Composite article and method of manufacturing a composite article

By imprinting the opposite texture coating on the functional texture layer, the air interception problem is solved, and the feasibility of protection and removal of the texture layer is achieved, and it is suitable for complex and large-area functional texture layer applications.

CN118974650APending Publication Date: 2024-11-15MORPHOTONICS HLDG BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026991.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-08
Filing Date
2023-01-17
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Functional texture layers are susceptible to air retention during manufacturing, resulting in irregular surface structures, and conventional protective layers are difficult to remove and may damage the texture.

Method used

Using a coating imprinted on the substrate texture, the coating is opposite to the substrate texture, and the air-enclosed setting is achieved through mechanical imprinting equipment, ensuring accurate mapping of the coating and substrate texture, preventing air interception, and providing removable protection.

Benefits of technology

Effectively prevent air interception, maintain the texture structure intact, simplify the coating removal process, reduce the risk of damage, and is suitable for complex surfaces and large-area applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005038274700000071
    Figure BDA0005038274700000071
  • Figure HDA0005038274710000011
    Figure HDA0005038274710000011
  • Figure HDA0005038274710000012
    Figure HDA0005038274710000012
Patent Text Reader

Abstract

The present invention relates to a composite article and a method of making such an article. A composite article includes a substrate and coatings wherein at least a portion of the substrate includes a texture wherein at least a portion of the at least one coating is opposite the texture of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite product and a method for manufacturing the composite product. Background Art

[0002] Functional texture layers are surfaces with a nano- or micro-scale texture. These can be random textures or, in particular, diffraction gratings, tilted gratings, blazed gratings, microlens arrays, lenses, strips, cones, prismatic lines or even blank surfaces. The use of functional texture layers on devices such as displays or solar cells is an important topic. Clever use of these layers can increase performance, reduce costs or improve the visual appearance of a product. For example, the use of diffuser layers in displays enables the use of thinner LED backlight concepts and the illumination of displays from the side. Other new high-tech possibilities are the integration of functional texture layers into solar panels to increase their efficiency or into organic light-emitting diode (OLED) lighting panels to extract more light.

[0003] Functional texture layers can be made by an imprinting process such as nanoimprint lithography. A stamp with a texture can be used to imprint its texture onto a (fluid) resin, lacquer or resist layer disposed on a substrate. After the stamp is pressed onto the substrate with the resin in between, the textured resin is cured into a solid phase. The curing method can be thermal or by using radiation such as UV light. Using this technique, texturing can be performed with micron or nanometer-sized features.

[0004] Given the small scale of the texture, the functional texture layer is prone to handling defects. To protect the functional texture layer, a foil combined with an adhesive layer is usually used as a protective layer. The combination of the protective foil and the adhesive layer is laminated to the surface texture to be protected (e.g., a wafer) by lamination or manual pressing processes. The foil can also be used to provide protection without a pressure-sensitive adhesive. The disadvantage of these methods is that the risk of air being entrained between the texture and the protective foil is high, because the foil and / or adhesive layer usually does not fully conform to the precise texture of the functional texture layer. If air is trapped between the foil and the texture, the air may have a negative impact on the surface structure of the texture. This usually results in irregular products, which is very undesirable. It can also be seen that the air causes changes in the surface of the substrate, such as changing the surface roughness. Alternatively, a protective coating can be applied to the texture of the functional texture layer. However, compared to the foil layer, conventional coatings have the same disadvantages when it comes to trapped air, in addition to which conventional coatings are more difficult to remove from the functional texture layer, thereby risking damage to the texture or leaving residues on the substrate or texture.

[0005] Therefore, it is an object of the present application to provide a solution to at least some of the above problems, or at least to provide an alternative solution for protecting the functional texture layer. Summary of the invention

[0006] The present invention provides a composite article comprising at least one substrate, wherein at least a portion of the substrate comprises a texture, and at least one coating, wherein at least a portion of the at least one coating is arranged on at least a portion of the texture of the substrate, in particular is embossed on at least a portion of the texture of the substrate, so that at least a portion of the coating (in particular the embossed coating) is opposite to the texture of the substrate.

[0007] The composite article according to the present invention has several advantages compared to the prior art. The use of a coating that is embossed on at least a portion of the texture of a substrate enables the provision of an embossed coating that is opposite to the texture of the substrate. In other words, the embossed coating follows the exact texture of the substrate. Therefore, the embossed texture of the coating is substantially an exact negative image of the texture of the substrate. By using embossing of the coating, air is prevented from being trapped in the texture of the substrate. The coating according to the present invention is arranged on the texture of the substrate without being surrounded by air. The embossed coating specifies a (negative) mapping of the texture of the substrate in a conformal manner, in particular so that all angles between intersecting curves remain unchanged, resulting in a conformal transformation in which angles and proportions are maintained. The present invention provides a composite article in which the coating is arranged on the texture of the substrate in an airless manner.

[0008] In particular, at least a portion of at least one coating is embossed on at least a portion of the texture of the substrate, such that at least a portion of the embossed coating has a texture that is opposite to the texture of the substrate. It can also be said that at least one coating comprises an embossed and / or opposite texture. Therefore, the present invention also relates to a composite product comprising at least one substrate, wherein at least a portion of the substrate comprises a texture, and at least one coating, at least one coating being arranged on at least a portion of the texture of the substrate, wherein at least a portion of the coating comprises an opposite texture that is embossed. The coating can be embossed, for example, by a mechanical embossing device, such as a roller-to-bottom plate device.

[0009] There are several benefits to using imprinted coating compared to applying the coating by, for example, spin coating. Spin coating is a common method for coating surfaces, for example for coating (round) wafers, but spin coating is complicated for larger surfaces. Spin coating of rectangular surfaces is also complicated. Thirdly, in the spin coating method, there may be no conformal protection for textured surfaces, which have a deep or steep texture without filling resin. Spin coating also generally requires more coating material, while imprinting enables minimal application and precise use of coating material without spillage. Finally, spin coating is limited to rigid substrates.

[0010] The composite article and method according to the present invention facilitates long-term storage, shipment and / or transportation of the article and stacking of multiple articles. The substrate, in particular its texture, remains clean and dust is prevented from accumulating thereon. Furthermore, harmful radiation or chemicals that could damage and / or alter the texture are kept away. Furthermore, the composite article is protected from undesirable climatic conditions, such as high humidity, which could cause damage due to, for example, delamination of the article.

[0011] When referring to a composite article, it may also refer to a composite material, an assembly or a composite device. The texture of a substrate may also be referred to as a functional texture, a surface texture or a surface substrate. The texture may be provided directly in the substrate. It is also conceivable that the substrate comprises at least one functional texture layer, the texture forming part of the functional texture layer. It is also conceivable that at least one substrate comprising at least one texture forms a functional texture layer, or that a substrate comprising a texture is referred to as a substrate comprising a functional texture layer.

[0012] The shape of the substrate generally depends on the intended use. For example, it is conceivable that the substrate is substantially rectangular, square, circular and / or a combination thereof. The substrate may also have a free form. This also applies to the texture or textured area of ​​the substrate. The substrate is preferably substantially planar. The substrate according to the invention may be relatively large. For example, it is conceivable that at least one substrate has at least 0.5 m 2 , at least 1m 2 or at least 2m 2 For example, the surface may be substantially rectangular, with a length in the range of 10 cm to 10 m and a width in the range of 10 cm to 5 m.

[0013] The coating is preferably at least partially fluid when applied to the substrate (particularly on the texture of the substrate). For example, it is conceivable that the viscosity of the coating ranges from 5 cP to 5000 cP, preferably from 5 cP to 500 cP, particularly at room temperature. For example, the viscosity of the coating may also be equal to the viscosity of water when applied. Preferably, the coating is applied to at least a portion of the texture of the substrate in the form of a liquid or viscous resin. Typical application techniques of the resin or coating resin forming the coating are printing methods that may be combined with lamination and / or embossing. As a printing method, for example, inkjet printing, dispense printing, screen printing, jet dispensing or any other printing techniques known to those skilled in the art may be used. Other coating methods known to those skilled in the art may be used, such as but not limited to spin coating, spraying and / or slit coating. For the embossing step, if applied, a roll-to-roll, plate-to-plate or roll-to-plate method may be applied. For the application of the coating resin, a textured or non-textured mold or stamp may be used. These examples may be applied to the method according to the present invention.

[0014] At least one coating according to the present invention may also be referred to as a protective layer or protective coating. At least one coating is preferably a removable coating. Within the scope of the present invention, such coatings that do not substantially damage or change the texture of the substrate when removed can be classified as removable. In addition, the coating is preferably configured to be removed as a whole. Therefore, the coating is preferably strong enough to not leave a part of the coating on the texture of the substrate when removed. No additional (chemical) removal aid is required to remove the coating according to the present invention from the substrate.

[0015] It is conceivable that the coating not only provides a protective function, but can also be used for other purposes after being removed from the substrate. In particular, because the coating is a replica of the texture of the substrate, the coating can also be used to indirectly check the quality of the texture of the substrate without the risk of damaging the primary texture during the inspection process. Therefore, it is beneficial if the coating is configured to be removed from the substrate, in particular from the texture of the substrate, without being damaged and / or permanently deformed.

[0016] The stripping force required for removing at least one coating from the texture of substrate is preferably lower than the cohesive force of substrate, for example the cohesive force of the texture of substrate. It can also be imagined that the stripping force required for removing at least one coating from the texture of substrate is lower than the cohesive force of coating, lower than the cohesive force and / or the bonding force of any optional additional layer that substrate is attached to thereon and / or lower than the cohesive force and / or the bonding force of any optional additional layer that coating is attached to thereon. The stripping force required for separating the texture of coating and substrate needs to be minimized, while ensuring good adhesion between these layers. When mentioning stripping force, it can also be referred to as peel strength. Stripping force can for example be determined by 180 degree peeling test according to the ISO 8510-2 test standard for rigid products and the ISO11339 test standard for flexible products or its equivalent alternative standard.

[0017] For example, it is conceivable that the peel force required to remove at least one coating from the texture of the substrate is less than 100 N / m, preferably less than 50 N / m, more preferably less than 20 N / m, even more preferably less than 10 N / m or 3 N / m. It is also conceivable that the peel force is in the range of 1 N / m to 10 N / m or in the range of 2.5 N / m to 7.5 N / m.

[0018] At least a portion of the texture of the substrate preferably has a relatively low surface free energy. The surface free energy can represent a low peeling force of the coating. In a possible embodiment, the surface free energy of the texture of the substrate is lower than 70mN / m, particularly lower than 40mN / m. It is also conceivable that the surface free energy of the coating is lower than 70mN / m, particularly lower than 40mN / m. It is also conceivable that the surface free energy of the texture of the substrate is lower than 30mN / m, particularly lower than 25mN / m, and / or the surface free energy of the coating is lower than 30mN / m, particularly lower than 25mN / m. Such a value will actively contribute to a low peeling force, which allows the coating to be easily removed from the texture of the substrate without damaging and / or leaving residues on the texture of the substrate and / or the coating, or at least minimizing damage and / or leaving residues on the texture of the substrate and / or the coating. For example, the required value of the surface free energy can be obtained by the surface treatment of the substrate, particularly by the surface treatment of the texture of the substrate. It is also conceivable that the surface free energy is controlled by controlling the composition of the coating. Low surface free energy is usually obtained by chemical groups located on the surface. Typical chemical groups for this purpose are fluorine-containing groups, such as fluoroalkyl, long alkyl and alkylsiloxane groups. Therefore, it is conceivable that at least a portion of the texture of the substrate contains fluoroalkyl, long alkyl and / or alkylsiloxane groups. For example, at least a portion of the texture of the substrate can be treated with a composition containing fluoroalkyl, long alkyl and / or alkylsiloxane groups. It is also conceivable that the coating contains fluoroalkyl, long alkyl and / or alkylsiloxane groups. It is also conceivable that the substrate and / or the coating includes at least one additive configured to reduce the surface free energy of the material. Non-limiting examples of such additives are perfluoropolyether (PFPE) monomers, perfluorinated monomers, silicone monomers and / or aliphatic monomers.

[0019] Another way to enhance the texture separation of the coating from the substrate is by reducing the interaction between the substrate and the coating. For example, this can be achieved by ensuring that a low density of strong covalent, ionic or metallic interface bonds and / or entanglements are formed between the coating and the substrate. In this way, the number and intensity of interactions between the two interfaces are limited. In a possible embodiment, the preferred interaction between the texture of the substrate and the coating is obtained by the texture of the substrate comprising at least one inorganic surface group, such as but not limited to SiO x 、SiN x , metals and / or metal oxides. These materials generally do not form strong bonds with organic (e.g., acrylate) surface groups. According to this principle, embodiments of composite articles comprising a coating comprising a UV-cured acrylic resin on textured glass or on a silicon substrate will result in successful separation of multiple layers.

[0020] It is also conceivable that a relatively low interaction between the texture of the substrate and the coating is obtained by passivating and / or deactivating the functional surface groups of the texture through a surface treatment. For example, such a surface treatment can consist of a deposition step that adds a passivation layer and / or another inactive layer on top of the texture. Another option is a plasma passivation or deactivation step that passivates a certain amount of surface groups that would otherwise be firmly bonded to the coating material. Therefore, it is conceivable that the substrate according to the present invention includes a plasma treated texture. It is also conceivable that the substrate and / or coating is subjected to an excimer treatment step.

[0021] In a possible embodiment of a composite article according to the present invention, the Young's modulus of the substrate is less than 4 GPa, preferably less than 3 GPa, and more preferably less than 2 GPa. It is also conceivable that the Young's modulus of the coating is less than 4 GPa, preferably less than 3 GPa, and more preferably less than 2 GPa. In another embodiment, it is conceivable that the composite article according to the present invention has a Young's modulus of less than 4 GPa, preferably less than 3 GPa, and more preferably less than 2 GPa. Alternatively, the substrate may include silicon, a nickel shim and / or a glass having a Young's modulus of about 70 GPa. Optionally, the carrier layer attached to the (removable) coating may be attached to a flexible film such as polyester (Young's modulus of 4 GPa). For example, the Young's modulus is measured according to ASTM E111. These embodiments contribute to easy removal of the coating, in particular without damaging the texture of the substrate and / or the coating.

[0022] In a preferred embodiment, at least a portion of the substrate includes an embossed texture. At least a portion of the texture can be obtained by an embossing process (e.g., nanoimprinting). It is also conceivable that the texture is obtained by a stamping process. For example, a resin may have been used. Typical application techniques for resins are printing and / or embossing. As an embossing method, roll-to-roll, plate-to-plate, or roll-to-plate technology can be used. For the application of resins, a texture mold or stamp is preferably applied. It is also conceivable that the texture is engraved, ground, etched, laser ablated, printed, injection molded, embossed, or otherwise textured. It is also conceivable that the substrate comprising the texture is configured to be applied in an embossing process. Therefore, the substrate according to the present invention can be, for example, a stamp.

[0023] The texture of the substrate is in particular a three-dimensional texture. For example, at least a portion of the texture of the substrate may comprise a repeating pattern. It is also conceivable that at least a portion of the texture is a randomized texture. The texture may comprise a diffraction grating, a tilted grating, a blazed grating, a microlens array, a lens, a strip, a cone, a prism line and / or a combination thereof. The substrate may comprise at least one active area, in particular, wherein the active area comprises a texture.

[0024] For example, the depth of the texture can be nanometer-scale to micrometer-scale. For example, it is conceivable that at least a portion of the texture has a depth in the range of 0.1 nm to 500 μm. It is also conceivable that at least a portion of the texture of the substrate includes a peak-to-valley height of at most 1 mm. Preferably, at least a portion of the texture of the substrate includes a peak-to-valley height of at most 10 μm, more preferably at most 5 μm, and even more preferably at most 2 μm. However, it is also conceivable that at least a portion of the texture of the substrate includes a peak-to-valley height of at most 100 nm, more preferably at most 50 nm, and even more preferably at most 20 nm or 10 nm.

[0025] The specification of the substrate may depend on the intended use. For example, it is conceivable that at least one substrate may include glass, metal, polycarbonate and / or polyester. More specifically, it is possible that at least one substrate contains polyethylene naphthalate (PEN), polyethylene terephthalate (PET) and / or polymethyl methacrylate (PMMA). Preferably, at least a portion of the substrate is substantially flexible. Alternatively, the substrate may be substantially rigid. For example, the substrate may be a rigid plate or block, preferably made of a durable material such as, but not limited to, glass, silicon dioxide, quartz, ceramic and / or metal. Non-limiting examples of possible metals are steel, copper and / or aluminum. It is also conceivable that the substrate includes at least one polymeric material, such as, but not limited to, at least one thermosetting resin and / or hard rubber. It is also conceivable that at least a portion of the substrate is formed as a thin sheet. For example, at least one substrate may include a metal sheet, a plastic sheet, a rubber sheet and / or a glass sheet. It is also conceivable that the substrate is made of substantially the same material as the coating. Therefore, it is conceivable that the coating and the substrate are made of substantially the same material. Any of the material examples mentioned for the coating may also be applied to the substrate.

[0026] Preferably, at least a portion of the coating is substantially transparent and / or translucent before curing. For example, at least a portion of the coating may be light-transmissive, in particular UV-transmissive. At least a portion of the coating preferably has a transparency of at least 10%, preferably at least 50%, more preferably at least 90%. At least a portion of the coating preferably has a UV-A transparency or UV-A permeability of at least 60%. For example, it is conceivable that at least a portion of the coating has a UV-A transparency in the range of 60% to 100%, in particular a UV-A transparency in the range of 70% to 90%. In a preferred embodiment, at least a portion of the coating has a cut-off wavelength in the range of 150nm to 400nm, more preferably in the range of 240 to 380nm, even more preferably in the range of 280nm to 315nm. The coating may be a UV-curable or cured coating. For example, at least a portion of the coating is curable when irradiated with a wavelength in the range of 200nm to 400nm, preferably in the range of 365nm to 405nm. It is also conceivable that at least one coating is a heat-curable coating.

[0027] In an embodiment, at least a portion of the substrate is preferably substantially transparent and / or translucent. For example, it is possible that at least a portion of the substrate is light-transmissive, in particular capable of transmitting UV light. At least a portion of the substrate preferably has a transparency of at least 10%, preferably at least 50%, more preferably at least 90%. At least a portion of the substrate preferably has a UV-A transparency or UV-A permeability of at least 60%. The substrate may include a UV-curable or cured layer. For example, it is possible that at least a portion of the substrate is curable when irradiated with a wavelength in the range of 300nm to 800nm, preferably 365nm to 405nm. It is also conceivable that at least a portion of the substrate is heat-curable.

[0028] Preferably, at least a portion of the bottom surface of the coating has a texture opposite to the texture of the substrate, and / or at least a portion of the upper surface of the coating is substantially flat. Applying the coating by an embossing method can provide a fairly uniform coating. The coating according to the present invention can have a substantially uniform thickness. Preferably, the coating according to the present invention is a substantially uniform coating. This is beneficial because each slight deviation will affect the texture of the substrate.

[0029] Preferably, at least one coating is in direct contact with the texture of the substrate, in particular without the interference of any other medium (such as air). As mentioned above, any medium present on the substrate or between the substrate and the coating will have a negative impact on the substrate and thus affect its performance. It is necessary to provide a coating that engages with the texture of the substrate in a shape-fitting manner. Preferably, the thickness of the coating is substantially uniform. This means that in practice the thickness deviation is at most 20%, preferably at most 10%, more preferably at most 5%.

[0030] Preferably, at least one coating comprises at least one polymer. For example, it is conceivable that, in particular before curing, at least one coating comprises at least one monomer and / or oligomer, wherein preferably at least one of the at least one monomer and / or oligomer is selected from the group of epoxides, thiols, polyvinyl resins, acrylates, methacrylates, polyethers, vinyl ethers, polyurethane acrylates, polyesters, fluorinated acrylates, fluorinated methacrylates, fluorinated polyethers, siloxanes, siloxane-acrylates and / or blends thereof. It is also conceivable that, in particular before curing, the coating comprises: a prepolymer composition and at least one multifunctional monomer component, the prepolymer composition comprising at least one monomer or oligomer component having at least one polymerizable C=C double bond, wherein the multifunctional monomer component comprises at least two functional groups, the two functional groups being selected from the group consisting of (meth)acrylates, methyl (meth)acrylates, vinyl ethers, allyl ethers, propenyl ethers, olefins, dienes, unsaturated esters, allyl triazines, allyl isocyanates and N-vinyl amides, wherein the monomer or oligomer having at least one polymerizable double bond The oligomer component is selected from the group consisting of (meth)acrylates, methyl (meth)acrylates, vinyl ethers, allyl ethers, propenyl ethers, olefins, dienes, unsaturated esters, allyl triazines, allyl isocyanates and N-vinyl amides, and at least one surface active anti-stick additive is selected from the group consisting of alkyl (meth)acrylates, polysiloxane (meth)acrylates, (per)fluoroalkyl (meth)acrylates, (per)fluoropolyether (meth)acrylates, alkyl vinyl ethers, polysiloxane vinyl ethers, (per)fluoroalkyl vinyl ethers and (per)fluoropolyether vinyl ethers. The coating or resin may also include at least one perfluorinated component.

[0031] At least one coating can include at least one additive. For example, it is conceivable that at least one additive is an initiator that is particularly configured to promote coating curing. For example, at least one coating can include at least one free radical initiator, cationic initiator, anionic initiator and / or photoinitiator. Non-limiting examples of applicable free radical initiators are azo compounds (such as azobisisobutyronitrile), peroxides (such as dibenzoyl peroxide or peroxydisulfate), phosphine oxides (such as diphenylphosphine oxide), aromatic ketones (such as 1-hydroxy-cyclohexyl phenyl-ketone or 2-hydroxy-2-methylphenylpropiophenone), or norrish II type initiators (such as methyl benzoyl formate). Possible cationic and anionic initiators are benzene sulfonates, alkyl sulfonium salts or photobase generators, such as triphenylsulfonium (cationic), tetrafluoroborate or 2-nitrobenzylcyclohexylcarbamate (anionic). Using at least one initiator can further enhance the controllability of coating curing process. Depending on the difference of initiators, curing can be initiated by heat, or by radiation (such as by UV radiation). In embodiments, the coating is fully curable, excluding any applied initiator. In possible embodiments, at least one coating, particularly a coating composition forming the coating, comprises at least 95 wt-%, at least 98 wt-% or at least 99 wt-% of curable material.

[0032] In a preferred embodiment, at least one coating layer comprises at least one resin (e.g., an acrylic resin), preferably comprising at least one siloxane group, epoxy group, and / or fluoroorganic group. For example, it is contemplated that the resin used for the coating layer comprises a monomer or oligomer comprising at least one polymerizable epoxy group and / or at least one multifunctional monomer component, wherein the multifunctional monomer component contains at least two functional epoxy groups per molecule. Any mixture of one of these epoxy group-containing formulations with the components in the previous paragraph may constitute a suitable formulation for forming a protective texture layer.

[0033] Preferably, at least one coating comprises at most 5 wt-% solvent. It is also conceivable that at least one coating is substantially free of solvent. In possible embodiments, the coating comprises at most 1 wt-% solvent, at most 2 wt-% solvent, at most 3 wt-% solvent, at most 4 wt-% solvent or at most 5 wt-% solvent. In an embodiment, the coating is a pressure sensitive adhesive, which is generated in situ depending on the application. The solvent can be classified as a fluid that is capable of dissolving a reasonable amount of resin while having a vapor pressure of 30 hPa or more at 25°C.

[0034] The composite product, in particular the coating, may also include at least one film layer. Preferably, this film layer is attached to the upper surface of the coating. If a film layer is applied, it is preferably attached to the side of the coating opposite to the side with the (embossed) texture. For example, the film layer may be a polymer film layer, a plastic film layer and / or a rubber film layer. The film layer may also be a foil layer. The film layer may be applied to the coating before or after solidification. The application method of the film layer may be lamination. The use of a film layer may simplify the removal of the coating from the substrate. In a possible embodiment, the film layer is adhered to the coating by an adhesive (preferably a pressure-sensitive adhesive).

[0035] In an advantageous embodiment, at least one coating layer comprises a plurality of coating sublayers. For example, it is conceivable that at least one coating layer comprises at least 3 coating sublayers, in particular at least 5 coating sublayers, more particularly at least 7 coating sublayers. It is conceivable that at least two coating sublayers are embossed coating sublayers. It is also conceivable that each coating sublayer is an embossed coating sublayer. The composition of each coating sublayer may be similar. It is also possible that at least two coating sublayers have different compositions.

[0036] The invention also relates to a substrate for a composite article according to the invention.The invention also relates to a coating for a composite article according to the invention.

[0037] The present invention also relates to a method for producing a composite article, in particular a composite article according to the present invention, comprising the following steps:

[0038] - providing at least one substrate, wherein at least a portion of the substrate comprises a texture;

[0039] - disposing at least one coating composition on at least a portion of the texture of the substrate; and

[0040] - Imprinting the coating composition onto at least a portion of the texture of the substrate, thereby forming an imprinted coating that is the inverse of the texture of the substrate.

[0041] The method is used to manufacture a composite product according to the present invention. Any of the embodiments described for the substrate and the coating can be applied. The method can also include a step of solidifying the coating. The solidification step can be a curing step, such as but not limited to heating and / or UV curing. Before applying the coating thereon, at least a portion of the substrate, preferably at least a portion of the texture, can be subjected to a surface treatment, such as but not limited to a plasma treatment.

[0042] The inventors provide experiments with composite articles discussed below. Typical peel force examples for successful and unsuccessful peeling are shown in Table 1. Peel tests were performed according to the ISO 8510-2 test standard using a 180° peel. In these tests, two types of materials were used as the coating resin for the substrate and coating:

[0043] Material A: UV-curable acrylic resin

[0044] Material B: UV-curable acrylate resin with perfluorinated components

[0045] The substrate tested had a texture formed by an array of pyramids, the pyramid array features being 30 μm high and 50×50 μm in base. Both the substrate and the coating were produced on a 250 μm thick PET substrate. The substrate was mounted on a rigid carrier for the peel test. The coating was applied by placing the coating resin on the texture of the substrate, in particular by embossing a solvent-free coating resin, subsequently laminating the coating resin onto the texture with a plastic foil, and subsequently UV curing the coating resin.

[0046] When both the textured substrate and the coating are made of material B (comprising a perfluorinated component), or when material A is surface treated, the results show that the removal of the coating is successful. In this case, the peeling force required to separate the coating from the first three-dimensional layer is low, i.e., below about 25 N / m. The application of the self-assembled passivation layer results in the easiest peeling (i.e., the lowest peeling force) because the passivation layer not only neutralizes the active surface groups, but also reduces the surface free energy to a value below 40 mN / m compared to the atmospheric plasma treatment. When the self-assembled passivation layer is not applied to the substrate, the combination of materials A and B (e.g., when the textured article is made of material A and the coating is made of material B, or vice versa) results in a peeling force in the medium range of about 25-80 N / m. In this medium range, the peeling force required to separate the two layers is high enough to make the bond between one of the texture layers and its corresponding substrate material the weakest link. When both materials consist of material A, the peel force required to separate the coating from the first three-dimensional layer is high, i.e., above 80 N / m, which results in a decrease in the cohesion within the stack.

[0047] Table 1: Peel test results for textured articles and coatings made from two materials (A and B). In two of the tests, the articles were surface treated to successfully separate from the coating.

[0048] BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The present invention will be further illustrated by means of non-limiting exemplary embodiments shown in the accompanying drawings, in which:

[0050] - Figure 1a and Figure 1b shows a detailed view of a composite article according to the prior art;

[0051] - Figure 2a-2d A possible embodiment of a composite article according to the invention is shown;

[0052] - Figure 3a and Figure 3b shows another possible embodiment of the composite article according to the invention; and

[0053] - Figure 4a-4c A 3D image of a substrate and a coating according to the invention is shown.

[0054] In the drawings, like reference numbers correspond to similar or equivalent elements or features. DETAILED DESCRIPTION

[0055] Figure 1a and Figure 1b Detailed views of the disadvantages of a composite article 10 according to the prior art are shown. These figures show detailed views of a side view of a composite article 10. The composite article 10 comprises a substrate 12 and a cover layer 13, such as a coating or a foil. The cover layer 13 is applied to the substrate 12. The figure shows that air bubbles 11 are trapped between the substrate 12 and the cover layer 13. When this happens in practice, the air bubbles 11 will affect the surface structure S of the substrate 12. Due to the influence of the air, the surface structure S of the texture T will become rough and / or changed. This is undesirable because it will affect the overall performance of the substrate 12.

[0056] Figure 2a-2d A schematic representation of a side view of a possible embodiment of a composite article 101 according to the present invention is shown. Each figure shows a composite article 101a, 101b, 101c, 101d, which includes a substrate 102a, 102b, 102c, 102d and a coating 103a, 103b, 103c, 103d. Each substrate 102a, 102b, 102c, 102d includes a texture T. In the non-limiting embodiment shown, the texture T has a repeated pattern. The design of the texture can depend on the intended use. The scale of the texture is usually at the nanometer level, with a maximum of micrometers. Thus, the coating 103a, 103b, 103c, 103d is imprinted on at least a portion of the texture T of the substrate 102a, 102b, 102c, 102d. It can be seen that the embossed coating 103a, 103b, 103c, 103d is the opposite of the texture T of the substrate 102a, 102b, 102c, 102d. Figure 3a and Figure 3b It is schematically shown in FIG. 1 that the coating 103a, 103b, 103c, 103d of each composite article 101a, 101b, 101c, 101d is removable. Figure 2a and Figure 2d An embodiment is shown in which the texture T is imprinted in the substrate 102a, 102d. Figure 2b and Figure 2cThe embodiment of shows an embodiment in which the substrate 102c, 102c includes a functional texture layer. The texture T is embossed in the functional texture layer.

[0057] Figure 3a and Figure 3b Another possible embodiment of a composite article 201 according to the invention is shown. The composite article 201 comprises a substrate 202 and a removable coating 203 , wherein the substrate 203 comprises a texture T. The coating 203 further comprises an additional layer 204 , in particular a foil layer 204 attached to the coating 203 . Figure 3a The composite article 201 is shown in an initial state, wherein a coating 203 is disposed on the texture T of a substrate 202. The coating 203 is an embossed coating 203 having a texture that is the opposite of the texture T of the substrate 202. Figure 3b The coating 203 is shown being removed from the substrate 202. The coating 203 is substantially peeled from the substrate 202. Due to the beneficial properties of the coating 203 and the substrate 202, the texture of both layers is not affected by the removal. The peel force required to remove the coating 203 from the texture T of the substrate 202 is generally lower than the cohesive force of the texture T of the substrate 202.

[0058] Figure 4a-4c The substrate 302 ( Figure 4a and Figure 4b ) and coating 303( Figure 4c ) Figure 4a and Figure 4b shows the coating before and after it is applied ( Figure 4a ) and after ( Figure 4b )The same texture T of the substrate 302. Figure 4c Coating 303 is shown after removal. It can be seen that there is no damage or residue on the texture T of substrate 302, and the texture of coating 303 is generally an exact negative image of the texture of substrate 302. These figures relate to experimental testing described in this application.

[0059] It is obvious that the present invention is not limited to the exemplary embodiments shown and described herein, but that numerous variations are possible within the framework of the appended claims, which will be apparent to those skilled in the art. In this case, it is conceivable that the different inventive concepts and / or technical measures of the above variant embodiments are fully or partially combined without departing from the inventive concept described in the appended claims.

[0060] The verb "comprise" and its conjugations used in this patent document are understood to mean not only "include", but also include the expressions "contain", "substantially include", "formed by..." and their conjugations.

Claims

1. Composite products, including: - at least one substrate, wherein at least a portion of said substrate comprises a texture; and - at least one coating; At least a portion of at least one coating is embossed on at least a portion of the texture of the substrate such that at least a portion of the embossed coating is opposite to the texture of the substrate.

2. The composite article of claim 1, wherein at least one coating is a removable coating.

3. The composite article according to any one of the preceding claims, wherein the peel force required to remove at least one coating from the texture of the substrate is lower than the cohesive force of the substrate.

4. The composite article according to any one of the preceding claims, wherein the peel force required to remove the coating is lower than 100 N / m, preferably lower than 20 N / m, more preferably lower than 3 N / m.

5. A composite article according to any one of the preceding claims, wherein the surface free energy of the texture of the substrate is lower than 70 mN / m, preferably lower than 40 mN / m, more preferably lower than 25 mN / m.

6. A composite article according to any one of the preceding claims, wherein the surface free energy of the coating is lower than 70 mN / m, preferably lower than 40 mN / m, more preferably lower than 25 mN / m.

7. A composite article according to any one of the preceding claims, wherein at least one coating comprises fluoroalkyl, long alkyl and / or alkylsiloxane groups.

8. A composite article according to any one of the preceding claims, wherein at least one coating has a Young's modulus of less than 4 GPa.

9. A composite article according to any one of the preceding claims, wherein at least one substrate has a Young's modulus of less than 4 GPa.

10. A composite article according to any one of the preceding claims, wherein at least a portion of the substrate comprises an embossed texture.

11. A composite article according to any one of the preceding claims, wherein at least a portion of the texture of the substrate comprises a repeating pattern.

12. A composite article according to any one of the preceding claims, wherein at least a portion of the texture of the substrate comprises a peak-to-valley height of at most 10 μm, preferably at most 5 μm, more preferably at most 2 μm.

13. A composite article according to any one of the preceding claims, wherein at least one substrate comprises glass, metal, polycarbonate and / or polyester.

14. A composite article according to any one of the preceding claims, wherein at least a portion of the bottom surface of the coating has a texture that is the opposite of the texture of the substrate, and wherein at least a portion of the upper surface of the coating is substantially flat.

15. A composite article according to any one of the preceding claims, wherein at least one coating is in direct contact with the texture of the substrate.

16. A composite article according to any one of the preceding claims, wherein the coating is substantially uniform in thickness.

17. Composite article according to any one of the preceding claims, wherein at least one coating comprises at least one monomer, oligomer or polymer monomer and / or oligomer, in particular before curing.

18. Composite article according to any one of the preceding claims, wherein at least one coating comprises at least one additive, preferably at least one initiator.

19. The composite article according to any one of the preceding claims, wherein at least one coating comprises at least one acrylic resin comprising at least one siloxane group, epoxy group and / or fluoroorganic group.

20. The composite article according to any one of the preceding claims, wherein at least one coating layer comprises at most 5 wt-% of solvent.

21. A composite article according to any one of the preceding claims, comprising at least one film layer attached to the upper surface of the coating.

22. A composite article according to any one of the preceding claims, wherein at least one coating comprises a plurality of coating sub-layers.

23. Method for manufacturing a composite article, in particular a method for manufacturing a composite article according to any one of the preceding claims, comprising the following steps: - providing at least one substrate, wherein at least a portion of said substrate comprises a texture; - disposing at least one coating composition on at least a portion of said texture of said substrate; - embossing the coating composition onto at least a portion of the texture of the substrate, thereby forming an embossed coating that is the inverse of the texture of the substrate.

24. A method according to claim 23, comprising the step of solidifying the coating.