 190°C to 230°C.
[0183] 23. The aqueous coating composition of any one of clauses 1 to 22, wherein the second polyurethane resin P2 is an anionic polyurethane resin.
[0184] 24. The aqueous coating composition of any one of clauses 1 to 23, wherein the second polyurethane resin P2 is an aliphatic polycarbonate-polyether based polyurethane resin.
[0185] 25. The aqueous coating composition according to any of clauses 1 to 24, wherein the aqueous dispersion D2 comprises the second polyurethane resin P2 in a total amount of 10 to 70% by weight, preferably 15 to 60% by weight, more preferably 25 to 50% by weight, very preferably 35 to 45% by weight, in each case based on the total weight of the aqueous dispersion D2.
[0186] 26. The aqueous coating composition according to any of clauses 1 to 25, wherein the aqueous coating composition comprises the aqueous dispersion D2 in a total amount of 5 to 60% by weight, preferably 10 to 50% by weight, very preferably 20 to 35% by weight, in each case based on the total weight of the aqueous coating composition.
[0187] 27. The aqueous coating composition according to any one of clauses 1 to 26, wherein the third polyurethane resin P3 has a glass transition temperature (Tg) of -40°C to -80°C, preferably -40°C to -60°C, very preferably -42°C to -55°C.
[0188] 28. The aqueous coating composition of any one of clauses 1 to 27, wherein the third polyurethane resin P3 is an anionic polyurethane resin.
[0189] 29. The aqueous coating composition of any one of clauses 1 to 28, wherein the third polyurethane resin P3 is an aliphatic polycarbonate-polyester based polyurethane resin.
[0190] 30. The aqueous coating composition of any of clauses 1 to 29, wherein the aqueous dispersion D3 has an average particle size (z-average) determined according to photon correlation spectroscopy of 20 to 200 nm, preferably 30 to 100 nm, very preferably 40 to 80 nm.
[0191] 31. The aqueous coating composition according to any of clauses 1 to 30, wherein the aqueous dispersion D3 comprises the third polyurethane resin P3 in a total amount of 10 to 60% by weight, preferably 20 to 50% by weight, very preferably 30 to 40% by weight, based in each case on the total weight of the aqueous dispersion D3.
[0192] 32. The aqueous coating composition according to any of clauses 1 to 31, wherein the aqueous coating composition comprises the aqueous dispersion D3 in a total amount of 1 to 40% by weight, preferably 5 to 30% by weight, very preferably 8 to 20% by weight, in each case based on the total weight of the aqueous coating composition.
[0193] 33. The aqueous coating composition according to any one of clauses 1 to 32, wherein the crosslinker is selected from amino resins, unblocked polyisocyanates, at least partially blocked polyisocyanates, polycarbodiimides and mixtures thereof, in particular unblocked polyisocyanates.
[0194] 34. An aqueous coating composition according to clause 33, wherein the unblocked polyisocyanate is selected from hexamethylene diisocyanate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, tetramethylhexane diisocyanate, isophorone diisocyanate (IPDI), 2-isocyanatopropylcyclohexyl isocyanate, dicyclohexylmethane 2,4'-diisocyanate, dicyclohexyl-methane 4,4'-diisocyanate, 1,4- or 1,3-bis(isocyanato-methyl)-cyclohexane, 1,4- or 1,3- or 1,2-diisocyanato-cyclohexane, and 2,4- or 2,6-diisocyanato-1-methyl-cyclohexane, dimers and trimers thereof, and also mixtures of these polyisocyanates.
[0195] 35. The aqueous coating composition of any one of clauses 1 to 34, wherein the aqueous coating composition comprises the at least one crosslinker in a total amount of 1 wt.% to 40 wt.% solids, preferably 2 to 30 wt.% solids, more particularly 6 to 12 wt.% or 15 to 25 wt.% solids, in each case based on the total weight of the aqueous coating composition.
[0196] 36. The aqueous coating composition according to any one of clauses 1 to 35, further comprising at least a polymer different from the polyurethane resins P1 to P3, a colorant and / or effect pigment, a matting agent, a thickener, a dispersant, a leveling agent, a pH adjuster, a defoamer, a biocide, a UV absorber, a crosslinking catalyst and mixtures thereof.
[0197] 37. The aqueous coating composition of any one of clauses 1 to 36, wherein the aqueous coating composition has a solids content of 10 to 70 wt.%, preferably 20 to 65 wt.%, in particular 35 to 55 wt.%, in each case based on the total weight of the aqueous coating composition.
[0198] 38. The aqueous coating composition of any one of clauses 1 to 37, wherein the aqueous coating composition has a viscosity of 10 to 1,000 mPa*s, preferably 40 to 600 mPa*s, in particular 100 to 250 mPa*s as determined according to DIN EN ISO 3219-1994-10.
[0199] 39. The aqueous coating composition of any one of clauses 1 to 38, wherein the aqueous coating composition comprises 10 to 100 g / L, preferably 10 to 60 g / L VOC.
[0200] 40. A method for producing a coating (C) on a substrate (S), the method comprising the steps of applying an aqueous coating composition as described in any one of clauses 1 to 39 to the substrate (S) and curing the applied coating composition.
[0201] 41. The method according to clause 40, wherein the substrate is selected from a metal substrate, a plastic substrate, a substrate comprising metal and plastic parts, wood or paper, in particular from a plastic substrate.
[0202] 42. A method as described in item 41, wherein the plastic substrate is selected from (i) thermoplastics, such as polyolefins, thermoplastic polyurethanes (TPU), thermoplastic rubbers (TPE), poly(meth)acrylates (PA), polystyrene, polyvinyl chloride (PVC), polyamides, polyurethanes, polycarbonates, polylactic acid (PLA), saturated polyesters like PET (polyethylene terephthalate), ethylene-propylene-diene (EPDM), acrylonitrile-styrene-butadiene (ABS), vinyl polymers selected from halogenated polymers other than PVC, (ii) thermosetting plastics, such as phenolic resins, epoxy resins, unsaturated polyester resins, resins with furan groups, resins with urea groups, melamine resins, polyurethane resins (PU), (iii) mixtures of the above-mentioned thermoplastics and thermosetting plastics, (iv) fiber-reinforced polymers or composite materials derived from the above-mentioned thermoplastics or thermosetting plastics; in particular selected from thermoplastic rubbers (TPE).
[0203] 43. The method of any one of clauses 40 to 42, wherein the aqueous coating composition, when applied to the substrate (S) at a wet thickness of up to 60 μm, forms a cured coating at a temperature of 18°C to 25°C in less than 1 minute, preferably in 10 to 40 seconds.
[0204] 44. A method as described in any of clauses 40 to 43, wherein the applied coating composition is cured for a duration of less than 3 minutes, in particular 10 seconds to 2 minutes, or wherein the applied coating composition is cured for a duration of 10 to 50 minutes, in particular 10 to 35 minutes, at a temperature of 18°C to 40°C, preferably 18°C to 25°C.
[0205] 45. A coating produced by the method of any one of clauses 40 to 44.
[0206] 46. A substrate (S) having a coating (C) according to clause 45.
[0207] Examples
[0208] The present invention will now be explained in more detail by using working examples, but the present invention is by no means limited to these working examples. In addition, unless otherwise indicated, the terms "part", "%" and "ratio" in these examples represent "part by mass", "mass %" and "mass ratio" respectively.
[0209] 1. Determine the method:
[0210] 1.1 Solid content (solid, non-volatile fraction)
[0211] Unless otherwise stated, the solids content (also called solids proportion, solids content, non-volatile matter proportion) is determined in accordance with DIN EN ISO 3251:2018-07 at 130° C.; 60 minutes, starting weight 1.0 g.
[0212] 1.2 Cross-cut Adhesion Test
[0213] The adhesion of the cured coating to the substrate is determined using the cross-cut adhesion test. The test is performed and evaluated on 2D panels according to DIN EN ISO 2409:2020-12.
[0214] 1.3 Stability against water
[0215] The stability of the coated substrate is determined by completely immersing the coated substrate in tap water at room temperature for a duration of 24 hours. If no visual change in the coating can be detected after 24 hours, the coated substrate is rated as "acceptable". Otherwise, the coated substrate is rated as "unacceptable".
[0216] 1.4 Wear test
[0217] The wear resistance of the coating on the substrate is determined in accordance with DIN EN ISO 20566:2021-06.
[0218] 1.5UV test
[0219] The UV resistance of the coated substrates is determined according to DIN EN ISO 4892-2:2021-11 by irradiating the coated substrates with UV light for 72 h. The UV resistance is assessed by visually comparing the irradiated coated objects with the coated objects that have not been irradiated with UV light in terms of color change.
[0220] 2. Preparation of different waterborne coating compositions of the present invention
[0221] 2.1 Preparation of basic components
[0222] Two different base components BC1 and BC2 were prepared by mixing the ingredients listed in Table 1.
[0223] Table 1: Ingredients for base components BC1 and BC2 (all amounts are given in wt. % based on the total weight of the corresponding base component)
[0224]
[0225]
[0226] 1) Solids content = 25%, containing polyurethane resin P1 with a Tg of -40°C (DIN EN ISO 11357-2-2020-08); prepared according to WO 92 / 15405 A1, pages 14 to 15, points 1.1 and 1.2;
[0227] 2) Solid content = 40%, aqueous dispersion of anionic aliphatic polycarbonate-polyether polyurethane resin, anionic aliphatic polycarbonate-polyether polyurethane having a 100% modulus of 1.7 MPa (DIN 53504:2017-03) (supplied by Covestro, Germany);
[0228] 3) Solid content = 34%-36%, aqueous dispersion of anionic aliphatic polyester-polycarbonate-based polyurethane resin, anionic aliphatic polycarbonate-polyether polyurethane having a Tg of -45°C to -51°C (DIN EN ISO 11357-2-2020-08) (supplied by Covestro, Germany);
[0229] 4) VOC and solvent-free wetting and dispersing additives (supplied by BYK Chemie GmbH);
[0230] 5) Solid content = 41%, prepared according to Example 1, paragraph
[0057] of EP 1 861 469 B1;
[0231] 6) Synthetic amorphous silica with high porosity used as a matting agent (supplied by WR Grace & Co.—Conn.);
[0232] 7) Aqueous dispersion of hydrophobic fumed silica (supplied by Evonik Operations GmbH);
[0233] 8)Hydroxy-functional polyurethane dispersion (supplied by Allnex);
[0234] 9) Anionic polyurethane aqueous dispersion (supplied by BASF AG);
[0235] 10) Silicone surfactants for waterborne coatings (supplied by BYK Chemical);
[0236] 11) Laponite RD (synthetic sheet silicate, supplied by BYK Chemical);
[0237] 12) Supplied by BASF AG.
[0238] 2.2 Preparation of waterborne coating compositions AC1 to AC12
[0239] The aqueous coating compositions AC1 to AC12 of the present invention are prepared by combining a base component, optionally a corresponding base color component (BCC) having a VOC of less than 250 g / L, and a hardener component in the mixing ratios given in Table 3 (weight ratios).
[0240]
[0241]
[0242] 3. Production of coated substrates
[0243] 3.1 Substrate
[0244] The molded thermoplastic rubber substrate (TPE substrate) and PVC substrate are produced by injecting molten thermoplastic rubber or PVC into 2D molds (plate forms) and 3D molds (various animal forms) and hardening the injected rubber or PVC. The molded TPE substrate and PVC substrate are cleaned for 3 to 4 minutes using an industrial washing machine with a washing liquid (Lavamatic liquid, supplied by DTL-Detergentes Técnicos, Unipessoal, Lda). Then, the cleaned substrate is dried.
[0245] 3.2 Coating of substrate
[0246] 3.2.1 Pneumatic spray application
[0247] The corresponding aqueous coating compositions AC1 to AC12 were each applied in a single coating system (pneumatic manual coating) with a wet film thickness of 15 to 25 μm directly to a portion of the cleaned TPE and PVC substrates prepared in point 3.1 and cured at 18° C. to 25° C. for 10 to 40 seconds. The remaining portions of the TPE and PVC substrates were then coated with the corresponding coating compositions as described above. In each case, the film thickness (cured) was 6-16 μm.
[0248] 3.2.2 Application by brush
[0249] The corresponding aqueous coating compositions AC1 to AC12 were each applied directly to a portion of the cleaned TPE and PVC substrates prepared in point 3.1 using a brush at a wet film thickness of 15 to 25 micrometers or at a wet film thickness of more than 60 to 70 micrometers. The applied coating compositions were each cured at 18° C. to 25° C. for 1 to 2 minutes or 15 to 30 minutes, depending on the applied wet film thickness of the applied aqueous coating compositions AC1 to AC12.
[0250] 3.2.3 Dipping application
[0251] The cleaned TPE and PVC substrates prepared in point 3.1 were immersed in a bath containing a 1:1 or 1:2 (v / v) dilution of the corresponding aqueous coating compositions AC1 to AC12 with water. After removing the coated substrate from the batch, the excess coating composition was drained off and the coated substrate was cured at 18 to 25° C. for 1 to 2 minutes.
[0252] 4. Results
[0253] 4.1 Visual Evaluation
[0254] Despite the aqueous nature of the coating compositions, no flow was detected when the aqueous coating compositions AC1 to AC12 were applied at high wet film thicknesses on TPE and PVC substrates using a brush application. Furthermore, the very fast curing times at room temperature prevented the applied aqueous coating compositions AC1 to AC12 from flowing on vertically oriented substrate areas. Overall, all coated substrates met the required qualities for coated toys and toy parts in terms of visual appearance.
[0255] 4.2 Cross-cut Adhesion Test
[0256] No peeling or splitting of the coatings formed from the aqueous coating compositions AC1 to AC12 on the TPE and PVC board substrates was detected in the cross-hatch adhesion test. Thus, the coatings formed from the aqueous coating compositions of the present invention exhibit high adhesion on the plastic substrates (despite their aqueous nature), very short curing times, and the absence of an adhesion-promoting layer on the substrate.
[0257] 4.3 Stability against water
[0258] After the coated TPE and PVC substrates were completely immersed in tap water for 24 hours, no visual defects were detected. Therefore, the coating formed by the aqueous coating composition has sufficient stability against dissolution, avoiding undesirable negative visual effects and release of coating substances during use of the coated substrate. All coated TPE and PVC substrates were accordingly rated as "qualified".
[0259] 4.4 Wear resistance
[0260] All coated TPE and PVC substrates showed slight or no wear, thus demonstrating high adhesion of the coatings on the TPE and PVC substrates despite the absence of an adhesion promoting layer and avoiding negative effects on the visual appearance and release of the coating substance during use of the coated substrates.
[0261] 4.5UV stability
[0262] All coated TPE and PVC substrates showed adequate stability against UV degradation. Thus, the coatings formed did not show undesirable visual color changes upon UV light exposure and thus showed good UV light stability. This avoids degradation of the color of the coating over time, which would render the visual appearance of the coated substrate unpleasant.
[0263] 5. Discussion of Results
[0264] The example shows that, if applied with thin wet film thickness, although its water-based properties, water-based coating composition also has extremely low curing time at room temperature. This allows to use them in the coating process of using water-based coating materials in need-due to existing safety regulations or environmental regulations-and does not greatly extend the curing time (compared with solvent-based coating materials) at room temperature. Although the formed coating does not have an adhesion-promoting layer, it also demonstrates excellent adhesion and good UV stability on various substrates. In addition, water-based coating composition can be applied with high wet film thickness, and does not form the sagging that causes the negative visual appearance of coated substrates. The extremely fast curing time at room temperature allows coating the substrate area of vertical orientation without forming sagging, thereby allowing to accurately coat the corresponding target area, regardless of its orientation on substrate.
Claims
1. A water-based coating composition, comprising: (a) at least one aqueous dispersion D1 comprising a first polyurethane resin P1 having a glass transition temperature (Tg) of less than or equal to -30°C as determined in accordance with DIN EN ISO 11357-2-2020-08, (b) at least one aqueous dispersion D2 comprising a second polyurethane resin P2 different from the first polyurethane resin P1, said second polyurethane resin P2 having a 100% modulus of at least 1 MPa as determined according to DIN 53504:2017-03, (c) at least one aqueous dispersion D3 comprising a third polyurethane resin P3 different from the first polyurethane resin P1 and the second polyurethane resin P2, said third polyurethane resin P3 having a glass transition temperature (Tg) less than or equal to -40°C as determined according to DIN EN ISO 11357-2-2020-08, and (d) at least one cross-linking agent.
2. The aqueous coating composition according to claim 1, wherein The first polyurethane resin P1 has a glass transition temperature (Tg) of -30°C to -50°C, preferably -35°C to -45°C, very preferably -38°C to -42°C.
3. The aqueous coating composition according to claim 1 or 2, wherein: The first polyurethane resin P1 is an aliphatic polyester-based polyurethane resin.
4. The aqueous coating composition according to any one of claims 1 to 3, wherein The aqueous coating composition comprises the aqueous dispersion D1 in a total amount of 5 to 60% by weight, preferably 10 to 50% by weight, very preferably 15 to 25% by weight, based in each case on the total weight of the aqueous coating composition.
5. The aqueous coating composition according to any one of claims 1 to 4, wherein The second polyurethane resin P2 has a 100% modulus, as determined in accordance with DIN 53504:2017-03, of 1 to 6 MPa, preferably 1 to 4 MPa, very preferably 1.4 to 1.9 MPa.
6. The aqueous coating composition according to any one of claims 1 to 5, wherein The second polyurethane resin P2 has a tensile strength, as determined in accordance with DIN 53504:2017-03, of 10 to 50 MPa, preferably 15 to 40 MPa, very preferably 22 to 28 MPa.
7. The aqueous coating composition according to any one of claims 1 to 6, wherein The second polyurethane resin P2 is an aliphatic polycarbonate-polyether-based polyurethane resin.
8. The aqueous coating composition according to any one of claims 1 to 7, wherein The aqueous coating composition comprises the aqueous dispersion D2 in a total amount of 5 to 60% by weight, preferably 10 to 50% by weight, very preferably 20 to 35% by weight, based in each case on the total weight of the aqueous coating composition.
9. The aqueous coating composition according to any one of claims 1 to 8, wherein The third polyurethane resin P3 has a glass transition temperature (Tg) of -40°C to -80°C, preferably -40°C to -60°C, very preferably -42°C to -55°C.
10. The aqueous coating composition according to any one of claims 1 to 9, wherein The third polyurethane resin P3 is an aliphatic polycarbonate-polyester based polyurethane resin.
11. The aqueous coating composition according to any one of claims 1 to 10, wherein The aqueous coating composition comprises the aqueous dispersion D3 in a total amount of 1 to 40% by weight, preferably 5 to 30% by weight, very preferably 8 to 20% by weight, based in each case on the total weight of the aqueous coating composition.
12. The aqueous coating composition according to any one of claims 1 to 11, wherein The aqueous coating composition contains 10 to 100 g / L, preferably 10 to 60 g / L of VOC.
13. A method for producing a coating (C) on a substrate (S), said method comprising the step of applying an aqueous coating composition as claimed in any one of claims 1 to 12 to the substrate (S) and the step of curing the applied coating composition.
14. A coating produced by the method of claim 13.
15. A substrate (S) having a coating (C) as claimed in claim 14.