Conductive paste, electronic component, and laminated ceramic capacitor
By controlling the glass transition temperature and additive types in the conductive paste, the tightness between the dry film and the substrate is improved, the problem of insufficient tightness in the manufacturing of laminated ceramic capacitors is solved, and efficient electrical characteristics are achieved .
Patent Information
- Application Number
- CN202380031152.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-15
AI Technical Summary
In the manufacturing process of laminated ceramic capacitors, shortening the crimping time and reducing the pressure lead to insufficient clinging between the dry film and the substrate, resulting in a decrease in electrical characteristics.
Develop a conductive slurry, including conductive powder, binder resin, additive and organic solvent, by controlling the glass transition temperature of the drying body to 30°C or below 55°C, and using an acid-based dispersant and ceramic powder, Improve the firmness of the dry film and the substrate.
It significantly improves the clinging of the dry film and ceramic green sheets, enhances the electrical characteristics of the laminated ceramic capacitors, and is suitable for miniaturized and high-capacity electronic devices.
Smart Images

Figure CN118974859A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a conductive paste, an electronic component, and a multilayer ceramic capacitor. Background Art
[0002] As electronic devices such as mobile phones and digital devices become smaller and more powerful, electronic components including multilayer ceramic capacitors are also expected to be smaller and have higher capacity. Multilayer ceramic capacitors have a structure in which multiple dielectric layers and multiple internal electrode layers are alternately stacked. By making the dielectric layers and internal electrode layers thinner, miniaturization and higher capacity can be achieved.
[0003] A multilayer ceramic capacitor is manufactured, for example, in the following manner. First, a conductive paste for internal electrodes is printed in a predetermined electrode pattern on the surface of a raw sheet containing a dielectric powder such as barium titanate (BaTiO3) and a binder resin, and the mixture is dried to form a dry film (conductive film). Next, the dry film and the raw sheet are stacked in an alternating overlapping manner to obtain a laminate. Next, the laminate is heated and pressed to form an integrated body to form a pressed body. The pressed body is cut, and after being treated to remove the organic binder in an oxidizing atmosphere or an inactive atmosphere, it is fired to obtain a fired chip. Next, a paste for external electrodes is applied to both ends of the fired chip, and after firing, the surface of the external electrode is plated with nickel, etc. to obtain a multilayer ceramic capacitor.
[0004] In the process of heating, pressing and cutting the laminated body formed by stacking the dry film and the green sheet, if the adhesion between the dry film and the green sheet (substrate) is insufficient, the dry film (conductive film) may peel off from the green sheet (substrate) or the layer structure may shift, and the resulting multilayer ceramic capacitor may not have the desired electrical properties.
[0005] For example, Patent Document 1 discloses a conductive paste, the purpose of which is to improve the adhesion of a conductive paste containing a (meth)acrylic resin as a binder resin to a ceramic green sheet. The conductive paste contains a (meth)acrylic resin as a binder resin, an organic solvent, and a metal powder, wherein the (meth)acrylic resin has a glass transition temperature Tg in the range of -60°C to 120°C, a hydroxyl group in the molecule in the range of 0.01 mass % to 5 mass %, an acid value in the range of 1 mgKOH / g to 50 mgKOH / g, and a weight average molecular weight in the range of 10,000 Mv to 350,000 Mv.
[0006] In addition, Patent Document 2 discloses a conductive paste, the purpose of which is to provide a conductive paste capable of forming a conductive film having excellent adhesion to a substrate, the conductive paste being used to form an electrode layer on a substrate, the conductive paste comprising a conductive powder, a resin binder, an organic additive and an organic solvent, the organic additive comprising a (meth)acrylate compound having two or more (meth)acryloyl groups in one molecule and a number average molecular weight of less than 1000.
[0007] In addition, Patent Document 3 discloses a dry film for internal electrodes of a multilayer ceramic capacitor for the purpose of providing a dry film for internal electrodes that can form internal electrodes that have excellent adhesion to a dielectric layer and whose shape does not significantly change before and after a heat treatment. The dry film is formed from a composition containing a conductive powder and an organic binder resin, and is characterized in that the dry film for internal electrodes has a Vickers hardness of 47 Hv or more and 51 Hv or less.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: International Publication No. 2013 / 187183
[0011] Patent Document 2: Japanese Patent Application Publication No. 2018-055933
[0012] Patent Document 3: Japanese Patent Application Publication No. 2019-121744 Summary of the invention
[0013] Problems to be solved by the invention
[0014] In recent years, in order to improve productivity and reduce costs, in the manufacturing process of multilayer ceramic capacitors, when a laminated body obtained by alternately laminating dry films and ceramic green sheets is subjected to heat compression, the pressing time during compression is sometimes shortened and the pressure is reduced.
[0015] However, when the pressing time during crimping is shortened or the pressure is reduced, conventional conductive pastes sometimes fail to achieve sufficient adhesion between the dry film and the substrate, resulting in positional deviation of the dry film and a reduction in yield. Therefore, conductive pastes that can further improve adhesion to the substrate when forming a dry film are required.
[0016] In view of such circumstances, an object of the present invention is to provide a conductive paste capable of further improving the adhesion with a substrate.
[0017] Means used to solve problems
[0018] In a first aspect of the present invention, a conductive paste is provided, wherein the conductive paste comprises a conductive powder, a binder resin, an additive and an organic solvent, and the binder resin, the additive and the organic solvent are mixed in the same content ratio as the conductive paste, and then dried to obtain a dried body having a glass transition temperature of 30° C. or more and 55° C. or less.
[0019] In addition, preferably, the additive includes a compound capable of lowering the glass transition temperature of the dried body, and the compound is included in an amount of 0.01% by mass or more and 2.0% by mass or less relative to the conductive paste as a whole. In addition, preferably, the temperature at which the weight reduction rate of the compound in thermogravimetric analysis reaches the maximum is above 200°C. In addition, preferably, the molecular weight of the compound is above 250 and below 3000. Preferably, the conductive paste also includes an acidic dispersant and / or an alkaline dispersant. In addition, preferably, the conductive powder includes at least one metal powder selected from Ni, Pd, Pt, Au, Ag, Cu and their alloys. In addition, preferably, the average particle size of the conductive powder is 0.05μm or more and 1.0μm or less. In addition, preferably, the binder resin includes a butyral resin. In addition, preferably, the conductive paste also includes ceramic powder. In addition, preferably, the ceramic powder includes barium titanate. In addition, preferably, the average particle size of the ceramic powder is 0.01μm or more and 0.5μm or less. Preferably, the conductive paste contains 1% by mass or more and 20% by mass or less of ceramic powder relative to the entire conductive paste. Preferably, the conductive paste is used for internal electrodes of a multilayer ceramic component.
[0020] In a second aspect of the present invention, there is provided an electronic component formed using the conductive paste.
[0021] According to a third aspect of the present invention, there is provided a multilayer ceramic capacitor including at least a laminated body in which dielectric layers and internal electrode layers are laminated, wherein the internal electrode layers are formed using the conductive paste.
[0022] Effects of the Invention
[0023] The conductive paste of the present invention can further improve the adhesion to the substrate. In addition, in the manufacturing process of a multilayer ceramic capacitor, the dried film (internal electrode layer) formed using the conductive paste of the present invention has high adhesion to the green sheet (dielectric layer). BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 1 and 2 are a perspective view and a cross-sectional view showing a multilayer ceramic capacitor according to an embodiment. DETAILED DESCRIPTION
[0025] 1. Conductive paste
[0026] The inventors of the present invention have conducted in-depth research to further improve the adhesion between the conductive paste and the substrate, and found that there is a correlation between the glass transition temperature of the components contained in the conductive paste and the adhesion of the substrate. That is, the conductive paste involved in this embodiment includes a conductive powder, a binder resin, an additive, and an organic solvent. By controlling the glass transition temperature of the components contained in the conductive paste within a specific range, the adhesion with the substrate (for example, a green sheet) can be further improved. The characteristics of the conductive paste involved in the embodiment are described below.
[0027] [Glass transition temperature]
[0028] Regarding the glass transition temperature of the conductive paste, it is difficult to accurately measure the glass transition temperature due to the influence of the powder material when the conductive paste contains a powder material such as a conductive powder. Therefore, in order to evaluate the glass transition temperature of the components contained in the conductive paste, the inventors of the present invention measured the glass transition temperature Tg of a dry body (for evaluation) prepared from a composition composed of components other than the powder material and exhibiting glass transition behavior, i.e., a paste for evaluation.
[0029] The dried product for evaluating the glass transition temperature (Tg) can be prepared, for example, by the following method: The binder resin, additives, and organic solvent (i.e., the components after removing the powder materials such as the conductive powder) contained in the conductive paste are weighed in the same proportion as in the conductive paste, and mixed at 2000 rpm for 4 minutes using a rotary mixer (manufactured by THINKY, ARE-310), and then the obtained liquid is applied to a PET film with a wet film thickness of 254 μm using an applicator, and dried at 120° C. for 40 minutes to remove the organic solvent, thereby obtaining a sample for evaluation.
[0030] The glass transition temperature Tg of the dried body (for evaluation) is 30°C or more and 55°C or less, preferably 30°C or more and 50°C or less. By controlling the glass transition temperature of the dried body (for evaluation) within the above range, the adhesion between the dried film and the green sheet is improved. The detailed reason is not clear, but it is believed that by setting the glass transition temperature Tg to a specific range, the dried film obtained using the conductive paste involved in this embodiment is moderately softened, and entanglement at the bonding interface is easily generated, thereby improving the adhesion between the dried film and the ceramic green sheet (dielectric layer).
[0031] In addition, when the conductive paste contains two or more resins as binder resins, multiple glass transition temperatures Tg are sometimes measured depending on the resins contained, but the glass transition temperature Tg of the evaluation sample in this specification represents the glass transition temperature Tg in the lowest temperature region. In addition, the glass transition temperature Tg of the above-mentioned dried body (evaluation sample) can be measured by the method described in the examples. In addition, as the evaluation sample, a dried body obtained by centrifuging the conductive paste after manufacturing the conductive paste, removing the filler (powder material such as conductive powder) and drying it can also be used.
[0032] [Vickers hardness (room temperature)]
[0033] In addition, when the conductive paste in the present embodiment is applied to the surface of a substrate and dried at 75° C. for 20 minutes to form a dry film, the Vickers hardness of the dry film surface at room temperature is preferably 10 or less, more preferably 9 or less, and further preferably 8 or less. In addition, the lower limit of the Vickers hardness (room temperature) is, for example, 3.5 or more.
[0034] [Vickers hardness (60℃)]
[0035] The Vickers hardness of the dry film surface at 60°C is preferably 8 or less, more preferably 7 or less, and further preferably 6 or less. The lower limit of the Vickers hardness (60°C) is, for example, 3 or more. When measuring the Vickers hardness (60°C) of the dry film, it is preferred to condition the dry film by leaving it at 60°C for 3 minutes in advance.
[0036] [Composition ingredients]
[0037] The conductive paste involved in this embodiment includes conductive powder, binder resin, additives and organic solvent. In addition, the conductive paste may further include ceramic powder. The glass transition temperature of the dried body (for evaluation) can be controlled within the above range by, for example, appropriately adjusting the type and content of the binder resin, additives and organic solvent. The specific conditions of each component are described in detail below.
[0038] (Conductive powder)
[0039] As the conductive powder, there is no particular limitation, and metal powder can be used, for example, powders of one or more selected from Ni, Pd, Pt, Au, Ag, Cu and their alloys can be used. Among them, from the viewpoints of conductivity, corrosion resistance and cost, powder of Ni or its alloy (hereinafter sometimes referred to as "Ni powder") is preferred. As Ni alloy, for example, alloys of Ni and at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt and Pd can be used. The content of Ni in the Ni alloy is, for example, 50% by mass or more, preferably 80% by mass or more. In addition, in order to suppress the rapid gas generation caused by the partial thermal decomposition of the binder resin during the debinding process, the Ni powder can contain about hundreds of ppm of element S.
[0040] The average particle size of the conductive powder is preferably 0.05 μm or more and 1.0 μm or less, and more preferably 0.1 μm or more and 0.5 μm or less. When the average particle size of the conductive powder is within the above range, it can be suitably used as a slurry for internal electrodes of thin-film multilayer ceramic capacitors (multilayer ceramic components). The average particle size is a value obtained by observation using a scanning electron microscope (SEM), and is an average value (SEM average particle size) obtained by measuring the particle size of each of a plurality of particles in an image obtained by observation at a magnification of 10,000 times using an SEM.
[0041] The content of the conductive powder is preferably 30% by mass or more and less than 70% by mass, more preferably 40% by mass or more and 60% by mass or less, relative to the entire conductive paste. When the content of the conductive powder is within the above range, the conductivity and dispersibility are excellent.
[0042] (Ceramic powder)
[0043] The ceramic powder is not particularly limited. For example, in the case of a slurry for internal electrodes of a multilayer ceramic capacitor, a known ceramic powder is appropriately selected according to the type of multilayer ceramic capacitor to be used. As the ceramic powder, for example, a perovskite oxide containing Ba and Ti can be used, preferably containing barium titanate (BaTiO3).
[0044] As the ceramic powder, a ceramic powder containing barium titanate as a main component and oxides as a secondary component may also be used. As oxides, oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb and one or more rare earth elements may be cited. In addition, as the ceramic powder, for example, a ceramic powder of a perovskite-type oxide ferroelectric in which the Ba atoms and Ti atoms of barium titanate (BaTiO3) are replaced by other atoms such as Sn, Pb, Zr, etc. may also be used.
[0045] When used as a conductive paste for internal electrodes, the ceramic powder may have the same composition as the dielectric ceramic powder constituting the green sheet of the multilayer ceramic capacitor (electronic component). This can suppress the generation of cracks caused by the mismatch of shrinkage at the interface between the dielectric layer and the internal electrode layer during the sintering process. Such ceramic powders include, in addition to the above, oxides such as ZnO, ferrite, PZT, BaO, Al2O3, Bi2O3, R (rare earth element) 2O3, TiO2, and Nd2O3. In addition, the ceramic powder may be used alone or in combination of two or more.
[0046] The average particle size of the ceramic powder is, for example, greater than 0.01 μm and less than 0.5 μm, preferably greater than 0.01 μm and less than 0.3 μm. By setting the average particle size of the ceramic powder to the above range, when used as an internal electrode slurry, a sufficiently fine and thin uniform internal electrode can be formed. The average particle size is a value obtained by observation using a scanning electron microscope (SEM), and is an average value (SEM average particle size) obtained by measuring the particle size of each of a plurality of particles from an image obtained by observation using an SEM at a magnification of 50,000 times.
[0047] The content of the ceramic powder is preferably 1% to 20% by mass, more preferably 3% to 15% by mass, relative to the entire conductive paste. When the content of the ceramic powder is within the above range, dispersibility and sinterability are excellent.
[0048] The content of the ceramic powder is preferably 1 part by mass or more and 30 parts by mass or less, and more preferably 3 parts by mass or more and 30 parts by mass or less, based on 100 parts by mass of the conductive powder.
[0049] (Binder resin)
[0050] As a binder resin, a butyral resin is preferably included. In addition, when used as an internal electrode paste, from the viewpoint of improving the bonding strength with the green sheet, a butyral resin may be included, or a butyral resin may be used alone. As a butyral resin, polyvinyl butyral (PVB) can be cited. When the conductive paste contains a butyral resin, the bonding strength with the green sheet can be further improved.
[0051] The lower limit of the content of the butyral resin is not particularly limited, and for example, it can be 20% by mass or more, 40% by mass or more, more than 50% by mass, or 60% by mass or more relative to the entire binder resin. When the content of the butyral resin is within the above range, the adhesiveness is further improved, and the bonding strength between the dry film and the green sheet (substrate) is improved.
[0052] In addition, the upper limit of the content of the butyral resin is not particularly limited, for example, it can be 90% by mass or less, or 80% by mass or less relative to the entire binder resin. When the content of the butyral resin is within the above range, since the conductive paste has a moderate hardness, it is not easy to cause undesirable situations such as the printed film not being peeled off from the support film and the electrode being broken during thermal compression bonding.
[0053] In addition, the weight average molecular weight (Mw) of the butyral resin can be 30,000 to 300,000, 50,000 to 200,000, or 100,000 to 150,000. In addition, the glass transition temperature Tg of the butyral resin can be 50°C to 90°C, or 60°C to 80°C. By including the additives described below together with the butyral resin having the above-mentioned characteristics, a conductive paste with further improved adhesion can be obtained. In addition, the butyral resin can include one alone or two or more.
[0054] In addition, resins other than butyral resins may also be included as binder resins. As binder resins other than the above, there are no particular limitations, and known resins may be used, for example, cellulose resins such as methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and nitrocellulose, acrylic resins, etc. Among them, from the viewpoints of solubility in solvents, combustion decomposition, etc., it is preferred to include a cellulose resin, and more preferably to include ethyl cellulose.
[0055] For example, when a cellulose resin is included as the binder resin, the weight average molecular weight (Mw) may be 10,000 or more and 300,000 or less. In addition, the hydroxyl value of the cellulose resin is not particularly limited, but is preferably 0.1 mgKOH / g or more and 15 mgKOH / g or less. In addition, the cellulose resin may include one type alone or two or more types.
[0056] In addition, when the binder resin includes a cellulose resin and a butyral resin, from the viewpoint of improving adhesion, relative to the total content (100% by mass) of the cellulose resin and the butyral resin, it can include more than 20% by mass of the butyral resin, or more than 40% by mass, or more than 50% by mass, or more than 60% by mass. When the content of the two resins is within the above range, sometimes the adhesion is further improved, and the bonding strength between the dry film and the raw sheet (substrate) is improved. In addition, the upper limit of the content of the butyral resin is not particularly limited, and can be less than 100% by mass, or less than 90% by mass, or less than 80% by mass. When the content of the two resins is within the above range, the conductive paste can have a moderate hardness, and it is not easy to have undesirable conditions such as the printed film not peeling off from the supporting film and the electrode breaking during hot pressing.
[0057] The content of the binder resin is preferably 0.5% by mass or more and 10% by mass or less, and more preferably 1% by mass or more and 7% by mass or less, relative to the entire conductive paste. When the content of the binder resin is within the above range, the conductivity and dispersibility are excellent.
[0058] The content of the binder resin is preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 14 parts by mass or less, based on 100 parts by mass of the conductive powder.
[0059] (Organic Solvent)
[0060] The organic solvent is not particularly limited, and any known organic solvent that can dissolve the binder resin can be used. Examples of the organic solvent include terpene solvents, acetate solvents, ether solvents, and ketone solvents.
[0061] Examples of the terpene solvent include terpineol, dihydroterpineol, and dihydroterpineol acetate.
[0062] Examples of the acetate solvent include isobornyl acetate, isobornyl propionate, isobornyl butyrate, and isobornyl isobutyrate; glycol ether acetates such as ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, 3-methoxy-3-methylbutyl acetate, and 1-methoxypropyl-2-acetate; glycol diacetates such as propylene glycol diacetate, 1,4-butanediol diacetate, 1,3-butanediol diacetate, and 1,6-hexanediol diacetate; and cyclohexanol acetate.
[0063] Examples of the ether solvent include propylene glycol monoalkyl ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether; glycol ethers such as diethylene glycol mono-2-ethylhexyl ether, ethylene glycol mono-2-ethylhexyl ether, diethylene glycol monohexyl ether, and ethylene glycol monohexyl ether; dipropylene glycol methyl-n-propyl ether, dipropylene glycol methyl-n-butyl ether, and dipropylene glycol dimethyl ether.
[0064] Examples of the ketone solvent include methyl isobutyl ketone, diisobutyl ketone, etc. When the ketone solvent is contained, the viscosity can be adjusted without impairing the dispersibility, and the drying property can be improved.
[0065] As the organic solvent, at least one selected from the group consisting of terpineol, dihydroterpineol, dihydroterpineol acetate, propylene glycol monobutyl ether, and diethylene glycol monobutyl ether acetate is preferably included. By including the above organic solvent, the compatibility with the binder resin is excellent, and the dispersibility of the filler is excellent.
[0066] The content of the organic solvent (total) is preferably 20% by mass or more and 60% by mass or less, and more preferably 25% by mass or more and 45% by mass or less, relative to the total amount of the conductive paste. When the content of the organic solvent is within the above range, the conductivity and dispersibility are excellent.
[0067] The content of the organic solvent is preferably 50 parts by mass or more and 130 parts by mass or less, and more preferably 60 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the organic solvent is within the above range, the conductivity and dispersibility are excellent.
[0068] In addition, the organic solvent may be used alone or in combination of two or more. For example, when two or more organic solvents are included, at least one selected from the group consisting of terpineol, dihydroterpineol, dihydroterpineol acetate, propylene glycol monobutyl ether (PNB), and diethylene glycol monobutyl ether acetate, and a hydrocarbon solvent may be included. In addition, at least one selected from methyl isobutyl ketone and diisobutyl ketone may be included together with the above organic solvents.
[0069] Examples of hydrocarbon solvents include solvents containing tridecane, nonane, cyclohexane, etc., mineral spirits, cycloalkane solvents, etc. Among them, mineral spirits are preferably contained. The content of the hydrocarbon solvent may be 10% by mass or more and 50% by mass or less, or 20% by mass or more and 40% by mass or less relative to the total amount of the organic solvent.
[0070] (additive)
[0071] The conductive paste according to the present embodiment contains an additive. As the additive, it is preferable to contain a compound capable of lowering the glass transition temperature of a dried product (for evaluation) to a specific range.
[0072] The above-mentioned compound is not particularly limited as long as it can adjust the glass transition temperature Tg of the dried body to a specific range. For example, it is preferably at least one compound selected from the group consisting of a compound having an ester structure, a compound having an amide structure, a compound having a phosphate group, and a compound having a rosin skeleton. Among them, a compound having an ester structure, a compound having an amide structure, and a compound having a phosphate group are more preferred.
[0073] It is believed that the above-mentioned compound can adjust the glass transition temperature of the dry film to a specific range by hindering the interaction between the resins contained in the conductive paste. In addition, it is believed that by adding the above-mentioned compound, the dry film is appropriately softened, and the surface of the dry film is easily deformed due to softening, thereby expanding the contact area with the bonded surface during pressure bonding, and the resins whose interactions are hindered are easily entangled at the bonding interface, thereby improving the adhesion between the dry film and the ceramic green sheet (dielectric layer).
[0074] In addition, as the above-mentioned compound, for example, a compound that can reduce the glass transition temperature Tg of the dry product (for evaluation) by preferably 10°C or more, more preferably 13°C or more, more preferably 15°C or more, and further preferably 20°C or more compared to the glass transition temperature Tg' of the dry product (for evaluation) not containing the above-mentioned compound can be selected.
[0075] In addition, the temperature at which the weight loss rate of the above-mentioned compound in thermogravimetric analysis reaches the maximum (maximum thermal decomposition temperature) can be, for example, 200°C or more, or 220°C or more, and preferably 250°C or more. When the maximum thermal decomposition temperature is within the above range, delamination and cracking of the laminate can be suppressed. In addition, the upper limit of the maximum thermal decomposition temperature is not particularly limited, and can be, for example, 450°C or less, 400°C or less, or 350°C or less.
[0076] In addition, the maximum thermal decomposition temperature refers to the value obtained by the thermogravimetric (TG) method using the following method. That is, using a thermal decomposition weight measuring device (NETZSCH manufactured, STA25000REGULUS), under a nitrogen atmosphere, the temperature is raised from 20°C to 550°C at a heating rate of 5°C / min, and when the weight loss at this time is measured, the temperature at which the differential heating loss reaches the maximum is taken as the maximum thermal decomposition temperature.
[0077] Specific examples of the compound that can lower the glass transition temperature of a dried product (for evaluation) to a specific range will be described below.
[0078] (a) Compounds having an ester structure
[0079] As the compound having an ester structure, a compound having a structural part represented by the following formula (A) or formula (B) (hereinafter also referred to as an “ester compound”) is preferred.
[0080]
Chemistry 1
[0081]
[0082] (Among them, R 1 It represents a saturated or unsaturated aliphatic hydrocarbon group having 2 to 12 carbon atoms. The aliphatic hydrocarbon group may be linear or branched, and one or more methylene groups (-CH2-) contained in the aliphatic hydrocarbon group may be substituted by oxygen (-O-).
[0083] The ester compound more preferably has a structure represented by the following structural formula (1) or the following structural formula (2).
[0084]
Chemistry 2
[0085]
[0086] In the above formulas (1) and (2), R 1 , R 2 , R 3 Each independently represents a saturated or unsaturated aliphatic hydrocarbon group having 2 to 12 carbon atoms, the aliphatic hydrocarbon group may be linear or branched, and one or more methylene groups (-CH2-) contained in the aliphatic hydrocarbon group may be substituted by oxygen (-O-). 1 , R 2 and R 3 The number of carbon atoms in the above-mentioned group includes the number of carbon atoms of a methylene group (-CH2-) substituted by oxygen (-O-).
[0087] In the above formulas (1) and (2), R 1 and R 3 The lower limit of the number of carbon atoms of each independently may be 3 or more, or 5 or more. 1 and R 3 The upper limit of the number of carbon atoms of each independently may be 10 or less, or 8 or less. 1 and R 3 The number of carbon atoms may also be the same.
[0088] In addition, R 1 and R 3 It may be an unsubstituted aliphatic hydrocarbon group or, for example, an aliphatic hydrocarbon group in which one methylene group (-CH2-) is replaced by oxygen (-O-). 1 and R 3 The same structure may also be used.
[0089] In (1) and (2) above, R 2 The lower limit of the number of carbon atoms may be 3 or more. 2 The upper limit of the number of carbon atoms in may be 10 or less, or 8 or less. 2 For example, it may be an aliphatic hydrocarbon group in which one or more methylene groups (-CH2-) are substituted with oxygen (-O-), or it may be an unsubstituted aliphatic hydrocarbon group.
[0090] The molecular weight of the ester compound is preferably 250 to 3000, more preferably 250 to 1000, and even more preferably 250 to 500. When the molecular weight of the ester compound is within the above range, adhesion to the ceramic green sheet (dielectric layer) is further improved.
[0091] In addition, the content of the above-mentioned ester compound can be appropriately adjusted so that the glass transition temperature Tg of the dried body (for evaluation) is within a specific range. The content of the above-mentioned ester compound is, for example, 0.01% by mass or more and 1.0% by mass or less relative to the conductive paste as a whole. When the content of the above-mentioned ester compound is within the above-mentioned range, the adhesion between the dry film and the ceramic green sheet (dielectric layer) can be improved. In addition, from the viewpoint of further improving the adhesion, the lower limit of the content of the ester compound can be 0.05% by mass or more relative to the conductive paste as a whole, or it can be 0.1% by mass or more. In addition, the upper limit of the content of the ester compound can be 0.7% by mass or less, or it can be 0.4% by mass or less.
[0092] The upper limit of the content of the ester compound is not particularly limited, and may be, for example, 2% by mass or less, 1.8% by mass or less, 1.5% by mass or less, or 1.0% by mass or less. When the content of the ester compound exceeds 1.0% by mass, although the adhesion is improved, when the pressed body of the laminate of the dry film and the ceramic green sheet is subjected to a binder removal treatment, thermal decomposition may occur to generate gas. The content of the ester compound may be appropriately adjusted within the above range according to the use environment, etc.
[0093] In addition, the content of the ester compound can be appropriately set according to the type and content of the above-mentioned binder resin. For example, the content of the ester compound can be set according to the content of the butyral resin. Regarding the content of the ester compound, for example, relative to 100 parts by mass of the butyral resin, the ester compound can be contained in an amount of 10 parts by mass or more and 90 parts by mass or less, or 10 parts by mass or more and 60 parts by mass or less, or 10 parts by mass or more and 50 parts by mass or less.
[0094] (b) Compounds having an amide structure
[0095] Examples of the compound having an amide structure include a compound having a structural portion represented by the following formula (3) (hereinafter also referred to as an “amide compound”).
[0096]
Chemistry 3
[0097]
[0098] In the above formula (3), R 11 represents a saturated or unsaturated aliphatic hydrocarbon group having 8 to 25 carbon atoms, the aliphatic hydrocarbon group may be linear or branched, and one or more methylene groups (-CH2-) of the aliphatic hydrocarbon group may be substituted by oxygen (-O-), R 12It represents hydrogen, a saturated or unsaturated aliphatic hydrocarbon group having 1 to 6 carbon atoms, and the aliphatic hydrocarbon group may be straight-chain or branched, and one or more methylene groups (-CH2-) of the aliphatic hydrocarbon group may be substituted by oxygen (-O-). In addition, the amide compound may not contain an acidic group (e.g., a carboxyl group). In the case of containing an acidic group, the softening effect of the dried film may be reduced.
[0099] In addition, the amide compound preferably has a structure represented by the following structural formula (4) or the following structural formula (5).
[0100]
Chemistry 4
[0101]
[0102]
Chemistry 5
[0103]
[0104] In the above formulas (4) and (5), R 11 , R 15 Each independently represents a saturated or unsaturated aliphatic hydrocarbon group having 8 to 25 carbon atoms, the aliphatic hydrocarbon group may be linear or branched, and one or more methylene groups (-CH2-) of the aliphatic hydrocarbon group may be substituted by oxygen (-O-), R 12 , R 13 , R 14 Each independently represents hydrogen, a saturated or unsaturated aliphatic hydrocarbon group having 1 to 6 carbon atoms, the aliphatic hydrocarbon group may be linear or branched, and one or more methylene groups (-CH2-) of the aliphatic hydrocarbon group may be substituted by oxygen (-O-), R 16 represents a saturated or unsaturated aliphatic hydrocarbon group having 1 to 6 carbon atoms, the aliphatic hydrocarbon group may be linear or branched, and one or more methylene groups (-CH2-) of the aliphatic hydrocarbon group may be substituted by oxygen (-O-). 11 ~R 16 The number of carbon atoms in the above-mentioned group includes the number of carbon atoms of a methylene group (-CH2-) substituted by oxygen (-O-).
[0105] In the above formulas (3) to (5), R 11 and R 15 The lower limit of the number of carbon atoms of each independently may be 8 or more, 12 or more, or 15 or more. 11 and R 15 The number of carbon atoms may also be the same.
[0106] In addition, R 11 and R 15It may be an aliphatic hydrocarbon group in which one or more methylene groups (-CH2-) are substituted with oxygen (-O-), or it may be an unsubstituted aliphatic hydrocarbon group. 11 and R 15 The same structure may also be used.
[0107] In the above formulas (3) to (5), R 12 , R 13 , R 14 The upper limit of the number of carbon atoms may be 5 or less, or 3 or less. 12 , R 13 , R 14 It may be an unsubstituted aliphatic hydrocarbon group, or an aliphatic hydrocarbon group in which, for example, one or more methylene groups (-CH2-) are substituted with oxygen (-O-), or may be hydrogen.
[0108] In the above formula (5), R 16 The upper limit of the number of carbon atoms in may be 5 or less, 3 or less, or 2 or less. 16 It may be a saturated hydrocarbon group in which one or more methylene groups (-CH2-) are substituted with oxygen (-O-), or it may be an unsubstituted saturated hydrocarbon group.
[0109] The molecular weight of the amide compound is preferably 250 to 3000, more preferably 250 to 1000, and even more preferably 250 to 500. When the molecular weight of the amide compound is within the above range, adhesion to the ceramic green sheet (dielectric layer) is further improved.
[0110] In addition, the content of the above-mentioned amide compound can be appropriately adjusted so that the glass transition temperature Tg of the dried body is within a specific range. The content of the above-mentioned amide compound is preferably 0.01% by mass or more and 1.0% by mass or less relative to the conductive paste as a whole. When the content of the above-mentioned amide compound is within the above-mentioned range, the adhesion between the dry film and the ceramic green sheet (dielectric layer) is improved. In addition, from the viewpoint of further improving the adhesion, the content of the amide compound can be 0.05% by mass or more relative to the conductive paste as a whole, or it can be 0.1% by mass or more. In addition, the upper limit of the content of the amide compound can be 0.7% by mass or less, or it can be 0.4% by mass or less.
[0111] The upper limit of the content of the amide compound may be 2% by mass or less, 1.8% by mass or less, 1.5% by mass or less, 1.0% by mass or less, or less than 1.0% by mass. When the content of the amide compound exceeds 1.0% by mass, although the adhesion is improved, when the pressed body of the laminate of the dry film and the ceramic green sheet is subjected to a debonding process, thermal decomposition sometimes occurs to generate gas. The content of the amide compound can be appropriately adjusted within the above range according to the use environment, etc.
[0112] In addition, the content of the amide compound can be appropriately set according to the type and content of the above-mentioned binder resin. For example, the content of the amide compound can be set according to the content of the butyral resin. For example, relative to 100 parts by mass of the butyral resin, the amide compound can be contained in an amount of 10 parts by mass or more and 90 parts by mass or less, or 10 parts by mass or more and 60 parts by mass or less, or 10 parts by mass or more and 50 parts by mass or less.
[0113] (c) Compounds having a phosphate group
[0114] The compound having a phosphoric acid group (phosphoric acid compound) is a compound having a phosphoric acid group at the terminal. The phosphoric acid compound may have a polymer structure, for example.
[0115] The phosphoric acid compound may have a structure represented by the following structural formula (6-1), for example.
[0116]
Chemistry 6-1
[0117]
[0118] In the above formula (6-1), R each independently represents hydrogen, or a structure comprising one or more of the group consisting of an alkyl chain, an ether chain, and an ester chain, and at least one of R represents a structure comprising one or more of the group consisting of an alkyl chain, an ether chain, and an ester chain. In addition, when R has an ether chain, the ether chain may have a single ether structure or a polyether chain having multiple ether structures. In the case where R has an ester chain, the ester chain may have a single ester structure or multiple ester structures. In addition, the terminal phosphate group (acidic group) may also be neutralized by an amine.
[0119] The phosphoric acid compound may have a structure represented by the following structural formula (6-2), for example.
[0120]
Chemistry 6-2
[0121]
[0122] In the above formula (6-2), R represents a structure including one or more of the group consisting of an alkyl chain, a polyether chain, and a polyester chain. The phosphoric acid compound may have, for example, a polyether chain, or may have both a polyether chain and a polyester chain. In addition, R may also be a straight chain structure. In addition, the terminal phosphoric acid group (acidic group) may also be neutralized by an amine.
[0123] The molecular weight of the phosphate compound is preferably 250 to 3000, more preferably 1000 to 3000, and even more preferably 1500 to 2500. When the molecular weight of the phosphate compound is within the above range, adhesion to the ceramic green sheet (dielectric layer) is further improved.
[0124] In addition, the content of the above-mentioned phosphate compound can be appropriately adjusted so that the glass transition temperature Tg of the dried body is within a specific range. The content of the above-mentioned phosphate compound is, for example, 0.01% by mass or more and 1.0% by mass or less relative to the conductive paste as a whole. When the content of the above-mentioned phosphate compound is within the above-mentioned range, the adhesion between the dry film and the ceramic green sheet (dielectric layer) can be improved. In addition, from the viewpoint of further improving adhesion, the content of the phosphate compound can be 0.05% by mass or more relative to the conductive paste as a whole, or it can be 0.1% by mass or more. In addition, the upper limit of the content of the phosphate compound can be 0.7% by mass or less.
[0125] The upper limit of the content of the phosphate compound may be 2% by mass or less, 1.8% by mass or less, 1.5% by mass or less, 1.0% by mass or less, or less than 1.0% by mass. When the content of the phosphate compound exceeds 1.0% by mass, when the pressed body of the laminate of the dry film and the ceramic green sheet is subjected to a debonding process, thermal decomposition may sometimes occur to generate gas. The content of the phosphate compound may be appropriately adjusted within the above range according to the use environment, etc.
[0126] In addition, the content of the phosphoric acid compound can be appropriately set according to the type and content of the above-mentioned binder resin. For example, the content of the phosphoric acid compound can be set according to the content of the butyral resin. For example, relative to 100 parts by mass of the butyral resin, the phosphoric acid compound can be contained in an amount of 10 parts by mass or more and 90 parts by mass or less, or 10 parts by mass or more and 60 parts by mass or less, or 10 parts by mass or more and 50 parts by mass or less.
[0127] (d) Compounds having a rosin skeleton
[0128] As the compound having a rosin skeleton, a rosin derivative having a hydroxyl group or an amine group (hereinafter, also simply referred to as a "rosin derivative") is preferably included.
[0129] Here, the rosin derivative refers to a compound derived from abietic acid and the like, and examples thereof include abietic acid and its derivatives such as dehydroabietic acid, dihydroabietic acid, tetrahydroabietic acid, diabietic acid, neoabietic acid, pimaric acid-type resin acids such as levorotatory pimaric acid, hydrogenated rosins obtained by hydrogenating these, and disproportionated rosins obtained by disproportionating these, and compounds having a rosin skeleton. In addition, the rosin skeleton may include a structure in which two or more rosins are bonded, or may include a rosin ester structure.
[0130] Preferably, it is a rosin derivative having a hydroxyl group, more preferably having one or two hydroxyl groups, and further preferably having two hydroxyl groups. The hydroxyl value of the rosin derivative can be, for example, 10 mgKOH / g or more, or 20 mgKOH / g or more, or 50 mgKOH / g or more, or further can be 100 mgKOH / g or more. In addition, the upper limit of the hydroxyl value is not particularly limited, for example, 200 mgKOH / g or less. In addition, the rosin derivative preferably does not have an acidic group such as a carboxyl group. The acid value of the rosin derivative can be, for example, 20.0 mgKOH / g or less, or 5.0 mgKOH / g or less.
[0131] The molecular weight of the rosin derivative is preferably 250 to 3000, more preferably 250 to 2000, and even more preferably 250 to 1200. When the molecular weight of the rosin derivative is within the above range, adhesion to the ceramic green sheet (dielectric layer) is further improved.
[0132] In addition, the content of the above-mentioned rosin derivative can be appropriately adjusted so that the glass transition temperature Tg of the dried body is within a specific range. The content of the above-mentioned ester compound is preferably 0.01% by mass or more and 1.0% by mass or less relative to the conductive paste as a whole. When the content of the above-mentioned rosin derivative is within the above-mentioned range, the adhesion between the dry film and the ceramic green sheet (dielectric layer) is improved. In addition, from the viewpoint of further improving the adhesion, the content of the rosin derivative can be 0.1% by mass or more relative to the conductive paste as a whole.
[0133] The upper limit of the content of rosin derivatives can be less than 2 mass %, can be less than 1.8 mass %, can be less than 1.5 mass %, can be less than 1.0 mass %, can be less than 1.0 mass %. When the content of rosin derivatives exceeds 1 mass %, although it has high adhesion, when the pressed body of the laminated body of the dry film and the ceramic green sheet is debonded, thermal decomposition sometimes occurs and gas is generated. The content of rosin derivatives can be appropriately adjusted according to the use environment, etc. within the above range. In addition, the upper limit of rosin derivatives can be less than 0.7 mass %, and can be less than 0.4 mass %. In the conductive paste of the present embodiment, even if the upper limit of rosin derivatives is the above range, it can have high adhesion.
[0134] In addition, the content of the rosin derivative can be appropriately set according to the type and content of the above-mentioned binder resin. For example, the content of the rosin derivative can be set according to the content of the butyral resin. For example, relative to 100 parts by mass of the butyral resin, the rosin derivative can be contained in an amount of 10 parts by mass or more and 90 parts by mass or less, 10 parts by mass or more and 60 parts by mass or less, or 10 parts by mass or more and 50 parts by mass or less.
[0135] (b) Dispersant
[0136] The conductive paste may contain a dispersant as an additive. When a dispersant is contained, the dispersibility of the conductive powder and the ceramic powder can be improved. As the dispersant, for example, an acidic dispersant, an alkaline dispersant, a nonionic dispersant, an amphoteric dispersant, etc. may be contained, preferably at least one of an acidic dispersant and an alkaline dispersant, and more preferably an acidic dispersant. In addition, the above-mentioned dispersants may be used alone or in combination of two or more.
[0137] As the acidic dispersant, there may be included carboxylic acid dispersants such as higher fatty acids, polycarboxylic acid dispersants, phosphoric acid dispersants, acidic dispersants having acidic groups such as polymer surfactants, etc., preferably at least one of polycarboxylic acid dispersants and phosphoric acid dispersants. In addition, the polycarboxylic acid dispersant may also be a comb-type carboxylic acid having a comb-type structure.
[0138] The higher fatty acid may be an unsaturated carboxylic acid or a saturated carboxylic acid, and is not particularly limited, and examples thereof include higher fatty acids having 11 or more carbon atoms, such as stearic acid, oleic acid, myristic acid, palmitic acid, linoleic acid, lauric acid, and linolenic acid. Among them, oleic acid or stearic acid is preferred.
[0139] Examples of the acidic dispersant include oleoylsarcosine, which is a compound of glycine and oleic acid, and alkyl monoamine salt-type amide compounds using higher fatty acids such as stearic acid and lauric acid instead of oleic acid.
[0140] In addition, from the viewpoint of further improving the separation inhibition effect of the conductive powder and the ceramic powder, a dicarboxylic acid may also be included. A dicarboxylic acid is a carboxylic acid having two carboxyl groups (COO- groups). In addition, the average molecular weight of the dicarboxylic acid is not particularly limited, and for example, may be 200 or more and 1000 or less.
[0141] Examples of alkaline dispersants include aliphatic amines such as laurylamine, abietamine, cetylamine, myristicamine, and stearylamine. When the conductive paste contains the acidic dispersant and the alkaline dispersant, the dispersibility is sometimes better and the viscosity stability over time is also excellent.
[0142] For example, the conductive paste contains 0.01% to 3% by mass of the dispersant relative to the entire conductive paste. The upper limit of the content of the dispersant may be 2% by mass or less, 1% by mass or less, or 0.5% by mass or less. When the content of the dispersant is within the above range, the dispersibility of the conductive paste can be improved, or sheet erosion and poor peeling of the green sheet can be suppressed.
[0143] (c) Other additives
[0144] The conductive paste of the present embodiment may contain other additives in addition to the above components as necessary. As other additives, for example, conventionally known additives such as a defoamer, a plasticizer, a surfactant, and a thickener may be used.
[0145] (Conductive paste)
[0146] The method for producing the conductive paste according to the present embodiment is not particularly limited, and a conventionally known method can be used. The conductive paste can be produced by stirring and kneading the above components using, for example, a three-roll mill, a ball mill, a mixer, or the like.
[0147] The conductive paste can be suitably used in electronic components such as multilayer ceramic capacitors. The multilayer ceramic capacitor has a dielectric layer formed using a dielectric green sheet and an internal electrode layer formed using a conductive paste.
[0148] [Multilayer Ceramic Capacitors]
[0149] Hereinafter, embodiments of the multilayer ceramic capacitor of the present invention will be described with reference to the accompanying drawings. In the accompanying drawings, the components may be shown schematically or with a changed scale. Figure 1 The position and direction of the components are described using an XYZ orthogonal coordinate system shown in FIG. In the XYZ orthogonal coordinate system, the X direction and the Y direction are horizontal directions, and the Z direction is a vertical direction (up and down direction).
[0150] Figure 1A in and Figure 1 B in FIG. 1 is a diagram showing a multilayer ceramic capacitor 1. The multilayer ceramic capacitor 1 includes a ceramic multilayer body 10 in which dielectric layers 12 and internal electrode layers 11 are alternately stacked, and external electrodes 20.
[0151] The following is a description of a method for manufacturing a multilayer ceramic capacitor using the above-mentioned conductive paste. First, a conductive paste is printed on a ceramic green sheet and dried to form a dry film. After a plurality of ceramic green sheets having the dry film on the upper surface are stacked by crimping to obtain a laminate, the laminate is fired to be integrated, thereby manufacturing a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are alternately stacked. Thereafter, a pair of external electrodes 20 are formed at both ends of the ceramic laminate 10 to manufacture a multilayer ceramic capacitor 1. The following is a more detailed description.
[0152] First, a green sheet as an unfired ceramic sheet is prepared. As the green sheet, for example, a dielectric layer slurry obtained by adding a binder resin such as polyvinyl butyral and a solvent such as terpineol to a raw material powder of a predetermined ceramic such as barium titanate is coated on a supporting film such as a PET film in a sheet shape and dried to remove the solvent. In addition, the thickness of the dielectric layer composed of the green sheet is not particularly limited, but from the perspective of the requirement for miniaturization of the multilayer ceramic capacitor, it is preferably 0.05 μm or more and 3 μm or less.
[0153] Next, a plurality of sheets are prepared in which the conductive paste is printed and applied on one side of a green sheet and dried to form a dry film on one side of the green sheet. In addition, from the viewpoint of the requirement for thinning the internal electrode layer 11, the thickness of the dry film formed by the conductive paste is preferably 1 μm or less after drying.
[0154] Next, the green sheet is peeled off from the support film, and the green sheets and the dry films formed on one surface of the green sheets are alternately stacked, and then heated and pressurized to obtain a laminate. In addition, a protective ceramic green sheet not coated with the conductive paste may be further arranged on both sides of the laminate.
[0155] Next, after the laminate is cut into a predetermined size to form a raw chip, the raw chip is subjected to a debinding treatment and fired in a reducing atmosphere, thereby manufacturing a laminated ceramic fired body (ceramic laminate 10). In addition, the atmosphere in the debinding treatment is preferably air or N2 gas atmosphere. The temperature during the debinding treatment is, for example, above 200°C and below 400°C. In addition, it is preferred that the holding time of the above temperature during the debinding treatment is set to be above 0.5 hours and below 24 hours. In addition, in order to suppress the oxidation of the metal used in the internal electrode layer, the firing is performed in a reducing atmosphere. In addition, the temperature during the firing of the laminate is, for example, above 1000°C and below 1350°C, and the holding time of the temperature during the firing is, for example, above 0.5 hours and below 8 hours.
[0156] By firing the green chip, the organic binder in the ceramic green sheet is completely removed, and the raw material powder of the ceramic is fired to form the ceramic dielectric layer 12. In addition, the organic vehicle in the dry film is removed, and the nickel powder or the alloy powder containing nickel as the main component is sintered or melted to form an internal electrode layer 11, thereby forming a laminated ceramic fired body in which a plurality of dielectric layers 12 and internal electrode layers 11 are alternately stacked. In addition, from the viewpoint of bringing oxygen into the interior of the dielectric layer to improve reliability and suppressing reoxidation of the internal electrode, the laminated ceramic fired body after firing may be subjected to annealing treatment.
[0157] Then, a pair of external electrodes 20 are provided on the manufactured multilayer ceramic fired body, thereby manufacturing the multilayer ceramic capacitor 1. For example, the external electrode 20 includes an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. In addition, as a material of the external electrode 20, for example, copper, nickel, or an alloy thereof can be preferably used. In addition, electronic components other than multilayer ceramic capacitors can also be used.
[0158] Example
[0159] Hereinafter, the present invention will be described in detail based on Examples and Comparative Examples, but the present invention is not limited to these Examples at all.
[0160] [Evaluation method]
[0161] (Adhesion evaluation)
[0162] A conductive paste (sample) is applied to the surface of a pre-made raw sheet containing barium titanate and polyvinyl butyral to form a conductive paste film with a wet film thickness of 35 μm. The obtained raw sheet and the sheet consisting of the conductive paste film for internal electrodes formed on the surface are dried at 75°C for 20 minutes to form a dry film on the raw sheet. The dried sheet (dry film-raw sheet) is overlapped with other raw sheets in the form of the surface coated with the conductive paste being sandwiched by the raw sheets, and then pressed at a temperature of 40°C and a pressure of 20 MPa for 20 seconds to produce a laminate (for evaluation).
[0163] The obtained laminate was cut into 1 cm squares, and both sides of the laminate were respectively set in the clamps of a tensile tester (AGS-50NX manufactured by Shimadzu Corporation) using adhesive tape, and a tensile test was performed. The force at break (the force when the dried film is peeled off from the green sheet) was recorded at a test speed of 20 mm / min. The force at break of Comparative Example 1 was set as 100%, and the force at break of each was evaluated in %.
[0164] (Hardness measurement)
[0165] Using a micro Vickers hardness tester (manufactured by Shimadzu Corporation, HMV-G21DT), under the condition of a test force of 98mN, the surface (dry film side) of the raw sheet formed with a conductive paste film (dry film) made under the same conditions as the adhesion evaluation was measured at n=5 points, and their average values were obtained. The hardness measurement was performed by attaching the sample to a glass substrate and placing it on a heated workbench as a sample stand of the hardness tester, at unheated room temperature (25°C) and heated to 60°C. In addition, when measuring the Vickers hardness (60°C), the previously measured dry film was placed at 60°C for 3 minutes for state adjustment, and then the measurement was performed while maintaining the state after heating at 60°C.
[0166] (Determination of glass transition temperature Tg)
[0167] The components other than the conductive powder and the ceramic powder in the conductive paste, namely, the ethyl cellulose resin, the polyvinyl butyral resin, the additives and the organic solvent were weighed in the same manner as the amounts contained in the conductive paste, and mixed at 2000 rpm for 4 minutes using a rotary mixer (manufactured by THINKY, ARE-310), and then the obtained liquid (mixture) was applied to a PET film with a wet film thickness of 254 μm using an applicator, and dried at 120° C. for 40 minutes to obtain a sample for evaluation. In addition, the organic solvent in the mixture was removed during drying.
[0168] Using a differential scanning calorimeter (NETZSCH Japan Co., Ltd., DSC3100), 10 mg of the dried evaluation sample was placed in an aluminum pan, and the temperature was increased from 0°C to 140°C at a heating rate of 10°C / min under a nitrogen gas flow of 100 mL / min. The glass transition temperature Tg on the low temperature side was determined from the peak of the obtained endothermic curve.
[0169] (Thermal decomposition temperature measurement)
[0170] The thermal decomposition temperature of the additive used in the conductive paste was measured using a thermal decomposition weight measuring device (NETZSCH, STA25000REGULUS). The measurement temperature atmosphere was nitrogen, and the temperature was increased from 20°C to 550°C at a heating rate of 5°C / min. The temperature at which the differential heating loss reached the maximum, that is, the temperature at which the weight loss rate in the thermogravimetric analysis reached the maximum, was taken as the thermal decomposition temperature (maximum thermal decomposition temperature).
[0171] [Materials used]
[0172] (Conductive powder)
[0173] As the conductive powder, Ni powder (SEM average particle size: 0.2 μm) was used.
[0174] (Ceramic powder)
[0175] As the ceramic powder, barium titanate (BaTiO 3 , SEM average particle size: 0.10 μm) was used.
[0176] (Binder resin)
[0177] As the binder resin, polyvinyl butyral resin (PVB) and ethyl cellulose resin (EC) were used.
[0178] (Dispersant)
[0179] In the examples and comparative examples, as the dispersant (additive) commonly contained, a polycarboxylic acid-based dispersant, which is an acid-based dispersant, was used.
[0180] (additive)
[0181] As additives for adjusting the glass transition temperature Tg (including comparative examples), the following compounds were used.
[0182] (1) Phosphoric acid compound A (copolymer having a phosphoric acid group and an ester structure, molecular weight: 1600)
[0183] (2) Phosphoric acid compound B (copolymer having a phosphoric acid group neutralized with an amine and an ester structure, molecular weight: 2000)
[0184] (3) Phosphoric acid compound C: Copolymer of phosphate ester salt (alkyl ammonium salt)
[0185] (4) Ester compound: having the structure (R) of the following formula (a): 1 =CH3(CH2)3OC2H4-, R 2 =-(CH2)4-, R 3 =-C2H4O(CH2)3CH3)
[0186] (5) Amide compound: having the structure of the following formula (b)
[0187] (6) Rosin derivatives: having the structure of the following formula (c) (R = -CH2NH2)
[0188] (7) Polycarboxylic acid (having polyoxyalkylene as graft chain)
[0189] (8) Dicarboxylic acid (2-(octadecen-1-yl)succinic acid)
[0190]
Chemistry 7
[0191]
[0192]
Chemistry 8
[0193]
[0194]
Chemistry 9
[0195]
[0196] (Organic Solvent)
[0197] As the organic solvent, dihydroterpineol (DHT) and mineral spirits (MSA) were used.
[0198] [Example 1]
[0199] Conductive powder 49 mass%, ceramic powder 12 mass%, acid dispersant 0.15 mass%, phosphoric acid compound A (additive) 0.3 mass%, binder resin 2.5 mass% (PVB:EC=7:3 (mass ratio)) and organic solvent (DHT:MSA=60:40 (mass ratio)) as the balance were added, and the total amount was 100 mass%, and these materials were mixed to prepare conductive paste. The content of each material in the conductive paste and the evaluation results are shown in Table 1.
[0200] [Examples 2 to 11, Comparative Examples 1 to 4]
[0201] A conductive paste was prepared and evaluated in the same manner as in Example 1 except that the types and contents of the additives shown in Table 1 were changed. Table 1 shows the contents of the respective materials of the conductive paste and the evaluation results.
[0202]
[0203] (Evaluation results)
[0204] The conductive pastes of Examples 1 to 11 had a glass transition temperature (Tg) of 55° C. or less in a low temperature range, and had improved adhesion, compared with the conductive pastes of Comparative Examples 1 to 4.
[0205] Industrial Applicability
[0206] When the conductive paste of the present invention is used to form the internal electrodes of a multilayer ceramic capacitor, a multilayer ceramic capacitor with high reliability can be obtained with high productivity. Therefore, the conductive paste of the present invention is particularly suitable for use as a chip component of an electronic device such as a mobile phone or a digital device, that is, an internal electrode of a multilayer ceramic capacitor.
[0207] In addition, the technical scope of the present invention is not limited to the methods described in the above-mentioned embodiments, etc. Sometimes one or more of the requirements described in the above-mentioned embodiments, etc. are omitted. In addition, the requirements described in the above-mentioned embodiments, etc. can be appropriately combined. In addition, as long as the law permits, the disclosure of all the documents cited in the above-mentioned embodiments, etc. is cited as part of the record of this article. In addition, as long as the law permits, the contents of Japanese Patent Application No. 2022-052668, which is a Japanese patent application, are cited as part of the record of this article.
[0208] The embodiments of the present invention may include the following configurations.
[0209] [1] A conductive paste, wherein the conductive paste comprises conductive powder, a binder resin, an additive and an organic solvent,
[0210] The binder resin, the additive, and the organic solvent are mixed at the same content ratio as that of the conductive paste, and then dried to obtain a dried product having a glass transition temperature of 30° C. or more and 55° C. or less.
[0211] [2] The conductive paste according to [1], wherein the additive includes a compound capable of lowering the glass transition temperature of the dried body, and the compound is contained in an amount of 0.01% by mass to 2.0% by mass based on the entire conductive paste.
[0212] [3] The conductive paste according to [1] or [2], wherein the temperature at which the weight loss rate of the compound in thermogravimetric analysis reaches a maximum is 200° C. or higher.
[0213] [4] The conductive paste according to any one of [1] to [3], wherein the molecular weight of the compound is 250 or more and 3000 or less.
[0214] [5] The conductive paste according to any one of [1] to [4], wherein the additive further includes an acidic dispersant and / or an alkaline dispersant.
[0215] [6] The conductive paste according to any one of [1] to [5], wherein the conductive powder includes at least one metal powder selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof.
[0216] [7] The conductive paste according to any one of [1] to [6], wherein the conductive powder has an average particle size of 0.05 μm or more and 1.0 μm or less.
[0217] [8] The conductive paste according to any one of [1] to [7], wherein the binder resin contains a butyral-based resin.
[0218] [9] The conductive paste according to any one of [1] to [8], further comprising ceramic powder.
[0219]
[10] The conductive paste according to [9], wherein the ceramic powder contains barium titanate.
[0220]
[11] The conductive paste according to [9] or
[10] , wherein the average particle size of the ceramic powder is 0.01 μm or more and 0.5 μm or less.
[0221]
[12] The conductive paste according to any one of [9] to
[11] , wherein the ceramic powder is contained in an amount of 1% by mass or more and 20% by mass or less based on the entire conductive paste.
[0222]
[13] The conductive paste according to any one of [1] to
[12] , wherein the conductive paste is used for an internal electrode of a multilayer ceramic component.
[0223]
[14] An electronic component formed using the conductive paste according to any one of [1] to
[13] .
[0224]
[15] A multilayer ceramic capacitor comprising at least a laminated body in which a dielectric layer and an internal electrode layer are laminated,
[0225] The internal electrode layer is formed using the conductive paste described in
[13] .
[0226] Description of Reference Numerals
[0227] 1: Multilayer ceramic capacitor;
[0228] 10: Ceramic laminate;
[0229] 11: internal electrode layer;
[0230] 12: dielectric layer;
[0231] 20: external electrode;
[0232] 21: external electrode layer;
[0233] 22: Electroplating layer.
Claims
1. A conductive paste, wherein: The conductive paste comprises conductive powder, a binder resin, an additive and an organic solvent. The binder resin, the additive, and the organic solvent are mixed at the same content ratio as that of the conductive paste, and then dried to obtain a dried product having a glass transition temperature of 30° C. or more and 55° C. or less.
2. The conductive paste according to claim 1, wherein The additive includes a compound capable of lowering the glass transition temperature of the dried body, and the compound is contained in an amount of 0.01 mass % to 2.0 mass % based on the entire conductive paste.
3. The conductive paste according to claim 1, wherein The temperature at which the weight reduction rate of the compound in thermogravimetric analysis reaches a maximum is 200° C. or higher.
4. The conductive paste according to claim 1, wherein The molecular weight of the compound is 250 or more and 3000 or less.
5. The conductive paste according to claim 1, wherein The additives further include an acidic dispersant and / or an alkaline dispersant.
6. The conductive paste according to claim 1, wherein The conductive powder includes at least one metal powder selected from the group consisting of Ni, Pd, Pt, Au, Ag, Cu and alloys thereof.
7. The conductive paste according to claim 1, wherein The conductive powder has an average particle size of 0.05 μm or more and 1.0 μm or less.
8. The conductive paste according to claim 1, wherein The binder resin includes a butyral-based resin.
9. The conductive paste according to claim 1, wherein: The conductive paste further includes ceramic powder.
10. The conductive paste according to claim 9, wherein: The ceramic powder includes barium titanate.
11. The conductive paste according to claim 9, wherein The ceramic powder has an average particle size of 0.01 μm or more and 0.5 μm or less.
12. The conductive paste according to claim 9, wherein: The ceramic powder is contained in an amount of 1 mass % or more and 20 mass % or less based on the entire conductive paste.
13. The conductive paste according to claim 1, wherein The conductive paste is used for internal electrodes of a multilayer ceramic component.
14. An electronic component, wherein: The electronic component is formed using the conductive paste according to any one of claims 1 to 13.
15. A multilayer ceramic capacitor, wherein: The multilayer ceramic capacitor includes at least a laminated body in which a dielectric layer and an internal electrode layer are laminated. The internal electrode layer is formed using the conductive paste according to claim 13 .