Adhesive film for semiconductor, dicing die-bonded film, and method for manufacturing semiconductor device

By using acrylic resin and thermosetting components of aromatic ring structural units in the adhesive film for semiconductors, combined with inorganic fillers, the problem of decreasing adhesion is solved, high adhesion and HAST resistance are achieved, and semiconductor packages are ensured at high temperature and high humidity stability under conditions.

CN118974899APending Publication Date: 2024-11-15RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029853.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-17
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

After the existing adhesive film for semiconductors has improved the test resistance of high acceleration temperature and humidity stress, the adhesive strength decreases, making it difficult to take into account both HAST resistance and adhesion.

Method used

Using acrylic resin with aromatic ring structural units as elastomer, combined with thermosetting components and inorganic fillers, a semiconductor adhesive film with moderate thickness is prepared to provide high adhesion and HAST resistance during the burial of semiconductor chips and wires. .

Benefits of technology

The high adhesion and HAST resistance of the adhesive film for semiconductors are achieved, ensuring the stability and reliability of the semiconductor package under high temperature and high humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974899A_ABST
    Figure CN118974899A_ABST
Patent Text Reader

Abstract

The invention discloses an adhesive film for a semiconductor. The adhesive film for a semiconductor contains a thermosetting component, an elastomer, and an inorganic filler. The elastomer contains an acrylic resin having a structural unit derived from a monomer having an aromatic ring.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive film for semiconductor, a dicing-die bonding integrated film and a method for manufacturing a semiconductor device. Background Art

[0002] Stacked MCP (MultiChip Package) has become popular, which realizes high capacity by stacking semiconductor chips in multiple layers. Examples of stacked MCP include wire-embedded type and chip-embedded type semiconductor packages. The structure of a semiconductor package in which the wire is embedded through an adhesive film is sometimes called FOW (Film Over Wire). The structure of a semiconductor package in which the semiconductor chip is embedded through an adhesive film is sometimes called FOD (Film Over Die). As an example of a semiconductor package using FOD, there is a semiconductor package having a controller chip arranged at the bottom layer and an adhesive film in which the controller chip is embedded (see Patent Document 1). In the manufacture of a semiconductor package having a FOD or FOW structure, it is required that the semiconductor chip or the wire be sufficiently embedded through the adhesive film.

[0003] In recent years, with the trend of high integration, the line / space gap of wiring has become narrower, and such adhesive films are required to have good HAST (Highly Accelerated Temperature and Humidity Stress Test) resistance. As a method for improving the HAST resistance of adhesive films, for example, a method of using an acrylic resin having a low ratio of structural units derived from acrylonitrile has been proposed (see Patent Document 2).

[0004] Previous technical literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-175459

[0007] Patent Document 2: International Publication No. 2020 / 067186 Summary of the invention

[0008] Technical issues to be solved by the invention

[0009] However, in the conventional method, although HAST resistance is improved, adhesive strength may be reduced. Therefore, an adhesive film is required to have both HAST resistance and adhesive strength.

[0010] Therefore, a main object of the present invention is to provide an adhesive film for a semiconductor having excellent HAST resistance and high adhesive strength.

[0011] Means for solving technical problems

[0012] According to the research of the present inventors, it was found that the use of an acrylic resin having a structural unit derived from a monomer having an aromatic ring as an elastomer enables both HAST resistance and adhesive strength of an adhesive film for a semiconductor to be achieved, thereby completing the present invention.

[0013] One aspect of the present invention relates to an adhesive film for a semiconductor. The adhesive film for a semiconductor (hereinafter, sometimes referred to as an "adhesive film") contains a thermosetting component, an elastomer, and an inorganic filler. The elastomer contains an acrylic resin having a structural unit derived from a monomer having an aromatic ring.

[0014] One embodiment of the adhesive film may have a thickness of 60 to 150 μm. In this case, the adhesive film may be an adhesive film for FOD for bonding a semiconductor chip to a substrate while embedding another semiconductor chip.

[0015] Another embodiment of the adhesive film may have a thickness of 25 to 80 μm. In this case, the adhesive film may be a FOW adhesive film for burying a part or the whole of a wire connected to another semiconductor chip and bonding to another semiconductor chip.

[0016] The elastomer may further contain an acrylic resin having no structural unit derived from a monomer having an aromatic ring. The weight average molecular weight of the acrylic resin having no structural unit derived from a monomer having an aromatic ring may be 500,000 or more.

[0017] The content of the elastomer may be 10 to 60% by mass based on the total amount of the adhesive film.

[0018] The content of the inorganic filler may be 30 to 250 parts by mass based on 100 parts by mass of the thermosetting component.

[0019] Another aspect of the present invention relates to a dicing die bonding integrated film including a dicing film and the adhesive film disposed on the dicing film.

[0020] Another aspect of the present invention relates to a method for manufacturing a semiconductor device. One aspect of the method for manufacturing a semiconductor device includes the step of bonding a second semiconductor chip to a substrate on which a first semiconductor chip is mounted, via the adhesive film. In this case, the first semiconductor chip is buried in the adhesive film.

[0021] Another embodiment of the method for manufacturing a semiconductor device includes the step of bonding the second semiconductor chip to the first semiconductor chip via the adhesive film. In this case, a part or the entirety of the wire is embedded in the adhesive film.

[0022] In one aspect or another aspect of the method for manufacturing a semiconductor device, the first semiconductor chip may be a controller chip.

[0023] The present invention includes [1] to

[12] .

[0024] [1] An adhesive film for a semiconductor, comprising a thermosetting component, an elastomer and an inorganic filler,

[0025] The elastomer contains an acrylic resin having a structural unit derived from a monomer having an aromatic ring.

[0026] [2] The adhesive film for a semiconductor according to [1], which has a thickness of 60 to 150 μm.

[0027] [3] The adhesive film for a semiconductor according to [1] or [2], which is used to bond a semiconductor chip to a substrate while embedding another semiconductor chip.

[0028] [4] The adhesive film for a semiconductor according to [1], which has a thickness of 25 to 80 μm.

[0029] [5] The adhesive film for a semiconductor according to [1] or [4], which is used to bond a semiconductor chip to another semiconductor chip while burying a part or the whole of a wire connected to the other semiconductor chip.

[0030] [6] The adhesive film for a semiconductor according to any one of [1] to [5], wherein

[0031] The elastomer further contains an acrylic resin having no structural unit derived from a monomer having an aromatic ring,

[0032] The acrylic resin having no structural unit derived from a monomer having an aromatic ring has a weight average molecular weight of 500,000 or more.

[0033] [7] The adhesive film for a semiconductor according to any one of [1] to [6], wherein

[0034] The content of the elastomer is 10 to 60% by mass based on the total amount of the adhesive film for semiconductor.

[0035] [8] The adhesive film for a semiconductor according to any one of [1] to [7], wherein

[0036] The content of the inorganic filler is 30 to 250 parts by mass based on 100 parts by mass of the thermosetting component.

[0037] [9] A dicing die bonding integrated film comprising:

[0038] Cutting film; and

[0039] The adhesive film for a semiconductor according to any one of [1] to [8] provided on the dicing film.

[0040]

[10] A method for manufacturing a semiconductor device, comprising the step of bonding a second semiconductor chip to a substrate on which a first semiconductor chip is mounted, using the adhesive film for a semiconductor according to [1] or [2].

[0041] The first semiconductor chip is embedded in the adhesive film.

[0042]

[11] A method for manufacturing a semiconductor device, comprising the step of bonding a second semiconductor chip to a first semiconductor chip using the adhesive film for a semiconductor according to [1] or [4],

[0043] A wire is connected to the first semiconductor chip,

[0044] A part or the whole of the wire is buried in the adhesive film.

[0045]

[12] The method for manufacturing a semiconductor device according to

[10] or

[11] , wherein:

[0046] The first semiconductor chip is a controller chip.

[0047] Effects of the Invention

[0048] According to the present invention, there is provided an adhesive film for semiconductors having excellent HAST resistance and high adhesive strength. Furthermore, according to the present invention, there is provided a dicing die bonding integrated film having such an adhesive film for semiconductors. Furthermore, according to the present invention, there is provided a method for manufacturing a semiconductor device using the adhesive film for semiconductors or the dicing die bonding integrated film. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 It is a schematic cross-sectional view showing one embodiment of the adhesive film.

[0050] Figure 2 This is a schematic cross-sectional view showing one embodiment of a laminate including an adhesive film.

[0051] Figure 3 This is a schematic cross-sectional view showing one embodiment of a laminate including an adhesive film.

[0052] Figure 4 It is a schematic cross-sectional view showing one embodiment of a semiconductor device.

[0053] Figure 5 The present invention is a process diagram showing an embodiment of a method for manufacturing a semiconductor device.

[0054] Figure 6The present invention is a process diagram showing an embodiment of a method for manufacturing a semiconductor device.

[0055] Figure 7 The present invention is a process diagram showing an embodiment of a method for manufacturing a semiconductor device.

[0056] Figure 8 The present invention is a process diagram showing an embodiment of a method for manufacturing a semiconductor device.

[0057] Fig. 9 The present invention is a process diagram showing an embodiment of a method for manufacturing a semiconductor device.

[0058] Fig.10 It is a schematic cross-sectional view showing another embodiment of a semiconductor device.

[0059] Fig.11 It is a schematic cross-sectional view showing another embodiment of a semiconductor device. DETAILED DESCRIPTION

[0060] The present invention is not limited to the following examples. In the following examples, except for the cases specifically indicated, the constituent elements (including steps, etc.) are not essential. The sizes of the constituent elements in each figure are conceptual sizes, and the relative relationship between the sizes of the constituent elements is not limited to the relationship shown in each figure. The numerical values ​​and their ranges exemplified below do not limit the present invention either.

[0061] In this specification, the numerical range represented by "~" indicates a range including the numerical values ​​recorded before and after "~" as the minimum value and the maximum value, respectively. In the numerical range recorded in stages in this specification, the upper limit value or lower limit value recorded in one numerical range can also be replaced by the upper limit value or lower limit value of other numerical ranges recorded in stages. In the numerical range recorded in this specification, the upper limit value or lower limit value of the numerical range can be replaced by the value shown in the embodiment.

[0062] In the present specification, (meth)acrylate refers to acrylate or its corresponding methacrylate. The same applies to other similar expressions such as (meth)acrylate, (meth)acryloyl, (meth)acrylic acid copolymer, etc.

[0063] Regarding the materials exemplified below, unless otherwise specified, one kind may be used alone or in combination of two or more kinds. Regarding the content of each component in the composition, when there are a plurality of substances equivalent to each component in the composition, unless otherwise specified, it refers to the total amount of the plurality of substances present in the composition.

[0064] [Adhesive film for semiconductors (Adhesive film)]

[0065] Figure 1It is a schematic cross-sectional view showing one embodiment of the adhesive film. Figure 1 The adhesive film 10 shown contains a thermosetting component (hereinafter, sometimes referred to as "(A) component"), an elastomer (hereinafter, sometimes referred to as "(B) component"), and an inorganic filler (hereinafter, sometimes referred to as "(C) component".). In addition to the (A) component, the (B) component, and the (C) component, the adhesive film 10 may also contain a curing accelerator (hereinafter, sometimes referred to as "(D) component"), a coupling agent (hereinafter, sometimes referred to as "(E) component"), and other components. The adhesive film 10 may be a film formed of a thermosetting adhesive containing the (A) component, the (B) component, the (C) component, and the like. The adhesive film 10 may be in a semi-cured (B stage) state. The adhesive film 10 can be in a cured (C stage) state after the curing treatment.

[0066] (A) Ingredients: Thermosetting ingredients

[0067] The component (A) may contain a thermosetting resin (A1) as a compound having a functional group that forms a crosslinked structure by a thermosetting reaction, and may further contain a curing agent (A2) that reacts with the thermosetting resin. From the viewpoint of adhesion, the thermosetting resin may contain an epoxy resin as a compound having an epoxy group. In this case, the curing agent may contain a phenolic resin as a compound having a phenolic hydroxyl group.

[0068] Examples of epoxy resins used as thermosetting resins include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A novolac epoxy resins, bisphenol F novolac epoxy resins, stilbene epoxy resins, epoxy resins containing triazine skeletons, epoxy resins containing fluorene skeletons, trisphenol methane epoxy resins, biphenyl epoxy resins, xylylene epoxy resins, biphenyl aralkyl epoxy resins, naphthalene epoxy resins, polyfunctional phenols, and diglycidyl ether compounds of polycyclic aromatics such as anthracene. These can also be used alone or in combination of two or more. Among these, the epoxy resin may contain a cresol novolac epoxy resin, a bisphenol F epoxy resin, a bisphenol A epoxy resin, or a combination thereof from the viewpoint of the tackiness and flexibility of the film.

[0069] The epoxy resin may contain a liquid epoxy resin that is liquid at 30°C (epoxy resin having a softening point of 40°C or less). That is, the epoxy resin may be a combination of a liquid epoxy resin and a solid epoxy resin that is solid at 30°C (epoxy resin having a softening point exceeding 40°C). In addition, in this specification, the softening point refers to a value measured by a ring and ball method in accordance with JIS K7234. The content of the liquid epoxy resin may be 3 to 15% by mass based on the total amount of the adhesive film. By containing a liquid epoxy resin in a thermosetting resin, the softness of the adhesive film tends to be improved. In addition, by combining a liquid epoxy resin and a solid epoxy resin, the embedding property of semiconductor chips and wires tends to be improved.

[0070] Commercially available products of liquid epoxy resins include, for example, EXA-830CRP (trade name, manufactured by DIC Corporation, liquid at 30°C), YDF-8170C (trade name, manufactured by NIPPON STEEL Chemical & Material Co., Ltd., liquid at 30°C), and EP-4088S (trade name, manufactured by ADEKA CORPORATION, liquid at 30°C).

[0071] The epoxy equivalent of the epoxy resin is not particularly limited and may be 90 to 300 g / eq or 110 to 290 g / eq. When the epoxy equivalent of the epoxy resin is within such a range, the bulk strength of the adhesive film is maintained and the fluidity of the thermosetting adhesive when forming the adhesive film tends to be easily ensured.

[0072] As the phenolic resin used as a curing agent, for example, phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, aminophenol and / or α-naphthol, β-naphthol, dihydroxynaphthalene and other phenols and compounds with aldehyde groups such as formaldehyde are condensed or co-condensed under an acidic catalyst to obtain a novolac type phenolic resin, a phenol aralkyl resin and a naphthol aralkyl resin synthesized by allylated bisphenol A, allylated bisphenol F, allylated naphthalene diol, phenol novolac, phenol and / or naphthols and dimethoxy-p-xylene or bis(methoxymethyl)biphenyl. These can also be used alone or in combination of two or more. The phenolic resin can contain a phenyl aralkyl type phenolic resin, a phenol novolac resin or a combination thereof.

[0073] The hydroxyl equivalent of the phenolic resin may be 70 g / eq or more, or 70 to 300 g / eq. When the hydroxyl equivalent of the phenolic resin is 70 g / eq or more, the storage elastic modulus of the adhesive film tends to be further increased. When the hydroxyl equivalent of the phenolic resin is 300 g / eq or less, the generation of foaming and degassing can be further suppressed.

[0074] Examples of commercially available phenolic resins include PSM-4326 (trade name, manufactured by Gunei Chemical Industry Co., Ltd., softening point: 120° C.), J-DPP-140 (trade name, manufactured by JFE Chemical Corporation, softening point: 140° C.), GPH-103 (trade name, manufactured by Nippon Kayaku Co., Ltd., softening point: 99 to 106° C.), MEH-7800M (trade name, manufactured by MEIWA PLASTIC INDUSTRIES, LTD., softening point: 80° C.), J-DPP-85 (trade name, manufactured by JFE Chemical Corporation, softening point: 85° C.), and MEH-5100-5S (trade name, manufactured by MEIWA PLASTIC INDUSTRIES, LTD., softening point: 65° C.).

[0075] When the thermosetting resin contains an epoxy resin and the curing agent contains a phenolic resin, from the perspective of curability, the ratio of the epoxy equivalent of the epoxy resin to the hydroxyl equivalent of the phenolic resin (epoxy equivalent: hydroxyl equivalent) can be 0.30 / 0.70 to 0.70 / 0.30, 0.35 / 0.65 to 0.65 / 0.35, 0.40 / 0.60 to 0.60 / 0.40, or 0.45 / 0.55 to 0.55 / 0.45. When the equivalent ratio is 0.30 / 0.70 or more, there is a tendency to obtain more sufficient curability. When the equivalent ratio is 0.70 / 0.30 or less, it is possible to prevent the viscosity from becoming too high and obtain more sufficient fluidity.

[0076] The softening point of the curing agent may be 50 to 200° C. or 60 to 150° C. A curing agent having a softening point of 200° C. or lower tends to have good compatibility with the thermosetting resin.

[0077] Based on the total amount of the adhesive film, the content of component (A) (the total content of the thermosetting resin and the curing agent) may be 10% by mass or more, or 15% by mass or more, 20% by mass or more, 23% by mass or more, 25% by mass or more, or 30% by mass or more. When the content of component (A) is 10% by mass or more based on the total amount of the adhesive film, the adhesive force of the adhesive film tends to be improved. From the viewpoint of film formability, the content of component (A) may be 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, or 45% by mass or less based on the total amount of the adhesive film.

[0078] (B) Component: Elastomer

[0079] The component (B) may contain an acrylic resin having a structural unit derived from a monomer having an aromatic ring (hereinafter, sometimes referred to as a "first acrylic resin"), and further contain an acrylic resin having no structural unit derived from a monomer having an aromatic ring (hereinafter, sometimes referred to as a "second acrylic resin").

[0080] The first acrylic resin is an acrylic resin (acrylic rubber) having a structural unit derived from a monomer having a (meth)acryloyl group as a main component. Examples of monomers having a (meth)acryloyl group include (meth)acrylate ((meth)acrylate), (meth)acrylic acid, (meth)acrylonitrile, and the like. Based on the total amount of structural units constituting the first acrylic resin, the content of structural units derived from monomers having a (meth)acryloyl group may be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more. The first acrylic resin may have structural units derived from (meth)acrylates having crosslinking functional groups such as epoxy groups, alcoholic or phenolic hydroxyl groups, and carboxyl groups. In the case where the first acrylic resin has structural units derived from (meth)acrylates having crosslinking functional groups, the adhesive strength after curing can be improved by heating to react with component (A).

[0081] The first acrylic resin has a structural unit derived from a monomer having an aromatic ring. The (B) component contains such a first acrylic resin, which tends to improve the adhesive force of the adhesive film. Examples of monomers having an aromatic ring include monomers having an aromatic ring and having a (meth)acryloyl group (monomers having an aromatic ring and having a (meth)acryloyl group), monomers having an aromatic ring and not having a (meth)acryloyl group (monomers having an aromatic ring and not having a (meth)acryloyl group), and the like.

[0082] Examples of the monomer having an aromatic ring and a (meth)acryloyl group include phenyl (meth)acrylate, benzyl (meth)acrylate, hydroxybenzyl (meth)acrylate, phenoxyethyl (meth)acrylate, hydroxyphenyl (meth)acrylate, (meth)acryloyloxyethyl phthalate, phenoxy polyethylene glycol (meth)acrylate, and ethoxylated nonylphenyl ether (meth)acrylate.

[0083] Examples of monomers having an aromatic ring and not having a (meth)acryloyl group include styrene; styrene derivatives such as α-methylstyrene, ethylstyrene, butylstyrene, isobutylstyrene, propylstyrene, isopropylstyrene, fluorostyrene, chlorostyrene, bromostyrene, styrenesulfonic acid, and hydroxystyrene (vinylphenol); and aromatic vinyl compounds and their derivatives such as vinyltoluene, vinylpyridine, isopropenylphenol, allylphenol, vinylnaphthalene, vinylanthracene, vinylphenanthrene, and vinylpyrene.

[0084] The content of the structural unit derived from the monomer having an aromatic ring may be 1 mass % or more, 3 mass % or more, or 5 mass % or more, and may be 30 mass % or less, 25 mass % or less, or 20 mass % or less, based on the total amount of structural units constituting the first acrylic resin.

[0085] The glass transition temperature (Tg) of the first acrylic resin may be above 0°C or above 3°C. When the Tg of the first acrylic resin is above 0°C, the adhesive strength of the adhesive film can be further improved, and the softness of the adhesive film can be prevented from becoming too high. As a result, the adhesive film is easily cut when the wafer is cut, and burrs can be prevented. The upper limit of the Tg of the first acrylic resin is not particularly limited, for example, it may be below 55°C, below 50°C, below 45°C, below 40°C, below 35°C, below 30°C, or below 25°C. When the Tg of the first acrylic resin is below 55°C, there is a tendency to improve the lamination of the wafer. As a result, the adhesive force is improved, and the effect of preventing the chip from flying after cutting is improved. In addition, it is possible to prevent the cracking during cutting caused by the reduced adhesion to the semiconductor wafer. In addition, in this specification, the glass transition temperature (Tg) refers to the value measured using a DSC (thermal differential scanning calorimeter) (for example, manufactured by Rigaku Corporation, ThermoPlus 2). By adjusting the type and content of the structural unit constituting the first acrylic resin, the Tg of the first acrylic resin can be adjusted to a desired range.

[0086] The weight average molecular weight (Mw) of the first acrylic resin can be more than 100,000, more than 200,000, or more than 300,000, and can be less than 3,000,000, less than 2,000,000, or less than 1,000,000. When the Mw of the first acrylic resin is within such a range, film formation, film strength, flexibility, viscosity, etc. can be properly controlled, and reflow (reflow) is excellent, and embedding can be improved. In addition, in this specification, Mw refers to the value obtained by measuring using gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene. In addition, when multiple peaks are observed in GPC, the weight average molecular weight of the peak caused by the highest peak intensity is defined as the weight average molecular weight in this specification.

[0087] Based on the total amount of component (B), the content of the first acrylic resin may be 20 to 100% by mass. When the content of the first acrylic resin is 20% by mass or more based on the total amount of component (B), it is easy to take into account both the HAST resistance and the adhesive force of the adhesive film. Based on the total amount of component (B), the content of the first acrylic resin may be 22% by mass or more or 25% by mass or more, and may be 90% by mass or less, 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, 45% by mass or less, or 40% by mass or less.

[0088] The second acrylic resin is an acrylic resin (acrylic rubber) having a structural unit from a monomer having a (meth) acryloyl group as a main component and not having a structural unit from a monomer having an aromatic ring. That is, the second acrylic resin can be called an acrylic resin (acrylic rubber) from which the structural unit from the monomer having an aromatic ring is removed from the first acrylic resin. Based on the total amount of structural units constituting the second acrylic resin, the content of the structural unit from the monomer having a (meth) acryloyl group can be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more. The second acrylic resin can have a structural unit from a (meth) acrylate having a crosslinking functional group such as an epoxy group, an alcoholic or phenolic hydroxyl group, a carboxyl group, etc. In the case where the second acrylic resin has a structural unit from a (meth) acrylate having a crosslinking functional group, the adhesive strength after curing can be improved by heating the reaction with the (A) component.

[0089] The glass transition temperature (Tg) of the second acrylic resin may be 5° C. or higher, or 8° C. or higher. The upper limit of Tg of the second acrylic resin is not particularly limited, and may be, for example, 55° C. or lower, 50° C. or lower, 45° C. or lower, 40° C. or lower, 35° C. or lower, 30° C. or lower, or 25° C. or lower.

[0090] The weight average molecular weight (Mw) of the second acrylic resin may be 500,000 or more, 600,000 or more, or 700,000 or more, and may be 3,000,000 or less, 2,000,000 or less, or 1,000,000 or less.

[0091] The content of the second acrylic resin may be 0 to 80% by mass based on the total amount of the component (B). The content of the second acrylic resin may be 78% by mass or less or 75% by mass or less, and may be 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 55% by mass or more, or 60% by mass or more based on the total amount of the component (B).

[0092] From the viewpoint of HAST resistance, the first acrylic resin and the second acrylic resin may be acrylic resins having a low ratio of structural units derived from (meth)acrylonitrile. For example, the first acrylic resin and the second acrylic resin may be acrylic resins having an area of ​​an absorption peak derived from stretching vibration of a carbonyl group in an infrared absorption spectrum (IR spectrum) as PA CO The area of ​​the peak derived from the stretching vibration of the nitrile group is defined as PA CN When , an acrylic resin that satisfies the conditions of the following formula (1) is used.

[0093] PA CN / PA CO ≤≤0.100 (1)

[0094] Here, the carbonyl group mainly originates from (meth)acrylate as a structural unit, and the nitrile group mainly originates from (meth)acrylonitrile as a structural unit. In addition, the area of ​​the absorption peak derived from the stretching vibration of the carbonyl group (PA CO ) and the peak area derived from the stretching vibration of the nitrile group (PA CN ) can be calculated, for example, by the following method.

[0095] First, the transmission IR spectrum of the mixture of the first acrylic resin and the second acrylic resin or the adhesive film containing them was measured by the KBr tablet method, with the vertical axis representing the absorbance and the horizontal axis representing the wave number (cm -1 ) to display the spectrum. For example, FT-IR6300 (manufactured by JASCO Corporation, light source: high brightness ceramic light source, detector: DLATGS) can be used to measure the IR spectrum. In the displayed spectrum, the area of ​​the absorption peak derived from the stretching vibration of the carbonyl group (PA CO ) is defined as the wavelength of 1650cm on the connecting spectrum. -1 and 1800cm -1 The straight line between these two points is the baseline and the area of ​​the absorbance enclosed by the spectrum and the baseline. The area of ​​the peak derived from the stretching vibration of the nitrile group (PA CN ) is defined as connecting 2230cm -1 and 2300cm -1 The straight line between these two points is the baseline and the area of ​​absorbance enclosed by the spectrum and the baseline. CO and PA CN , which can calculate PA CN / PA CO .

[0096] PA of the first acrylic resin and the second acrylic resin CN / PA COIt may be 0.100 or less, or 0.090 or less, 0.080 or less, 0.070 or less, 0.060 or less, 0.050 or less, 0.040 or less, 0.030 or less, or 0.020 or less. CN / PA CO When it is 0.100 or less, the cohesive force of the acrylic resin decreases, so there is a tendency that embedding properties improve.

[0097] In addition to the first acrylic resin and the second acrylic resin, the component (B) may further contain other elastomers. Examples of other elastomers include polyester resins, polyamide resins, polyimide resins, silicone resins, butadiene resins, and modified forms of these resins. The content of other elastomers may be 0 to 20% by mass based on the total amount of the component (B).

[0098] The content of component (B) may be 10 to 60% by mass based on the total amount of the adhesive film. When the content of component (B) is 10% by mass or more based on the total amount of the adhesive film, the embedding property of the adhesive film tends to be improved, and when it is 60% by mass or less, the adhesive force of the adhesive film tends to be improved. Based on the total amount of the adhesive film, the content of component (B) may be 15% by mass or more, 20% by mass or more, 25% by mass or more, or 30% by mass or more, and may be 55% by mass or less, 50% by mass or less, 45% by mass or less, 40% by mass or less, or 38% by mass or less.

[0099] (C) Ingredients: Inorganic filler

[0100] (C) component can be at least one selected from the group consisting of aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, boron nitride and silicon dioxide. (C) component can contain silicon dioxide from the viewpoint of adjusting the melt viscosity.

[0101] From the perspective of fluidity, the average particle size of the (C) component can be 0.01 μm (10 nm) or more, 0.03 μm (30 nm) or more, 0.05 μm (50 nm) or more, or 0.1 μm (100 nm) or more, and can be 1.5 (1500 nm) μm or less, 1.0 μm (1000 nm) or less, 0.8 μm (800 nm) or less, or 0.6 μm (600 nm) or less. Two or more (C) components with different average particle sizes can also be combined. Here, the average particle size refers to the particle size with a cumulative frequency of 50% in the particle size distribution obtained by the laser diffraction / scattering method. In addition, the average particle size of the (C) component can also be obtained by using an adhesive film containing the (C) component. In this case, the average particle size of the component (C) can be determined by applying a laser diffraction / scattering method to prepare a dispersion liquid, and then dispersing the residue obtained by decomposing the resin component by heating the adhesive film in a solvent to obtain a particle size distribution.

[0102] The adhesive film may contain the first inorganic filler and the second inorganic filler satisfying the following conditions: The adhesive film contains the first inorganic filler and the second inorganic filler, so that embedding property can be improved, and further, after curing, breaking strength, adhesive force, etc. can be improved.

[0103] The average particle size of the first inorganic filler is 300 to 1000 nm.

[0104] The average particle size of the second inorganic filler is 0.05 to 0.70 times the average particle size of the first inorganic filler.

[0105] The total content of the first inorganic filler and the second inorganic filler (component (C)) is 10 to 60% by mass based on the total amount of the adhesive film.

[0106] The average particle size of the first inorganic filler is 300 to 1000 nm, and may be 350 nm or more, 400 nm or more, or 450 nm or more, and may be 900 nm or less, 800 nm or less, 700 nm or less, or 600 nm or less.

[0107] The average particle size of the second inorganic filler may be less than 300 nm, or may be 250 nm or less, 220 nm or less, or 200 nm or less. The average particle size of the second inorganic filler may be, for example, 10 nm or more, 50 nm or more, or 100 nm or more.

[0108] These average particle sizes refer to the particle sizes with a cumulative frequency of 50% in the particle size distribution obtained by the laser diffraction / scattering method. In addition, the average particle sizes of the first inorganic filler and the second inorganic filler can also be obtained by using an adhesive film containing the first inorganic filler and the second inorganic filler. In this case, the residue obtained by decomposing the resin component by heating the adhesive film is dispersed in a solvent to prepare a dispersion liquid, and based on the particle size distribution obtained by applying the laser diffraction / scattering method thereto, the value of the peak in the range of 300 to 1000 nm can be used as the average particle size of the first inorganic filler, and the value of the peak in the range of less than 300 nm can be used as the average particle size of the second inorganic filler.

[0109] The average particle size of the second inorganic filler is 0.05 to 0.70 times the average particle size of the first inorganic filler. The average particle size of the second inorganic filler may be 0.10 times or more, 0.20 times or more, or 0.30 times or more, and 0.60 times or less, 0.50 times or less, or 0.40 times or less.

[0110] Based on the total amount of the adhesive film, the content of the first inorganic filler can be 5 to 60 mass%, or it can be more than 6 mass%, more than 8 mass%, or more than 10 mass%, and it can be less than 55 mass%, less than 45 mass%, less than 40 mass%, less than 35 mass%, or less than 30 mass%.

[0111] Based on the total amount of the adhesive film, the content of the second inorganic filler can be 0 to 40 mass%, or it can be more than 3 mass%, more than 5 mass%, more than 10 mass%, more than 12 mass%, or more than 15 mass%, and can be less than 35 mass%, less than 30 mass%, or less than 25 mass%.

[0112] Based on the total amount of the adhesive film, the total content of the first inorganic filler and the second inorganic filler (component (C)) is 10 to 60 mass %, and can be greater than 15 mass %, greater than 18 mass %, greater than 20 mass %, greater than 25 mass %, or greater than 30 mass %, and can be less than 55 mass %, less than 52 mass %, or less than 50 mass %.

[0113] The mass ratio of the first inorganic filler to the total of the first inorganic filler and the second inorganic filler (component (C)) can be 40 to 100 mass%, or can be greater than 45 mass%, greater than 50 mass%, or greater than 55 mass%, and can be less than 95 mass%, less than 90 mass%, or less than 85 mass%.

[0114] The mass ratio of the second inorganic filler relative to the total of the first inorganic filler and the second inorganic filler (component (C)) can be 0 to 60 mass%, or can be 5 mass% or more, 10 mass% or more, or 15 mass% or more, and can be 55 mass% or less, 50 mass% or less, or 45 mass% or less.

[0115] The content of component (C) may be 30 to 250 parts by mass relative to 100 parts by mass of component (A) (the total of thermosetting resin and curing agent). When the content of component (C) is within such a range, the adhesive force of the adhesive film tends to be improved. The content of component (C) may be 35 parts by mass or more, 40 parts by mass or more, 50 parts by mass or more, or 55 parts by mass or more relative to 100 parts by mass of component (A) (the total of thermosetting resin and curing agent), and may be 220 parts by mass or less, 200 parts by mass or less, 180 parts by mass or less, 160 parts by mass or less, 150 parts by mass or less, 140 parts by mass or less, 130 parts by mass or less, 120 parts by mass or less, or 100 parts by mass or less.

[0116] (D) Component: Curing Accelerator

[0117] As (D) component, for example, imidazoles and derivatives thereof, organophosphorus compounds, secondary amines, tertiary amines, quaternary ammonium salts, etc. can be cited. These can also be used alone or in combination of two or more. Among these, from the viewpoint of reactivity, (D) component can also be imidazoles and derivatives thereof.

[0118] Examples of the imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole, etc. These may be used alone or in combination of two or more.

[0119] (E) Ingredient: Coupling agent

[0120] (E) component may also be a silane coupling agent. As the silane coupling agent, for example, γ-ureidopropyl triethoxysilane, γ-mercaptopropyl trimethoxysilane, 3-phenylaminopropyl trimethoxysilane, 3-(2-aminoethyl)aminopropyl trimethoxysilane, etc. may be cited. These may also be used alone or in combination of two or more.

[0121] The adhesive film may further contain other components. Examples of other components include pigments, ion scavengers, antioxidants, and the like.

[0122] Based on the total amount of the adhesive film, the total content of component (D), component (E) and other components can be greater than 0.1 mass %, greater than 0.3 mass %, or greater than 0.5 mass %, or less than 30 mass %, less than 20 mass %, less than 10 mass %, or less than 5 mass %.

[0123] The adhesive film 10 can be formed, for example, by coating a thermosetting adhesive on a support film. In forming the adhesive film 10, a varnish of a thermosetting adhesive (adhesive varnish) can also be used. When using an adhesive varnish, the (A) component, the (B) component, and the (C) component, as well as components added as needed, are mixed or kneaded in a solvent to prepare the adhesive varnish, and the obtained adhesive varnish is coated on a support film, and heated and dried to remove the solvent, thereby obtaining the adhesive film 10.

[0124] The support film is not particularly limited as long as it is a film that can withstand the above-mentioned heating and drying, and can be, for example, a polyester film, a polypropylene film, a polyethylene terephthalate film, a polyimide film, a polyetherimide film, a polyethylene naphthalate film, a polymethylpentene film, etc. The support film can be a multilayer film formed by combining two or more types, or a film whose surface is treated with a silicone-based, silica-based release agent, etc. The thickness of the support film can be, for example, 10 to 200 μm or 20 to 170 μm.

[0125] The mixing or kneading can be carried out using a common disperser such as a stirrer, a pestle, a three-roll mill, or a ball mill, or by combining them as appropriate.

[0126] The solvent used to prepare the adhesive varnish is not limited as long as it can evenly dissolve, mix or disperse the various components, and conventionally known solvents can be used. Examples of such solvents include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, toluene, and xylene. From the viewpoint of drying speed and price, the solvent may be methyl ethyl ketone or cyclohexanone.

[0127] As a method for coating the adhesive varnish on the support film, a known method can be used, for example, a knife coating method, a roll coating method, a spray coating method, a gravure coating method, a rod coating method, a curtain coating method, etc. The heating and drying conditions are not particularly limited as long as the used solvent is fully volatilized, and for example, it can be 1 to 30 minutes at 50 to 150°C.

[0128] The thickness of the adhesive film 10 may be, for example, 1 μm or more, 3 μm or more, 20 μm or more, 25 μm or more, 30 μm or more, 35 μm or more, 40 μm or more, 50 μm or more, 60 μm or more, 70 μm or more, or 80 μm or more, and may be 200 μm or less, 150 μm or less, 120 μm or less, 100 μm or less, 80 μm or less, or 60 μm or less. When the adhesive film 10 is an adhesive film for FOD, in order to properly embed the entire semiconductor chip (for example, a controller chip), the thickness of the adhesive film 10 may be, for example, 40 to 200 μm, 60 to 150 μm, or 80 to 120 μm. When the adhesive film 10 is an adhesive film for FOW, the thickness of the adhesive film 10 may be, for example, 20 to 120 μm, 25 to 80 μm, or 30 to 60 μm in order to embed the wire so that the wire does not contact the semiconductor chip.

[0129] From the viewpoint of preventing damage or contamination, the adhesive film 10 produced on the support film may also have a covering film on the surface of the adhesive film opposite to the support film. Examples of the covering film include polyethylene film, polypropylene film, and surface release agent treated film. The thickness of the covering film may be, for example, 15 to 200 μm or 30 to 170 μm.

[0130] The adhesive film 10 can be used, for example, as a protective sheet for protecting the back surface of a semiconductor element (semiconductor chip) of a flip-chip semiconductor device or as a sealing sheet for sealing between the surface of a semiconductor element (semiconductor chip) of a flip-chip semiconductor device and an adherend.

[0131] [Dicing and Die Bonding Integrated Film]

[0132] Figure 2 and Figure 3 FIG. 1 is a schematic cross-sectional view showing an embodiment of a laminate having an adhesive film. Figure 2 or Figure 3 The laminated body is provided in the form shown. Figure 2 The laminated body 100 shown includes a base material layer 20 and an adhesive film 10 provided on the base material layer 20 . Figure 3 The laminated body 110 shown further includes a protective film 30 provided on a surface of the adhesive film 10 on the opposite side to the base material layer 20 with respect to the laminated body 100 .

[0133] The base layer 20 may be a resin film similar to the support film. The thickness of the base layer 20 may be, for example, 10 to 200 μm or 20 to 170 μm.

[0134] The base material layer 20 may be a dicing film. A laminated body in which the base material layer 20 is a dicing film can be used as a dicing die bonding integrated film. The dicing die bonding integrated film may be in a film, sheet, or tape shape.

[0135] As a dicing film, for example, resin films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, and polyimide film can be cited. As needed, the dicing film can also be a resin film that has been surface-treated by primer coating, UV treatment, corona discharge treatment, grinding treatment, and etching treatment. The dicing film can have adhesiveness. The dicing film with adhesiveness can be, for example, a resin film that is endowed with adhesiveness, or a laminated film having a resin film and an adhesive layer disposed on one side thereof. The adhesive layer can be formed by a non-ultraviolet curing type or ultraviolet curing type adhesive. A non-ultraviolet curing type adhesive is an adhesive that shows constant adhesiveness under short-term pressure. An ultraviolet curing type adhesive is an adhesive that has the property of reducing adhesiveness by irradiating ultraviolet rays. The thickness of the adhesive layer can be appropriately set according to the shape and size of the semiconductor device, for example, it can be 1 to 100 μm, 5 to 70 μm, or 10 to 40 μm. From the viewpoint of economic efficiency and film handling properties, the thickness of the base material layer 20 as a dicing film may be 60 to 150 μm or 70 to 130 μm.

[0136] The protective film 30 may be a resin film similar to the cover film, and the thickness of the protective film 30 may be, for example, 15 to 200 μm or 30 to 170 μm.

[0137] [Semiconductor device and method of manufacturing the same]

[0138] Figure 4 It is a schematic cross-sectional view showing one embodiment of a semiconductor device, and shows an example of a semiconductor device manufactured using an adhesive film. Figure 4 The semiconductor device 200 shown is mainly composed of a substrate 14, a first semiconductor chip Wa and a second semiconductor chip Waa mounted on the substrate 14, a sealing layer 42 for sealing the second semiconductor chip Waa, and an adhesive film 10 for bonding the second semiconductor chip Waa to the substrate 14. The substrate 14 has an organic substrate 90 and circuit patterns 84 and 94 provided on the organic substrate 90. The first semiconductor chip Wa is bonded to the substrate 14 by an adhesive 41. The first wire 88 is connected to the first semiconductor chip Wa, and the first semiconductor chip Wa is electrically connected to the circuit pattern 84 via the first wire 88. The first semiconductor chip Wa as a whole and the first wire 88 as a whole are buried in the adhesive film 10. The second wire 98 is connected to the second semiconductor chip Waa, and the second semiconductor chip Waa is electrically connected to the circuit pattern 84 via the second wire 98. The second semiconductor chip Waa as a whole and the second wire 98 as a whole are buried in the sealing layer 42.

[0139] Figure 5 , Figure 6 , Figure 7 , Figure 8 and Fig. 9 is a process diagram showing an embodiment of a method for manufacturing a semiconductor device, Figure 4 FIG. 2 is a process diagram of an example of a method for manufacturing a semiconductor device 200 shown in FIG. Figures 5 to 9 The method shown includes the following steps: bonding the first semiconductor chip Wa to the substrate 14 via the adhesive 41; setting the first wire 88 connecting the first semiconductor chip Wa and the substrate 14 (circuit pattern 84); preparing a chip with adhesive having a second semiconductor chip Wbb and an adhesive film 10 attached thereto; pressing the chip with adhesive onto the substrate 14, thereby bonding the second semiconductor chip Waa to the substrate 14 in a manner that the first semiconductor chip Wa and the first wire 88 are buried by the adhesive film 10; setting the second wire 98 connecting the second semiconductor chip Waa and the substrate 14 (circuit pattern 84). Afterwards, by forming the sealing layer 44, it is possible to obtain Figure 4 A semiconductor device 200 is shown.

[0140] The thickness of the first semiconductor chip Wa may be 10 to 170 μm. The first semiconductor chip Wa may be a controller chip for driving the semiconductor device 200. The first semiconductor chip Wa may be a flip chip chip. The size of the first semiconductor chip Wa is generally smaller than the size of the second semiconductor chip Waa. The adhesive 41 between the first semiconductor chip Wa and the substrate 14 may be a well-known semiconductor adhesive used in the field.

[0141] like Figure 5 As shown, the substrate 14 (circuit pattern 84) is electrically connected to the first semiconductor chip Wa via the first wire 88. The first wire 88 connecting the first semiconductor chip Wa and the substrate 14 (circuit pattern 84) can be, for example, a gold wire, an aluminum wire, or a copper wire. The heating temperature for connecting the first wire 88 can be in the range of 80 to 250° C. or 80 to 220° C. The heating time for connecting the first wire 88 can be from a few seconds to a few minutes. In order to connect the first wire 88, vibration energy generated by ultrasound and crimping energy generated by applying pressure can also be applied.

[0142] The chip with adhesive formed by the second semiconductor chip Waa and the adhesive film 10 can be used, for example, with Figure 2The laminate 100 shown in the figure is prepared by a dicing die bonding integrated film of the same structure as that of the laminate 100. In this case, for example, the laminate 100 (dicing die bonding integrated film) is attached to a single surface of the semiconductor wafer in a direction in which its adhesive film 10 contacts the semiconductor wafer. The surface to which the adhesive film 10 is attached can be the circuit surface of the semiconductor wafer, or it can be the back surface on the opposite side thereof. The semiconductor wafer to which the laminate 100 (dicing die bonding integrated film) is attached is divided by cutting, thereby forming a single-piece second semiconductor chip Waa. As cutting, there can be cited blade cutting using a rotating knife, making a modified area on the semiconductor wafer by laser, invisible cutting of expanding the substrate layer, etc. The second semiconductor chip Waa is picked up together with the divided adhesive film 10. In the case where the adhesive layer of the dicing film is formed by an ultraviolet curing adhesive, before picking up the second semiconductor chip Waa, the adhesive force of the adhesive layer can be reduced by irradiating the adhesive layer with ultraviolet rays as needed.

[0143] The second semiconductor chip Waa may have a size of 20 mm or less in width. The width (or length of one side) of the second semiconductor chip Waa may be 3 to 15 mm or 5 to 10 mm.

[0144] The semiconductor wafer used to form the second semiconductor chip Waa may be, for example, a thin semiconductor wafer having a thickness of 10 to 100 μm. In addition to single crystal silicon, the semiconductor wafer may also be a compound semiconductor wafer such as polycrystalline silicon, various ceramics, or gallium arsenide. The second semiconductor chip Waa may also be formed from the same semiconductor wafer.

[0145] like Figure 7 As shown in FIG. 1 , the chip with adhesive formed by the adhesive film 10 and the second semiconductor chip Waa is placed so that the first wire 88 and the first semiconductor chip Waa are covered by the adhesive film 10. Figure 8 As shown, the second semiconductor chip Waa is fixed to the substrate 14 by pressing the second semiconductor chip Waa onto the substrate 14. The heating temperature for pressing can be 50 to 200°C or 100 to 150°C. If the heating temperature for pressing is high, the adhesive film 10 becomes soft, so there is a tendency for the embedding property to be improved. The pressing time can be 0.5 to 20 seconds or 1 to 5 seconds. The pressure for pressing can be 0.01 to 5 MPa or 0.02 to 2 MPa.

[0146] After the crimping, the structure including the adhesive film 10 may be further heated to cure the adhesive film 10. The temperature and time for curing may be appropriately set according to the curing temperature of the adhesive film 10. The temperature may also be changed in stages. The heating temperature may be, for example, 40 to 300° C. or 60 to 200° C. The heating time may be, for example, 30 to 300 minutes.

[0147] like Fig. 9 As shown, the substrate 14 and the second semiconductor chip Waa are electrically connected via the second wire 98. The type and connection method of the second wire 98 can be the same as those of the first wire 88.

[0148] After that, a sealing layer 42 is formed by a sealing material to seal the circuit pattern 84, the second wire 98, and the second semiconductor chip Waa. The sealing layer 42 can be formed by a common method using a mold, for example. After the sealing layer 42 is formed, the adhesive film 10 and the sealing layer 42 can be further thermally cured by heating. The heating temperature for this purpose can be, for example, 165 to 185° C., and the heating time can be about 0.5 to 8 hours.

[0149] Fig.10 2 is a schematic cross-sectional view showing another embodiment of a semiconductor device. The semiconductor device 201 is mainly composed of a substrate 14, a first semiconductor chip Wa and a second semiconductor chip Waa mounted on the substrate 14, a sealing layer 42 for sealing the first semiconductor chip Wa and the second semiconductor chip Waa, and an adhesive film 10 for bonding the second semiconductor chip Waa to the first semiconductor chip Wa. The substrate 14 has an organic substrate 90, circuit patterns 84 and 94 provided on the organic substrate 90, and a connection terminal 95 provided on the surface of the organic substrate 90 on the side opposite to the circuit patterns 84 and 94. The first semiconductor chip Wa is bonded to the substrate 14 by an adhesive 41. The first wire 88 is connected to the first semiconductor chip Wa, and the first semiconductor chip Wa is electrically connected to the circuit pattern 84 via the first wire 88. A portion of the first wire 88 is buried in the adhesive film 10. The second wire 98 is connected to the second semiconductor chip Waa, and the second semiconductor chip Waa is electrically connected to the circuit pattern 84 via the second wire 98.

[0150] Fig.10 The semiconductor device 201 shown can be manufactured by the same method as the method for manufacturing the semiconductor device 200 , which method includes the step of bonding the second semiconductor chip Waa to the first semiconductor chip Wa via the adhesive film 10 .

[0151] Fig.11 2 is a schematic cross-sectional view showing another embodiment of a semiconductor device. The semiconductor device 202 is mainly composed of a substrate 14 (organic substrate 90), a first semiconductor chip Wa and a second semiconductor chip Waa mounted on the substrate 14, a sealing layer 42 for sealing the first semiconductor chip Wa and the second semiconductor chip Waa, and an adhesive film 10 for burying the entire first semiconductor chip Wa and bonding the second semiconductor chip Waa to the substrate 14. The first semiconductor chip Wa is a flip chip type chip and is electrically connected to the substrate 14 via a plurality of electrodes 96. An underfill 50 is filled between the first semiconductor chip Wa and the substrate 14.

[0152] Example

[0153] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these.

[0154] [Adhesive film production]

[0155] (Examples 1 to 7 and Comparative Examples 1 to 3)

[0156] <Preparation of Adhesive Varnish>

[0157] Cyclohexanone was added to a composition consisting of components (A) and (C) according to the product names and composition ratios (unit: parts by mass) shown in Tables 1 and 2, and the mixture was stirred and mixed. Component (B) shown in Tables 1 and 2 was added thereto and stirred, and then components (D) and (E) shown in Tables 1 and 2 were added and stirred until the components were uniform, thereby preparing an adhesive varnish. In addition, the values ​​of components (B) and (C) shown in Tables 1 and 2 refer to parts by mass of the solid content.

[0158] (A) Component: Thermosetting resin component

[0159] (A1) Ingredients: Thermosetting resin

[0160] (A1-1) N-500P-10 (trade name, manufactured by DIC Corporation, o-cresol novolac type epoxy resin, epoxy equivalent: 204 g / eq, softening point: 75 to 85° C.)

[0161] (A1-2) EXA-830CRP (trade name, manufactured by DIC Corporation, liquid bisphenol F type epoxy resin, epoxy equivalent: 159 g / eq)

[0162] (A2) Ingredient: Curing agent

[0163] (A2-1) MEH-7800M (trade name, manufactured by Meiwa Chemical Industry Co., Ltd., phenyl aralkyl type phenolic resin, hydroxyl equivalent: 174 g / eq, softening point: 80° C.)

[0164] (A2-2) PSM-4326 (trade name, manufactured by Gunei Chemical Co., Ltd., phenol novolac resin, hydroxyl equivalent: 105 g / eq, softening point: 120° C.)

[0165] (B) Component: Elastomer

[0166] (B1) Component: First Acrylic Resin

[0167] (B1-1) Acrylic resin A (acrylic resin as a copolymer of butyl acrylate / ethyl acrylate / ethyl methacrylate / glycidyl methacrylate / styrene, content of structural units derived from styrene: 9% by mass (based on total structural units), weight average molecular weight: 400,000, Tg: 5°C)

[0168] (B2) Component: Second acrylic resin

[0169] (B2-1) Acrylic resin B (HTR-860P-3CSP (trade name), manufactured by Nagase ChemteX Corporation, acrylic resin, weight average molecular weight: 800,000, Tg: 12° C.)

[0170] (B2-2) Acrylic resin C (acrylic resin obtained by removing structural units derived from acrylonitrile from acrylic resin SG-P3 (trade name, manufactured by Nagase ChemteX Corporation), weight average molecular weight: 600,000, Tg: 12° C.)

[0171] (C) Ingredients: Inorganic filler

[0172] (C-1) Silica filler A (SC2050-HLG (trade name), manufactured by Admatechs Co., Ltd., silica filler dispersion, average particle size: 0.50 μm)

[0173] (C-2) Silica filler B (silica filler dispersion, average particle size: 0.18 μm)

[0174] (D) Curing accelerator

[0175] (D-1) 2PZ-CN (trade name, manufactured by SHIKOKU CHEMICALS CORPORATION, 1-cyanoethyl-2-phenylimidazole)

[0176] <Adhesive film production>

[0177] The produced adhesive varnish was filtered through a 100 mesh filter and vacuum defoamed. As a substrate layer, a 38 μm thick polyethylene terephthalate film (PET) film that had been subjected to demolding treatment was prepared, and the vacuum defoamed adhesive varnish was applied to the PET film. The applied adhesive varnish was heated and dried in two stages: heating and drying at 90°C for 5 minutes and then heating and drying at 140°C for 5 minutes, to obtain adhesive films of Examples 1 to 7 and Comparative Examples 1 to 3 in the B stage state. In the adhesive film, the thickness was adjusted to 60 μm according to the coating amount of the adhesive varnish. Two sheets of the obtained adhesive film with a thickness of 60 μm were prepared, and they were bonded together at 70°C to produce an adhesive film with a thickness of 120 μm.

[0178] [Evaluation of adhesive film]

[0179] <Measurement of the Ratio of Nitrile Groups in Acrylic Resin>

[0180] The IR spectrum of the adhesive film of Example 3 was measured and the PA CN / PA CO First, the transmission IR spectrum of the adhesive film was measured by the KBr tablet method, with the vertical axis showing the absorbance and the horizontal axis showing the wave number (cm -1 ). FT-IR6300 (manufactured by JASCO Corporation, light source: high brightness ceramic light source, detector: DLATGS) was used for the IR spectrum measurement. Next, the wavelength of the wavelength connected to 1650 cm -1 and 1800cm -1 The straight line between these two points is the baseline and the absorbance area enclosed by the spectrum and the baseline is the PA CO . And, the calculation is to connect the 2230cm -1 and 2300cm -1 The straight line between these two points is the baseline and the absorbance area enclosed by the spectrum and the baseline is the PA CN According to the calculated PA CO and PA CN , and find PA CN / PA CO Perform this operation 3 times in total to find PA CN / PA CO The average of 3 times is 0.014.

[0181] <Evaluation of HAST resistance>

[0182] A printed wiring board substrate (manufactured by ShowaDenko Materials co., Ltd., trade name: MCL-E-679) was prepared in which a copper foil with a thickness of 70 μm was laminated on a glass epoxy substrate. The copper surface of the printed wiring board substrate was etched to form a comb-shaped electrode with a line / space of 40 μm / 40 μm. On the substrate forming the comb-shaped electrode, adhesive films (5 mm×12 mm) of Examples 1 to 7 and Comparative Examples 1 to 3 with a thickness of 120 μm were attached at a temperature of 120°C, a time of 2 seconds, and a pressure of 0.2 MPa. Next, in a reduced pressure dryer, after heating at a temperature of 90°C, a time of 1 hour, and a pressure of 0.6 MPa, it was further heated at a temperature of 130°C, a time of 1 hour, and a pressure of 0.6 MPa, thereby producing an evaluation substrate. The evaluation substrate was exposed to a voltage of DC13.2V under the conditions of 130°C and 85%RH, and the voltage was applied to measure the resistance value between the lines. In the measurement of the resistance value, the number of times when the resistance value decreased by more than two digits was observed was calculated, and the time from the start of the test to the observation of the 50th resistance value decrease was evaluated according to the following criteria. The results are shown in Tables 1 and 2.

[0183] A: The time from the start of the test to the observation of the 50th resistance drop exceeded 100 hours.

[0184] B: The time from the start of the test to the time when the 50th decrease in resistance value was observed was more than 50 hours and less than 100 hours.

[0185] C: The time from the start of the test to the observation of the 50th decrease in resistance value was 50 hours or less.

[0186] <Evaluation of Adhesion Strength>

[0187] (Manufacturing of semiconductor chips with adhesive films)

[0188] A dicing film (manufactured by Showa Denko Materials Co., Ltd., with a thickness of 100 μm) having a resin film and an adhesive layer was prepared, and the adhesive films (thickness of 120 μm) of Examples 1 to 7 and Comparative Examples 1 to 3 prepared were attached respectively to prepare a dicing die bonding integrated film having a dicing film and an adhesive film arranged on one surface of the dicing film. Next, a semiconductor wafer (thickness of 400 μm) was attached to the adhesive film side of the dicing die bonding integrated film at a stage temperature of 70°C. A semiconductor chip having a size of 2 mm × 2 mm was formed by cutting using a fully automatic cutting machine DFD-6361 (manufactured by DISCO Corporation). A semiconductor chip with an adhesive film formed by a semiconductor chip and an adhesive film attached thereto was picked up to obtain a semiconductor chip with an adhesive film.

[0189] (Adhesion to organic substrate (solder resist))

[0190] Using the obtained semiconductor chip with adhesive film, the shear strength of the chip after curing was measured. The semiconductor chip was thermally pressed onto the solder resist (TAIYO HOLDINGS CO., LTD., trade name: SR-1). The pressing conditions were a temperature of 120°C, a time of 1 second, and a pressure of 0.1 MPa. Next, the evaluation sample obtained by pressing was placed in a dryer, heated at 110°C for 1 hour, heated for 30 minutes, and then heated at 175°C for 5 hours to cure it. Next, in the cured evaluation sample, the semiconductor chip was hung and stretched by a universal bonding strength tester (manufactured by Nordson Advanced Technology KK, trade name: Series 4000), thereby measuring the chip shear strength of the semiconductor chip and the organic substrate after curing. The measurement of the chip shear strength was carried out under the conditions of 6.7 MPa, 260°C, and a stage holding time of 20 seconds. The results are shown in Tables 1 and 2.

[0191] (Adhesion to gold substrate)

[0192] The bonding strength was evaluated using a gold substrate that is less likely to bond than an organic substrate. That is, the bonding strength to the gold substrate is an evaluation method under stricter conditions than the bonding strength to the organic substrate (solder resist). Using the obtained semiconductor chip with an adhesive film, the chip shear strength after curing was measured. The semiconductor chip was thermally pressed onto the gold substrate. The pressing conditions were a temperature of 120°C, a time of 1 second, and a pressure of 0.1MPa. Next, the evaluation sample obtained by pressing was placed in a dryer, heated at 110°C for 1 hour, heated for 30 minutes, and then heated at 175°C for 5 hours to cure it. Then, in the cured evaluation sample, the semiconductor chip was hung and stretched by a universal bonding strength tester (manufactured by Nordson Advanced Technology KK, trade name: Series 4000), thereby measuring the chip shear strength after curing of the semiconductor chip and the gold substrate. The measurement of the chip shear strength was carried out under the conditions of 6.7MPa, 260°C, and a stage holding time of 20 seconds. The results are shown in Tables 1 and 2. In Comparative Example 1, the wafer shear strength was lower than the lower limit of measurement of the measuring device and could not be measured.

[0193] [Table 1]

[0194]

[0195] As shown in Table 1, the adhesive films of Examples 1 and 2 containing an acrylic resin having a structural unit derived from a monomer having an aromatic ring as an elastomer have excellent HAST resistance and excellent adhesion compared to the adhesive film of Comparative Example 1 that does not contain an acrylic resin having a structural unit derived from a monomer having an aromatic ring as an elastomer.

[0196]

[0197] As shown in Table 2, the adhesive films of Examples 3 to 7 containing an acrylic resin having a structural unit derived from a monomer having an aromatic ring as an elastomer are superior in both HAST resistance and adhesive strength compared to the adhesive films of Comparative Examples 2 and 3 not containing an acrylic resin having a structural unit derived from a monomer having an aromatic ring as an elastomer.

[0198] From the above results, it was confirmed that the adhesive film for a semiconductor of the present invention is excellent in HAST resistance and has high adhesive strength.

[0199] Explanation of symbols

[0200] 10-adhesive film, 14-substrate, 20-base material layer (cutting film), 30-protective film, 41-adhesive, 42-sealing layer, 84, 94-circuit pattern, 88-first conductor, 90-organic substrate, 98-second conductor, 100, 110-laminated body, 200, 201, 202-semiconductor device, Wa-first semiconductor chip, Waa-second semiconductor chip.

Claims

1. An adhesive film for semiconductors, comprising a thermosetting component, an elastomer and an inorganic filler, The elastomer contains an acrylic resin having a structural unit derived from a monomer having an aromatic ring. 2 . The adhesive film for a semiconductor according to claim 1 , which has a thickness of 60 to 150 μm. 3 . The adhesive film for a semiconductor according to claim 1 , which is used to bond a semiconductor chip to a substrate while embedding another semiconductor chip. The adhesive film for a semiconductor according to claim 1 , which has a thickness of 25 to 80 μm. 5 . The adhesive film for a semiconductor according to claim 1 , which is used to bond a semiconductor chip to another semiconductor chip while burying a part or the whole of a wire connected to the other semiconductor chip.

6. The adhesive film for semiconductor according to any one of claims 1, 2 and 4, wherein The elastomer further contains an acrylic resin having no structural unit derived from a monomer having an aromatic ring, The acrylic resin having no structural unit derived from a monomer having an aromatic ring has a weight average molecular weight of 500,000 or more.

7. The adhesive film for semiconductor according to any one of claims 1, 2 and 4, wherein The content of the elastomer is 10 to 60% by mass based on the total amount of the adhesive film for semiconductor.

8. The adhesive film for semiconductor according to any one of claims 1, 2 and 4, wherein The content of the inorganic filler is 30 to 250 parts by mass based on 100 parts by mass of the thermosetting component.

9. A dicing die bonding integrated film comprising: Cutting film; and The adhesive film for a semiconductor according to any one of claims 1, 2 and 4 provided on the dicing film.

10. A method for manufacturing a semiconductor device, comprising the step of bonding a second semiconductor chip to a substrate on which a first semiconductor chip is mounted, using the adhesive film for a semiconductor according to claim 1 or 2, The first semiconductor chip is embedded in the adhesive film.

11. A method for manufacturing a semiconductor device, comprising the step of bonding a second semiconductor chip to a first semiconductor chip by using the adhesive film for a semiconductor according to claim 1 or 4, A wire is connected to the first semiconductor chip, A part or the whole of the wire is buried in the adhesive film.

12. The method for manufacturing a semiconductor device according to claim 10, wherein: The first semiconductor chip is a controller chip.

13. The method for manufacturing a semiconductor device according to claim 11, wherein: The first semiconductor chip is a controller chip.