Film, method for producing same, and image display device

By adding acrylic resin to the polyimide film and performing stretching treatment, the problem of reducing transparency of the polyimide film when heating is solved, and a film with high transparency and mechanical strength is realized, which is suitable for flexible displays. cover.

CN118974146APending Publication Date: 2024-11-15KANEKA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032211.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-04-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Polyimide films are prone to color when heated, resulting in a decrease in transparency and making it difficult to take into account both transparency and mechanical strength.

Method used

A film containing polyimide and an acrylic resin is used to improve transparency through compatibility, and mechanical strength is imparted by tensile treatment, so as to ensure the refractive index anisotropy and high transparency of the film.

Benefits of technology

The film with excellent transparency and high mechanical strength is achieved, suitable for the coverage of flexible displays, and can be stretched at low temperatures, avoiding the coloring problem caused by high temperature heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005068877360000041
    Figure BDA0005068877360000041
  • Figure BDA0005068877360000042
    Figure BDA0005068877360000042
  • Figure BDA0005068877360000051
    Figure BDA0005068877360000051
Patent Text Reader

Abstract

The present invention relates to a film containing a polyimide and an acrylic resin, wherein the average value nH of the refractive index n1 in a first direction in which the refractive index in the film plane is maximum and the refractive index n2 in a second direction orthogonal to the first direction in the film plane, and the refractive index n3 in the film thickness direction satisfy nH-n3 > = 0.0140. The total light transmittance of the film is preferably 85% or more, the haze is preferably 10% or less, and the yellowness is preferably 5 or less. The film can be produced, for example, by stretching an unstretched film containing a polyimide and an acrylic resin in at least one direction. The film may be a biaxially stretched film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a film, a method for producing the film, and an image display device including the film. Background Art

[0002] Liquid crystal display devices, organic EL (Electroluminescence) display devices, electronic paper and other display devices, or electronic devices such as solar cells and touch panels require thinning or lightness, and further require flexibility. By replacing the glass materials used in these devices with film materials, flexibility, thinness and lightness can be achieved. Transparent polyimide films have been developed as glass substitutes for display substrates or cover films (cover windows) arranged on the outermost surface of display devices (e.g., Patent Document 1). In addition, it is also proposed to use polyimide with an amide structure (so-called "polyamide-imide") as a material for the cover film (e.g., Patent Document 2).

[0003] In order to apply to bendable applications such as flexible displays, research is being conducted to improve the bending resistance of transparent polyimide films. For example, Patent Document 1 describes that the bending resistance is improved by stretching a polyimide film.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-6933

[0007] Patent Document 2: International Publication No. 2013 / 048126 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] Although polyimide has excellent heat resistance, it has a high glass transition temperature, so it needs to be heated to a high temperature of 250° C. or higher to stretch the polyimide film. When polyimide is heated to a high temperature, it tends to be colored yellow and has a tendency to reduce transparency, making it difficult to achieve both transparency and high mechanical strength.

[0010] In view of the above circumstances, an object of the present invention is to provide a transparent film having excellent transparency and excellent mechanical strength which can also be applied to a flexible display.

[0011] Solutions for solving problems

[0012] The present invention relates to a film comprising polyimide and acrylic resin and having anisotropic refractive index, wherein the average refractive index n in the film surface is H The difference n between the refractive index n3 in the thickness direction of the filmH - n3 is greater than 0.0140.

[0013] The average refractive index n in the film plane H The refractive index n1 in the first direction and the refractive index n2 in the second direction perpendicular to the first direction may satisfy 100×(n1-n2) / n2<1.0.

[0014] The total light transmittance of the film is preferably 85% or more, the haze is preferably 10% or less, and the yellowness is preferably 5 or less. The glass transition temperature of the film may be 110° C. or more and less than 250° C. The ratio of the polyimide resin to the acrylic resin contained in the film may be in the range of 98:2 to 2:98 by weight.

[0015] The polyimide contained in the film has a structure derived from diamine and a structure derived from tetracarboxylic dianhydride. In one embodiment, the polyimide preferably has a fluoroalkyl group in at least one of the structure (diamine component) derived from diamine and the structure (acid dianhydride component) derived from tetracarboxylic dianhydride. The polyimide may also be a polyamide-imide that includes a structure derived from dicarboxylic acid in addition to the structure derived from diamine and the structure derived from tetracarboxylic dianhydride.

[0016] The polyimide preferably contains a diamine having a fluoroalkyl group as a diamine component. Examples of the diamine having a fluoroalkyl group include fluoroalkyl-substituted benzidines such as 2,2'-bis(trifluoromethyl)benzidine (TFMB).

[0017] It is preferable that the polyimide contains one or more types selected from the group consisting of tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride having a fluoroalkyl group as the acid dianhydride component.

[0018] In one embodiment, in the acrylic resin contained in the film, the total amount of methyl methacrylate and the modified structure of methyl methacrylate is 60 wt % or more relative to the total amount of monomer components. The acrylic resin may have a glass transition temperature of 80° C. or more.

[0019] Both the tensile elastic modulus in the first direction and the tensile elastic modulus in the second direction of the film may be 3.5 GPa or more.

[0020] The film is obtained, for example, by stretching a film (unstretched film) comprising polyimide and acrylic resin in at least one direction. That is, the film of the present invention may be a stretched film stretched in at least one direction. The film may also be a biaxially stretched film. The temperature during stretching may be lower than 250°C.

[0021] In one embodiment, a resin solution containing polyimide and acrylic resin dissolved in an organic solvent is applied to a support, and the organic solvent is removed to obtain an unstretched film. The film is stretched in at least one direction to obtain a stretched film having anisotropy of refractive index.

[0022] Effects of the Invention

[0023] The film has excellent transparency and high mechanical strength such as bending resistance, and therefore can be suitably used as a cover film for a flexible display or the like. DETAILED DESCRIPTION

[0024] The film of one embodiment of the present invention comprises a polyimide resin and an acrylic resin, and exhibits transparency due to the compatibility of the polyimide resin and the acrylic resin. The film of the present invention has anisotropy of refractive index, and the average refractive index n in the film plane is H The difference n between the refractive index n3 in the thickness direction of the film H -n3 is 0.0140 or more. That is, the average refractive index n in the film surface is H The refractive index n3 in the thickness direction satisfies n H -n3≥0.0140.

[0025] The average refractive index n in the film plane H The refractive index n1 in the first direction with the largest refractive index in the film plane and the refractive index n2 in the second direction orthogonal to the first direction in the film plane are averaged. The refractive index n1 in the first direction and the refractive index n2 in the second direction preferably satisfy 100×(n1-n2) / n2<1.0.

[0026] The method for producing a film having anisotropy of refractive index is not particularly limited. For example, a film is produced from a resin composition (resin mixture) containing a polyimide resin and an acrylic resin showing compatibility, and the film is stretched in at least one direction to impart anisotropy of refractive index. A film satisfying 100×(n1-n2) / n2<1.0 is obtained, for example, by biaxially stretching the film.

[0027] [Polyimide]

[0028] As the polyimide showing compatibility with the acrylic resin, it is preferably soluble in an organic solvent. The polyimide soluble in an organic solvent is preferably soluble in a concentration of 1% by weight or more relative to N,N-dimethylformamide (DMF). In particular, it is preferably soluble in non-amide solvents in addition to amide solvents such as DMF.

[0029] Polyimide is a polymer having a structural unit shown in general formula (I), obtained by dehydrating and cyclizing a polyamic acid obtained by the addition polymerization of tetracarboxylic dianhydride (hereinafter, sometimes described as "acid dianhydride") and diamine. That is, polyimide is a polycondensate of tetracarboxylic dianhydride and diamine, having a structure derived from acid dianhydride (acid dianhydride component) and a structure derived from diamine (diamine component). It should be noted that polyimide can also be synthesized by condensation based on decarboxylation of diisocyanate and acid dianhydride.

[0030]

[0031] In the general formula (I), Y is a divalent organic group, and X is a tetravalent organic group. Y is a diamine residue, which is an organic group obtained by removing two amino groups from a diamine represented by the following general formula (II). X is a tetracarboxylic dianhydride residue, which is an organic group obtained by removing two carboxylic anhydride groups from a tetracarboxylic dianhydride represented by the following general formula (III).

[0032]

[0033] In other words, the polyimide includes a structural unit represented by the following general formula (IIa) and a structural unit represented by the following general formula (IIIa), and has a structural unit represented by the general formula (I) through the imide bond formed by the structure (IIa) derived from the diamine and the structure (IIIa) derived from the tetracarboxylic dianhydride.

[0034]

[0035] The polyimide may contain a structural unit (amide structural unit) represented by the following general formula (IV) in addition to the imide structural unit represented by the general formula (I). A polyimide containing an amide structural unit in addition to the imide structural unit is also referred to as a polyamideimide.

[0036]

[0037] In the general formula (IV), Y and Z are divalent organic groups. As in the general formula (I), Y is a diamine residue. Z is a dicarboxylic acid residue, and is an organic group formed by removing two carboxyl groups from a dicarboxylic acid represented by the following general formula (V). It should be noted that in the synthesis of polyamide-imide, a dicarboxylic acid dichloride represented by the general formula (V') can be preferably used instead of a dicarboxylic acid. A dicarboxylic anhydride can also be used instead of a dicarboxylic acid.

[0038]

[0039] The amide structural unit represented by the general formula (V) is formed by forming an amide bond between the diamine-derived structure represented by the general formula (IIa) and the dicarboxylic acid-derived structure represented by the following general formula (Va). That is, the polyamideimide includes the diamine-derived structure (IIa), the tetracarboxylic dianhydride-derived structure (IIIa) and the dicarboxylic acid-derived structure (Va).

[0040]

[0041] In addition, polyamideimide contains the structure of the following general formula (VI) in which the structure (IIa) derived from a diamine is bonded to both ends of the structure (Va) derived from a dicarboxylic acid.

[0042]

[0043] In the general formula (VI), Y1 and Y2 are diamine residues, and Z1 is a dicarboxylic acid residue. When the [-Y1-NH-CO-Z1-CO-NH-Y2-] portion in the general formula (VI) is regarded as a divalent organic group, the divalent organic group can be regarded as a diamine residue Y containing two amide bonds. That is, the polyimide in which the diamine residue Y in the general formula (I) contains an amide bond is a polyamideimide, and it can be said that polyamideimide is a type of polyimide. Hereinafter, unless otherwise specified, "polyimide" includes "polyamideimide".

[0044] As mentioned above, polyimide can be synthesized by the condensation of tetracarboxylic dianhydride and diamine decarbonation of diisocyanate, etc., except the method of synthesizing by tetracarboxylic dianhydride and diamine via polyamic acid, but no matter in which synthesis method, the obtained polyimide has the structure (tetracarboxylic dianhydride residue) X of the acid dianhydride having four carboxyl groups removed from tetracarboxylic dianhydride and the structure (diamine residue) Y of the diamine having two amino groups removed from diamine. Therefore, even if the starting material for synthesizing polyimide is not tetracarboxylic dianhydride or diamine, the structure equivalent to the tetracarboxylic dianhydride residue contained in the polyimide is expressed as "acid dianhydride component", and the structure equivalent to the diamine residue is expressed as "diamine component". In addition, although dicarboxylic acid derivatives such as dicarboxylic acid dichloride or dicarboxylic anhydride are used in the synthesis of polyamide-imide, the obtained polyamide-imide has the structure Z (dicarboxylic acid residue) formed by removing 2 carboxyl groups from dicarboxylic acid. Therefore, even when the starting material used for synthesis of the polyimide is a dicarboxylic acid derivative, the structure corresponding to the dicarboxylic acid residue is represented as a "dicarboxylic acid component".

[0045] The polyimide may contain a plurality of diamine residues Y, a plurality of tetracarboxylic dianhydride residues X, and a plurality of dicarboxylic acid residues Z. Hereinafter, examples of the diamine component and the tetracarboxylic dianhydride component as monomer units constituting the polyimide and the dicarboxylic acid component when the polyimide is a polyamideimide will be described.

[0046] <Diamine>

[0047] The diamine component of the polyimide is not particularly limited, but preferably contains a diamine having a fluoroalkyl group from the viewpoint of improving compatibility with an acrylic resin. Among the diamines having a fluoroalkyl group, a fluoroalkyl-substituted benzidine is particularly preferred. By containing a fluoroalkyl-substituted benzidine as a diamine component, the solubility and transparency of the polyimide are improved, and the compatibility with an acrylic resin tends to be improved.

[0048] (Fluoroalkyl substituted benzidine)

[0049] Examples of fluoroalkyl-substituted benzidines include 2-fluorobenzidine, 3-fluorobenzidine, 2,3-difluorobenzidine, 2,5-difluorobenzidine, 2,6-difluorobenzidine, 2,3,5-trifluorobenzidine, 2,3,6-trifluorobenzidine, 2,3,5,6-tetrafluorobenzidine, 2,2'-difluorobenzidine, 3,3'-difluorobenzidine, 2,3'-difluorobenzidine, 2,2',3-trifluorobenzidine, 2,3,3'-trifluorobenzidine, 2,2 ',5-trifluorobenzidine, 2,2',6-trifluorobenzidine, 2,3',5-trifluorobenzidine, 2,3',6-trifluorobenzidine, 2,2',3,3'-tetrafluorobenzidine, 2,2',5,5'-tetrafluorobenzidine, 2,2',6,6'-tetrafluorobenzidine, 2,2',3,3',6,6'-hexafluorobenzidine, 2,2',3,3',5,5',6,6'-octafluorobenzidine, 2-(trifluoromethyl)benzidine, 3-(trifluoromethyl)benzidine 2,3-Bis(trifluoromethyl)benzidine, 2,5-Bis(trifluoromethyl)benzidine, 2,6-Bis(trifluoromethyl)benzidine, 2,3,5-Tris(trifluoromethyl)benzidine, 2,3,6-Tris(trifluoromethyl)benzidine, 2,3,5,6-tetrakis(trifluoromethyl)benzidine, 2,2'-Bis(trifluoromethyl)benzidine, 3,3'-Bis(trifluoromethyl)benzidine, 2,3'-Bis(trifluoromethyl)benzidine, 2,2',3-Tris(trifluoromethyl)benzidine 2,3,3'-tris(trifluoromethyl)benzidine, 2,2',5-tris(trifluoromethyl)benzidine, 2,2',6-tris(trifluoromethyl)benzidine, 2,3',5-tris(trifluoromethyl)benzidine, 2,3',6,-tris(trifluoromethyl)benzidine, 2,2',3,3'-tetrakis(trifluoromethyl)benzidine, 2,2',5,5'-tetrakis(trifluoromethyl)benzidine, 2,2',6,6'-tetrakis(trifluoromethyl)benzidine and the like.

[0050] Among the fluoroalkyl-substituted benzidines, the fluoroalkyl group of the fluoroalkyl-substituted benzidine is preferably a perfluoroalkyl group from the viewpoint of taking into account both the solubility and transparency of the polyimide. As the perfluoroalkyl group, a trifluoromethyl group is preferred. Among them, from the viewpoint of the solubility of the polyimide in an organic solvent and the compatibility with an acrylic resin, a perfluoroalkyl-substituted benzidine having a perfluoroalkyl group at the 2-position of the biphenyl is preferred, and 2,2'-bis(trifluoromethyl)benzidine (hereinafter referred to as "TFMB") is particularly preferred. By having a trifluoromethyl group at the 2-position and 2'-position of the biphenyl, in addition to the reduction in the π electron density due to the electron-withdrawing property of the trifluoromethyl group, the bond between the two benzene rings of the biphenyl is twisted due to the steric hindrance of the trifluoromethyl group, and the planarity of the π conjugation is reduced, so that the absorption end wavelength is shifted to a short wavelength, which can reduce the coloring of the polyimide.

[0051] The content of the fluoroalkyl-substituted benzidine is preferably 50 mol% or more, more preferably 60 mol% or more, further preferably 70 mol% or more, and may be 80 mol% or more, 85 mol% or more, or 90 mol% or more relative to the total amount of the diamine component. When the content of the fluoroalkyl-substituted benzidine is relatively large, the compatibility with the acrylic resin is improved, the coloring of the film is suppressed, and the mechanical strength such as the pencil hardness and the elastic modulus tends to be increased.

[0052] (Diamine having an amide bond)

[0053] As the diamine component of the polyimide, a diamine having an amide bond can be used. For example, an amide formed by bonding a diamine to the carboxyl groups at both ends of a dicarboxylic acid is represented by the general formula (VII).

[0054]

[0055] In the general formula (VII), Y is a diamine residue, and Z is a dicarboxylic acid residue. The diamine having an amide structure shown in the general formula (VII) is composed of one dicarboxylic acid (derivative) and two diamines, and therefore, in the calculation of the composition of the polyimide (polyamide-imide), it is regarded as having one dicarboxylic acid residue and two diamine residues. The general formula (VII) shows a structure in which one dicarboxylic acid is condensed with two diamines, but it may be a structure in which two dicarboxylic acids are condensed with three diamines, or it may be a structure in which three or more dicarboxylic acids are condensed with four or more diamines.

[0056] The polyimide containing the diamine having an amide structure represented by the general formula (VII) as the diamine component contains an amide bond in addition to an imide bond, and is therefore equivalent to a polyamideimide. In the synthesis of the polyamideimide, an amide oligomer having an amine terminal can be used instead of a dicarboxylic acid derivative as a monomer to synthesize a polyimide having a structure represented by the general formula (IV) (i.e., a polyamideimide). An amide oligomer having an amine terminal can also be used in combination with a dicarboxylic acid derivative.

[0057] The dicarboxylic acid in the diamine having an amide structure represented by the general formula (VII) is not particularly limited, and various aliphatic dicarboxylic acids, aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and heterocyclic dicarboxylic acids used in the synthesis of polyamide-imide can be applied. The details of the dicarboxylic acid component are described below. In the preparation of a compound having a condensation structure of a diamine and a dicarboxylic acid, a dicarboxylic acid derivative such as a dicarboxylic acid dichloride or a dicarboxylic acid anhydride can also be used instead of a dicarboxylic acid.

[0058] Specific examples of diamines containing a condensation structure of fluoroalkyl-substituted benzidine and dicarboxylic acid include condensates of TFMB and dicarboxylic acid. As dicarboxylic acid, terephthalic acid and / or isophthalic acid are particularly preferred. For example, a diamine in which TFMB is condensed at both ends of terephthalic acid has a structure of the following formula (4).

[0059]

[0060] (Diamine having a fluoroalkyl group)

[0061] Examples of the diamine having a fluoroalkyl group (other than the above-mentioned fluoroalkyl-substituted benzidine) include diamines having an aromatic ring to which a fluoroalkyl group is bonded, such as 1,4-diamino-2-(trifluoromethyl)benzene, 1,4-diamino-2,3-bis(trifluoromethyl)benzene, 1,4-diamino-2,5-bis(trifluoromethyl)benzene, 1,4-diamino-2,6-bis(trifluoromethyl)benzene, 1,4-diamino-2,3,5-tris(trifluoromethyl)benzene, and 1,4-diamino-2,3,5,6-tetrakis(trifluoromethyl)benzene; and diamines having a fluoroalkyl group not directly bonded to an aromatic ring, such as 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis(3-aminophenyl)hexafluoropropane, and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane.

[0062] The polyimide may contain a diamine not containing a fluoroalkyl group as a diamine component. Examples of the diamine component in the polyimide not containing a fluoroalkyl group that exhibits compatibility with an acrylic resin include alicyclic diamines, diamines having a fluorene skeleton, diamines having a sulfone group, and fluorine-containing diamines.

[0063] (Fluorinated diamine)

[0064] Examples of the fluorinated diamines (those not containing a fluoroalkyl group) include 2-fluorobenzidine, 3-fluorobenzidine, 2,3-difluorobenzidine, 2,5-difluorobenzidine, 2,6-difluorobenzidine, 2,3,5-trifluorobenzidine, 2,3,6-trifluorobenzidine, 2,3,5,6-tetrafluorobenzidine, 2,2'-difluorobenzidine, 3,3'-difluorobenzidine, 2,3'-difluorobenzidine, 2,2',3-trifluorobenzidine, 2,3,3'-trifluorobenzidine, 2,2',5-trifluorobenzidine, 2,2',6-trifluorobenzidine, 2,3',5-trifluorobenzidine, 2,3',6-trifluorobenzidine Aniline, 2,2',3,3'-tetrafluorobenzidine, 2,2',5,5'-tetrafluorobenzidine, 2,2',6,6'-tetrafluorobenzidine, 2,2',3,3',6,6'-hexafluorobenzidine, 2,2',3,3',5,5',6,6'-octafluorobenzidine, 1,4-diamino-2-fluorobenzene, 1,4-diamino-2,3-difluorobenzene, 1,4-diamino-2,5-difluorobenzene, 1,4-diamino-2,6-difluorobenzene, 1,4-diamino-2,3,5-trifluorobenzene, 1,4-diamino-2,3,5,6-tetrafluorobenzene, 2,2'-dimethylbenzidine, etc.

[0065] (Alicyclic diamine)

[0066] Examples of the diamine having an alicyclic structure include isophoronediamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(aminomethyl)norbornene, 4,4′-methylenebis(cyclohexylamine), bis(4-aminocyclohexyl)methane, 4,4′-methylenebis(2-methylcyclohexylamine), adamantane-1,3-diamine, 2,6-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,5-bis(aminomethyl)bicyclo[2.2.1]heptane, and 1,1-bis(4-aminophenyl)cyclohexane.

[0067] (Diamine having a fluorene skeleton)

[0068] As an example of the diamine having a fluorene skeleton, 9,9-bis(4-aminophenyl)fluorene can be mentioned.

[0069] (Diamine having a sulfone group)

[0070] Examples of the diamine having a sulfone group include 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]diphenyl sulfone, and 4,4'-bis[4-(4-aminophenoxy)phenoxy]diphenyl sulfone. Among these, diaminodiphenyl sulfones such as 3,3'-diaminodiphenyl sulfone (3,3'-DDS) and 4,4'-diaminodiphenyl sulfone (4,4'-DDS) are preferred.

[0071] (Other diamines)

[0072] Examples of diamines other than those described above include p-phenylenediamine, m-phenylenediamine, o-phenylenediamine, p-xylylenediamine, m-xylylenediamine, o-xylylenediamine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 2-(3-aminophenyl)propane, 2- ... )-2-(4-aminophenyl)propane, 1,1-bis(3-aminophenyl)-1-phenylethane, 1,1-bis(4-aminophenyl)-1-phenylethane, 1-(3-aminophenyl)-1-(4-aminophenyl)-1-phenylethane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminobenzoyl)benzene, 1,3-bis(4-aminobenzoyl)benzene, 1,4-bis(3-aminobenzoyl)benzene, 1,4-bis(4-aminobenzoyl)benzene, 1,3-bis(3-amino-α,α-dimethylbenzyl)benzene, 1,3-bis(4 1,4-bis(3-amino-α,α-dimethylbenzyl)benzene, 1,4-bis(4-amino-α,α-dimethylbenzyl)benzene, 2,6-bis(3-aminophenoxy)benzonitrile, 2,6-bis(3-aminophenoxy)pyridine, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, 2,2- Bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene, 1,3-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,4-bis[4-(3-aminophenoxy)benzoyl]benzene, 1,4-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,3-bis[4-(3-aminophenoxy)-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-aminophenoxy)-α,α-dimethylbenzyl]benzene, 1,4-bis[4-(3-aminophenoxy)-α,α-dimethylbenzyl]benzene, 1,4-bis[4-(4-aminophenoxy)-α,α-dimethylbenzyl] benzene, 4,4'-bis[4-(4-aminophenoxy)benzoyl]diphenyl ether, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]benzophenone, 3,3'-diamino-4,4'-diphenoxybenzophenone, 3,3'-diamino-4,4'-diphenyloxybenzophenone, 3,3'-diamino-4-phenoxybenzophenone, 3,3'-diamino-4-biphenyloxybenzophenone, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane and the like aromatic diamines. ,

[0073] As the diamine, bis(aminomethyl)ether, bis(2-aminoethyl)ether, bis(3-aminopropyl)ether, bis[(2-aminomethoxy)ethyl]ether, bis[2-(2-aminoethoxy)ethyl]ether, bis[2-(3-aminopropoxy)ethyl]ether, 1,2-bis(aminomethoxy)ethane, 1,2-bis(2-aminoethoxy)ethane, 1,2-bis[2-(aminomethoxy)ethoxy]ethane, 1,2-bis[2-(2-aminoethoxy)ethoxy]ethane, ethylene glycol bis(3-aminopropyl)ether, diethylene glycol bis(3-aminopropyl)ether, triethylene glycol bis( 3-aminopropyl) ether, ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1,3-bis(4-aminobutyl)tetramethyldisiloxane, α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminobutyl)polydimethylsiloxane and the like chain diamines.

[0074] <Tetracarboxylic dianhydride>

[0075] The acid dianhydride component of the polyimide is not particularly limited. From the viewpoint of improving compatibility with acrylic resins, the polyimide preferably contains at least one of tetracarboxylic dianhydride having a fluoroalkyl group and alicyclic tetracarboxylic dianhydride as the acid dianhydride component. By containing tetracarboxylic dianhydride having a fluoroalkyl group or alicyclic tetracarboxylic dianhydride as the acid anhydride component, the solubility and transparency of the polyimide are improved, and the compatibility with acrylic resins tends to be improved.

[0076] (Tetracarboxylic dianhydride having a fluoroalkyl group)

[0077] Examples of the tetracarboxylic dianhydride having a fluoroalkyl group include 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]hexafluoropropane dianhydride, 1,4-bis(trifluoromethyl)pyromellitic anhydride, 4-(trifluoromethyl)-1H,3H-benzo[1,2-c:4,5-c']difuran-1,3,5,7-tetraone, 3,6-bis[3',5'-bis(trifluoromethyl)phenyl]pyromellitic anhydride, and 1-(3',5'-bis(trifluoromethyl)phenyl)pyromellitic anhydride. Among them, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA) is particularly preferred from the viewpoint of achieving both transparency and mechanical strength of the polyimide.

[0078] (Alicyclic tetracarboxylic dianhydride)

[0079] Cyclic tetracarboxylic dianhydride is a tetracarboxylic dianhydride having an alicyclic structure. From the viewpoint of transparency of the polyimide and compatibility with an acrylic resin, it is preferred that the alicyclic tetracarboxylic dianhydride does not contain an aromatic ring and that the acid anhydride group is bonded to the alicyclic ring.

[0080] Examples of the alicyclic tetracarboxylic dianhydride include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 1,1'-bicyclohexane-3,3',4,4'tetracarboxylic dianhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride, 2,2'-bisnorbornane-5,5', Among them, from the viewpoint of transparency and mechanical strength of the polyimide, 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA), 1,2,3,4-cyclopentanetetracarboxylic dianhydride (CPDA), 1,2,4,5-cyclohexanetetracarboxylic dianhydride (H-PMDA), 1,1'-bicyclohexane-3,3',4,4'-tetracarboxylic acid-3,4:3',4'-dianhydride (H-BPDA) are preferred, and CBDA is particularly preferred.

[0081] (Other acid dianhydrides)

[0082] Polyimide may also include tetracarboxylic dianhydrides other than the above as acid dianhydride components. As tetracarboxylic dianhydrides other than the above, aromatic tetracarboxylic dianhydrides containing no fluorine atoms may be exemplified. By including aromatic tetracarboxylic dianhydrides containing no fluorine, the compatibility of polyimide resin with acrylic resin is sometimes improved, and the mechanical strength of the film is improved.

[0083] Examples of fluorine-free aromatic tetracarboxylic dianhydrides include: dianhydrides having two anhydride groups bonded to one benzene ring, such as pyromellitic dianhydride and phthalic dianhydride; dianhydrides having two anhydride groups bonded to one condensed polycyclic ring, such as 2,3,6,7-naphthalenetetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, and terphenyltetracarboxylic dianhydride; bis(trimellitic anhydride) esters, 3,3',4,4'-biphenyltetracarboxylic dianhydride, Acid dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, 3,4'-oxydiphthalic anhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidene diphenyloxy) diphthalic anhydride, 5,5'-dimethylmethylenebis(phthalic anhydride), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 11,11-dimethyl -1H-difurano[3,4-b:3',4'-i]xanthene-1,3,7,9(11H)-tetraone, 1,4-bis(3,4-dicarboxyphenoxy)phthalic anhydride, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride, ethylene glycol bis(trimellitic anhydride), N,N'-(9H-fluorene-9-ylidenedi-4,1-phenylene)bis[1,3-di Acid dianhydrides having an acid anhydride group bonded to different aromatic rings include: 1,3-dihydro-1,3-dioxo-5-isobenzofurancarboxamide], 2,2-bis(4-hydroxyphenyl)propane dibenzoate-3,3',4,4'-tetracarboxylic dianhydride, and the like.

[0084] From the viewpoint of transparency and solubility of polyimide and compatibility with acrylic resin, the fluorine-free aromatic tetracarboxylic dianhydride is preferably pyromellitic dianhydride (PMDA), benzimidazole dianhydride (MPDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 4,4'-oxydiphthalic anhydride (ODPA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride (BPADA), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), and bis(trimellitic anhydride) ester.

[0085] Bis(trimellitic anhydride)ester is represented by the following general formula (1).

[0086]

[0087] Q in the general formula (1) is an arbitrary divalent organic group, and carboxyl groups are bonded to carbon atoms of Q at both ends of Q. The carbon atom bonded to the carboxyl group may form a ring structure. Specific examples of the divalent organic group Q include the following (A) to (K).

[0088]

[0089] R in formula (A) 1 is an alkyl group having 1 to 20 carbon atoms, and m is an integer of 0 to 4. The group represented by formula (A) is a group obtained by removing two hydroxyl groups from a hydroquinone derivative which may have a substituent on the benzene ring. Examples of hydroquinone having a substituent on the benzene ring include tert-butyl hydroquinone, 2,5-di-tert-butyl hydroquinone, and 2,5-di-tert-amyl hydroquinone. In the general formula (1), when Q is (A) and m=0 (i.e., there is no substituent on the benzene ring), the bis(trimellitic anhydride) ester is p-phenylene bis(trimellitic anhydride) ester (abbreviated as: TAHQ).

[0090] R in formula (B) 2 is an alkyl group having 1 to 20 carbon atoms, and n is an integer of 0 to 4. The group represented by formula (B) is a group obtained by removing two hydroxyl groups from a biphenol which may have a substituent on the benzene ring. Examples of biphenol derivatives having a substituent on the benzene ring include 2,2'-dimethylbiphenyl-4,4'-diol, 3,3'-dimethylbiphenyl-4,4'-diol, 3,3',5,5'-tetramethylbiphenyl-4,4'-diol, and 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diol.

[0091] The group represented by formula (C) is a group obtained by removing two hydroxyl groups from 4,4'-isopropylidene diphenol (bisphenol A). The group represented by formula (D) is a group obtained by removing two hydroxyl groups from resorcinol.

[0092] p in formula (E) is an integer of 1 to 10. The group represented by formula (E) is a group obtained by removing two hydroxyl groups from a linear diol having 1 to 10 carbon atoms. Examples of the linear diol having 1 to 10 carbon atoms include ethylene glycol and 1,4-butanediol.

[0093] The group represented by the formula (F) is a group obtained by removing two hydroxyl groups from 1,4-cyclohexanedimethanol.

[0094] R in formula (G) 3 is an alkyl group having 1 to 20 carbon atoms, and q is an integer of 0 to 4. The group represented by formula (G) is a group obtained by removing two hydroxyl groups from bisphenol fluorene which may have a substituent on the benzene ring having a phenolic hydroxyl group. Examples of bisphenol fluorene derivatives having a substituent on the benzene ring having a phenolic hydroxyl group include biscresol fluorene and the like.

[0095] Bis(trimellitic anhydride)ester is preferably an aromatic ester. As Q, (A)(B)(C)(D)(G)(H)(I) is preferred among the above (A) to (K). Among them, (A) to (D) are preferred, and a group having a biphenyl skeleton of (B) is particularly preferred. When Q is a group represented by the general formula (B), from the viewpoint of the solubility of the polyimide in an organic solvent, Q is preferably 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diyl represented by the following formula (B1).

[0096]

[0097] The acid dianhydride in which Q in the general formula (1) is a group represented by the formula (B1) is bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)-2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diester (abbreviation: TAAMBP) represented by the following formula (3).

[0098]

[0099] As an example of tetracarboxylic dianhydride other than the above, ethylene tetracarboxylic dianhydride, butane tetracarboxylic dianhydride, etc. are mentioned.

[0100] <Dicarboxylic Acid>

[0101] As described above, dicarboxylic acids or dicarboxylic acid derivatives are used in the preparation of polyimide (polyamide-imide) having an amide structure. Examples of dicarboxylic acids include aliphatic dicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-oxybisbenzoic acid, 4,4'-biphenyldicarboxylic acid, and 2-fluoroterephthalic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-hexahydroterephthalic acid, hexahydroisophthalic acid, 1,3-cyclopentanedicarboxylic acid, and bi(cyclohexyl)-4,4'-dicarboxylic acid; and heterocyclic dicarboxylic acids such as 2,5-thiophenedicarboxylic acid and 2,5-furandicarboxylic acid.

[0102] As the dicarboxylic acid derivative, dicarboxylic acid dichloride, dicarboxylic acid ester, dicarboxylic acid anhydride and the like can be used. Among them, dicarboxylic acid dichloride is preferred because of its high reactivity.

[0103] From the viewpoint of solubility of polyamide-imide and compatibility with acrylic resin, dicarboxylic acid is preferably aromatic dicarboxylic acid and alicyclic dicarboxylic acid, and aromatic dicarboxylic acid is particularly preferred. Among aromatic dicarboxylic acids, terephthalic acid, isophthalic acid, 4,4'-biphenyl dicarboxylic acid, and 4,4'-oxydibenzoic acid are preferred, among which terephthalic acid and isophthalic acid are preferred, and terephthalic acid is particularly preferred. Among alicyclic dicarboxylic acids, 1,4-cyclohexane dicarboxylic acid and bi(cyclohexyl)-4,4'-dicarboxylic acid are preferred, and 1,4-cyclohexane dicarboxylic acid is particularly preferred.

[0104] <Composition of polyimide>

[0105] The polyimide used in the present embodiment has no particular limitation on its composition as long as it is soluble in an organic solvent and is compatible with the acrylic resin, and may be a polyamideimide having an amide bond derived from a dicarboxylic acid component as described above.

[0106] It is preferred that at least one of the diamine and the acid dianhydride in the polyimide contains a fluoroalkyl group. Both the diamine containing a fluoroalkyl group and the acid dianhydride containing a fluoroalkyl group may be used. When at least one of the acid dianhydride and the diamine contains a fluoroalkyl group, there is a tendency to improve the solubility in organic solvents and the compatibility with acrylic resins.

[0107] In particular, since the polyimide exhibits compatibility with acrylic resins in various solvents, it is preferred that the polyimide contain a diamine having a fluoroalkyl group as a diamine component. As described above, the diamine having a fluoroalkyl group is preferably a fluoroalkyl-substituted benzidine such as TFMB.

[0108] The ratio of the diamine having a fluoroalkyl group to the total amount of the diamine component of the polyimide is preferably 50 mol% or more, more preferably 60 mol% or more, further preferably 70 mol% or more, and may be 80 mol% or more, 85 mol% or more, or 90 mol% or more. The amount of the fluoroalkyl-substituted benzidine is preferably within the above range, and the amount of TFMB is particularly preferably within the above range. By increasing the content of the fluoroalkyl-substituted benzidine such as TFMB, the coloring of the film is suppressed, and the mechanical strength such as the pencil hardness or elastic modulus tends to be increased.

[0109] When the polyimide contains a diamine having no fluoroalkyl group as a diamine component, the diamine having no fluoroalkyl group is preferably a diamine having an alicyclic structure, a diamine having an ether structure, a diamine having a fluorene structure, a diamine having a sulfone group, or a diamine having a fluorine-containing group other than a fluoroalkyl group.

[0110] For example, by using diaminodiphenyl sulfone as a diamine in addition to the fluoroalkyl-substituted benzidine, the solubility and transparency of the polyimide resin in the solvent may be improved. On the other hand, if the ratio of diaminodiphenyl sulfone is large, the compatibility with the acrylic resin may be reduced. The content of diaminodiphenyl sulfone may be 1 to 40 mol%, 3 to 30 mol%, or 5 to 25 mol% relative to the total amount of diamine.

[0111] Regardless of whether or not the polyimide contains a diamine having a fluoroalkyl group as a diamine component, it is preferred that the polyimide contains at least one of an acid dianhydride having a fluoroalkyl group and an alicyclic tetracarboxylic dianhydride as an acid dianhydride component.

[0112] When the polyimide does not contain a diamine having a fluoroalkyl group as a diamine component, it is preferred to contain an acid dianhydride having a fluoroalkyl group as an acid dianhydride component from the viewpoint of having compatibility with an acrylic resin. In this case, the ratio of the acid dianhydride having a fluoroalkyl group is preferably 40 mol% or more, more preferably 50 mol% or more, further preferably 60 mol% or more, and may also be 70 mol% or more, 80 mol% or more, or 90 mol% or more, relative to the total amount of the acid dianhydride component of the polyimide. Among them, it is particularly preferred that the amount of 6FDA is within the above range.

[0113] When the polyimide contains a diamine having a fluoroalkyl group as a diamine component, it may not contain an acid dianhydride having a fluoroalkyl group as an acid dianhydride component. Even when the polyimide contains a diamine having a fluoroalkyl group as a diamine component, it may contain an acid dianhydride having a fluoroalkyl group as an acid dianhydride component.

[0114] From the viewpoint of improving the compatibility of the polyimide resin with the acrylic resin, the total content of the tetracarboxylic dianhydride having a fluoroalkyl group and the alicyclic tetracarboxylic dianhydride is preferably 15 mol% or more, more preferably 20 mol% or more, further preferably 25 mol% or more, and may be 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, or 90 mol% or more, relative to the total amount of the acid dianhydride component.

[0115] When the polyimide contains a diamine having a fluoroalkyl group as a diamine component and does not contain an acid dianhydride having a fluoroalkyl group as an acid dianhydride, it is preferred to contain alicyclic tetracarboxylic dianhydride as the acid dianhydride component. The polyimide may also contain a diamine having a fluoroalkyl group as a diamine component, and contain an acid dianhydride having a fluoroalkyl group and an alicyclic tetracarboxylic dianhydride as the acid dianhydride components.

[0116] When the acid dianhydride component includes a tetracarboxylic dianhydride having a fluoroalkyl group and does not include alicyclic tetracarboxylic dianhydride, the content of the tetracarboxylic dianhydride having a fluoroalkyl group is preferably 30 mol% or more, more preferably 35 mol% or more, further preferably 40 mol% or more, and may be 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, or 90 mol% or more relative to the total amount of the acid dianhydride component. The total amount of the acid dianhydride component may also be a tetracarboxylic dianhydride having a fluoroalkyl group.

[0117] When the acid dianhydride component includes alicyclic tetracarboxylic dianhydride and does not include tetracarboxylic dianhydride having a fluoroalkyl group, the content of alicyclic tetracarboxylic dianhydride is preferably 15 mol% or more, more preferably 20 mol% or more, and may be 25 mol% or more or 30 mol% or more relative to the total amount of the acid dianhydride component.

[0118] When tetracarboxylic dianhydride having a fluoroalkyl group and alicyclic tetracarboxylic dianhydride are included as the acid dianhydride components, the total content of the tetracarboxylic dianhydride having a fluoroalkyl group and the alicyclic tetracarboxylic dianhydride is preferably 20 mol% or more, more preferably 25 mol% or more, further preferably 30 mol% or more, and may be 35 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, or 90 mol% or more, relative to the total amount of the acid dianhydride components.

[0119] Whether or not tetracarboxylic dianhydride with fluoroalkyl is included as acid dianhydride component, from the viewpoint of ensuring the solubility of polyimide resin in organic solvent, relative to the total amount of acid dianhydride component, the content of alicyclic tetracarboxylic dianhydride is preferably 80 mol% or less, more preferably 70 mol% or less, further preferably 65 mol% or less, and can also be 60 mol% or less, 55 mol% or less or 50 mol% or less. In order to make acrylic resin compatible with polyimide resin in low-boiling non-amide solvents (for example, halogen solvents such as dichloromethane), relative to the total amount of acid dianhydride component of polyimide, the content of alicyclic tetracarboxylic dianhydride is preferably 45 mol% or less, more preferably 40 mol% or less, and can also be 35 mol% or less. Relative to the total amount of acid dianhydride component of polyimide, the content of alicyclic tetracarboxylic dianhydride can also be 1 mol% or more, 5 mol% or more, 10 mol% or more, 15 mol% or more or 2 mol% or more.

[0120] When alicyclic tetracarboxylic dianhydride is included as an acid dianhydride component, in order to make the polyimide resin compatible with the acrylic resin in an organic solvent, the polyimide preferably includes a tetracarboxylic dianhydride with a fluoroalkyl group and / or a fluorine-free aromatic tetracarboxylic dianhydride as an acid dianhydride component in addition to alicyclic tetracarboxylic dianhydride. As described above, as alicyclic tetracarboxylic dianhydride, CBDA is preferred, as a tetracarboxylic dianhydride with a fluoroalkyl group, 6FDA is preferred, as a fluorine-free aromatic tetracarboxylic dianhydride, PMDA, MPDA, BPDA, ODPA, BTDA, BPADA, BPAF, bis (trimellitic anhydride) ester are preferred. As bis (trimellitic anhydride) ester, TAHQ and TAMBP are preferred, and TAMBP is particularly preferred.

[0121] When tetracarboxylic dianhydride having a fluoroalkyl group is included as an acid dianhydride component, even if the total amount of the acid dianhydride is tetracarboxylic dianhydride having a fluoroalkyl group, the polyimide resin and the acrylic resin can be compatible in an organic solvent. In order to make the acrylic resin and the polyimide resin compatible in a low-boiling non-amide solvent (for example, a halogen solvent such as dichloromethane), the content of the tetracarboxylic dianhydride having a fluoroalkyl group is preferably 90 mol% or less, more preferably 85 mol% or less, and can also be 80 mol% or less, 70 mol% or less, 65 mol% or less, or 60 mol% or less.

[0122] When the acid dianhydride component includes a tetracarboxylic dianhydride having a fluoroalkyl group but does not include alicyclic tetracarboxylic dianhydride, in order to make the acrylic resin and the polyimide resin compatible in a low-boiling non-amide solvent, the content of the tetracarboxylic dianhydride having a fluoroalkyl group is preferably 30 to 90 mol%, more preferably 35 to 80 mol%, and further preferably 40 to 75 mol% relative to the total amount of the acid dianhydride component. From the same point of view, the content of the aromatic tetracarboxylic dianhydride without fluorine is preferably 10 to 70 mol%, more preferably 20 to 65 mol%, and further preferably 25 to 60 mol% relative to the total amount of the acid dianhydride component. As described above, as the tetracarboxylic dianhydride having a fluoroalkyl group, 6FDA is preferred, and as the aromatic tetracarboxylic dianhydride without fluorine, PMDA, MPDA, BPDA, ODPA, BTDA, BPADA, BPAF, and bis(trimellitic anhydride) ester are preferred. As bis(trimellitic anhydride) ester, TAHQ and TAMBP are preferred, and TAMBP is particularly preferred.

[0123] When the polyimide includes a dicarboxylic acid-derived structure represented by the general formula (Va), that is, when it is a polyamide-imide, the total amount of the structure derived from the tetracarboxylic dianhydride represented by the general formula (IIIa) and the dicarboxylic acid-derived structure represented by the general formula (Va) is preferably 90 to 110 parts by mole relative to 100 parts by mole of the diamine-derived structure represented by the general formula (IIa). The total amount of the structure of the general formula (IIa) and the structure of the general formula (Va) may be 93 to 107 parts by mole, 95 to 105 parts by mole, 97 to 103 parts by mole, or 99 to 101 parts by mole relative to 100 parts by mole of the structure of the general formula (IIa).

[0124] In the polyamide-imide, the ratio of the structure of the general formula (Va) is preferably 1 to 70 mol%, more preferably 2 to 60 mol%, further preferably 3 to 50 mol%, and may be 5 to 45 mol% or 10 to 40 mol% relative to the total of the structure of the general formula (IIIa) and the structure of the general formula (Va). The ratio of the structure of the general formula (II) to the structure of the general formula (Va) is roughly equal to the ratio of the imide structure of the general formula (I) to the amide structure of the general formula (IV). The higher the ratio of the structure derived from dicarboxylic acid of the general formula (Va), that is, the higher the ratio of the amide structure, the higher the solubility of the polyamide-imide in the organic solvent. If the ratio of the structure derived from dicarboxylic acid of the general formula (Va) is 70 mol% or less, excellent compatibility can be shown for acrylic resin. From the perspective of compatibility with acrylic resin and mechanical strength of the film, the ratio of the structure derived from dicarboxylic acid is preferably 50 mol% or less.

[0125] As described above, as the dicarboxylic acid component of the polyamideimide, terephthalic acid, isophthalic acid, 4,4'-biphenyldicarboxylic acid, 4,4'-oxydibenzoic acid, 1,4-cyclohexanedicarboxylic acid and bi(cyclohexyl)-4,4'-dicarboxylic acid are preferred. Among them, terephthalic acid and isophthalic acid are preferred, and terephthalic acid is particularly preferred.

[0126] Polyamide-imide preferably contains one or more of these dicarboxylic acids as dicarboxylic acid components. Relative to the total amount of dicarboxylic acid components of polyamide-imide, the total amount of terephthalic acid, isophthalic acid, 4,4'-biphenyl dicarboxylic acid, 4,4'-oxydibenzoic acid, 1,4-cyclohexane dicarboxylic acid and bi (cyclohexyl) -4,4'- dicarboxylic acid is preferably 50 mol% or more, more preferably 60 mol% or more, further preferably 70 mol% or more, and can also be 75 mol% or more, 80 mol% or more, 85 mol% or more, 90 mol% or more or 95 mol% or more. Relative to the total amount of dicarboxylic acid components of polyamide-imide, the total amount of terephthalic acid and isophthalic acid can also be 50 mol% or more, 60 mol% or more, 70 mol% or more, 75 mol% or more, 80 mol% or more, 85 mol% or more, 90 mol% or more or 95 mol% or more, and the amount of terephthalic acid can also be this range.

[0127] When the polyimide is a polyamide-imide having a structure derived from a dicarboxylic acid represented by the general formula (Va), it is preferred that at least one of the diamine and the acid dianhydride has a fluoroalkyl group from the viewpoint of solubility in an organic solvent and compatibility with an acrylic resin. The polyamide-imide preferably contains a diamine having a fluoroalkyl group as a diamine component, and preferably contains a fluoroalkyl-substituted benzidine such as TFMB.

[0128] The ratio of the fluoroalkyl-substituted benzidine is preferably 30 mol% or more relative to the total amount of the diamine components of the polyamideimide. In other words, it is preferred that 30% or more of the diamine residues Y contained in the polyamideimide are structural units in which at least one hydrogen atom on the benzene ring of 4,4'-biphenylene is substituted by a fluoroalkyl group. The ratio of the diamine having a fluoroalkyl group relative to the total amount of the diamine components of the polyamideimide is more preferably 50 mol% or more, further preferably 70 mol% or more, and may also be 80 mol% or more, 85 mol% or more, or 90 mol% or more. It is particularly preferred that the amount of TFMB is within the above range relative to the total amount of the diamine components.

[0129] When the polyimide is a polyamideimide containing a structure derived from a dicarboxylic acid represented by general formula (Va), it preferably contains at least one of an acid dianhydride having a fluoroalkyl group and an alicyclic tetracarboxylic dianhydride as the acid dianhydride component from the viewpoint of solubility in an organic solvent and compatibility with an acrylic resin.

[0130] <Preparation of polyimide>

[0131] The method for producing polyamide-imide is not particularly limited. In general, polyamic acid, which is a polyimide precursor, is produced by reaction between diamine and tetracarboxylic dianhydride, and polyimide is obtained by dehydration cyclization (imidization) of the polyamic acid.

[0132] The preparation method of polyamic acid is not particularly limited, and any known method can be applied. For example, diamine and tetracarboxylic dianhydride are dissolved in an organic solvent with approximately equal molar amounts (95: 100 to 105: 100 molar ratio) and stirred to obtain a polyamic acid solution. The concentration of the polyamic acid solution is generally 5 to 35 weight %, preferably 10 to 30 weight %. At a concentration in this range, the polyamic acid obtained by polymerization has an appropriate molecular weight, and the polyamic acid solution has an appropriate viscosity.

[0133] When preparing polyamideimide, in addition to diamine and tetracarboxylic dianhydride, dicarboxylic acid or its derivative (dicarboxylic acid dichloride, dicarboxylic acid anhydride, etc.) can also be used as a monomer to prepare polyamideimide. In this case, the amount of each monomer can be adjusted so that the total amount of tetracarboxylic dianhydride and dicarboxylic acid or its derivative becomes a molar amount roughly equivalent to that of diamine.

[0134] In order to suppress the ring opening of the acid dianhydride during the polymerization of the polyamic acid, it is preferred to add the acid dianhydride and the dicarboxylic acid or its derivative to the diamine. When adding multiple diamines, multiple acid dianhydrides, multiple dicarboxylic acids or their derivatives, they can be added at one time or in multiple times. The physical properties of the polyimide can be controlled by adjusting the order of adding the monomers.

[0135] In the preparation of the polyamic acid, a method of adding the remaining monomers to an oligomer prepared by preliminarily polymerizing a part of the monomers and polymerizing the oligomer may be adopted. Examples of the oligomer include the above-mentioned amine-terminated oligomers.

[0136] The organic solvent used in the polymerization of polyamic acid is not particularly limited as long as it is a solvent that does not react with the monomer and can dissolve polyamic acid. As an organic solvent, urea solvents such as methyl urea, N, N-dimethylethyl urea, dimethyl sulfoxide, diphenyl sulfone, tetramethyl sulfone and other sulfoxide or sulfone solvents, N, N-dimethylacetamide (DMAc), N, N-dimethylformamide (DMF), N, N'-diethylacetamide, N-methyl-2-pyrrolidone (NMP), γ-butyrolactone, hexamethylphosphoric acid triamide and other amide solvents, chloroform, dichloromethane and other halogenated alkyl solvents, benzene, toluene and other aromatic hydrocarbon solvents, tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, dimethyl ether, diethyl ether, p-cresol methyl ether and other ether solvents can be listed. These solvents are usually used alone or in combination as needed. Two or more. From the viewpoint of the solubility and polymerization reactivity of polyamic acid, DMAc, DMF, NMP and the like can be preferably used.

[0137] Polyimide is obtained by dehydration cyclization of polyamic acid. As a method for preparing polyimide from polyamic acid solution, a method for imidization in a solution by adding a dehydrating agent, an imidization catalyst, etc. in a polyamic acid solution can be cited. In order to promote the progress of imidization, the polyamic acid solution can be heated. The solution containing the polyimide generated by the imidization of polyamic acid is mixed with a poor solvent, so that the polyimide resin is precipitated in the form of a solid. By separating the polyimide resin in the form of a solid, the impurities generated during the synthesis of polyamic acid, or the residual dehydrating agent and imidization catalyst, etc. can be cleaned and removed using a poor solvent, and the coloring or yellowness of the polyimide can be prevented from rising. In addition, by separating the polyimide resin in the form of a solid, when preparing a solution for making a film, a solvent suitable for filmization such as a low boiling point solvent can be applied.

[0138] The molecular weight of the polyimide (weight average molecular weight in terms of polyethylene oxide measured by gel permeation chromatography (GPC)) is preferably 10,000 to 300,000, more preferably 20,000 to 250,000, and further preferably 40,000 to 200,000. When the molecular weight is too small, the strength of the film may be insufficient. When the molecular weight is too large, the compatibility with the acrylic resin may be poor.

[0139] The polyimide resin is preferably soluble in a non-amide solvent such as a ketone solvent or a halogenated alkyl solvent. The polyimide resin showing solubility in a solvent means dissolving at a concentration of 5% by weight or more. In one embodiment, the polyimide resin shows solubility in dichloromethane. Dichloromethane has a low boiling point, and it is relatively easy to remove the residual solvent when making a film. Therefore, by using a polyimide resin soluble in dichloromethane, it can be expected that the productivity of the film can be improved.

[0140] From the viewpoint of thermal stability and light stability of the resin composition and the film, the polyimide preferably has a lower reactivity. The acid value of the polyimide is preferably 0.4mmol / g or less, more preferably 0.3mmol / g or less, and further preferably 0.2mmol / g or less. The acid value of the polyimide may also be 0.1mmol / g or less, 0.05mmol / g or less, or 0.03mmol / g or less. From the viewpoint of reducing the acid value, the polyimide preferably has a higher imidization rate. The imidization rate of the polyimide is preferably 93% or more, more preferably 95% or more, further preferably 97% or more, and may also be 98% or more, or 99% or more. By making the acid value smaller, the stability of the polyimide can be improved, and there is a tendency to improve the compatibility with the acrylic resin.

[0141] [Acrylic resin]

[0142] Examples of acrylic resins include poly(meth)acrylates such as polymethyl methacrylate, methyl methacrylate-(meth)acrylic acid copolymers, methyl methacrylate-(meth)acrylic acid ester copolymers, methyl methacrylate-(meth)acrylic acid ester copolymers, methyl methacrylate-acrylic acid ester-(meth)acrylic acid copolymers, and methyl (meth)acrylate-styrene copolymers. The stereoregularity of the polymer is not particularly limited, and may be any of isotactic, syndiotactic, and atactic.

[0143] From the viewpoint of transparency, compatibility with polyamide-imide, and mechanical strength of the film, the acrylic resin preferably has methyl methacrylate as a main structural unit. The amount of methyl methacrylate in the acrylic resin relative to the total amount of monomer components is preferably 60% by weight or more, and may be 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. The acrylic resin may be a homopolymer of methyl methacrylate.

[0144] The acrylic resin may be one in which an imide structure or a lactone ring structure is introduced. Such a modified polymer is preferably one in which an imide structure or a lactone ring structure is introduced into an acrylic polymer having a methyl methacrylate content within the above range. That is, in the acrylic resin modified by introducing an imide structure or a lactone ring structure, the total amount of methyl methacrylate and the modified structure of methyl methacrylate is preferably 60% by weight or more, and may also be 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. The modified polymer may also be one in which an imide structure or a lactone ring structure is introduced into a homopolymer of methyl methacrylate.

[0145] By introducing an imide structure into an acrylic polymer such as methyl methacrylate, there is a tendency to increase the glass transition temperature of the acrylic resin. In addition, when the acrylic resin contains an imide structure, the compatibility with polyimide is sometimes improved. For example, although polyamide-imide having a large ratio of a structure derived from dicarboxylic acid (ratio of amide structure) sometimes has poor compatibility with acrylic resin, acrylic resin having an imide structure also shows excellent compatibility with polyamide-imide having a high ratio of a structure derived from dicarboxylic acid.

[0146] The acrylic resin having a glutarimide structure can be obtained by heating and melting a polymethyl methacrylate resin and treating it with an imidizing agent, as described in Japanese Patent Application Publication No. 2010-261025. Commercially available products such as "PLEXIMID TT70" and "PLEXIMID 8805" manufactured by EVONIK can also be used as imide-modified polymethyl methacrylate.

[0147] When the acrylic resin has a glutarimide structure, the glutarimide content may be 3% by weight or more, 10% by weight or more, 20% by weight or more, 30% by weight or more, or 50% by weight or more. The greater the glutarimide content, the easier it is to show compatibility with polyamide-imide having a high ratio of the structure of the general formula (Va) (high ratio of amide structure).

[0148] The glutarimide content is calculated as follows: 1 The introduction rate (imidization rate) of the glutarimide structure is determined from the H-NMR spectrum, and the imidization rate is converted by weight. For example, in methyl methacrylate into which the glutarimide structure is introduced, the imidization rate Im=B / (A+B) is determined from the area A of the peak (near 3.5 to 3.8 ppm) derived from the O-CH3 proton of methyl methacrylate and the area B of the peak (near 3.0 to 3.3 ppm) derived from the N-CH3 proton of glutarimide.

[0149] From the viewpoint of heat resistance of the resin composition and the film, the glass transition temperature of the acrylic resin is preferably 80°C or higher, more preferably 90°C or higher, further preferably 100°C or higher, and may be 110°C or higher, 115°C or higher, or 120°C or higher.

[0150] From the viewpoint of solubility in organic solvents, compatibility with the above-mentioned polyamide-imide and mechanical strength of the film, the weight average molecular weight (polystyrene equivalent) of the acrylic resin is preferably 5,000 to 5,000,000, more preferably 10,000 to 2,000,000, further preferably 15,000 to 1,000,000, and may be 20,000 to 500,000, 30,000 to 300,000 or 50,000 to 200,000.

[0151] From the viewpoint of thermal stability and light stability of resin composition and film, acrylic resin preferably has less content of reactive functional groups such as ethylenically unsaturated groups and carboxyl groups. The iodine value of acrylic resin is preferably 10.16g / 100g (0.4mmol / g) or less, more preferably 7.62g / 100g (0.3mmol / g) or less, and further preferably 5.08g / 100g (0.2mmol / g) or less. The iodine value of acrylic resin can also be 2.54g / 100g (0.1mmol / g) or less or 1.27g / 100g (0.05mmol / g) or less. The acid value of acrylic resin is preferably 0.4mmol / g or less, more preferably 0.3mmol / g or less, and further preferably 0.2mmol / g or less. The acid value of acrylic resin can also be 0.1mmol / g or less, 0.05mmol / g or less or 0.03mmol / g or less. By reducing the acid value, the stability of the acrylic resin tends to be improved, and the compatibility with the polyimide tends to be enhanced.

[0152] [Resin composition]

[0153] By mixing the above-mentioned polyimide resin with an acrylic resin, a resin composition containing a polyimide resin and an acrylic resin can be obtained. The above-mentioned polyimide resin and acrylic resin can show compatibility in any ratio, so the ratio of the polyimide resin to the acrylic resin in the resin composition is not particularly limited. The mixing ratio (weight ratio) of the polyimide resin and the acrylic resin can be 98:2 to 2:98, 95:5 to 10:90, or 90:10 to 15:85. The higher the ratio of the polyimide resin, the higher the elastic modulus and pencil hardness of the film, the excellent mechanical strength, and the tendency that the tensile elastic modulus and bending resistance generated by stretching become significantly improved. The higher the ratio of the acrylic resin, the less coloring of the film and the higher the transparency, and the glass transition temperature becomes lower, and the processability of the film such as stretching tends to improve.

[0154] In order to give full play to the effect of improving transparency and processability brought about by mixing the polyimide resin and the acrylic resin, the ratio of the acrylic resin is preferably 10% by weight or more relative to the total of the polyimide resin and the acrylic resin, and may be 15% by weight or more, 20% by weight or more, 25% by weight or more, 30% by weight or more, 35% by weight or more, 40% by weight or more, 45% by weight or more, 50% by weight or more, 60% by weight or more, or 70% by weight or more. On the other hand, from the viewpoint of obtaining a film with excellent mechanical strength, the ratio of the polyimide resin is preferably 10% by weight or more relative to the total of the polyimide resin and the acrylic resin, more preferably 20% by weight or more, further preferably 30% by weight or more, and may be 40% by weight or more, 50% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, or 80% by weight or more.

[0155] Polyimide is a polymer having a special molecular structure. Generally speaking, it has low solubility in organic solvents and is not compatible with other polymers. However, as mentioned above, polyimide containing specific diamine components and acid dianhydride components has high solubility in organic solvents and is compatible with acrylic resins.

[0156] The resin composition comprising the polyimide resin and the acrylic resin preferably has a single glass transition temperature in differential scanning calorimetry (DSC) and / or dynamic viscoelasticity measurement (DMA). When the resin composition has a single glass transition temperature, it can be considered that the polyimide resin and the acrylic resin are completely compatible. The film comprising the polyimide resin and the acrylic resin also preferably has a single glass transition temperature.

[0157] From the viewpoint of heat resistance, the glass transition temperature of the resin composition and the film is preferably 110° C. or higher, and may be 115° C. or higher, 120° C. or higher, 125° C. or higher, 130° C. or higher, 135° C. or higher, 140° C. or higher, 145° C. or higher, or 150° C. or higher. On the other hand, from the viewpoint of processability such as stretching, the glass transition temperature of the resin composition and the film is preferably lower than 250° C., and may be 240° C. or lower, 230° C. or lower, 220° C. or lower, or 210° C. or lower.

[0158] The resin composition may be a mixture of only the polyimide resin and the acrylic resin precipitated as a solid component, or may be a mixture of the polyimide resin and the acrylic resin. In addition, when a polyimide solution is mixed with a poor solvent to precipitate the polyimide resin, an acrylic resin may be mixed in the solution to precipitate the resin composition mixed with the polyimide and the acrylic resin as a solid (powder).

[0159] The resin composition may also be a mixed solution comprising a polyimide resin and an acrylic resin. The resin mixing method is not particularly limited, and the resins may be mixed in a solid state or in a liquid to form a mixed solution. A polyimide solution and an acrylic resin solution may be prepared separately, and the two may be mixed to prepare a mixed solution of polyimide and acrylic resin.

[0160] The solvent of the solution containing the polyimide resin and the acrylic resin is not particularly limited as long as it is soluble in both the polyimide resin and the acrylic resin. Examples of the solvent include: amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; ether solvents such as tetrahydrofuran and 1,4-dioxane; ketone solvents such as acetone, methyl ethyl ketone, methyl acetone, methyl isopropyl ketone, methyl isobutyl ketone, diethyl ketone, cyclopentanone, cyclohexanone, and methylcyclohexanone; and halogenated alkyl solvents such as chloroform, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, chlorobenzene, dichlorobenzene, and dichloromethane.

[0161] From the viewpoint of solubility of polyimide resin and compatibility of polyimide resin and acrylic resin in solution, amide solvents are preferred. On the other hand, from the viewpoint of solvent removal during film production, low-boiling-point non-amide solvents are preferred, and ketone solvents and alkyl halide solvents are preferred from the viewpoint of excellent solubility in both polyimide resin and acrylic resin and low boiling point, and easy removal of residual solvent during film production.

[0162] For the purpose of improving the processability of the film or imparting various functions, organic or inorganic low molecular weight compounds, polymer compounds (such as epoxy resins), etc. can be mixed in the resin composition (solution). The resin composition may include flame retardants, ultraviolet absorbers, crosslinking agents, dyes, pigments, surfactants, leveling agents, plasticizers, microparticles, sensitizers, etc. Microparticles include organic microparticles such as polystyrene and polytetrafluoroethylene, inorganic microparticles such as colloidal silica, carbon, and layered silicates, etc., which may be porous or hollow structures. Fiber-reinforced materials include carbon fibers, glass fibers, aromatic polyamide fibers, etc.

[0163] [film]

[0164] <Film Forming>

[0165] The film comprising polyimide resin and acrylic resin can be manufactured by known methods such as melting method and solution method. As mentioned above, polyimide resin and acrylic resin can be mixed in advance or mixed when thin film is formed. It is also possible to use a composite formed by kneading polyimide resin and acrylic resin.

[0166] The resin composition containing polyimide resin and acrylic resin tends to have a lower melt viscosity than the case of polyimide alone, and has excellent formability such as melt extrusion molding. In addition, the solution of the resin composition containing polyimide resin and acrylic resin tends to have a lower solution viscosity than the solution of polyimide resin alone at the same solid content concentration. Therefore, the solution has excellent operability such as transportation, and has high coating properties, which is conducive to reducing uneven thickness of the film.

[0167] As mentioned above, the film can be formed by a melting method or a solution method. From the perspective of producing a film having excellent transparency and uniformity, the solution method is preferred. In the solution method, a film can be obtained by applying the solution containing the polyimide resin and the acrylic resin on a support and removing the solvent by drying.

[0168] As a method for coating the resin solution on a support, a known method using a rod coater or a comma coater can be applied. A glass substrate, a metal substrate such as SUS, a metal roller, a metal belt, a plastic film, etc. can be used as a support. From the viewpoint of improving productivity, it is preferred to use an annular support such as a metal roller, a metal belt, or a long plastic film as a support, and manufacture the film by a roll-to-roll method. When using a plastic film as a support, a material that is insoluble in the solvent doped with the film can be appropriately selected.

[0169] It is preferred to heat when drying the solvent. The heating temperature is not particularly limited, as long as it is a temperature that can remove the solvent and suppress the coloring of the resulting film, and is appropriately set at about room temperature to 250°C, preferably 50°C to 220°C. The heating temperature can be increased in stages. In order to improve the removal efficiency of the solvent, the resin film can be peeled off from the support and dried after a certain degree of drying. In order to promote the removal of the solvent, heating can be performed under reduced pressure.

[0170] <Stretch>

[0171] The film immediately after film formation (in the case of the solution method, after the solvent is dried) is an unstretched film and generally has no refractive index anisotropy. By stretching the film in at least one direction, the refractive index anisotropy within the film plane becomes larger and the mechanical strength of the film tends to be improved.

[0172] The film stretching conditions are not particularly limited, and may be a method of stretching the film in the conveying direction between a pair of rollers with different rotation speeds (free-end uniaxial stretching), a method of fixing both ends of the film in the width direction with pins or clamps and stretching in the width direction (fixed-end uniaxial stretching), etc. Biaxial stretching may also be performed, such as sequential biaxial stretching in which fixed-end uniaxial stretching is performed after free-end uniaxial stretching, or biaxial stretching is performed simultaneously in the conveying direction and the width direction while fixing both ends of the film in the width direction.

[0173] In order to obtain a small in-plane refractive index difference (in-plane birefringence) n1-n2 and an in-plane average refractive index n H The difference between the refractive index n3 in the thickness direction (out-of-plane birefringence) n H -n3 larger film is preferably biaxially stretched. In biaxial stretching, the stretching ratio in one direction and the stretching ratio in the orthogonal direction may be the same or different. By making the difference between the stretching ratio in one direction and the stretching ratio in the orthogonal direction smaller, there is a tendency for n1-n2 to become smaller.

[0174] Generally speaking, the film comprising polyimide resin and acrylic resin has a tendency that the refractive index in the stretching direction becomes larger. In the compatible system of polyimide resin and acrylic resin, the stretching elastic modulus in the stretching direction of the film becomes larger, and the rise of the stretching elastic modulus when the stretching ratio is increased is remarkable. In addition, by the stretching of the film, there is a tendency that the bending resistance in the stretching direction (bending resistance when the direction orthogonal to the stretching direction is used as the bending axis) is improved.

[0175] In the direction orthogonal to the stretching direction, there is a tendency for the stretching elastic modulus to become smaller than before stretching (unstretched film). If the film is biaxially stretched, both the refractive index n1 in one direction in the plane and the refractive index n2 in the direction orthogonal thereto become larger, and the refractive index n3 in the thickness direction becomes smaller than before stretching. As a result, the tensile elastic modulus of the obtained film in all directions in the plane becomes larger, and the bending resistance is higher when any direction is set as the bending axis.

[0176] The heating temperature during stretching is not particularly limited, and may be set, for example, within the range of about ±40° C. of the glass transition temperature of the film. The lower the stretching temperature, the greater the refractive index anisotropy of the film. In addition, the greater the stretching ratio, the greater the refractive index anisotropy of the film.

[0177] From the viewpoint of suppressing the coloring of the film caused by heating during stretching and obtaining a film with high transparency (low yellowness), the stretching temperature is preferably lower than 250°C, more preferably lower than 245°C, and may be lower than 240°C, lower than 230°C, lower than 225°C, lower than 220°C, lower than 215°C, lower than 210°C, lower than 205°C, lower than 200°C, lower than 195°C, or lower than 190°C. The glass transition temperature of the resin composition of the compatible system of the polyimide resin and the acrylic resin is lower than that of the single polyimide resin, and therefore it has good stretching processability even at a temperature lower than 250°C.

[0178] From the viewpoint of suppressing an increase in the haze of the film due to stretching, the stretching temperature is preferably 100°C or higher, more preferably 110°C or higher, and may be 120°C or higher, 130°C or higher, 140°C or higher, 150°C or higher, 160°C or higher, 170°C or higher, or 180°C or higher.

[0179] The stretching ratio can be expressed as the out-of-plane birefringence n of the stretched film. H -n3 is set to be greater than 0.0140. The stretching ratio is, for example, 1 to 300%, or may be greater than 5%, greater than 10%, greater than 30%, greater than 50%, greater than 70%, greater than 90%, or greater than 120%, or may be less than 250%, less than 200%, or less than 150%. It should be noted that the stretching ratio (%) is expressed as 100×(L1-L0) / L0, where L0 is the length of the film in the stretching direction before stretching (original length), and L1 is the length of the film in the stretching direction after stretching. In biaxial stretching, at a stretching ratio smaller than that of uniaxial stretching, n H -n3 tends to increase.

[0180] [Thin film properties]

[0181] The thickness of the film is not particularly limited and can be appropriately set according to the purpose. The thickness of the film (thickness after stretching) is, for example, 5 to 300 μm. From the perspective of taking into account both self-supporting properties and flexibility and making a film with higher transparency, the thickness of the film is preferably 20 μm to 100 μm, and may also be 30 μm to 90 μm, 40 μm to 85 μm, or 50 μm to 80 μm. The thickness of the film used as a cover film for a display is preferably 30 μm or more, more preferably 40 μm or more, and may also be 50 μm or more.

[0182] As mentioned above, the stretched film has anisotropy of refractive index, and the average refractive index n in the film plane is H The difference n between the refractive index n3 in the thickness direction of the film H -n3 is 0.0140 or more. The average refractive index n in the film surface HIt is the average value of the refractive index n1 in the first direction where the refractive index is the largest within the film plane and the refractive index n2 in the second direction orthogonal to the first direction within the film plane.

[0183] The direction of the maximum refractive index in the plane (first direction) is determined using a phase difference meter. The slow axis direction determined by the phase difference measurement is the first direction. The refractive index n1 in the first direction, the refractive index n2 in the second direction, and the refractive index n3 in the thickness direction are measured values ​​obtained using the prism coupling method. The refractive index n3 in the thickness direction is the average value of the refractive index in the thickness direction on the cross section orthogonal to the first direction and the cross section orthogonal to the second direction.

[0184] The larger the stretching ratio, the higher the molecular orientation in the film plane. H The difference between the refractive index n3 in the thickness direction of the film is the out-of-plane birefringence n H -n3 has a tendency to be larger. H -n3 may be 0.0145 or more, 0.0150 or more, 0.0155 or more, or 0.0160 or more, or 0.018 or more, 0.020 or more, 0.022 or more, 0.024 or more, or 0.025 or more. H -n3 may be 0.080 or less, 0.060 or less, 0.050 or less, or 0.045 or less.

[0185] The index of the refractive index anisotropy in the plane of the film R (%): 100 × (n1-n2) / n2 is preferably less than 1.0%, and can also be less than 0.9%, less than 0.8%, less than 0.7% or less than 0.6%. The smaller R is, the smaller the anisotropy of the mechanical strength in the film plane is, and there is a tendency to show excellent mechanical strength in all directions in the plane. As described above, by biaxially stretching the film, there is a tendency for the anisotropy of the refractive index in the film plane to become smaller, and there is a tendency for R to be smaller as the difference in the stretching ratio in a direction orthogonal to one direction is smaller.

[0186] The total light transmittance of the film is preferably 85% or more, more preferably 86% or more, further preferably 87% or more, and may be 88% or more, 89% or more, 90% or more, or 91% or more. The haze of the film is preferably 10% or less, more preferably 5% or less, further preferably 4% or less, and may be 3.5% or less, 3% or less, 2% or less, or 1% or less. In the compatible system of polyimide resin and acrylic resin, even if n is used as the H Even when the film is stretched so that -n3 is 0.0140 or more, high transparency is maintained, so that a transparent film with high total light transmittance and low haze can be obtained.

[0187] From the viewpoint of intensity, it is preferred that the tensile modulus of elasticity in the first direction and the tensile modulus of elasticity in the second direction are more than 3.5GPa. The tensile modulus of elasticity in the first direction and the second direction is more preferably more than 3.7GPa, and can also be more than 3.9GPa or more than 4.0GPa. The difference of the tensile modulus of elasticity in the first direction and the tensile modulus of elasticity in the second direction can also be less than 2.0GPa, less than 1.5GPa, less than 1.2GPa, less than 1.0GPa, less than 0.8GPa, less than 0.6GPa or less than 0.5GPa. By biaxial stretching, there is a tendency that the difference of the tensile modulus of elasticity in the first direction and the second direction diminishes.

[0188] From the viewpoint of intensity, it is preferred that the tensile modulus of elasticity in the first direction and the tensile modulus of elasticity in the second direction are more than 3.5GPa. The tensile modulus of elasticity in the first direction and the second direction is more preferably more than 3.7GPa, and can also be more than 3.9GPa or more than 4.0GPa. The difference of the tensile modulus of elasticity in the first direction and the tensile modulus of elasticity in the second direction can also be less than 2.0GPa, less than 1.5GPa, less than 1.2GPa, less than 1.0GPa, less than 0.8GPa, less than 0.6GPa or less than 0.5GPa. By biaxial stretching, there is a tendency that the difference of the tensile modulus of elasticity in the first direction and the second direction diminishes.

[0189] The unstretched film formed from a resin composition comprising a polyimide resin and an acrylic resin has a smaller tensile elastic modulus than a film of a single polyimide resin. However, when a film of a compatible system of a polyimide resin and an acrylic resin is stretched, the tensile elastic modulus increases significantly, thereby achieving a high tensile elastic modulus comparable to or exceeding that of a film of a single polyimide resin.

[0190] The pencil hardness of the film is preferably F or more, and may be H or more or 2H or more. In a compatible system of polyimide resin and acrylic resin, the pencil hardness is not easily reduced even if the ratio of acrylic resin is increased, and the pencil hardness does not change significantly even if it is stretched. Therefore, a film with less coloring and excellent transparency can be obtained without reducing the excellent mechanical strength unique to polyimide.

[0191] Under the conditions of a bending radius of 1.0 mm, a bending angle of 180°, and a bending speed of 1 time / second, the bending resistance number of the film during a dynamic bending test of repeated bending (the number of bending times until the film cracks or breaks) is preferably 100,000 times or more, and may also be 150,000 times or more or 200,000 times or more. By stretching the film, the bending resistance in the stretching direction is improved, so the bending resistance number during the dynamic bending test with the direction orthogonal to the stretching direction as the bending axis is greatly increased compared to the bending resistance number of the unstretched film.

[0192] For the film, the number of bending resistances when the dynamic bending test is performed with the second direction as the bending axis is preferably within the above range, and the number of bending resistances in both the case where the first direction is set as the bending axis and the case where the second direction is set as the bending axis is particularly preferably within the above range. The mechanical strength of the biaxially stretched film is high in all directions in the plane, so when any direction is set as the bending axis, a large number of bending resistances can be exhibited.

[0193] [Application of film]

[0194] The above film has high transparency and excellent mechanical strength, so it can be suitably used as a cover film configured on the recognition side surface of an image display panel, or a transparent substrate for a display, a transparent substrate for a touch panel, a substrate for a solar cell, etc. When the film is actually used, an antistatic layer, an easy-adhesion layer, a hard coating layer, an antireflection layer, etc. can also be provided on the surface.

[0195] The film has high bending resistance and can be used particularly suitably as a cover film for the viewing side surface of a curved display or a bendable display. For example, it can be used suitably as a cover film for a foldable image display device (foldable display) that is repeatedly bent along a bending axis at the same location.

[0196] Example

[0197] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples. It should be noted that the present invention is not limited to the following examples.

[0198] [Production Example of Polyimide Resin]

[0199] Dimethylformamide (DMF) was placed in a separable flask and stirred under a nitrogen atmosphere. Diamine and tetracarboxylic dianhydride were added at the ratio (mol %) shown in Table 1 and stirred for 5 to 10 hours under a nitrogen atmosphere to react and obtain a polyamic acid solution having a solid content concentration of 18 wt %.

[0200] Add 6.0g of pyridine as an imidization catalyst to 100g of polyamic acid solution, add 8g of acetic anhydride after complete dispersion, and stir at 90°C for 3 hours. After cooling to room temperature, add 100g of 2-propanol (hereinafter referred to as IPA) at a rate of 2 to 3 drops / second while stirring the solution to precipitate polyimide. Then add 150g of IPA, stir for about 30 minutes, and filter using a Kiriyama funnel. After washing the obtained solid with IPA, dry it in a vacuum oven set at 120°C for 12 hours to obtain polyimide resins A to C.

[0201] [Preparation of polyamide-imide resin]

[0202] Diamine, tetracarboxylic dianhydride and dicarboxylic acid dichloride were added at the ratio (mol %) shown in Table 1. Polymerization (preparation of polyamic acid solution), imidization, resin precipitation, washing and drying were carried out in the same manner as in the preparation of polyimide resin to obtain polyimide resins D to G.

[0203] [Example of film production]

[0204] <Reference Example 1>

[0205] The polyimide resin A obtained in the above manufacturing example and a commercially available polymethyl methacrylate resin ("parapet HM1000" manufactured by Kuraray Co., Ltd., glass transition temperature: 120°C; acid value: 0.0 mmol / g; hereinafter referred to as "acrylic resin 1") were dissolved in dichloromethane (DCM) at a weight ratio shown in Table 1 to prepare a solution containing 11% by weight of the resin component. This solution was applied on an alkali-free glass plate, and heat-dried at 60°C for 15 minutes, 90°C for 15 minutes, 120°C for 15 minutes, 150°C for 15 minutes, 180°C for 15 minutes, and 200°C for 15 minutes in an air atmosphere to prepare a film having a thickness shown in Table 1.

[0206] <Reference Examples 2 to 9>

[0207] Films were prepared in the same manner as in Reference Example 1 except that the type of polyimide resin, the type of acrylic resin, and the mixing ratio of polyimide to acrylic resin were changed as shown in Table 1. In Reference Examples 4, 7, 8, and 9, polyimide resin and acrylic resin were incompatible in the dichloromethane solution and the solution became turbid, so DMF was used as a solvent instead of dichloromethane to prepare films.

[0208] The details of acrylic resins 2 and 3 used in Reference Examples 3, 5, and 8 are as follows.

[0209] Acrylic resin 2: copolymer of methyl methacrylate / methyl acrylate (monomer ratio 87 / 13) ("Parapet G-1000" manufactured by Kuraray Co., Ltd., glass transition temperature 109°C, acid value 0.0 mmol / g)

[0210] Acrylic resin 3: an acrylic resin having a glutarimide ring prepared according to the "Acrylic Resin Production Example" of Japanese Patent Laid-Open No. 2018-70710 (glutarimide content 4 wt%, glass transition temperature 125°C, acid value 0.4 mmol / g)

[0211] <Comparative Example 1>

[0212] A dichloromethane solution of polyimide resin C was prepared, and a thin film having a thickness of about 50 μm was produced under the same conditions as in Reference Example 1.

[0213] <Comparative Example 2>

[0214] A methylene chloride solution of acrylic resin 1 was prepared, and a film having a thickness of about 50 μm was produced under the same conditions as in Reference Example 1 except that the drying conditions were changed to 60° C. for 30 minutes, 80° C. for 30 minutes, 100° C. for 30 minutes, and 110° C. for 30 minutes.

[0215] [Example of Production of Stretch Film]

[0216] <Example 1>

[0217] A film containing polyimide resin A and acrylic resin 1 was prepared in the same manner as in Reference Example 1, and cut into a rectangle with the casting direction (MD) during film formation as the long side. The short sides (both ends in the longitudinal direction) of the film cut into a rectangle were clamped and the clamping distance was changed in an oven at the temperature shown in Table 1, thereby performing free-end uniaxial stretching at the stretching ratio shown in Table 1.

[0218] <Example 7>

[0219] A film containing polyimide resin C and acrylic resin 2 was prepared in the same manner as in Reference Example 5, and free-end uniaxial stretching was performed under the conditions shown in Table 1.

[0220] <Comparative Example 3>

[0221] A film of acrylic resin 1 was prepared in the same manner as in Comparative Example 2, and free-end uniaxial stretching was performed under the conditions shown in Table 1.

[0222] <Example 2>

[0223] In the same manner as in Example 1, free-end uniaxial stretching was performed under the conditions shown in Table 1 in such a manner that the length in the MD direction became 1.43 times (stretching ratio 43%). Thereafter, while both ends in the MD direction were clamped and fixed, both ends in the short-side direction (TD) were gripped by clamps, and the distance between the clamps was changed to perform fixed-end uniaxial stretching in such a manner that the length in the TD direction became 1.45 times that before free-end uniaxial stretching (stretching ratio 45%), thereby obtaining a biaxially stretched film having a stretching ratio of 43% in MD and 45% in TD.

[0224] <Examples 3 to 6, 8 to 12>

[0225] The film type and stretching conditions were changed as shown in Table 1, and sequential biaxial stretching (free-end uniaxial stretching and fixed-end uniaxial stretching) was performed in the same manner as in Example 2 to obtain a biaxially stretched film.

[0226] [evaluate]

[0227] <Glass transition temperature>

[0228] Differential scanning calorimetry (DSC) of the films of Reference Examples 1 to 9 and Comparative Example 1 was performed using a differential scanning calorimeter ("DSC7000X" manufactured by Hitachi High-Tech) under a nitrogen atmosphere at a heating rate of 10°C / min and a temperature range of 50°C to 270°C, and the inflection point of the DSC curve was defined as the glass transition temperature. In Reference Examples 1 to 9, no inflection point was confirmed near the glass transition temperature of the acrylic resin, and in the resin compositions constituting the films of Reference Examples 1 to 9 (and Examples 1 to 12), it was confirmed that the polyimide resin and the acrylic resin were completely compatible.

[0229] <Haze and Total Light Transmittance>

[0230] The film was cut into 3 cm squares, and the haze and total light transmittance (TT) were measured using a haze meter "HZ-V3" manufactured by Suga Test Instruments Co., Ltd. in accordance with JIS K7136 and JIS K7361-1.

[0231] <Yellowness>

[0232] The film was cut into 3 cm squares, and the yellowness (YI) was measured using a spectrocolorimeter "SC-P" manufactured by Suga Test Instruments Co., Ltd. in accordance with JIS K7373.

[0233] <Determination of the First Direction>

[0234] The phase difference measurement device "KOBRA" manufactured by Oji Scientific Instruments was used to measure the phase difference at a wavelength of 589 nm by the parallel Nicol rotation method, and the direction of the orientation axis (slow axis direction), that is, the direction with the maximum refractive index in the plane was taken as the first direction. The direction in the film plane orthogonal to the first direction (fast axis direction) was taken as the second direction.

[0235] <Refractive Index>

[0236] The film was cut into 3 cm squares, and the refractive index n1 in the first direction and the refractive index n2 in the second direction were measured using a prism coupler (Metricon "2010 / M"). Furthermore, the refractive index in the thickness direction in the cross section orthogonal to the first direction and the cross section orthogonal to the second direction were measured, and the average value was set as the refractive index n3 in the thickness direction.

[0237] Calculate the average refractive index n in the plane from n1, n2 and n3 H=(n1+n2) / 2, the index of in-plane refractive index anisotropy R(%): 100×(n1-n2) / n2 and the out-of-plane birefringence n H -n3.

[0238] <Tensile elastic modulus>

[0239] The film was cut into short strips with a width of 10 mm and the first direction as the long side, and after standing for 1 day at 23°C / 55%RH for humidity adjustment, a tensile test was performed using "AUTOGRAPH AGS-X" manufactured by Shimadzu Corporation under the following conditions with the first direction as the stretching direction, and the tensile elastic modulus in the first direction was measured. For the stretched films of Examples 1 to 12, a sample cut into short strips with the second direction as the long side was used, and a tensile test was performed with the second direction as the stretching direction, and the tensile elastic modulus in the second direction was also measured.

[0240] Distance between fixtures: 100mm

[0241] Stretching speed: 20.0mm / min

[0242] Measurement temperature: 23°C

[0243] <Pencil Hardness>

[0244] The pencil hardness of the film was measured by JIS K5600-5-4 "Pencil Scratch Test" with the first direction being the scratch direction (direction of pencil movement). The pencil hardness of the stretched films of Examples 1, 3 to 12 and Comparative Example 3 was also measured with the second direction being the scratch direction.

[0245] <Dynamic bending test>

[0246] The film was cut into short strips of 20 mm × 150 mm with the first direction as the long side. The short side of the sample was mounted on a U-shaped telescopic test fixture ("DMX-FS" manufactured by YUASA SYSTEM Co., Ltd.), and the second direction of the film was used as the bending axis under a temperature of 23°C and a relative humidity of 55%. The bending test was repeated using a desktop durability tester ("DMLHB" manufactured by YUASA SYSTEM Co., Ltd.), with a bending radius of 1.0 mm, a bending angle of 180°, and a bending speed of 1 time / second to determine the bending resistance. Specifically, the film was confirmed to have cracks or breaks every 1,000 bends (every 50,000 for more than 100,000 times), and the maximum number of bends without cracks or breaks was taken as the bending resistance.

[0247] For the stretched films of Examples 1 to 12, the bending resistance number was also measured for the case where the first direction was used as the bending axis using a sample cut into short strips with the second direction as the long side. The bending resistance number when the sample with the first direction as the long side was used and the bending resistance number when the test was carried out with the second direction as the bending axis was taken as the bending resistance number in the first direction, and the bending resistance number when the sample with the second direction as the long side was used and the bending resistance number when the test was carried out with the first direction as the bending axis was taken as the bending resistance number in the second direction.

[0248] [Evaluation results]

[0249] Regarding Reference Examples 1 to 9, Examples 1 to 12, and Comparative Examples 1 and 2, the resin composition (composition of polyimide, type of acrylic resin, and mixing ratio), glass transition temperature, film production conditions (type of solvent and stretching conditions), film thickness, haze, total light transmittance (TT), and yellowness are shown in Table 1, and the evaluation results of tensile modulus, pencil hardness, number of bending resistance in a dynamic bending test, and refractive index are shown in Table 2. Those for which the tensile modulus, pencil hardness, dynamic bending test, and refractive index were not evaluated are described as "ND" in the table.

[0250] In Table 1, the compounds are described by the following abbreviations.

[0251] <Tetracarboxylic dianhydride>

[0252] 6FDA: 4,4'-(hexafluoroisopropylidene) diphthalic anhydride

[0253] CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride

[0254] TAAHBP: Bis(1,3-oxo-1,3-dihydroisobenzofuran-5-carboxylic acid)-2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diester

[0255] BPDA: 3,3'4,4'-biphenyltetracarboxylic dianhydride

[0256] BPADA: 4,4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride

[0257] PMDA: Pyromellitic Dianhydride

[0258] <Dicarboxylic acid dichloride>

[0259] TPC: Terephthaloyl chloride

[0260] IPC: Isophthaloyl dichloride

[0261] <Diamine>

[0262] TFMB: 2,2'-bis(trifluoromethyl)benzidine

[0263] DDS: 3,3'-Diaminodiphenyl sulfone

[0264] [Table 1]

[0265]

[0266] [Table 2]

[0267]

[0268] The unstretched films of Reference Examples 1 to 9 comprising polyimide resin and acrylic resin, and the stretched films of Examples 1 to 12 in which these films are stretched, all have a haze of less than 2% and a total light transmittance of more than 90%, and have the same high transparency as the acrylic films of Comparative Examples 1 and 2.

[0269] The yellowness of the polyimide film of Comparative Example 1 is 7.5, whereas the yellowness of the films of Reference Example 5 and Examples 7 and 8 is smaller than that of Comparative Example 1. This shows that by mixing polyimide with an acrylic resin, a film with less coloration than when polyimide is used alone can be obtained.

[0270] The refractive index in the film plane of the unstretched film of Reference Example 1 is not anisotropic, the tensile elastic modulus is 3.9 GPa, and the bending resistance in the dynamic bending test is 13,000 times. Compared with Reference Example 1, the average refractive index in the plane of Examples 1 to 3 obtained by stretching the film of Reference Example 1 is n H becomes larger, the refractive index n3 in the thickness direction becomes smaller, and the out-of-plane birefringence n H -n3 increases accordingly.

[0271] Compared with Reference Example 1, the tensile modulus in the first direction of Examples 1 to 3 becomes larger. Compared with Reference Example 1, in Examples 2 and 3 as biaxially stretched films, the refractive index n2 in the second direction becomes larger, and the tensile modulus in the second direction also becomes larger. On the other hand, compared with Reference Example 1, in the uniaxially stretched film of Example 1, the refractive index n2 in the second direction becomes smaller, and the tensile modulus in the second direction becomes smaller. From these results, it can be seen that the refractive index in the stretching direction increases with stretching, and the tensile modulus in the stretching direction increases accordingly. It can be seen that biaxial stretching can obtain a film with a large tensile modulus in all directions within the plane.

[0272] In addition, it can be seen that the out-of-plane birefringence n H In the stretched films of Examples 1 to 3 in which -n3 is larger than that of Reference Example 1, the bending resistance in the first direction and the bending resistance in the second direction are both 400,000 or more, and the bending resistance is significantly improved compared with the unstretched film of Reference Example 1.

[0273] It can also be seen from the comparison between Reference Example 2 and Example 4 in which the ratio of the polyimide resin to the acrylic resin is changed that the out-of-plane birefringence increases by stretching, the tensile elastic modulus in the stretching direction increases, and the bending resistance times in the first direction and the second direction increase. The same tendency is also found in the comparison between Reference Example 3 and Example 5 in which the type of acrylic resin is changed. The same tendency is also found in the comparison between Reference Example 4 and Example 6 in which the type of polyimide resin is changed, and in the comparison between Reference Example 5 and Example 8.

[0274] The biaxially stretched films of Examples 9 to 12 including polyamideimide and acrylic resin also had larger out-of-plane birefringence and improved tensile elastic modulus and bending resistance in the first and second directions compared to the unstretched films of Reference Examples 6 to 9.

[0275] It should be noted that in Reference Examples 4, 7, 8, 9, and Examples 6, 10, 11, and 12, polyimide (polyamide-imide) and acrylic resin did not show compatibility in DCM, so DMF was used as a solvent to prepare the film. However, it can be seen that in these examples, the in-plane refractive index also increases due to stretching, and the mechanical strength is also greatly improved.

[0276] In Example 7, which is obtained by uniaxially stretching the film of Reference Example 5, the refractive index n1 in the first direction (stretching direction) increases, and the tensile elastic modulus and bending resistance in the first direction are improved accordingly, but the refractive index n2 in the second direction decreases, and the tensile elastic modulus decreases. From the comparison between Example 7 and Example 8, it can be seen that by biaxially stretching the film, a film having excellent mechanical strength in all directions in the plane can be obtained.

[0277] Compared with the unstretched film of Comparative Example 1, the film of Comparative Example 2, which was obtained by stretching a film containing only acrylic resin 1, did not show a significant change in the difference in refractive index between the in-plane and out-of-plane, and did not show a significant difference in tensile elastic modulus. In addition, the mechanical strength of the films of Comparative Examples 1 and 2 was inferior to that of the examples.

[0278] The above results show that the film of the compatible system of polyimide and acrylic resin has excellent transparency comparable to that of a film of a single acrylic resin, and that a transparent film can be obtained in which the refractive index anisotropy increases due to stretching, and along with this, the tensile elastic modulus and bending resistance are greatly improved, and the film has excellent mechanical strength that cannot be achieved by an acrylic resin film.

Claims

1. A film comprising polyimide and acrylic resin, The average value n of the refractive index n1 in the first direction with the largest refractive index in the film plane and the refractive index n2 in the second direction orthogonal to the first direction in the film plane is H , and the refractive index n3 in the thickness direction of the film satisfies n H -n3 ≥ 0.0140, The film has a total light transmittance of more than 85%, a haze of less than 10%, and a yellowness of less than 5.

2. The film according to claim 1, wherein The refractive index n1 in the first direction and the refractive index n2 in the second direction satisfy 100×(n1-n2) / n2<1.

0.

3. The film according to claim 1 or 2, wherein The tensile elastic modulus in the first direction and the tensile elastic modulus in the second direction are both 3.5 GPa or more. The film according to claim 1 or 2, which is a stretched film stretched in at least one direction. The film according to claim 4 , which is a biaxially stretched film. 6 . The film according to claim 1 , which has a glass transition temperature of 110° C. or higher and lower than 250° C.

7. The film according to claim 1 or 2, wherein: The polyimide has a diamine-derived structure represented by the general formula (IIa) and a tetracarboxylic dianhydride-derived structure represented by the general formula (IIIa). Y is a diamine residue belonging to a divalent organic group, X is a tetracarboxylic dianhydride residue belonging to a tetravalent organic group, At least one of the structure derived from diamine and the structure derived from tetracarboxylic dianhydride has a fluoroalkyl group.

8. The film according to claim 7, wherein The polyimide includes a structure derived from a diamine having a fluoroalkyl group as the structure derived from a diamine.

9. The film according to claim 8, wherein The diamine having a fluoroalkyl group is a fluoroalkyl-substituted benzidine.

10. The film according to claim 8, wherein The diamine having a fluoroalkyl group is 2,2'-bis(trifluoromethyl)benzidine.

11. The film according to claim 7, wherein The polyimide includes, as the structure derived from tetracarboxylic dianhydride, a structure derived from one or more tetracarboxylic dianhydrides selected from the group consisting of tetracarboxylic dianhydrides having a fluoroalkyl group and alicyclic tetracarboxylic dianhydrides.

12. The film according to claim 7, wherein The polyimide further comprises a dicarboxylic acid-derived structure represented by general formula (Va): Z is a dicarboxylic acid residue which is a divalent organic group.

13. The film according to claim 1 or 2, wherein: In the acrylic resin, the total amount of methyl methacrylate and the modified structure of methyl methacrylate is 60% by weight or more based on the total amount of monomer components.

14. The film according to claim 1 or 2, wherein The acrylic resin has a glass transition temperature of 80° C. or higher. 15 . The film according to claim 1 , comprising the polyimide and the acrylic resin at a weight ratio in the range of 98:2 to 2:

98.

16. A method for producing a thin film, which is the method for producing a thin film according to claim 1 or 2, wherein: An unstretched film comprising polyimide and acrylic resin is stretched in at least one direction.

17. The method for producing a thin film according to claim 16, wherein: The unstretched film is biaxially stretched.

18. The method for producing a thin film according to claim 16, wherein: The temperature during stretching is lower than 250°C.

19. The method for producing a thin film according to claim 16, wherein: The unstretched film is produced by applying a resin solution prepared by dissolving polyimide and acrylic resin in an organic solvent onto a support, and removing the organic solvent.

20. An image display device comprising the film according to claim 1 or 2 on a viewing side surface of an image display panel.

21. The image display device according to claim 20, which is bendable.