Coated anode composition

By using coated micro-silicon active material particles as the anode composition in lithium-ion battery packs, the mechanical degradation and SEI instability problems caused by volume changes in silicon anodes are solved, achieving high capacity and long lifespan performance of the battery.

CN118974968APending Publication Date: 2024-11-15ANTEO ENERGY TECH PTY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026047.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-07
Filing Date
2023-03-07
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

When existing lithium-ion battery packs use silicon as the anode material, they face problems such as mechanical degradation due to volume changes and instability of the solid electrolyte interface (SEI), which affect cycle life and electrochemical reactivity.

Method used

The anode composition uses coated micro-silicon active material particles. The coating material is selected from carbon, graphene, graphite, metal oxides and polymers, etc., to control the expansion effect of silicon, reduce the formation and decomposition of SEI, and improve the stability and cycle life of the electrode.

Benefits of technology

It significantly extends the anode stability and cycle life of lithium-ion battery packs, reduces electrode impedance, improves electrochemical reactivity, and achieves high-capacity and long-life battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005031505980000431
    Figure BDA0005031505980000431
  • Figure BDA0005031505980000432
    Figure BDA0005031505980000432
  • Figure BDA0005031505980000433
    Figure BDA0005031505980000433
Patent Text Reader

Abstract

The present disclosure generally relates to coated microsilicon active material particles and / or coated anodes comprising an anode composition. The present disclosure also relates to an anode of a lithium ion battery and an anode composition thereof. The present disclosure also relates to a method of incorporating the anode composition into an electrochemical cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to coated micro-silicon active material particles and / or coated anodes comprising an anode composition. The present disclosure also relates to an anode of a lithium-ion battery and an anode composition thereof. The present disclosure also relates to a method of incorporating the anode composition into an electrochemical cell. Background Art

[0002] Conventional lithium-ion (Li-ion) batteries typically use graphite-based anodes as the lithium intercalation material. However, silicon-based anodes offer improvements over graphite-based Li-ion batteries. 3.75 Si) exhibits higher gravimetric capacity (3579 mAh / g compared to 372 mAh / g for graphite) and volumetric capacity (about 2194 mAh / cm 3 Compared to about 750 mAh / cm in fully lithiated graphite 3 ). In addition, silicon-based anodes have a relative + A low lithiation / delithiation voltage plateau of about 0.3-0.4 V, which allows it to maintain an open circuit potential that avoids undesirable Li plating and dendrite formation. Although silicon shows excellent electrochemical activity, achieving a stable cycle life for silicon-based anodes is challenging due to the large volume change of silicon during lithiation and delithiation. Silicon active materials and regions may lose electrical contact with the anode because the large volume change coupled with its low electrical conductivity separates silicon from the surrounding materials in the anode.

[0003] In addition, large silicon volume changes exacerbate the formation of solid electrolyte interface (SEI), which may further lead to electrical isolation and, therefore, capacity loss. The expansion and contraction of silicon particles during charge-discharge cycles causes silicon particles to pulverize, which increases the specific surface area of ​​silicon particles. As the silicon surface area changes and increases during cycling, SEI repeatedly splits and reforms. Therefore, during cycling to thick electronic and ionic insulating layers, SEI continues to accumulate around the pulverized silicon areas. This accumulated SEM increases the impedance of the electrode and reduces the electrochemical reactivity of the electrode, which is detrimental to the cycle life. Due to its high specific capacity, abundance, and low cost, silicon is a promising active material for Li-ion anodes. However, its large volume change during lithiation and delithiation (Li 3.75 The volume change of Si1 phase >280% produces mechanical degradation of the electrode and unstable SEI, which leads to electrode swelling and poor battery cycle life.

[0004] Therefore, there is a need to provide new and alternative anode compositions for lithium-ion batteries, particularly lithium-ion batteries containing a majority of silicon active materials, which can control the expansion effects of silicon and significantly extend the stability and / or cycle life of the anode. Summary of the invention

[0005] The present disclosure provides coated micro-silicon active material particles and / or coated anodes comprising an anode composition. The anode composition may comprise micro-silicon active material particles or coated micro-silicon active material particles, wherein the silicon content is at least 60wt.% based on the total weight of the anode composition. The present disclosure also provides a method for incorporating an anode comprising an anode composition into an electrochemical cell and an electrochemical cell so formed, whereby the anode paired with the method integrated into the electrochemical cell can extend the stability and / or cycle life of the anode. The anode composition and / or the formed anode may be coated.

[0006] In one aspect, an anode composition is provided, comprising micro-silicon active material particles, wherein the micro-silicon active material particles have one or more of the following: (i) a BET surface area of ​​about 0.1 m 2 / g and about 10m 2 / g, (ii)D 50 The particle size is between about 0.1 μm and about 10 μm, and (iii) D 50 The ratio of the surface area of ​​the micro-silicon active material to that of the micro-silicon active material is between about 0.1 and about 10, wherein the amount of the micro-silicon active material particles present in the anode composition is between about 60 wt.% and about 95 wt.% based on the total weight % of the anode composition, and wherein the anode composition comprises a coating. In some embodiments, the coating can be a coating of the micro-silicon active material particles. The coating can be selected from the group comprising: carbon, graphene, graphite, metal oxides, polymers and combinations thereof to form coated micro-silicon active material particles.

[0007] In some embodiments, the surface area of ​​the coated micro-silicon active material particles will be reduced compared to the surface area of ​​the uncoated micro-silicon active material particles. It should be understood that in some examples, if the micro-silicon active material particles have a roughened surface, the surface area may be reduced, wherein the coating may actually fill these defects. In other embodiments, the surface area of ​​the coated micro-silicon active material particles will be increased compared to the surface area of ​​the uncoated micro-silicon active material particles. In some embodiments, the measured BET surface area of ​​the coated micro-silicon active material particles may be between about 1 m 2 / g and about 100m 2 / g. In some embodiments, the amount of micro-silicon active material particles or coated micro-silicon active material particles present in the anode composition may be between about 70 wt.% and about 95 wt.%, based on the total weight % of the anode composition. In some embodiments, the purity of the micro-silicon active material particles (excluding oxygen) may be at least 95 wt.%, preferably 98 wt.%. In some embodiments, the thickness of the coating may be between about 0.1 nm and about 200 nm.

[0008] In some embodiments, the anode composition may further include one or more binders. The binder may be present in the anode composition in an amount of about 2.5 wt.% to about 15 wt.%, based on the total weight of the anode composition.

[0009] In some embodiments, the anode composition may further include one or more conductive materials. The conductive materials may be present in the anode composition in an amount of about 2.5 wt.% to about 40 wt.%, based on the total weight of the anode composition.

[0010] In some embodiments, the micro silicon active material particles or coated active material particles and / or the anode composition may be pre-lithiated. The pre-lithiation level of the micro silicon active material particles or coated active material particles and / or the anode composition may be between about 1% and about 30% silicon lithiation.

[0011] In another aspect, an electrochemical cell is provided, comprising: an anode; a cathode; an electrolyte; and a separator, wherein the anode comprises an anode composition defined in any one or more embodiments or examples described herein, wherein the lithium uptake capacity of the anode is greater than the lithium release capacity of the cathode. In some embodiments, the capacity of the lithium uptake capacity of the anode may not be fully utilized during charging of the lithium ion battery. In one example, the anode may be only partially lithiated in a fully charged state. In some embodiments, the degree of silicon lithiation may be limited to about 20% to about 80% of the theoretical maximum. In some embodiments, the capacity ratio of the anode to the cathode (N / P ratio) may be between about 1.05 and about 7. In other embodiments, the lower cutoff voltage may be between about 2.0V and 3.5V.

[0012] In some embodiments, the pre-lithiation level of the anode may be from about 1% to about 30% silicon lithiation. The cathode may include an active material selected from the group consisting of lithium nickel cobalt manganese oxide (NCM), lithium iron phosphate (LFP), lithium nickel manganese spinel (LNMO), lithium nickel cobalt aluminum oxide (NCA), lithium manganese oxide (LMO), lithium cobalt oxide (LCO), and sulfur or sulfur composites. The electrolyte may be selected from a non-aqueous electrolyte solution comprising one or more lithium salts.

[0013] In some embodiments, the electrochemical cell may be an energy storage device. The energy storage device may be a battery, preferably a secondary battery. For example, the battery may be a lithium-ion battery.

[0014] In another aspect, a method for improving the cycling stability of a lithium ion battery is provided, the lithium ion battery having an anode and a cathode, at least one electrolyte and a separator, wherein the anode composition is defined by any one or more embodiments or examples described herein. In some embodiments, the anode in the battery delivers a specific capacity of at least about 450 mAh / g, 500 mAh / g, 600 mAh / g, 800 mAh / g, 1000 mAh / g, 1200 mAh / g or 1500 mAh / g, and retains at least about 80% of its initial capacity after 100, 200, 400, 600, 800, 1000 or 1500 cycles of the battery.

[0015] In another aspect, there is provided a use of an anode composition in an electrochemical cell, wherein the anode composition is at least partially applied to a current collector material, and wherein the anode composition is defined by any one or more embodiments or examples described herein.

[0016] In another aspect, a method for preparing an anode of an electrochemical cell is provided, the method comprising the steps of: (i) preparing an anode slurry comprising microsilicon active material particles or coated microsilicon active material particles, optionally one or more additional active materials, optionally one or more binders, optionally one or more conductive materials, optionally one or more additives and a solvent system; and (ii) casting a layer of the anode slurry onto a current collector material to provide an anode composition layer on the current collector material, and (iii) optionally coating the anode composition, wherein the microsilicon active material particles have one or more of the following: (a) a BET surface area measured between about 0.1 m 2 / g and about 10m 2 / g, (b)D 50 The particle size is between about 0.1 μm and about 10 μm, and (c) D 50 The ratio of the BET surface area is between about 0.1 and about 10.

[0017] In another aspect, an anode prepared as defined in the method of any one or more embodiments or examples described herein is provided.

[0018] In another aspect, a method for assembling an electrochemical cell is provided, wherein the method comprises the following steps: preparing an anode defined by the method in any one or more embodiments or examples described herein, wherein the anode comprises an anode composition as defined in any one or more embodiments or examples described herein; and assembling the anode into an electrochemical cell.

[0019] In any of the above aspects and embodiments, the microsilicon active material particles and / or the anode comprising the anode composition comprises a coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Preferred embodiments of the present disclosure will be further described and illustrated, by way of example only, with reference to the accompanying drawings, in which:

[0021] Figure 1a is a graph showing the specific coating capacity at C / 2 for a full cell (anode) of 70 wt% mSi limited capacity (with Al2O3 coating versus uncoated mSi).

[0022] Figure 1b is a graph showing the discharge capacity retention at C / 2 for a 70 wt % mSi limited capacity (with Al 2 O 3 coating versus uncoated mSi) full cell (anode).

[0023] Figure 2a is a graph showing the specific coating capacity at C / 2 for a 70 wt% mSi limited capacity (with PR coating versus uncoated mSi) full cell (anode).

[0024] Figure 2b is a graph showing the discharge capacity retention at C / 2 for a 70 wt% mSi limited capacity (with PR coating vs. uncoated mSi) full cell (anode).

[0025] Figure 3a is a graph showing the specific coating capacity at C / 2 for a 70 wt% mSi limited capacity (PVP-SPD coating versus uncoated) full cell (anode).

[0026] Figure 3b is a graph showing the discharge capacity retention of 70 wt% mSi limited capacity (PVP-SPD coating vs. uncoated) full cells (anode) at C / 2.

[0027] Figure 4a is a graph showing the specific coating capacity at C / 2 for a 70 wt% mSi limited capacity (with PAN coating versus uncoated mSi) full cell (anode).

[0028] Figure 4b is a graph showing the discharge capacity retention at C / 2 for a 70 wt% mSi limited capacity (with PAN coating versus uncoated mSi) full cell (anode).

[0029] Figure 5a is a graph showing the specific coating capacity (anode) of pre-lithiated 70 wt % mSi anodes (at 0% and 10% pre-lithiation) at C / 2.

[0030] Figure 5b is a graph showing the discharge capacity retention of full cells of pre-lithiated 70 wt % mSi anodes (at 0% and 10% pre-lithiation) at C / 2 rate. DETAILED DESCRIPTION

[0031] The present disclosure describes the following various non-limiting examples relating to studies conducted to identify alternative and improved anodes comprising a predominantly micro-silicon anode composition for lithium-ion batteries, any methods of incorporating the anodes into electrochemical cells, the electrochemical cells so formed, and uses thereof.

[0032] General Definitions and Terminology

[0033] In the following description, reference is made to the accompanying drawings, which form a part of the present invention and show several embodiments by way of illustration. It is to be understood that other embodiments may be utilized and structural changes may be made without departing from the scope of the present disclosure.

[0034] With respect to the definitions provided herein, unless otherwise stated or implied from the context, the defined terms and phrases include the meanings provided. In addition, unless otherwise expressly stated or apparent from the context, the following terms and phrases do not exclude that a person skilled in the relevant art has acquired the meaning of the term or phrase. These definitions are provided to help describe specific embodiments, and these definitions are not intended to limit the claimed invention, as the scope of the present invention is limited only by the claims. In addition, unless the context otherwise requires, singular terms shall include the plural and plural terms shall include the singular.

[0035] All publications discussed and / or cited herein are incorporated in their entirety.

[0036] Throughout this disclosure, references to individual steps, compositions of matter, groups of steps, or groups of compositions of matter are to be considered to encompass both one and plural (i.e., one and more) of such steps, compositions of matter, groups of steps, or groups of compositions of matter, unless expressly stated otherwise or the context requires otherwise. Thus, as used herein, the singular forms "a," "an," and "the" include plural aspects unless the context expressly dictates otherwise. For example, reference to "a" includes a single as well as two or more; reference to "an" includes a single as well as two or more; reference to "the" includes a single as well as two or more, etc.

[0037] Those skilled in the art will appreciate that the present disclosure herein is susceptible to variations and modifications other than those specifically described. It should be understood that the present disclosure includes all such variations and modifications. The present disclosure also includes, individually or collectively, all examples, steps, features, methods, compositions and processes mentioned or indicated in this specification, as well as any and all combinations or any two or more of the steps or features.

[0038] The term "and / or", such as "X and / or Y", should be understood to mean "X and Y" or "X or Y", and should be considered to provide clear support for both meanings or either meaning.

[0039] Unless otherwise indicated, the terms "first," "second," etc. are used herein merely as labels and are not intended to impose order, position, or hierarchy requirements on the items to which these terms refer. Furthermore, reference to a "second" item does not require or preclude the existence of lower-numbered items (e.g., a "first" item) and / or higher-numbered items (e.g., a "third" item).

[0040] As used herein, when used with a list of items, the phrase "at least one of" means that different combinations of one or more of the listed items may be used, and only one of each item in the list may be needed. An item may be a specific object, thing, or category. In other words, "at least one of" means that any combination or any number of items in the list may be used, but not all items in the list will be needed. For example, "at least one of item A, item B, and item C" may mean item A; item A and item B; item B; item A, item B, and item C; or item B and item C. In some cases, "at least one of item A, item B, and item C" may mean, for example, but not limited to, two of item A, one of item B, and ten of item C; four of item B and seven of item C; or some other suitable combination.

[0041] It should be appreciated that certain features described herein in the context of separate embodiments for clarity may also be provided in combination in a single embodiment. Conversely, various features described in the context of a single embodiment for brevity may also be provided separately or in any sub-combination.

[0042] Throughout this specification, various aspects and components of the present invention can be presented in range format. The range format is included for convenience and should not be interpreted as a fixed limitation on the scope of the present invention. Therefore, unless otherwise specified, the description of the range should be considered to have clearly disclosed all possible sub-ranges and individual numerical values ​​within the range. For example, the description of a range such as 1 to 5 should be considered to have specifically disclosed sub-ranges, such as 1 to 3, 1 to 4, 1 to 5, 2 to 4, 2 to 5, 3 to 5, etc., and individual numbers and partial numbers within the range, such as 1, 2, 3, 4, 5, 5.5 and 6, unless an integer is required or an integer is implied from the context. Regardless of the width of the disclosed range, this applies. Where specific values ​​are required, these values ​​will be indicated in the specification.

[0043] Throughout this specification, the word "comprise" or variations such as "comprises" or "comprising" should be understood to imply the inclusion of stated elements, integers or steps or groups of elements, integers or steps, but not the exclusion of any other elements, integers or steps or groups of elements, integers or steps.

[0044] Throughout the specification, the term "consisting essentially of is intended to exclude elements that would substantially affect the properties of the claimed composition.

[0045] In the present document, the terms "comprising", "comprise" and "comprises" are intended to be optionally replaced by the terms "consisting essentially of", "consist essentially of", "consists essentially of", "consisting of", "consist of" and "consists of", in each instance.

[0046] As used herein, the term "about" encompasses a tolerance of 10% of any value or values ​​associated with the term.

[0047] Herein, the term "weight %" may be abbreviated as "wt. %".

[0048] Specific terms

[0049] As used herein, the term "lithiation" encompasses lithiation of either the anode or cathode and is intended to mean Li + Intercalated with or alloyed with active materials.

[0050] Herein, the term "delithiation" encompasses the lithiation of the anode or cathode and is intended to mean Li + and extraction or dealloying of active materials.

[0051] The term "charge" can be used in the context of both full cells and half cells. In a full cell, the term "charge" covers the amount of charge that is forced to + A non-spontaneous process of migration from the cathode into the anode (initial pairing of the anode and cathode) and represents a rise in the cell voltage. In a half-cell, the term "charge" covers the extraction of Li from the working electrode. + The non-spontaneous process of deposition on the reference electrode (lithium metal foil) and indicating an increase in the cell voltage.

[0052] The term "discharge" can be used in the context of both full cells and half cells. In a full cell, the term "discharge" covers the extraction of Li from the anode. + The spontaneous process by which ions migrate from the anode to the cathode when assembled and represents a decrease in the cell voltage. In a half-cell, the term "discharge" covers the Li + Dissolution from the reference electrode (lithium metal foil) and Li + A spontaneous process that inserts into the working electrode and represents a decrease in the cell voltage.

[0053] As used herein, the term "half-cell" describes a reference test system consisting of a working electrode (electrode of interest) and a reference electrode (eg, lithium metal foil) used for research and development purposes.

[0054] As used herein, the term "full cell" describes a conventional electrochemical cell system that pairs a commercially relevant anode (graphite, silicon, LTO) with a commercially relevant cathode (LFP, LCO, NCM, NCA, LMO).

[0055] The term “prelithiation” describes the addition of Li to the cathode electrode prior to pairing with the cathode electrode in full cell format. + Inserted into the anode or anode active material.

[0056] The term "N / P ratio" or "negative-positive ratio" refers to the mass balance between the anode (negative electrode) and the cathode (positive electrode). The mass balance is calculated by the mass per cm of the respective electrodes. 2 Determined by the available area capacity.

[0057] The term "areal capacity" refers to the available capacity per unit area of ​​the electrode (anode or cathode). It is determined by the type and wt.% of active material in the coating and the amount of active material in mg / cm 2 (or g / m 2 The coating loading applied to the current collector substrate is determined in mg / cm 2The higher the load per cm 2 The higher the area capacity.

[0058] Coated microsilicon particles

[0059] The present disclosure relates at least in part to coated micro-silicon active material particles and / or coated anodes comprising the anode compositions described herein. It is believed that the coating applied to the micro-silicon active material particles, as described herein, can improve cycle stability and reduce electrolyte decomposition due to electrochemical protection of the anode surface. It should be understood that the coating can provide one or more of a variety of properties to the micro-silicon active particles and / or anodes, including, for example, structural strength, lower surface area, reduced pulverization, electronic conductivity, Li ion conductivity, passivation and / or insulation, and ultimately improve silicon anode capacity retention.

[0060] In some embodiments, the coating can protect the surface of the micro-silicon particles from continuous contact with the electrolyte, and thus can help reduce or eliminate the continuous reformation of the SEI layer and the associated lithium loss in each charge and discharge cycle. To achieve this result, the coating should be thick enough to form an effective barrier; flexible enough to withstand the expansion behavior of the micro-silicon active material; but thin enough to avoid or minimize the obstruction of the transfer of lithium ions or electrons from the electrolyte to the active material, and vice versa. The coating is preferably electrochemically inert, and thus forms a passivation layer on the surface of the micro-silicon particle active material.

[0061] In another embodiment, the coating may be highly conductive. A highly conductive coating may further reduce the interfacial resistance between the micro silicon particles and between these particles and the current collector.

[0062] In some embodiments, the coating can adjust the chemistry of the active material to provide greater affinity with the chemistry of the binder. For example, if the binder is more hydrophobic, the more hydrophobic active material surface will have greater affinity (and vice versa).

[0063] In some embodiments, the coating can reduce the charge transfer resistance at the interface and increase the electronic conductivity of the microsilicon particles.

[0064] In another embodiment, the coating may form a passivation layer. Once integrated into the water-based anode slurry, the coating acting as a passivation layer may prevent oxidation of the micro-silicon active material, thereby preventing the formation of hydrogen during processing, while keeping a maximum amount of the micro-silicon active material electrochemically active.

[0065] The coating may have different morphologies. The resulting coating morphology may be affected by the coating method used to apply the coating and / or the chemical properties of the precursor material or coating material used. In one embodiment, the coating may include loose aggregates or particles placed on the outer surface of the microsilicon particles or embedded in the outer surface, including nano- or micron-sized fibers, flakes, fine particles, etc. The particles may include micron- or nano-sized powders, fibers, or flakes. In another embodiment, the coating may include a discontinuous layer. In another embodiment, the coating may include a continuous layer. In another embodiment, the coating may include a conformal layer. In other embodiments, the coating may present a pinhole-free or quasi-pinhole-free coating.

[0066] The coating may be present in the anode layer at about 0.1 wt.% to about 20 wt.%, or about 0.1 wt.% to about 15 wt.%, or about 0.1 wt.% to about 10 wt.%. It is understood that the coating wt.% will be minimized to the amount that gives the most beneficial properties to achieve the desired results.

[0067] In some embodiments, the coating layer may be selected from the group consisting of carbon, graphene, graphite, metal oxides, polymers, and combinations thereof to form coated micro silicon active material particles or coated anode compositions.

[0068] In some embodiments or examples, the coating may have a thickness between about 0.1 nm and about 200 nm, or between about 0.2 nm and about 150 nm, or between about 0.3 nm and about 100 nm, or between about 0.3 nm and about 75 nm, or between about 0.3 nm and about 50 nm, or between about 0.3 nm and about 25 nm, or between about 0.3 nm and about 0.20 nm, or between about 0.3 nm and about 10 nm. The coating may have a thickness (in nm) of less than about 200, 175, 150, 125, 100, 90, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 8, 6, 5, 4, 3, 2, 1, 0.8, 0.5, 0.2, or 0.1. The thickness (in nm) of the coating can be at least about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 12, 14, 16, 18, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 100, 150, or 200. The thickness (in nm) of the coating can be within a range provided by any two of these upper and / or lower amounts.

[0069] In some embodiments, the ratio of the coating thickness to the uncoated silicon particle diameter (t / d, in the form of X:1) may be between about 0.0001:1 and about 0.2:1, or between about 0.0001:1 and about 0.15:1, or between about 0.0001:1 and about 0.12:1, or between about 0.0001:1 and about 0.1:1, or between about 0.0001:1 and about 0.09:1, or between about 0.0001:1 and about 0.085:1. Viewed from another perspective, in some embodiments, the ratio of silicon particle diameter to coating thickness (d / t, in the form of 1:X) may be between about 1:100,000 and about 1:5, or between about 1:100,000 and about 1:8, or between about 1:100,000 and about 1:10, or between about 1:100,000 and about 1:12.

[0070] The silicon active material particles herein may be coated in the form of carbon. The carbon coating may mainly comprise sp 2 Hybridized carbon or mainly contains sp 3 Hybridized carbon. The carbon coating may also contain varying degrees of sp 2 and sp 3 Hybridization. Some embodiments of the coating may contain high levels of sp 2 Hybridization and low levels of sp 3 hybridization, or vice versa. In some embodiments, relative to the sp 2 The hybridization level may be between 1% and 100%. In another embodiment, the sp3 hybridization level may be between 1% and 100%. Specific coating embodiments may include 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 99% or 100% sp 2 hybridization level, which can be compared with 1-% sp 2 Hybridization*100 sp3 hybridization level combination. In other words, regardless of sp 2 What is the level of hybridization? 2 / sp 3 In the hybrid coating, the rest of the coating consists of sp 3 Another coating embodiment may include 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or 100% sp 3 Hybridization level, while sp 2 Hybridization level is 1-% sp 3 Hybridization*100.

[0071] Carbon-coated silicon active material particles can be provided by coating micro silicon active material particles as described herein with carbon using one or more carbon precursors. As used herein, the term "carbon" can refer to an amorphous or non-graphitizable carbon coating, a graphitic carbon coating, or graphene. A non-graphitizable material is a carbon material that remains substantially amorphous even when exposed to high temperatures. As discussed above, the carbon coating can exhibit a range of mixed sp 2 / sp 3 Hybridization. Carbon coatings can be applied using a range of techniques known in the art including, but not limited to, CVD, PVD, pyrolysis, and the like.

[0072] In embodiments, the amorphous carbon coating may be a coating having soft carbon or hard carbon, as known in the art. It should be understood that a wide range of precursor materials are commercially available to achieve such amorphous carbon coatings with carbon black, petroleum pitch, coal tar pitch, acetylene gas, decomposable polymers, preferably decomposable polymers with low oxygen content, such as PVP (polyvinyl pyrrolidone), polyacrylonitrile (PAN), polyaniline (PANi), polypyrrole (PPy), melanin resins, phenolic resins, polydopamine, resorcinol formaldehyde resins, citric acid and glucose (just some non-limiting examples). The amorphous carbon layer can generally be obtained via a pyrolysis process, in which the microsilicon particles are exposed to a decomposable gas such as acetylene, which is then deposited as a carbon layer on the surface when heated to a sufficiently high temperature. Alternatively, it can be obtained by coating the microsilicon particles in a precursor material such as asphalt or a combustible polymer and pyrolyzing the asphalt or polymer to form a carbon layer. Different carbon precursors can be selected to form carbon layers of different qualities. For example, aromatic compounds may form compounds that may have a higher degree of sp 2 Hybridized high-quality coatings. More linear organic compounds (such as acetylene or certain polymers) can form more sp 3 Hybrid amorphous structure.

[0073] In some embodiments, graphene-coated micro-silicon active material particles as described herein may be provided by coating micro-silicon active material particles as described herein with graphene. In some embodiments, graphene may be selected from the group comprising graphene, graphene oxide or reduced graphene oxide and derivatives thereof. Graphite-coated micro-silicon active material particles may be provided by coating micro-silicon active material particles as described herein with graphite. In some embodiments, graphite may be selected from the group comprising graphite, nanographite, graphite oxide and derivatives thereof.

[0074] Metal oxide-coated microsilicon particles can be provided by coating microsilicon active material particles as described herein with metal oxides. In some embodiments, the metal oxide can be selected from the group comprising: aluminum oxide, hydroxide aluminum oxide (γ-AlO(OH)), aluminum hydroxide (Al(OH)3), aluminum nitrate (Al(NO3)3) or other similar aluminum-containing substances. In some embodiments, aluminum hydroxide or aluminum nitrate can form a precursor for subsequent conversion into hydroxide aluminum oxide or aluminum oxide. In some embodiments, the aluminum oxide may include alpha aluminum oxide. In another embodiment, the metal oxide may include a titanium- or niobium-based metal oxide. The metal oxide coating may include titanium oxide (TiO2) or niobium oxide (Nb2O5). In another embodiment, the metal oxide coating may include a magnesium-based oxide. The magnesium-based oxide may be magnesium oxide (MgO).

[0075] In an embodiment, metal oxides, such as α-alumina and other aluminum species, can be applied to microsilicon particles via a precipitation process followed by calcination at higher temperatures of >400°C, or via processes such as atomic layer deposition (ALD). The precipitation process approach typically involves dissolving an appropriate metal salt in water at an appropriate concentration and at a controlled pH, and manipulating the pH so that the metal salt is uniformly precipitated on the surface of the microsilicon active material. Typically, this involves increasing the pH of the environment. The concentration of the metal salt in the solution determines the final coating thickness. Excess components and metal salts can be gently washed, and the microsilicon active material can be transferred to a furnace. The precipitate can be heated to a temperature of up to 1200°C under air or an inert gas, which converts the metal salt precursor into the corresponding metal oxide.

[0076] The polymer-coated micro-silicon active material particles can be provided by coating the micro-silicon active material particles as described herein with a polymer. In some embodiments, the polymer can be selected from the group comprising starch, lignin, cellulose, polyacrylamide, polymethacrylamide, polyamic acid, polystyrene-4-sulfonate (PSS), 3,4-ethylenedioxythiophene / polystyrene-4-sulfonate (PEDOT:PSS), polydiallyldimethylammonium chloride PDDA, polydiallyldimethylammonium / polystyrene-4-sulfonate (PDDA:PSS), urea-pyrimidone (UPy), urea-oligo-amide 1,4-diisoprene (including cis-1,4-polyisoprene natural rubber and trans-1,4-polyisoprene gutta-percha), synthetic polyisoprene, polybutadiene, chloroprene rubber, polychloroprene, Butyl rubber (including halogenated butyl rubber), styrene-butadiene rubber, nitrile rubber, ethylene propylene rubber, ethylene propylene diene rubber, epichlorohydrin rubber, polyacrylic rubber, silicone rubber, fluorosilicone rubber, fluoroelastomer, perfluoroelastomer, polyether block amide, chlorosulfonated polyethylene, ethylene-vinyl acetate, thermoplastic elastomer, protein elastin, protein elastin, ethylene oxide-epichlorohydrin copolymer, polyurethane, urethane-urea copolymer, polyaniline, polypyrrole, polythiophene, polyfuran, bicyclic polymer, poly(ethylene oxide) (PEO), polypropylene oxide (PPO), poly(acrylonitrile) (PAN), poly(methyl methacrylate) (PMMA), poly(vinylidene fluoride) (PVDF), poly((bis-(methoxyethoxy)ethoxy)phosphazene), polyvinyl chloride, polydimethylsiloxane, poly(vinylidene fluoride)-hexafluoropropylene (PVDF-HFP), any derivative thereof (e.g., sulfonated derivative), phenol resin, or any combination thereof.

[0077] In some embodiments, the coated microsilicon active material particles may be provided by precipitation, pyrolysis, or by chemical vapor deposition, physical vapor deposition, atomic layer deposition sputtering, or mechanical deposition of a precursor formulation coating.

[0078] In some embodiments or examples, the coating may be in the form of a single layer on the surface of the micro-silicon active material particles. In another embodiment, the coating may be in the form of two or more layers, for example, a multilayer located on the surface of the micro-silicon active material particles. The coating may include about 1 to 5 layers. The coating may include less than 5 layers, 4 layers, 3 layers, or less than 2 layers. The coating may include at least about 1 layer, 2 layers, 3 layers, 4 layers, or at least about 5 layers. The coating may include a layer within the range provided by any lower limit and / or upper limit as previously described. It should be understood that each layer may be provided by a different coating. For example, a coated micro-silicon active material particle may include a coating, wherein the coating includes graphene, and another coating includes a metal oxide (e.g., aluminum oxide) applied to the micro-silicon in any order.

[0079] In one embodiment, the coated micro-silicon active material particles may be in any form, for example, the micro-silicon active material particles may take the form of flakes, agglomerates, particles, powders, spheres, crushed materials, and the like, and combinations thereof. The coated micro-silicon active material particles may have any desired shape, including but not limited to cubes, rods, plates, polyhedrons, spheres or hemispheres, quasi-spheres, circles or semicircles, angles, irregular shapes, and the like. In one embodiment, the aspect ratio (i.e., the ratio of length to width, where the length and width are measured perpendicular to each other, and the length refers to the longest linear measurement dimension) of the coated micro-silicon active material particles is 1.0 to 10.0, or 1.0 to 5.0, or 1.0 to 4.0. In one embodiment, the aspect ratio of the coated micro-silicon active material particles is about 1.0 to 4.0, for example, about 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, or 4.0.

[0080] In some embodiments, the particle size (in μm) of the coated microsilicon active material particles may be at least about 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, or 50. In some embodiments, the particle size (in μm) of the coated microsilicon active material particles may be less than about 50, 45, 40, 35, 30, 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, or 0.5. Combinations of any two or more of these upper and / or lower particle sizes are also possible, for example, the particle size (in μm) of the coated microsilicon active material particles may be between about 1 and about 50, about 2 and about 40, or about 3 and about 30. The particle size is taken as the longest cross-sectional diameter across the coated microsilicon active material particles. For non-spherical coated microsilica active material particles, the particle size is taken as the distance corresponding to the longest cross-sectional dimension across the particle.

[0081] The coated micro-silicon active material particles may have a certain particle size distribution, wherein 90% of the micro-silicon active material particles (D90 ) has a particle size of less than about 50, 45, 40, 35, 34, 32, 30, 28, 24, 20, 18, 16, 14, 12, 10, 8, 6, 5 or 4 μm, wherein 50% of the microsilicon active material particles (D 50 ) has a particle size (in μm) of less than about 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, 0.8, 0.6, 0.4, 0.2, 0.1, or 10% of the microsilicon active material particles (D 10 ) is less than about 4, 3, 2 or 1 μm. In some embodiments, the microsilicon active material particles have a particle size of (D 50 ) particle size (in μm) is at least about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10. In some embodiments, the (D 50 ) particle size (in μm) is less than about 10, 9, 8, 7, 6, 5, 4, 3.5, 3, 2.5, 2, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.5, 0.4, 0.3, 0.2 or 0.1. Combinations of any two or more of these upper and / or lower particle sizes are also possible, for example, the (D) of the microsilicon active material particles 50 ) particle size (in μm) is between about 0.1 to about 10, about 0.1 to about 9, about 0.1 to about 8, about 0.1 to about 7, about 0.1 to about 6, about 0.1 to about 5, about 0.5 to about 10, about 0.5 to about 9, about 0.5 to about 8, about 0.5 to about 7, about 0.5 to about 6, about 0.5 to about 5, about 1 to about 10, about 1 to about 9, about 1 to about 8, about 1 to about 7, about 1 to about 6, or about 1 to about 5.

[0082] In some embodiments or examples, the BET surface area of ​​the coated micro-silicon active material particles may be about 0.1 m 2 / g to about 100m 2 The BET surface area (m 2 The molecular weight (m / g) may be at least about 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 60, 70, 80, 90, or 100 m / g. 2 In other embodiments or examples, the surface area (m 2 / g) may be less than about 100, 90, 80, 70, 60, 50, 45, 40, 35, 30, 25, 20, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, 0.5 or 0.1 m 2Combinations of these surface area values ​​to form various ranges are also possible.

[0083] In some embodiments or examples, the tap density of the coated micro-silicon active material particles may be about 0.5 g / cm 3 To about 1.5g / cm 3 The tap density of the coated microsilicon active material particles may be at least about 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.2, 1.3, or 1.5 g / cm 3 In other embodiments or examples, the tap density of the coated microsilicon active material particles may be less than about 1.5, 1.4, 1.3, 1.2, 1.0, 0.95, 0.9, 0.85, 0.8, 0.75, 0.7, 0.65, 0.6, 0.55, or 0.5 g / cm 3 Combinations of these density values ​​to form various ranges are also possible. For example, the tap density of the coated micro-silicon active material particles may be between about 0.5 g / cm 3 To about 1.2g / cm 3 Density can be measured by any standard method, for example according to ASTM D7481-18.

[0084] Advantageously, the microsilicon active material particles of the present disclosure can be provided in high purity. In one embodiment or example, the purity of the microsilicon active material particles (excluding oxygen) may be in the range of about 95 to about 99.9 (by wt.%). The purity of the microsilicon active material particles (excluding oxygen) may be at least (by wt.%) about 95, 96, 97, 98, 99, 99.5 or 99.9. The purity of the microsilicon active material particles (excluding oxygen) may be less than (by wt.%) about 99.9, 99.5, 99, 98, 97, 96 or 95. The purity of the microsilicon active material particles (excluding oxygen) may be within the range provided by any lower limit and / or upper limit as previously described.

[0085] In one embodiment or example, the purity of the microsilicon active material particles (containing oxygen) may be in the range of about 79 to about 99.5 (by wt.%). The purity of the microsilicon active material particles (containing oxygen) may be at least (by wt.%) about 75, 80, 85, 90, 95, 96, 97, 98, 99 or 99.5. The purity of the microsilicon active material particles (containing oxygen) may be less than (by wt.%) about 99.5, 99, 98, 97, 96, 95, 90, 85, 80 or 75. The purity of the microsilicon active material particles (containing oxygen) may be within the range provided by any lower limit and / or upper limit as previously described.

[0086] The combination of novel and inventive features of the coated micro-silicon active material particles according to the present disclosure and their use in anode compositions for anodes in lithium-ion batteries can also unexpectedly lead to improvements in battery cycling behavior. It was unexpectedly shown that the lithium-ion battery as described herein has a small irreversible capacity loss in the first charging cycle and has stable electrochemical behavior and minimal decay in subsequent cycles. Therefore, by using the coated micro-silicon active material particles as described herein, a lower initial capacity loss and a low continuous capacity loss of the lithium-ion battery can be achieved. Overall, the lithium-ion battery as described herein provides very good stability and cycle life. Therefore, a large number of cycles can be achieved with minimal fatigue, for example, fatigue caused by mechanical damage to the anode coating, anode material or SEI formation.

[0087] Anode composition

[0088] The present disclosure is directed to providing improvements in anodes for lithium-ion batteries. The present disclosure encompasses various studies and developments aimed at identifying and better understanding the failure mechanisms of anodes containing a majority of silicon anode compositions, and subsequently optimizing their formulations so that degradation (e.g., cracking and delamination) of the solid electrolyte interface, silicon particle fracture and instability can be controlled, reduced or in some way ameliorated to improve the stability and cyclability of lithium-ion batteries.

[0089] It has been unexpectedly discovered that, at least according to some examples as described herein, most silicon anode compositions can exhibit significant anode stability and / or cycle life. It has further been unexpectedly discovered that most silicon anode compositions paired with methods for integration into electrochemical cells can control SEI formation and silicon expansion and degradation, and thus significantly extend the stability and / or cycle life of the anode.

[0090] It has also been discovered that, at least according to some examples as described herein, a majority of silicon anode compositions for electrochemical cells (e.g., batteries) can provide one or more additional advantages, such as:

[0091] (a) Long-term cycling stability of lithium-ion (Li-ion) batteries;

[0092] (b) Controlled expansion and contraction of silicon during charge and discharge cycles of lithium-ion batteries, which minimizes silicon particle cracking, pulverization, and SEM growth;

[0093] (c) cell capacity fade during cycle life due to controlled silicon expansion / contraction and reduced silicon anode voltage window; and / or

[0094] (d) High rate capacity.

[0095] The anode composition described herein may include microsilicon active material particles, wherein the microsilicon active material particles have one or more of the following: (i) a BET surface area measured between about 0.1 m 2 / g and about 10m 2 / g; (ii) D 50 The particle size is between about 0.1 μm and about 10 μm; and (iii) D 50 :BET surface area ratio is between about 0.1 and 10, and the amount of silicon present in the anode composition is between about 60 wt.% and about 95 wt.%, based on the total weight % of the anode composition.

[0096] In some embodiments, the anode composition as described herein may include micro-silicon active material particles, wherein the micro-silicon active material particles have a BET surface area measured by (i) between about 0.1 m 2 / g and about 10m 2 / g; and (ii) D 50 The particle size is between about 0.1 μm and about 10 μm; or (iii) D 50 :BET surface area ratio is between about 0.1 and 10, and the amount of silicon present in the anode composition is between about 60 wt.% and about 95 wt.%, based on the total weight % of the anode composition.

[0097] The anode composition as described herein may comprise or consist of microsilicon active material particles as described herein, optionally one or more additional active materials, optionally one or more binders, optionally one or more conductive materials, and optionally one or more additives. In one example, the anode composition as described herein may comprise or consist of microsilicon active material particles, wherein the microsilicon active material particles have one or more of the following: (i) a BET surface area measured between about 0.1 m 2 / g and about 10m 2 / g; (ii) D 50 The particle size is between about 0.1 μm and about 10 μm; and (iii) D 50 :BET surface area ratio is between about 0.1 and 10, wherein the microsilicon active material particles are coated, and wherein the amount of coated microsilicon active material particles present in the anode composition is between about 60 wt.% and about 95 wt.% based on the total weight % of the anode composition; optionally one or more additional active materials; optionally one or more binders; optionally one or more conductive materials; and optionally one or more additives.

[0098] In some embodiments, the anode composition as described herein may include the following: microsilicon active material particles, wherein the microsilicon active material particles have a BET surface area of ​​(i) between about 0.1 m 2 / g and about 10m 2 / g; and (ii) D 50 The particle size is between about 0.1 μm and about 10 μm; or (iii) D 50 :BET surface area ratio is between about 0.1 and 10, wherein the microsilicon active material particles are coated, and wherein the amount of coated microsilicon active material particles present in the anode composition is between about 60 wt.% and about 95 wt.% based on the total weight % of the anode composition; optionally one or more additional active materials, optionally one or more binders; optionally one or more conductive materials; and optionally one or more additives.

[0099] In some embodiments or examples, the micro-silicon active material particle content of the anode composition may be about 60wt.% to about 95wt.%, based on the total weight of the anode composition. It should be understood that when the micro-silicon active material particle content of the anode composition is greater than 60wt.%, preferably greater than 70wt.%, additional advantages may be exhibited. The micro-silicon active material particle content may be less than about 95wt.%, 90wt.%, 85wt.%, 80wt.%, 75wt.%, 70wt.%, 65wt.% or 60wt.%. The micro-silicon active material particle content may be at least about 60wt.%, 65wt.%, 70wt.%, 75wt.%, 80wt.%, 85wt.%, 90wt.% or 95wt.%. The micro-silicon active material particle content of the anode composition may be within the range provided by any two of these upper and / or lower limits.

[0100] In some embodiments or examples, the thickness of the anode composition may be substantially uniform and in the range of about 5 μm to about 70 μm. The thickness (μm) of the anode composition may be less than about 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10 or 5. The thickness (μm) of the anode composition may be at least about 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 or 65. The thickness of the anode composition may be within the range provided by any two of these upper and / or lower limits.

[0101] In some embodiments or examples, the anode composition may be loaded on the current collector material. In some embodiments or examples, the anode composition may be applied to the current collector material as a coating or film. It should be understood that the current collector may be at least partially coated with the anode composition. For example, the anode composition may be applied only to one side of the current collector material. The current collector material for the anode may be selected from the group comprising the following: copper, aluminum, stainless steel, titanium, carbon, perforated metal foil, metal foam, and porous and non-porous films based on metal-coated polymers. It should be understood that the current collector material will have appropriate size, porosity and pore size, covering the above materials and acting as a current collector. For example, the anode composition may be applied to a copper current collector material (such as copper foil). For example, a micro-silicon active material particle, one or more optional additional active materials, one or more optional adhesives, one or more optional conductive materials, and one or more optional additives or an anode composition consisting thereof may be loaded on a copper current collector material (such as copper foil). In some embodiments, the thickness of the current collector material for the anode may be between about 4 μm and about 25 μm. The thickness of the current collector (in μm) may be less than about 25, 20, 15, 10, 8, 6, or 4. The thickness of the current collector (in μm) may be at least about 4, 5, 6, 7, 8, 9, 10, 12, 14, 16, 18, 20, or 25. The thickness of the current collector (in μm) may be within the range provided by any two of these upper and / or lower limits. In one example, the current collector material for the anode may be a copper foil having a thickness between about 6 μm and about 12 μm.

[0102] In some embodiments or examples, the anode composition can be an anode of a battery. For example, the anode composition can be an anode of a lithium-ion battery.

[0103] The present disclosure may also relate to an anode composition comprising a coating. In some embodiments or examples, the coating may be a coating of micro-silicon active material particles, which are subsequently incorporated into the anode composition. In other embodiments or examples, the coating may be a coating of the anode composition or the anode itself. In other words, the coating may be present on at least a portion of the surface of the anode composition and the anode so formed. In some embodiments or examples, the portion (%) may be at least about 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95 or 100.

[0104] In some embodiments, the coating layer may be selected from the group consisting of carbon, graphene, graphite, metal oxides, polymers, and combinations thereof to form coated micro silicon active material particles or coated anode compositions.

[0105] The silicon active material particles herein may be coated in the form of carbon. The carbon coating may mainly comprise sp 2 Hybridized carbon or mainly contains sp 3 Hybridized carbon. The carbon coating may also contain varying degrees of sp 2 and sp 3 Hybridization. Some embodiments of the coating may contain high levels of sp 2 Hybridization and low levels of sp 3 hybridization, or vice versa. In some embodiments, relative to the sp 2 The hybridization level may be between 1% and 100%. In another embodiment, the sp3 hybridization level may be between 1% and 100%. Specific coating embodiments may include 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 99% or 100% sp 2 hybridization level, which can be compared with 1-% sp 2 Hybridization*100 sp3 hybridization level combination. In other words, regardless of sp 2 What is the level of hybridization? 2 / sp 3 In the hybrid coating, the rest of the coating consists of sp 3 Another coating embodiment may include 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or 100% sp 3 Hybridization level, while sp 2 Hybridization level is 1-% sp 3 Hybridization*100.

[0106] Carbon-coated silicon active material particles can be provided by coating micro silicon active material particles as described herein with carbon using one or more carbon precursors. As used herein, the term "carbon" can refer to an amorphous or non-graphitizable carbon coating, a graphitic carbon coating, or graphene. A non-graphitizable material is a carbon material that remains substantially amorphous even when exposed to high temperatures. As discussed above, the carbon coating can exhibit a range of mixed sp 2 / sp 3 Hybridization. Carbon coatings can be applied using a range of techniques known in the art including, but not limited to, CVD, PVD, pyrolysis, and the like.

[0107] In embodiments, the amorphous carbon coating may be a coating having soft carbon or hard carbon, as known in the art. It should be understood that a wide range of precursor materials are commercially available to achieve such amorphous carbon coatings with carbon black, petroleum pitch, coal tar pitch, acetylene gas, decomposable polymers, preferably decomposable polymers with low oxygen content, such as PVP (polyvinyl pyrrolidone), polyacrylonitrile (PAN), polyaniline (PANi), polypyrrole (PPy), melanin resins, phenolic resins, polydopamine, resorcinol formaldehyde resins, citric acid and glucose (just some non-limiting examples). The amorphous carbon layer can generally be obtained via a pyrolysis process, in which the microsilicon particles are exposed to a decomposable gas such as acetylene, which is then deposited as a layer on the surface when heated to a sufficiently high temperature. Alternatively, it can be obtained by coating the microsilicon particles in a precursor material such as asphalt or a combustible polymer and pyrolyzing the asphalt or polymer to form a carbon layer. Different carbon precursors can be selected to form carbon layers of different qualities. For example, aromatic compounds can form compounds that may have a higher degree of sp 2 Hybridized high-quality coatings. More linear organic compounds (such as acetylene or certain polymers) can form more sp 3 Hybrid amorphous structure.

[0108] In some embodiments, graphene-coated micro-silicon active material particles as described herein may be provided by coating micro-silicon active material particles as described herein with graphene. In some embodiments, graphene may be selected from the group comprising graphene, graphene oxide or reduced graphene oxide and derivatives thereof. Graphite-coated micro-silicon active material particles may be provided by coating micro-silicon active material particles as described herein with graphite. In some embodiments, graphite may be selected from the group comprising graphite, nanographite, graphite oxide and derivatives thereof.

[0109] Metal oxide-coated microsilicon particles can be provided by coating microsilicon active material particles as described herein with metal oxides. In some embodiments, the metal oxide can be selected from the group comprising: aluminum oxide, hydroxide aluminum oxide (γ-AlO(OH)), aluminum hydroxide (Al(OH)3), aluminum nitrate (Al(NO3)3) or other similar aluminum-containing substances. In some embodiments, aluminum hydroxide or aluminum nitrate can form a precursor for subsequent conversion into hydroxide aluminum oxide or aluminum oxide. In some embodiments, the aluminum oxide may include alpha aluminum oxide. In another embodiment, the metal oxide may include a titanium- or niobium-based metal oxide. The metal oxide coating may include titanium oxide (TiO2) or niobium oxide (Nb2O5). In another embodiment, the metal oxide coating may include a magnesium-based oxide. The magnesium-based oxide may be magnesium oxide (MgO).

[0110] In an embodiment, metal oxides, such as α-alumina and other aluminum species, can be applied to microsilicon particles via a precipitation process followed by calcination at higher temperatures of >400°C, or via processes such as atomic layer deposition (ALD). The precipitation process approach typically involves dissolving an appropriate metal salt in water at an appropriate concentration and at a controlled pH, and manipulating the pH so that the metal salt is uniformly precipitated on the surface of the microsilicon active material. Typically, this involves increasing the pH of the environment. The concentration of the metal salt in the solution determines the final coating thickness. Excess components and metal salts can be gently washed, and the microsilicon active material can be transferred to a furnace. The precipitate can be heated to a temperature of up to 1200°C under air or an inert gas, which converts the metal salt precursor into the corresponding metal oxide.

[0111] The polymer-coated micro-silicon active material particles can be provided by coating the micro-silicon active material particles as described herein with a polymer. In some embodiments, the polymer can be selected from the group comprising starch, lignin, cellulose, polyacrylamide, polymethacrylamide, polyamic acid, polystyrene-4-sulfonate (PSS), 3,4-ethylenedioxythiophene / polystyrene-4-sulfonate (PEDOT:PSS), polydiallyldimethylammonium chloride PDDA, polydiallyldimethylammonium / polystyrene-4-sulfonate (PDDA:PSS), urea-pyrimidone (UPy), urea-oligo-amide 1,4-diisoprene (including cis-1,4-polyisoprene natural rubber and trans-1,4-polyisoprene gutta-percha), synthetic polyisoprene, polybutadiene, chloroprene rubber, polychloroprene, Butyl rubber (including halogenated butyl rubber), styrene-butadiene rubber, nitrile rubber, ethylene propylene rubber, ethylene propylene diene rubber, epichlorohydrin rubber, polyacrylic rubber, silicone rubber, fluorosilicone rubber, fluoroelastomer, perfluoroelastomer, polyether block amide, chlorosulfonated polyethylene, ethylene-vinyl acetate, thermoplastic elastomer, protein elastin, protein elastin, ethylene oxide-epichlorohydrin copolymer, polyurethane, urethane-urea copolymer, polyaniline, polypyrrole, polythiophene, polyfuran, bicyclic polymer, poly(ethylene oxide) (PEO), polypropylene oxide (PPO), poly(acrylonitrile) (PAN), poly(methyl methacrylate) (PMMA), poly(vinylidene fluoride) (PVDF), poly((bis-(methoxyethoxy)ethoxy)phosphazene), polyvinyl chloride, polydimethylsiloxane, poly(vinylidene fluoride)-hexafluoropropylene (PVDF-HFP), any derivative thereof (e.g., sulfonated derivative), phenol resin, or any combination thereof.

[0112] The silane coupling agent-derived coating on the micro-silicon active material particles can be provided by a silane coupling agent represented by the following formula (1): Y-(CH2) n -Si-X3, wherein Y represents a non-hydrolyzable group capable of forming, when polymerized on the surface of the active material, a conductive polymer moiety, a conductive coating, a lithium ion conductive coating, a layer that interacts with an electrode binder advantageously via physical attraction or adhesion, a layer that interacts with an electrode binder advantageously via formation of chemical bonds, or a combination of any of the above;

[0113] each X independently represents a hydroxyl group or a hydrolyzable group selected from the group consisting of a halogen atom, an alkoxy group, an ether group, and a siloxy group;

[0114] The three X groups may be the same as or different from each other; and

[0115] n represents an integer of 0 to 3.

[0116] In some examples, Y can include an amino group, an epoxy group, a polyethylene glycol methyl ether, a polyethylene glycol, an acryloxy group, a methacryloxy group, or any combination thereof.

[0117] Examples of the silane coupling agent represented by formula (1) may include, but are not limited to, aminopropyltriethoxysilane, aminopropyltrimethoxysilane, bis-gammatrimethoxysilanepropylamine, aminoneohexyltrimethoxysilane.

[0118] In embodiments, the coated microsilica active material particles or coated anode composition may be provided in any manner or embodiment as described above, including pyrolysis of the coating or by chemical vapor deposition, physical vapor deposition, sputtering, or mechanical deposition.

[0119] In some embodiments or examples, the coating may be in the form of a single layer. In another embodiment, the coating may be in the form of two or more layers (e.g., multiple layers). The coating may include about 1 to 5 layers. The coating may include less than 5 layers, 4 layers, 3 layers, or less than 2 layers. The coating may include at least about 1 layer, 2 layers, 3 layers, 4 layers, or at least about 5 layers. The coating may be included in a layer within the range provided by any lower limit and / or upper limit as previously described. It should be understood that each layer may be provided by a different coating. For example, a coated micro-silicon active material particle or a coated anode composition may include a coating, wherein one coating includes a carbon material, another coating includes a metal oxide (e.g., aluminum oxide), and another layer includes a polymer coating applied to the micro-silicon in any order. Alternatively, the coating may be a carbon material coating and a metal oxide coating applied to the micro-silicon in any order. In addition, the coating may be a carbon material coating and a polymer coating applied to the micro-silicon in any order.

[0120] It is believed that the coating on the micro silicon active material particles or anode composition, as described herein, can improve the cycling stability and reduce the electrolyte decomposition due to the electrochemical protection of the anode surface. It should be understood that the coating can provide a variety of properties to the micro silicon active particles or anode composition, including, for example, structural strength, lower surface area, reduced pulverization, electronic conductivity, Li ion conductivity, passivation and / or insulation, and ultimately improve the silicon anode capacity retention rate.

[0121] Silicon particles

[0122] The present invention relates to an anode composition comprising optionally coated micro-silicon active material particles. The present invention also relates to an anode composition comprising coated micro-silicon active material particles.

[0123] In some embodiments or examples, the micro silicon active material particles may be selected from the group consisting of: metallurgical silicon, polycrystalline silicon and single crystal silicon. In a preferred example, the micro silicon active material particles are metallurgical silicon.

[0124] It will be appreciated that the raw material for any type of elemental silicon is quartz sand (silicon dioxide (SiO2)). In conventional manufacturing processes, SiO2 is reacted with carbon in an electric arc furnace, where the carbon may be supplied to the process in the form of coke, and where high temperatures (about 1800°C) are applied to reduce SiO2 to Si and CO according to the following reaction:

[0125] SiO2+2C→Si+2CO………………………………………………………………(1)

[0126] This reaction produces metallurgical grade silicon, which may contain impurities such as Al, Ca, Fe, Ti, P, Cu, Cr, K, V, Ni, Na, etc. at levels ranging from hundreds to thousands of parts per million (ppm). Metallurgical silicon can be used in various industrial applications, including steel production. However, due to the impurities, it cannot be used in electronic applications. The crystal structure of metallurgical silicon is well defined, but it is neither as pure as single crystal silicon nor as efficient at conducting electricity as single crystal silicon. Metallurgical silicon has a metallic crystal structure, which is characterized by metallic bonding between its atoms. In a metallic crystal structure, the atoms are arranged in a repeating pattern, but lack order.

[0127] To reduce the impurities in metallurgical silicon to a few parts per billion (ppb), further refining is required. This process can produce semiconductor-grade or electronic-grade Si (also known as polysilicon). The reaction between metallurgical silicon and anhydrous HCl will form trichlorosilane (SiHCl3), which is a liquid with a boiling point of 32°C:

[0128] Si+3HCl→SiHCl3+H2………………………………………………………………(2)

[0129] It should be understood that some chloride impurities, such as FeCl3, may also be formed, but due to the difference between the boiling points of these impurities and SiHCl3, fractional distillation techniques can be used to separate the impurities. During this process, a mixture of SiHCl3 and chloride impurities is heated, with the vapors condensed in different distillation columns and maintained at appropriate temperatures. This will enable the separation of pure SiHCl3 from the impurities. The reaction between SiHCl3 and H2 will result in the formation of pure polysilicon.

[0130] 2SiHCl3+2H2→2Si+6HCl……………………………………………………(3)

[0131] The crystal structure of polycrystalline silicon is ill-defined, and the small crystals (grains) that make up the material are randomly oriented and are typically less than 100 microns in size. The grains are separated by grain boundaries and typically have random crystal orientations. This produces a material that is weaker and less efficient at conducting electricity than single crystal silicon.

[0132] The Czochralski method is used to convert pure polysilicon into single crystals of single silicon. A seed crystal is required to grow the single crystal material, which will act as a template for growth. The Czochralski method involves heating the polysilicon in a quartz-lined graphite crucible by resistively heating it to the melting point of Si (1412°C). The seed crystal is then placed in the molten material and slowly raised, allowing the crystal to grow onto the seed crystal. During crystal growth, slow rotation is required to average out any temperature variations that may cause uneven solidification.

[0133] The resulting single crystal silicon is often referred to as single-crystalline silicon. It consists of silicon characterized by a regular and repeating arrangement of its atoms in a three-dimensional lattice and without grain confinement. Single crystal silicon can be considered an intrinsic semiconductor consisting only of superpure silicon. Silicon single crystals are well known for their high efficiency and high purity, making them ideal for electronic applications. By incorporating other elements, single crystal silicon can be p-type silicon and n-type silicon.

[0134] It is well known in the art that impurities may be present in any micro-silicon active material particles. It is also well known that impurities may be selectively added to any micro-silicon active material particles. In some embodiments, impurities selected from the group consisting of Al, Ca, Fe, Ti, P, Cu, Cr, K, V, Ni and Na may be present in the micro-silicon active material particles, for example, in a total amount or in an individual amount of less than about 5000 ppm, less than about 4500 ppm, less than about 4000 ppm, less than about 3500 ppm or less than about 3000 ppm. In one embodiment, the total impurities or individual impurities selected from the group consisting of Al, Ca, Fe, Ti, P, Cu, Cr, K, V, Ni and Na may be present in the micro-silicon active material particles in a range between about 0 ppm and about 5000 ppm, preferably between about 0 ppm and about 4000 ppm, and more preferably between about 0 ppm and about 3000 ppm.

[0135] In preferred embodiments or examples of the present disclosure, the micro silicon active material particles are coated micro silicon active material particles as described herein, and the anode composition including the coated micro silicon active material particles may or may not be additionally coated.

[0136] In some embodiments, the micro silicon active material particle coating may be selected from the group consisting of carbon, graphene, graphite, metal oxides, polymers, and combinations thereof to form coated micro silicon active material particles or coated anode compositions.

[0137] In some embodiments or examples, the thickness of the coating may be between about 0.1 nm and about 200 nm, or between about 0.2 nm and about 150 nm, or between about 0.3 nm and about 100 nm, or between about 0.3 nm and about 75 nm, or between about 0.3 nm and about 50 nm, or between about 0.3 nm and about 25 nm, or between about 0.3 nm and about 20 nm, or between about 0.3 nm and about 10 nm. The thickness of the coating (in nm) may be less than about 200, 175, 150, 125, 100, 90, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 8, 6, 5, 4, 3, 2, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, or 0.1.

[0138] In some embodiments, the ratio of the coating thickness to the uncoated silicon particle diameter (t / d, in the form of X:1) may be between about 0.0001:1 and about 0.2:1, or between about 0.0001:1 and about 0.15:1, or between about 0.0001:1 and about 0.12:1, or between about 0.0001:1 and about 0.1:1, or between about 0.0001:1 and about 0.09:1, or between about 0.0001:1 and about 0.085:1. Viewed from another perspective, in some embodiments, the ratio of silicon particle diameter to coating thickness (d / t, in the form of 1:X) may be between about 1:100,000 and about 1:5, or between about 1:100,000 and about 1:8, or between about 1:100,000 and about 1:10, or between about 1:100,000 and about 1:12.

[0139] The silicon active material particles herein may be coated in the form of carbon. The carbon coating may mainly comprise sp 2 Hybridized carbon or mainly contains sp 3 Hybridized carbon. The carbon coating may also contain varying degrees of sp 2 and sp 3 Hybridization. Some embodiments of the coating may contain high levels of sp 2 Hybridization and low levels of sp 3 hybridization, or vice versa. In some embodiments, relative to the sp 2 The hybridization level may be between 1% and 100%. In another embodiment, the sp3 hybridization level may be between 1% and 100%. Specific coating embodiments may include 10%, 20%, 30%, 50%, 60%, 70%, 80%, 90%, 99% or 100% sp 2 hybridization level, which can be compared with 1-% sp 2 Hybridization*100 sp3 hybridization level combination. In other words, regardless of sp 2 What is the level of hybridization? 2 / sp 3 In the hybrid coating, the rest of the coating consists of sp 3 Another coating embodiment may include 10%, 20%, 30%, 50%, 60%, 70%, 80%, 90% or 100% sp 3 Hybridization level, while sp 2 Hybridization level is 1-% sp 3 Hybridization*100.

[0140] Carbon-coated silicon active material particles can be provided by coating micro silicon active material particles as described herein with carbon using one or more carbon precursors. As used herein, the term "carbon" can refer to an amorphous or non-graphitizable carbon coating, a graphitic carbon coating, or graphene. A non-graphitizable material is a carbon material that remains substantially amorphous even when exposed to high temperatures. As discussed above, the carbon coating can exhibit a range of mixed sp 2 / sp 3 Hybridization. Carbon coatings can be applied using a range of techniques known in the art including, but not limited to, CVD, PVD, pyrolysis, and the like.

[0141] In embodiments, the amorphous carbon coating may be a coating having soft carbon or hard carbon, as known in the art. It should be understood that a wide range of precursor materials are commercially available to achieve such amorphous carbon coatings with carbon black, petroleum pitch, coal tar pitch, acetylene gas, decomposable polymers, preferably decomposable polymers with low oxygen content, such as PVP (polyvinyl pyrrolidone), polyacrylonitrile (PAN), polyaniline (PANi), polypyrrole (PPy), melanin resins, phenolic resins, polydopamine, resorcinol formaldehyde resins, citric acid and glucose (just some non-limiting examples). The amorphous carbon layer can generally be obtained via a pyrolysis process, in which the microsilicon particles are exposed to a decomposable gas such as acetylene, which is then deposited as a layer on the surface when heated to a sufficiently high temperature. Alternatively, it can be obtained by coating the microsilicon particles in a precursor material such as asphalt or a combustible polymer and pyrolyzing the asphalt or polymer to form a carbon layer. Different carbon precursors can be selected to form carbon layers of different qualities. For example, aromatic compounds may form compounds that may have a higher degree of sp 2 Hybridized high-quality coatings. More linear organic compounds (such as acetylene or certain polymers) can form more sp 3 Hybrid amorphous structure.

[0142] In some embodiments, graphene-coated micro-silicon active material particles as described herein may be provided by coating micro-silicon active material particles as described herein with graphene. In some embodiments, graphene may be selected from the group comprising graphene, graphene oxide or reduced graphene oxide and derivatives thereof. Graphite-coated micro-silicon active material particles may be provided by coating micro-silicon active material particles as described herein with graphite. In some embodiments, graphite may be selected from the group comprising graphite, nanographite, graphite oxide and derivatives thereof.

[0143] Metal oxide-coated microsilicon particles can be provided by coating microsilicon active material particles as described herein with metal oxides. In some embodiments, the metal oxide can be selected from the group comprising: aluminum oxide, hydroxide aluminum oxide (γ-AlO(OH)), aluminum hydroxide (Al(OH)3), aluminum nitrate (Al(NO3)3) or other similar aluminum-containing substances. In some embodiments, aluminum hydroxide or aluminum nitrate can form a precursor for subsequent conversion into hydroxide aluminum oxide or aluminum oxide. In some embodiments, the aluminum oxide may include alpha aluminum oxide. In another embodiment, the metal oxide may include a titanium- or niobium-based metal oxide. The metal oxide coating may include titanium oxide (TiO2) or niobium oxide (Nb2O5). In another embodiment, the metal oxide coating may include a magnesium-based oxide. The magnesium-based oxide may be magnesium oxide (MgO).

[0144] In an embodiment, metal oxides, such as α-alumina and other aluminum species, can be applied to microsilicon particles via a precipitation process followed by calcination at higher temperatures of >400°C, or via processes such as atomic layer deposition (ALD). The precipitation process approach typically involves dissolving an appropriate metal salt in water at an appropriate concentration and at a controlled pH, and manipulating the pH so that the metal salt is uniformly precipitated on the surface of the microsilicon active material. Typically, this involves increasing the pH of the environment. The concentration of the metal salt in the solution determines the final coating thickness. Excess components and metal salts can be gently washed, and the microsilicon active material can be transferred to a furnace. The precipitate can be heated to a temperature of up to 1200°C under air or an inert gas, which converts the metal salt precursor into the corresponding metal oxide.

[0145] The polymer-coated micro-silicon active material particles can be provided by coating the micro-silicon active material particles as described herein with a polymer. In some embodiments, the polymer can be selected from the group comprising starch, lignin, cellulose, polyacrylamide, polymethacrylamide, polyamic acid, polystyrene-4-sulfonate (PSS), 3,4-ethylenedioxythiophene / polystyrene-4-sulfonate (PEDOT:PSS), polydiallyldimethylammonium chloride PDDA, polydiallyldimethylammonium / polystyrene-4-sulfonate (PDDA:PSS), urea-pyrimidone (UPy), urea-oligo-amide 1,4-diisoprene (including cis-1,4-polyisoprene natural rubber and trans-1,4-polyisoprene gutta-percha), synthetic polyisoprene, polybutadiene, chloroprene rubber, polychloroprene, Butyl rubber (including halogenated butyl rubber), styrene-butadiene rubber, nitrile rubber, ethylene propylene rubber, ethylene propylene diene rubber, epichlorohydrin rubber, polyacrylic rubber, silicone rubber, fluorosilicone rubber, fluoroelastomer, perfluoroelastomer, polyether block amide, chlorosulfonated polyethylene, ethylene-vinyl acetate, thermoplastic elastomer, protein elastin, protein elastin, ethylene oxide-epichlorohydrin copolymer, polyurethane, urethane-urea copolymer, polyaniline, polypyrrole, polythiophene, polyfuran, bicyclic polymer, poly(ethylene oxide) (PEO), polypropylene oxide (PPO), poly(acrylonitrile) (PAN), poly(methyl methacrylate) (PMMA), poly(vinylidene fluoride) (PVDF), poly((bis-(methoxyethoxy)ethoxy)phosphazene), polyvinyl chloride, polydimethylsiloxane, poly(vinylidene fluoride)-hexafluoropropylene (PVDF-HFP), any derivative thereof (e.g., sulfonated derivative), phenol resin, or any combination thereof.

[0146] In some embodiments, the coated microsilicon active material particles may be provided by precipitation, pyrolysis, or by chemical vapor deposition, physical vapor deposition, atomic layer deposition sputtering, or mechanical deposition of a precursor formulation coating.

[0147] In some embodiments or examples, the coating may be in the form of a single layer. In another embodiment, the coating may be in the form of two or more layers (e.g., multiple layers). The coating may include about 1 to 5 layers. The coating may include less than 5 layers, 4 layers, 3 layers, or less than 2 layers. The coating may include at least about 1 layer, 2 layers, 3 layers, 4 layers, or at least about 5 layers. The coating may be included in a layer within the range provided by any lower limit and / or upper limit as previously described. It should be understood that each layer may be provided by a different coating. For example, a coated micro-silicon active material particle or a coated anode composition may include a coating, wherein one coating includes a carbon material, another coating includes a metal oxide (e.g., aluminum oxide), and another layer includes a polymer coating applied to the micro-silicon in any order. Alternatively, the coating may be a carbon material coating and a metal oxide coating applied to the micro-silicon in any order. In addition, the coating may be a carbon material coating and a polymer coating applied to the micro-silicon in any order.

[0148] It is believed that, as described herein, the coating on the micro silicon active material particles can improve the cycling stability and reduce the electrolyte decomposition due to the electrochemical protection of the anode surface. It should be understood that the coating can provide a variety of properties to the micro silicon active particles, including, for example, structural strength, lower surface area, reduced pulverization, electronic conductivity, Li ion conductivity and / or insulation, and ultimately improve the silicon anode capacity retention.

[0149] In one embodiment, the microsilicon active material particles or coated microsilicon active material particles may be in any form, for example, they may take the form of flakes, agglomerates, particles, powders, spheres, crushed materials, etc., and combinations thereof. The microsilicon active material particles or coated microsilicon active material particles may have any desired shape, including but not limited to cubes, rods, plates, polyhedrons, spheres or hemispheres, quasi-spheres, circles or semicircles, angles, irregular shapes, etc. In one embodiment, the aspect ratio (i.e., the ratio of length to width, where the length and width are measured perpendicular to each other and the length refers to the longest linear measurement dimension) of the microsilicon active material particles or coated microsilicon active material particles is 1.0 to 10.0, 1.0 to 5.0, or 1.0 to 2.0. In one embodiment, the aspect ratio of the microsilicon active material particles or coated microsilicon active material particles may be about 1.0 to 5.0, or about 1.0 to 4.0, or about 1.0 to about 3.0, or about 1.0 to about 2.0, for example about 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5 or 5.0.

[0150] In some embodiments, the particle size (in μm) of the microsilicon active material particles or coated microsilicon active material particles may be at least about 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, or 30. In some embodiments, the particle size (in μm) of the microsilicon active material particles or coated microsilicon active material particles may be less than about 30, 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, or 0.5. Combinations of any two or more of these upper and / or lower particle sizes are also possible, for example, the particle size (in μm) of the microsilicon active material particles or coated microsilicon active material particles may be between about 1 and about 10, about 2 and about 8, about 3 and about 6, or about 2 and about 5. The particle size is taken as the longest cross-sectional diameter across the microsilicon active material particles or coated microsilicon active material particles. For non-spherical microsilicon active material particles or non-spherical coated microsilicon active material particles, the particle size is taken as the distance corresponding to the longest cross-sectional dimension across the particle.

[0151] The micro-silicon active material particles may have a certain particle size distribution, wherein 90% of the micro-silicon active material particles (D 90 ) has a particle size of less than about 50, 45, 40, 35, 34, 32, 30, 28, 24, 20, 18, 16, 14, 12, 10, 8, 6, 5 or 4 μm, wherein 50% of the microsilicon active material particles (D 50 ) has a particle size (in μm) of less than about 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2 or 0.1, or 10% of the microsilicon active material particles (D 10 ) is less than about 4, 3, 2, or 1. In some embodiments, the microsilicon active material particles have a particle size of (D 50 ) particle size (in μm) is at least about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10. In some embodiments, the (D 50 ) particle size (in μm) is less than about 10, 9, 8, 7, 6, 5, 4, 3.5, 3, 2.5, 2, 1.5, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2 or 0.1. Combinations of any two or more of these upper and / or lower particle sizes are also possible, for example, the (D) of the microsilicon active material particles 50) particle size (in μm) is between about 0.1 to about 10, about 0.1 to about 9, about 0.1 to about 8, about 0.1 to about 7, about 0.1 to about 6, about 0.1 to about 5, about 0.5 to about 10, about 0.5 to about 9, about 0.5 to about 8, about 0.5 to about 7, about 0.5 to about 6, about 0.5 to about 5, about 1 to about 10, about 1 to about 9, about 1 to about 8, about 1 to about 7, about 1 to about 6, or about 1 to about 5.

[0152] In some embodiments or examples, the BET surface area of ​​the micro-silicon active material particles may be about 0.1 m 2 / g to about 10m 2 / g, for example, about 0.1 m 2 / g to about 5m 2 / g. The BET surface area of ​​the micro-silicon active material particles (m 2 / g) can be at least about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 m / g. 2 In other embodiments or examples, the surface area (m 2 / g) may be less than about 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, or 0.1 m 2 / g. Combinations of these surface area values ​​to form various ranges are also possible, for example, the surface area of ​​the microsilicon active material particles can be from about 0.1 to about 10, from about 0.1 to about 9, from about 0.1 to about 8, from about 0.1 to about 7, from about 0.1 to about 6, from about 0.1 to about 5, from about 0.5 to about 10, from about 0.5 to about 9, from about 0.5 to about 8, from about 0.5 to about 7, from about 0.5 to about 6, from about 0.5 to about 5, from about 1 to about 10, from about 1 to about 9, from about 1 to about 8, from about 1 to about 7, from about 1 to about 6, or from about 1 to about 5.

[0153] In some embodiments or examples, the BET surface area of ​​the coated micro-silicon active material particles may be about 0.1 m 2 / g to about 90m 2 The BET surface area (m 2 / g) can be at least about 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 60, 70, 80 or 90 m / g. 2 In other embodiments or examples, the surface area (m 2 / g) may be less than about 90, 80, 70, 60, 50, 40, 30, 20, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, 0.5 or 0.1 m 2 Combinations of these surface area values ​​to form various ranges are also possible.

[0154] The inventors unexpectedly found that the D 50 Particle size (in μm) and BET surface area (m 2 There is a relationship between the D of the micro-silicon active material particles and the ratio of these parameters to the electrochemical performance of the anode. 50 Particle size (in μm) and BET surface area (m 2 / g) may be in the range of about 0.1 to about 10. In some embodiments or examples, the D 50 Particle size (in μm) and BET surface area (m 2 The ratio of D / g) may be at least about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10. In some embodiments or examples, the D of the uncoated micro-silicon active material particles is 50 Particle size (in μm) and BET surface area (m 2 The ratio of D / g) can be less than about 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2 or 0.1. Combinations of these ratios to form various ranges are also possible, for example, the D of the microsilicon active material particles is less than about 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2 or 0.1. 50 Particle size (in μm) and BET surface area (m 2 The ratio of D / g) may be in the range of about 0.1 to about 10, about 0.1 to about 9, about 0.1 to about 8, about 0.1 to about 7, about 0.1 to about 6, about 0.1 to about 5, about 0.5 to about 10, about 0.5 to about 9, about 0.5 to about 8, about 0.5 to about 7, about 0.5 to about 6, about 0.5 to about 5, about 1 to about 10, about 1 to about 9, about 1 to about 8, about 1 to about 7, about 1 to about 6, or about 1 to about 5. For example, the D of the microsilicon active material particles may be about 0.1 to about 10, about 0.1 to about 9, about 0.1 to about 8, about 1 to about 7, about 1 to about 6, or about 1 to about 5. 50 Particle size (in μm) and BET surface area (m 2 / g) is in the range of about 0.1 to about 6, and the ratio of the nanostructured carbon nanotubes to the nanostructured carbon nanotubes is about 2 μm to about 8 μm and about 1 μm, respectively. 2 / g to about 5m 2 / gD50 The BET surface area range provides an improvement in the initial Coulombic efficiency and capacity retention of the anode. Specifically, the D 50 Particle size (in μm) and BET surface area (m 2 / g) is in the range of about 1.0 to about 3.5, and the ratio of the nanostructured carbon nanotubes to the nanostructured carbon nanotubes is from about 3.0 μm to about 6.0 μm and from about 1.0 μm to about 1.5 μm, respectively. 2 / g to about 3.5m 2 / gD 50 The particle size and BET surface area ranges provide, advantageously, the maximum improved capacity retention in a full cell configuration of a micro-silicon anode design. It will be appreciated that when D 50 When the particle size / BET surface area ratio is higher than 3.5 and lower than 1.0, the electrochemical performance is found to decrease gradually. 50 Particle size ranges from 0.1 μm to 2.0 μm and BET surface area > 5 m 2 / g makes D 50 When the particle size / BET surface area ratio is between 0.01 and 0.10, the ICE and capacity retention are found to drop sharply. Without wishing to be bound by theory, this phenomenon may be caused by the low surface reactivity of the micro-silicon active material particles with the electrolyte, thereby forming a thinner and less resistive SEI layer.

[0155] It is surprising to find that when various micro-Si anode grades are cycled in half-cell and full-cell designs, there is an inverse relationship in cycling stability, which is determined by their respective particle size, BET surface area, and d 50 The ratio between particle size and BET surface area is determined.

[0156] In the half-cell format tested under fully lithiated conditions, for d 50 >2.0μm, BET surface area <5m 2 / g and d 50 Rapid capacity degradation is evident for samples with particle size:BET surface area ratios above 0.01 to 0.1. The cycling stability observed from half-cell tests is reversed when the micro-Si materials are tested in a full-cell design with limited capacity. 50 Particle size (preferably 2.0-8.0 μm), low BET surface area (preferably 1.0-5.0 m 2 / g) and high d 50 Micro-silicon materials with a particle size:BET surface area ratio (preferably 0.1-6.0) produce stable cycling performance with higher ICE and capacity retention.

[0157] The expansion and contraction of silicon particles during charge-discharge cycles causes the silicon particles to pulverize, which increases the specific surface area of ​​the silicon particles. In the half-cell, Li is supplied unlimitedly by the Li metal counter electrode. + In the case of a large Si surface area, a low average particle size and thus reduced stress on the particles make it possible to have a low d 50 , high BET surface area and d 50 Micro-Si particles with a particle size:BET surface area ratio < 0.1 will take longer to reach full depletion of the Si electrode, resulting in relatively stable cycling performance.

[0158] In the full cell design with limited Li reservoir, the 50 <2.0μm, BET surface area>5m 2 / g and d 50 The larger surface area of ​​the micro-Si particles, which consist of a particle size:BET surface area ratio < 0.1, increases the reactivity during charge-discharge, resulting in Li + Consumption is accelerated, resulting in poor capacity retention and cycle life. 50 Particle size (preferably 2.0-8.0 μm), low BET surface area (preferably 1.0-5.0 m 2 / g) and high d 50 Li in micro-silicon materials with particle size: BET surface area ratio (preferably 0.1-6.0) + The low surface reactivity of ions and hence low irreversible consumption extend the capacity retention and cycle life. 50 The specific combination of MgO and BET surface area can lead to exceptionally good performance in full cells.

[0159] In some embodiments or examples, the tap density of the micro-silicon active material particles or the coated micro-silicon active material particles may be about 0.5 g / cm 3 To about 1.5g / cm 3 The tap density of the microsilicon active material particles or coated microsilicon active material particles may be at least about 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.2, 1.3, or 1.5 g / cm 3 In other embodiments or examples, the tap density of the microsilicon active material particles or coated microsilicon active material particles may be less than about 1.5, 1.4, 1.3, 1.2, 1.0, 0.95, 0.9, 0.85, 0.8, 0.75, 0.7, 0.65, 0.6, 0.55, or 0.5 g / cm3 Combinations of these density values ​​to form various ranges are also possible. For example, the tap density of the micro-silicon active material particles or coated micro-silicon active material particles may be between about 0.5 g / cm 3 To about 1.2g / cm 3 Density can be measured by any standard method, for example according to ASTM D7481-18.

[0160] Advantageously, the microsilicon active material particles of the present disclosure can be provided in high purity. In one embodiment or example, the purity of the microsilicon active material particles (excluding oxygen) may be in the range of about 95 to about 99.9 (by wt.%). The purity of the microsilicon active material particles (excluding oxygen) may be at least (by wt.%) about 95, 96, 97, 98, 99, 99.5 or 99.9. The purity of the microsilicon active material particles (excluding oxygen) may be less than (by wt.%) about 99.9, 99.5, 99, 98, 97, 96 or 95. The purity of the microsilicon active material particles (excluding oxygen) may be within the range provided by any lower limit and / or upper limit as previously described.

[0161] In one embodiment or example, the purity of the microsilicon active material particles (containing oxygen) may be in the range of about 79 to about 99.5 (by wt.%). The purity of the microsilicon active material particles (containing oxygen) may be at least (by wt.%) about 75, 80, 85, 90, 95, 96, 97, 98, 99 or 99.5. The purity of the microsilicon active material particles (containing oxygen) may be less than (by wt.%) about 99.5, 99, 98, 97, 96, 95, 90, 85, 80 or 75. The purity of the microsilicon active material particles (containing oxygen) may be within the range provided by any lower limit and / or upper limit as previously described.

[0162] The combination of novel and inventive features of the micro-silicon active material particles according to the present disclosure, their optional coating, and their use in the optionally coated anode composition for the anode in the lithium-ion battery pack unexpectedly leads to an improvement in the battery pack cycling behavior. Alternatively, the coated micro-silicon active material particles according to the present disclosure and their use in the optionally coated anode composition for the anode in the lithium-ion battery pack may also unexpectedly lead to an improvement in the battery cycling behavior. It is unexpectedly shown that the lithium-ion battery pack as described herein has a small irreversible capacity loss in the first charging cycle and has stable electrochemical behavior and minimal decay in subsequent cycles. Therefore, by using micro-silicon active material particles or coated micro-silicon active material particles as described herein, a lower initial capacity loss and a low continuous capacity loss of the lithium-ion battery pack can be achieved. Overall, the lithium-ion battery pack as described herein provides very good stability and cycle life. Therefore, a large number of cycles can be achieved with minimal fatigue, for example, fatigue caused by mechanical damage to the anode coating, anode material or SEI formation.

[0163] Pre-lithiation

[0164] The SEI layer is formed during lithium ion insertion, where the organic electrolyte is reduced on the surface of the anode when the anode potential is below about 1 V relative to Li+ / Li. The SEI layer is critical to preventing the electrolyte ions from being co-intercalated into the bulk electrode material by creating an electrically insulating but ionically conductive film. This prevents the electrolyte from continuing to decompose excessively. However, during the formation of the SEM layer film on the surface of the anode active material, some lithium ions may be irreversibly trapped in the electrode, resulting in lithium ion depletion.

[0165] The initial irreversible lithium loss of the anode can be compensated by adding lithium to the anode via pre-lithiation. Pre-lithiation methods can be roughly divided into electrochemical pre-lithiation and chemical pre-lithiation. Electrochemical pre-lithiation can be further divided into half-cell pre-lithiation or short-circuit pre-lithiation. Chemical pre-lithiation can be further divided into chemical synthesis, solution impregnation and mechanical processing. Additional pre-lithiation methods that can be used at the active material particles at the level of the anode coating are represented by chemical vapor deposition (CVD) type methods and physical vapor deposition methods (PVD). Preferred methods for pre-lithiating the anode coating include also pre-forming SEM layers and can be performed in a roll-to-roll process and are essentially cost-effective. It should be understood that the preferred pre-lithiation method for pre-lithiating the active material particles before incorporating the active material particles into the anode coating may be different from the method for pre-lithiating the anode composition. It should be understood that pre-lithiation at the particle level can be performed before the coating is applied to the particles. It should be noted that the present disclosure is not limited to a specific pre-lithiation method, and the most appropriate method will be selected to achieve the desired results.

[0166] Pre-lithiation can be applied to the anode electrode. For example, pre-lithiation can be applied to compensate for lithium lost in the first cycle, which constitutes one full charge and one full discharge of the electrochemical cell. If the amount of pre-lithiation is selected so that the SEI layer is formed before assembly into a full cell but no lithium is intercalated into the active material or alloyed with the active material, once incorporated into the full cell, the first cycle loss of the anode will be minimized, and any further loss of lithium is expected to be caused by other sources, such as the cathode electrode. As a result, the electrochemical cell now cycles at a higher cell capacity because more lithium is available in subsequent cycles to transfer back and forth between the anode and the cathode during repeated charge and discharge cycles.

[0167] In addition to compensating for any lithium loss that occurs during the first cycle and more generally the initial formation cycle, pre-lithiation can also provide a lithium reservoir in the anode before the anode is assembled into a battery assembly. The lithium reservoir can compensate for the lithium loss that continues over multiple cycles, thereby reducing capacity decay and extending the service life of the full battery. In other words, pre-lithiation can provide one or more advantages for silicon-containing anodes, especially anodes containing a high percentage of silicon. Providing a lithium reservoir to the anode using a method that also applies an SEI layer to the active material can also maximize the first cycle efficiency of the battery.

[0168] Optionally, the anode composition can provide a pre-lithiated anode composition. Pre-lithiation can occur at the anode active material level before incorporating the active material into the anode composition, or pre-lithiation can occur after preparing the anode composition. One or more advantages of the present disclosure are provided by a pre-lithiated anode composition that, once incorporated into a full cell arrangement, can provide a lithium reservoir in the anode, thereby compensating for the Li ions that persist during the charge / discharge cycle. + loss to extend its cycle life.

[0169] In some embodiments, the microsilicon active material particles or coated microsilicon active material particles may be pre-lithiated microsilicon active material particles or coated microsilicon active material particles, wherein pre-lithiation occurs before the active material is incorporated into the anode composition. It should be understood that the microsilicon active material particles may be pre-lithiated before forming the coated microsilicon active material particles. In other embodiments, the microsilicon active material particles or coated microsilicon active material particles may be pre-lithiated microsilicon active material particles or coated microsilicon active material particles, wherein pre-lithiation occurs after the active material has been incorporated into the anode composition. The degree of pre-lithiation can be selected so that the phase produced is between Li0Si1 (0% pre-lithiation) and Li 4.40 Si1 (100% pre-lithiation). Any phase composition in between may be desirable, including Li1Si1, Li 1.71 Si2、Li2Si1、Li 3.5 Si1 and Li 3.75Si1. In some embodiments or examples, the pre-lithiation amount of the microsilicon active material particles and / or the anode composition may be between about 1% and about 30%. The pre-lithiation amount of the microsilicon active material particles or the coated microsilicon active material particles and / or the anode composition may be less than about 30%, 25%, 20%, 15%, 10%, 5% or 1%. The pre-lithiation amount of the microsilicon active material particles or the coated microsilicon active material particles and / or the anode composition may be at least about 1%, 5%, 10%, 15%, 20%, 25% or 30%. The pre-lithiation amount of the microsilicon active material particles or the coated microsilicon active material particles and / or the anode composition may be within the range provided by any two of these upper and / or lower limits.

[0170] Pre-lithiation of the micro-silicon active material particles or coated micro-silicon active material particles can be carried out via physical vapor deposition (PVD) or chemical vapor deposition (CVD) or mechanical alloying process or chemical process or electrochemical process. It should be understood that a series of suitable methods can be applied to produce a silicon-lithium alloy phase before incorporating the pre-lithiated micro-silicon active material particles into the anode composition.

[0171] Additional active materials

[0172] The anode composition as described herein may further comprise one or more additional active materials. In some embodiments, the additional active material may be graphite or silicon. For example, flake graphite, natural graphite, artificial graphite, silicon oxide (SiOx) where x = 0.8 to 2, silicon-carbon composite materials, silicon alloys, or any combination thereof.

[0173] Adhesives

[0174] The anode composition as disclosed herein may further include one or more binders. The binder may be a polymer. In some embodiments, the polymer may be selected from the group consisting of: gum arabic; carboxymethyl cellulose (CMC) / citric acid; CMC / styrene-butadiene rubber (SBR); polytetrafluoroethylene (PTFE); polyvinylidene fluoride (PVDF); poly (1-trimethylsilyl-1-propyne) (PTMSP); gum binders such as gum arabic, xanthan gum and guar gum; natural cellulose-based binders; polysaccharides such as sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium alginate; polyacrylates; aliphatic polymers such as polyvinyl butyral; aromatic polymers such as styrene-butadiene rubber. For example, the polymer can be selected from the group consisting of polyvinyl pyrrolidone, carboxymethyl cellulose, polyacrylic acid (PAA), poly(methacrylic acid), maleic anhydride copolymers including poly(ethylene and maleic anhydride) copolymers, polyvinyl alcohol, carboxymethyl chitosan, natural polysaccharides, xanthan gum, alginate, polyimide and PAA copolymers including one or more of the following: polyvinyl alcohol (PVA), polyurethane (PU), polyimide (PI) or polyacrylonitrile (PAN). In one example, the binder is PAA. The binder can be dissolved in H2O or ethanol or a mixture of H2O and ethanol or N,N' dimethylformamide or any other solvent suitable for the intended purpose. Some binders can exist in the form of water-based emulsions.

[0175] In some embodiments or examples, the ratio of the binder to the micro-silicon active material particles or the coated micro-silicon active material particles may be about 1:40, 1:35, 1:32, 1:30, 1:25, 1:23, 1:20, 1:15, 1:10, 1:9, 1:6 or 1:4. The ratio of the binder to the micro-silicon active material particles or the coated micro-silicon active material particles may be in the range of about 1:4 to about 1:32. The ratio of the binder to the micro-silicon active material particles or the coated micro-silicon active material particles may be in the range of about 1:8 to about 1:23. The ratio of the binder to the micro-silicon active material particles or the coated micro-silicon active material particles may be in the range of about 1:9 to about 1:15.

[0176] In some embodiments or examples, the binder (in wt.%) may be present in the anode composition in a range of about 2.5 to 15. The binder (in wt.%) may be present in the anode composition in an amount less than about 15, 12, 10, 8, 5, or 2.5. The binder (in wt.%) may be present in the anode composition in an amount of at least about 2.5%, 5%, 8%, 10%, 12%, or 15%. The amount of binder (in wt.%) present in the anode composition may be within the range provided by any two of these upper and / or lower limits. For example, the binder (in wt.%) may be present in the anode composition in a range of about 3 to about 8 or about 4 to about 8.

[0177] It has been found that the pH of the binder may affect the electrochemical performance of the anode composition. In some embodiments or examples, the pH of the binder may be less than 9, 8, 7, 6, 5, 4, 3 or 2. In some embodiments or examples, the pH of the binder may be at least 2, 3, 4, 5, 6, 7, 8 or 9. The pH of the binder may be within the range provided by any two of these upper and / or lower limits. For example, the pH of the binder may be in the range of 4 to 8.

[0178] Conductive Materials

[0179] Anode compositions as described herein may further include one or more conductive materials. In some embodiments or examples, the conductive material may be a carbon-based material. In one embodiment or example, the carbon-based material may be nanoscale or micron-sized carbon particles or flakes, or a combination thereof. In one embodiment or example, the carbon-based material may be selected from the group consisting of: activated carbon, carbon nanoparticles, graphite, single-walled (SWCNT) or multi-walled (MWCNT) carbon nanotubes, branched carbon nanotubes, carbon nanofibers, graphene, graphene oxide, MXene, nano- or micron-sized hard carbon, nano- or micron-sized porous carbon, and conductive polymers. The carbon-based material may be selected from the group consisting of: graphene, graphene oxide, graphite, single-walled (SWCNT) or multi-walled (MWCNT) carbon nanotubes, branched carbon nanotubes, carbon nanofibers, MXene, nano- or micron-sized hard carbon, nano- or micron-sized porous carbon, and conductive polymers.

[0180] In some embodiments or examples, the ratio of the conductive material to the micro-silicon active material particles or the coated micro-silicon active material particles may be about 1:50, 1:48, 1:45, 1:40, 1:35, 1:30, 1:25, 1:20, 1:18, 1:15, 1:10, 1:8, 1:6, 1:4, 1:3, 1:2 or 1:1.3. The ratio of the conductive material to the micro-silicon active material particles or the coated micro-silicon active material particles may be in the range of about 1:2 to about 1:30. The ratio of the conductive material to the micro-silicon active material particles or the coated micro-silicon active material particles may be in the range of about 1:2 to about 1:18. The ratio of the conductive material to the micro-silicon active material particles may be in the range of about 1:2 to about 1:15.

[0181] In some embodiments or examples, the conductive material may be present in the anode composition in the range of about 2.5 to 40 wt.% (based on the total weight of the anode composition). The conductive material may be present in the anode composition in an amount of less than about 40 wt.%, 30 wt.%, 20 wt.%, 15 wt.%, 10 wt.%, 7 wt.%, 5 wt.% or 2.5 wt.% (based on the total weight of the anode composition). The conductive material may be present in the anode composition in an amount of at least about 2.5 wt.%, 5 wt.%, 7 wt.%, 10 wt.%, 15 wt.%, 20 wt.%, 30 wt.% or 40 wt.% (based on the total weight of the anode composition). The conductive material may be present in the anode composition in an amount provided by any two of these upper and / or lower limits. For example, the conductive material may be present in the anode composition in an amount of about 7 wt.% to about 25 wt.%.

[0182] Electrochemical Cells

[0183] The present disclosure is directed to providing improvements in anodes for electrochemical cells. In some embodiments or examples, the present disclosure is directed to an anode for an electrochemical cell, the anode comprising an anode composition according to at least some embodiments or examples as described herein.

[0184] In some embodiments or examples, the electrochemical cell may comprise: a negative electrode, a positive electrode, at least one electrolyte, and a separator, wherein the anode comprises an anode composition as defined herein. For example, the electrochemical cell may comprise or consist of: an anode; a cathode; at least one electrolyte, the at least one electrolyte comprising one or more electrolyte solvents; and a separator, wherein the anode comprises an anode composition as defined herein, and wherein the lithium uptake capacity of the anode is greater than the lithium release capacity of the anode.

[0185] One or more advantages of the present disclosure are provided by the arrangement of the anode and cathode in an electrochemical cell, which has been found to be very important in increasing the stability and cycle life of the anode compositions described herein.

[0186] In some embodiments, capacity limitation can be considered based on mass loading or area capacity. Mass loading or area capacity refers to an electrochemical cell assembly in which the capacity of the anode may be significantly too large relative to the cathode. Capacity limitation may limit the capacity of an overly large electrode (anode) by allowing only partial lithiation to occur, because the amount of lithium contained in the electrochemical cell is limited by the lithium contained in the cathode when the cell is assembled. For example, in an electrochemical cell assembly in which the anode has an area capacity of x and the cathode has an area capacity of y, the estimated capacity limitation percentage generated is calculated by y / x*100. It should be understood that this capacity limitation method may be particularly useful in the case where the anode contains a high percentage of elemental silicon as an active material, which provides a specific capacity of more than 3500mAh / g.

[0187] It should be understood that the specific area capacity (in mAh / cm 2 The specific loading weight (in mg / cm2) provided by the amount of anode composition applied to the current collector corresponds to 2 Specific load weight (in mg / cm 2 The specific area capacity (in mAh / cm2) is based on the total weight of the anode composition, which includes micro-silicon active material particles, one or more optional additional active materials, one or more optional binders, and one or more optional conductive materials. 2 The silicon content in the anode composition is in units of silicon (in units) depending on the thickness of the anode composition coating on the current collector, the silicon content in the anode composition and the utilization of silicon.

[0188] In some embodiments, the specific areal capacity (in mAh / cm2) corresponding to complete utilization of the active material contained in the anode composition of the anode is 2 The unit is between 2.5 mAh / cm 2 Up to 20mAh / cm 2 between.

[0189] In some embodiments, the specific loading weight (in mg / cm 2 Units) can be between 0.95mg / cm 2 Up to 7.5 mg / cm 2 between.

[0190] In some embodiments, the anode and cathode are arranged in such a manner that the anode can deliver about 0.5 mAh / cm 2 to about 6 mAh / cm 2, and the anode can deliver about 1500mAh / g, 1200mAh / g, 1000mAh / g, 800mAh / g, 600mAh / g, 500mAh / g or 400mAh / g. In another embodiment, the anode and the cathode are arranged in such a way that the anode can deliver about 0.5mAh / cm 2 to about 6 mAh / cm 2 , and the anode may be used for about 80%, 75%, 70%, 65%, 60%, 55%, 50%, 45%, 40%, 35%, 30%, 25% or 20%.

[0191] In other embodiments, the capacity limitation can be considered based on the phase composition of the LiSi alloy. 3.75 Si1 or Li 4.4 Si1 corresponds to a maximum achievable capacity of 3590 mAh / g or a maximum theoretical lithiation state of 4200 mAh / g. It should be understood that if the utilization of the anode is limited, this can be translated into a specific phase composition of the LiSi alloy. The specific phase composition can also be translated into specific capacity (mAh / g). For example, Li 1.71 Si1 can correspond to a specific capacity of up to 1636 mAh / g, Li 2.33 Si1 can correspond to a specific capacity of up to 2227 mAh / g, Li 3.25 Si1 can correspond to a specific capacity of up to 3101 mAh / g, Li 3.75 Si1 can correspond to a specific capacity of up to 3579 mAh / g, and Li 4.4 Si1 can correspond to a specific capacity of up to 4199 mAh / g.

[0192] In another embodiment, the capacity limitation may be considered based on the voltage of the anode during charge and / or discharge. It should be understood that the amount of silicon lithiation after discharge may be configured by the discharge voltage of the anode.

[0193] For example, it will be appreciated that the N / P ratio balance between the anode and cathode may be between about 1.05 and about 7, and / or that the voltage range may be controlled relative to the discharge level of the electrochemical cell. In some embodiments or examples, the capacity of the lithium uptake capacity of the anode may not be fully utilized during charging of a lithium-ion battery. In some embodiments or examples, the specific area capacity of the anode may be greater than the specific area capacity of the cathode. In other words, the anode is only partially lithiated in a fully charged state. Fully charged refers to the state of an electrochemical cell (e.g., a Li-ion battery) in which the anode, specifically the micro-silicon active material, has its highest degree of lithiation according to the invention described herein. Partial lithiation of the anode means that the maximum lithium uptake capacity of the anode active material in the anode is not fully utilized. In some embodiments, the amount of lithium stored in the cathode (mAh / cm 2) can be compared to the lithium storage capacity of the anode (mAh / cm 2 ) is at least 0.05 to 7.0 times smaller.

[0194] In some embodiments, the Li / Si ratio of an electrochemical cell (e.g., a Li-ion battery) may be set by the anode to cathode ratio (N / P). In some embodiments, the N / P ratio between the anode and cathode may be between about 1.05 and about 7, about 2 and about 5, or about 3 and about 4. The N / P ratio may be greater than about 7, 6, 5, 4, 3, 2, or 1.05. The N / P ratio may be at least about 1.05, 2, 3, 4, 5, 6, or 7. The N / P ratio may be within a range provided by any two of these upper and / or lower limits. For example, the N / P ratio between the anode and cathode may be between about 1.5 and about 4 or between about 1.8 and about 3.5.

[0195] In some embodiments, the capacity limit (in %) may be at least about 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 0, 85, 90, 95, or 99. In some embodiments, the capacity limit (in %) may be less than about 99, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, or 20. The capacity limit (in %) may be within the range provided by any two of these upper and / or lower values. For example, the capacity limit (in %) may be between about 25 and about 90, or between about 30 and about 80.

[0196] The present disclosure advantageously provides an electrochemical cell designed so that the lithium uptake capacity of the anode is greater than the lithium release capacity of the cathode. This results in the lithium uptake capacity of the anode being not fully utilized, that is, in a fully charged state, the silicon active material particles of the anode are only partially lithiated, and advantageously reduces or prevents the high volume changes commonly found in silicon anodes during lithiation / delithiation cycles, which degrades its structure and shortens the life of the battery pack. In other words, a high N / P ratio may limit the degree of lithiation of micro-silicon because the amount of Li ions is fixed by the cathode when the battery is assembled. For example, the anode may be significantly too large relative to the amount of lithium contained in the battery and provided by the cathode. Since the degree of lithiation is limited by an overly large anode, the expansion level of the micro-silicon active material particles or the coated micro-silicon active material particles and their degradation are also limited. In some embodiments or examples, the degree of silicon lithiation may be in the range of about 20% to about 80%. Unexpectedly, the degree of silicon lithium within this range may have a stabilizing effect on the performance of the electrochemical cell.

[0197] In another embodiment, the capacity of the electrochemical cell may be limited by limiting the lower cutoff voltage. In some embodiments or examples, the lower cutoff voltage may be between about 2.5V and about 3.0V. For example, the lower cutoff voltage may be between 2.8V and about 3.0V. It should be understood that the voltage limit may be imposed by limiting the lower cutoff voltage. This can prevent the micro-silicon active material particles or coated micro-silicon active material particles from completely de-lithiating at each cycle and reduce their expansion, thereby reducing degradation and thus extending the cycle life.

[0198] In another embodiment, the capacity of the electrochemical cell can be limited by limiting the upper cutoff voltage. In some embodiments or examples, the upper cutoff voltage can be between about 3.6V and about 4.25V.

[0199] It will be appreciated that both capacity and voltage limitations may be used simultaneously.

[0200] It should be understood that the anode composition may be pre-lithiated as described in any one or more of the embodiments or examples described herein. In some embodiments, pre-lithiation may occur before the active material is incorporated into the anode composition. In other embodiments, pre-lithiation may occur after the active material has been incorporated into the anode composition. In some embodiments or examples, the pre-lithiation amount of the anode composition may be between about 1% and about 30%. The pre-lithiation amount of the anode composition may be less than about 30%, 25%, 20%, 15%, 10%, 5%, or 1%. The pre-lithiation amount of the anode composition may be at least about 1%, 5%, 10%, 15%, 20%, 25%, or 30%. The pre-lithiation amount of the anode composition may be within the range provided by any two of these upper and / or lower limits.

[0201] In some embodiments, the amount of lithium contained in the anode may be about 30% of its maximum storage capacity, while the amount of lithium contained in the cathode may be 100% of its maximum storage capacity. In some embodiments, the amount of lithium contained in the anode may be about 20% of its maximum storage capacity, while the amount of lithium contained in the cathode may be 100% of its maximum storage capacity. In some embodiments, the amount of lithium contained in the anode may be about 10% of its maximum storage capacity, while the amount of lithium contained in the cathode may be 100% of its maximum storage capacity.

[0202] In one embodiment, for electrochemical pre-lithiation, a half-cell approach may be used. The silicon-containing electrode is assembled in a half-cell setup using a lithium foil reference electrode, and the degree of pre-lithiation is controlled by setting appropriate parameters in a constant current charge / discharge cycle program. In order to produce an SEI layer and a lithium reservoir of up to 0% lithium in the anode, the half-cell will undergo a first cycle by partially or fully lithiating the silicon-containing electrode, followed by complete delithiation.

[0203] When a lithium reservoir is produced in the anode, a lithium reservoir that is partially lithiated to the desired degree is required. According to the composition of the silicon-containing anode and the relevant material properties, the first cycle loss can be estimated when the corresponding composition is tested for the lithium metal foil reference electrode in the half-cell and the anode composition first cycle loss is determined in this way. If the first cycle loss is estimated to be x%, then in order to produce a y% lithium reservoir, the initial lithiation step during the pre-lithiation process required to achieve the lithiation level of the z% silicon anode composition needs to consider x% + y%. If in a specific embodiment, the anode composition shows a 10% first cycle loss, this loss needs to be considered when calculating the desired pre-lithiation degree to obtain the resulting lithium reservoir. For example, in order to achieve a 10% lithium reservoir, the anode can be lithiated up to 20% of its expected design capacity (mAh / g), of which the initial approximately 10% is intended to compensate for the irreversible lithium loss during the first cycle, and the additional lithium reservoir is stored in the anode or silicon material to form the desired lithium reservoir. It should be understood that higher levels of pre-lithiation can be applied to achieve other desired levels of lithium reservoirs. The maximum desired level of lithium storage may be 30%.

[0204] It is believed that pairing pre-lithiation and capacity limitation can provide one or more additional advantages to the electrochemical cells of the present disclosure. For example, despite any lithium loss during the first cycle, the anode capacity occupied by lithium supplied by the cathode and stored in the anode during the first lithiation will be the same with and without pre-lithiation, but the lithium reservoir in the anode can compensate for the gradual loss of lithium during repeated charge and discharge cycles over multiple cycles.

[0205] In some embodiments, the anode composition can be applied to a current collector material as a coating or film. The current collector material for the anode can be selected from the group consisting of copper, aluminum, stainless steel, titanium, carbon, perforated metal foil, metal foam, and porous and non-porous films based on metal-coated polymers. For example, the anode composition can be applied to a copper current collector material (e.g., copper foil).

[0206] In some embodiments, the thickness of the current collector material for the anode may be between about 4 μm and about 25 μm. The thickness of the current collector (in μm) may be less than about 25, 20, 15, 10, 8, 6 or 4. The thickness of the current collector (in μm) may be at least about 4, 5, 6, 7, 8, 9, 10, 12, 14, 16, 18, 20 or 25. The thickness of the current collector (in μm) may be within the range provided by any two of these upper and / or lower limits. In one example, the current collector material for the anode may be a copper foil having a thickness between about 6 μm and about 12 μm.

[0207] In some embodiments or examples, the thickness of the anode composition may be substantially uniform and in the range of about 5 μm to about 70 μm. The thickness (μm) of the anode composition may be less than about 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10 or 5. The thickness (μm) of the anode composition may be at least about 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 or 65. The thickness of the anode composition may be within the range provided by any two of these upper and / or lower limits.

[0208] It should be understood that the cathode active material is also applied to the current collector material. The current collector material for the anode can be selected from the group comprising: copper, aluminum, stainless steel, titanium, carbon, perforated metal foil, metal foam, and porous and non-porous films based on metal-coated polymers. For example, the cathode composition can be applied to an aluminum current collector material (e.g., aluminum foil).

[0209] In some embodiments, the thickness of the current collector material for the cathode may be between about 10 μm and about 30 μm. The thickness of the current collector (in μm) may be less than about 30, 25, 20, 15 or 10. The thickness of the current collector (in μm) may be at least about 10, 12, 14, 16, 18, 20, 25 or 30. The thickness of the current collector (in μm) may be within the range provided by any two of these upper and / or lower limits. In one example, the current collector material for the cathode may be an aluminum foil with a thickness between about 10 μm and about 30 μm.

[0210] In some embodiments, the cathode may be selected from the group consisting of lithium nickel cobalt manganese oxide (NCM), lithium iron phosphate (LFP), lithium nickel manganese spinel (LNMO), lithium nickel cobalt aluminum oxide (NCA), lithium manganese oxide (LMO), lithium cobalt oxide (LCO), and sulfur or a sulfur composite material including a mixture of sulfur and carbon.

[0211] In some embodiments or examples, the electrolyte may be selected from a non-aqueous solution of one or more lithium salts (e.g., in a Li-ion battery). One or more lithium salts may be selected from the group consisting of: lithium bis(trifluoromethanesulfone)imide, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium bis(trifluorosulfonylimide), lithium trifluoromethanesulfonate, lithium fluoroalkylsulfonylimide, lithium fluoroarylsulfonylimide, lithium bis(oxalatoborate), tris(trifluoromethylsulfonylimide)methyl lithium, lithium difluoromethanesulfonate, lithium trifluoromethanesulfonate salt (lithium trifluoromethanesulfonate), lithium bis(oxalate)borate, lithium tetrafluoroborate, lithium perchlorate, lithium tetrachloroaluminate, lithium hexafluoroarsenate, lithium hexafluoroantimonate, 4,5-dicyano-2-(trifluoromethyl)imidazolidine (LiTDI), LiPF3(C2F5)3(LiFAP), LiBF3(C2F5), lithium chloride, and combinations thereof. For example, the electrolyte may include lithium hexafluorophosphate.

[0212] In some embodiments or examples, the lithium salt is soluble in an organic solvent. The lithium salt is soluble in an organic solvent selected from ethers, esters, carbonates and acetals. In one example, the solvent can be selected from dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene carbonate, propylene carbonate, dimethyl carbonate, tetrahydrofuran and dioxolane. In some embodiments or examples, the lithium salt can be dissolved in an organic solvent selected from the group consisting of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, dipropyl carbonate, cyclopentanone, sulfolane, dimethyl sulfoxide, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, 1,2-diethoxymethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 1,2-dimethoxyethane, methyl acetate, ethyl acetate, nitromethane, 1,3-propane sultone, γ-valerolactone, methyl isobutyryl acetate, 2-methoxyethyl acetate, 2-ethoxyethyl acetate, diethyl oxalate, ionic liquids, and any combination thereof. In some embodiments or examples, the lithium salt may be dissolved in an organic solvent selected from the group consisting of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and any combination thereof.

[0213] The electrolyte may include an additive of one or more alkali metal salts selected from the group consisting of LiPF6 LiBF4, LiAsF6, LiSbF6, LiClO4, LiAlCl4, LiGaCl4, LiC(SO2CF3)3, LiN(SO2CF3)2, LiSCN, LiSO2CF2CF3, LiC6F5SO3, LiO2CCF3, LiSO3F, LiB(C6H5)4, LiCF3SO3, LiNO3, and mixtures thereof. In other embodiments, the additive may be selected from one or more of the following: fluoroethylene carbonate (FEC), vinylethylene carbonate (VEC), ethylene carbonate (VC), propylene carbonate (PC), ethyl methyl carbonate (EMC), propane sultone (PS), and mixtures thereof. Electrolyte additives may further improve certain features of the battery. For example, an electrolyte (e.g., lithium hexafluorophosphate) may include an additive (e.g., fluoroethylene carbonate) dissolved in an organic solvent (e.g., diethyl carbonate).

[0214] In some embodiments or examples, the lithium salt may be dissolved in one or more organic solvents as described above, wherein the one or more organic solvents are present in a volume to volume ratio ranging from 10: 1 to 1: 10. For example, a lithium salt (e.g., 1M LiPF6) may be dissolved in FEC / DEC (2:8) v%, FEC:EMC (3:7) w / w+2wt.%VC, EC / EMC / DEC (3 / 5 / 2vol%)+1wt.%VC+10wt.%FEC, or EC / EMC (3:7) wt.%+1wt.%VC.

[0215] In some embodiments or examples, the separator is used to separate the anode from the cathode and allows the lithium ions in the electrolyte to pass freely. The separator can be selected from a series of different porous polymer films. It should be understood that any porous polymer film with suitable porosity, tortuosity and thickness can be selected as a separator. For example, a separator material based on a polymer film can be selected. In one embodiment or example, the separator can be selected from polyethylene (PE), polypropylene (PP) or polyethylene terephthalate (PET). In another embodiment, a nonwoven fiber material is selected as a separator, and the nonwoven fiber material comprises a fiber selected from nylon, polyethylene terephthalate (PET), cellulose, aramid or polyacrylonitrile.

[0216] In some embodiments or examples, the electrochemical cell may be an energy storage device. The energy storage device may be a battery. For example, the battery may be a secondary battery. In a specific example, the battery may be a lithium-ion battery (Li-ion battery).

[0217] Anode compositions for lithium-ion batteries

[0218] In some embodiments or examples, the present disclosure also provides a method for improving the cycle stability of a battery pack, the battery pack having an anode and a cathode, at least one electrolyte and an optional separator, wherein the anode comprises an anode composition as described herein. It has been found that an anode comprising an anode composition provides a particularly effective anode for a battery pack (e.g., a Li-ion battery pack) capable of maintaining a long-term capacity retention rate. In some embodiments or examples, the discharge capacity of the anode inside the battery pack may be at least about 800 mAh / g within at least 100 cycles of the battery pack. In some embodiments or examples, the specific capacity (mAh / g) may be at least about 500, 600, 800, 1000, 1200, 1400, 1600, 1800, 2000, 2200, 2400, 2600, 2800, 3000 or 3500. In some embodiments or examples, the specific capacity (mAh / g) may be less than about 3500, 3400, 3200, 3000, 2800, 2600, 2400, 2200, 2000, 1800, 1600, 1400, 1200, 1000, 800, 600 or 500. The specific capacity (mAh / g) may be within the range provided by any two of these upper and / or lower limits. In some embodiments or examples, the number of cycles may be at least 80, 100, 120, 140, 160, 180, 200, 220, 240, 260, 280, 300, 320, 340, 360, 380, 400, 420, 440, 460, 480, 500, 1000 or 1500.

[0219] The long-term cycling performance of an electrochemical cell (e.g., a Li-ion battery) comprising the anode composition can be tested for high silicon content anodes (i.e., about 70% silicon content) with different capacity limits. According to at least some embodiments or examples as described herein, the initial discharge capacity of the anode comprising the anode composition can be at least about (in mAh / g) 600, 800, 1100, 1200, 1300, 1400, 1500, or 1600. At least according to some embodiments or examples, after 100, 200, 300, 400, 500, 800, 1000, or 1500 cycles, 80% of the discharge capacity can be retained.

[0220] It should be understood that constant current charge-discharge cycle experiments can generally be used to evaluate the performance indicators of battery packs: capacity during cycling, rate capacity, coulombic efficiency and capacity retention.

[0221] In some embodiments or examples, the present disclosure also relates to the use of an anode comprising an anode composition as described herein in an electrochemical cell. For example, the electrochemical cell can be an energy storage device, such as a battery, preferably a secondary battery. More specifically, the battery can be a lithium ion battery.

[0222] In some embodiments or examples, the present disclosure also relates to an anode comprising the anode composition, wherein the anode can be a battery anode, more specifically, a lithium-ion battery anode.

[0223] It has been found that the optionally coated anode composition, which may include or consist of optionally coated micro-silicon active material particles, optionally one or more binders, optionally one or more conductive materials, and optionally one or more additives, significantly reduces the effects shown by SEI formation and silicon expansion and degradation, and thus provides improved Li-ion battery performance. The anode composition provides high first cycle efficiency, as well as the additional advantage of providing controlled silicon utilization, which in turn improves the high current response and performance of the battery. For example, an electrochemical cell (e.g., a Li-ion cell) containing an anode composition as described herein allows partial utilization / lithiation of silicon, and the specific capacity of the anode is reduced and controlled by the amount of lithium that the anode can supply, thereby providing an improved average coulombic efficiency (CE) of at least about 75%, 80%, 85%, 90%, 95%, 98%, 99%, 99.5%, 99.8%, 99.9% or more or less than 100% over at least 200 cycles. In another example, using the anode composition as an anode provides improved performance of a lithium ion battery, the improved performance exhibiting cycling stability after at least 200 cycles at C / 2.

[0224] Furthermore, it has been unexpectedly discovered that if the N / P ratio of an anode containing mainly micro-silicon (e.g., >70%) is controlled to a value above 3 (e.g., 3.3), stable cycling of the anode can be provided to achieve more than 200 cycles at a capacity retention of greater than 80%. In other words, a high N / P ratio limits the degree of lithiation of micro-silicon because Li + The amount of silicon is fixed by the cathode when the cell is assembled. This results in a degree of silicon lithiation of about 20% to about 80%, rather than 80% to 90% as seen in conventional cell assemblies where the anode comprises primarily graphite, which has a stabilizing effect on cell performance. It will be appreciated that the anode is significantly oversized relative to the amount of lithium contained in the cell and provided by the cathode. Advantageously, because the degree of lithiation is limited by an oversized anode, the level of expansion of the silicon and its degradation is also limited.

[0225] Preparation method

[0226] In some embodiments or examples, the present disclosure relates to a method for preparing an anode of an electrochemical cell. The method will include at least one of the following: incorporating coated microsilicon active material particles into the anode; or coating the anode itself during or after the anode is formed. The method can be used to prepare an anode according to any embodiment or example as described herein. It should be understood that the anode prepared by the method may include an anode composition, the anode composition comprising microsilicon active material particles or coated microsilicon active material particles. It should be understood that the anode prepared by the method may include an anode composition or consist of an anode composition, the anode composition comprising microsilicon active material particles, optionally one or more additional active materials, optionally one or more binders, optionally one or more conductive materials, optionally one or more additives, and optionally solvents. It should also be understood that the anode prepared by the method may include an anode composition or consist of an anode composition, the anode composition comprising coated microsilicon active material particles, optionally one or more additional active materials, optionally one or more binders, optionally one or more conductive materials, optionally one or more additives, and optionally solvents. The microsilicon active material particles, coated microsilicon active material particles, one or more additional active materials, one or more optional binders, one or more optional conductive materials, one or more optional additives and one or more optional solvents may be selected from any one or more of the embodiments or examples described herein.

[0227] In some embodiments or examples, a method for preparing coated micro-silicon active material particles is provided, the method comprising: (i) providing a plurality of micro-silicon active material particles, wherein the micro-silicon active material particles have one or more of the following: (i) a measured BET surface area of ​​between about 0.1 m 2 / g and about 10m 2 / g; (ii) D 50 The particle size is between about 0.1 μm and about 10 μm; and (iii) D 50 :BET surface area ratio is between about 0.1 and about 10; and (ii) applying a coating to the surface of the microsilicon active material particles.

[0228] In some embodiments or examples, a method for preparing coated micro-silicon active material particles is provided, the method comprising: (i) providing a plurality of micro-silicon active material particles, wherein the micro-silicon active material particles have a BET surface area (i) measured between about 0.1 m 2 / g and about 10m 2 / g; and (ii) D 50 The particle size is between about 0.1 μm and about 10 μm; or (iii) D 50:BET surface area ratio is between about 0.1 and about 10; and (ii) applying a coating to the surface of the microsilicon active material particles.

[0229] In some embodiments or examples, a method for preparing an anode of an electrochemical cell is provided, the method comprising the following steps: (i) preparing an anode slurry, the anode slurry comprising microsilicon active material particles or coated microsilicon active material particles, optionally one or more additional active materials, optionally one or more binders, optionally one or more conductive materials, optionally one or more additives and a solvent system; (ii) casting a layer of the anode slurry onto a current collector material to provide an anode composition layer on the current collector material; and (iii) optionally coating an anode composition, wherein the microsilicon active material particles have one or more of the following: (a) a measured BET surface area of ​​between about 0.1 m 2 / g and about 10m 2 / g, (b)D 50 The particle size is between about 0.1 μm and about 10 μm, and (c) D 50 The ratio of the BET surface area is between about 0.1 and about 10.

[0230] In some embodiments or examples, a method for preparing an anode of an electrochemical cell is provided, the method comprising the following steps: (i) preparing an anode slurry, the anode slurry comprising microsilicon active material particles or coated microsilicon active material particles, optionally one or more additional active materials, optionally one or more binders, optionally one or more conductive materials, optionally one or more additives and a solvent system; (ii) casting a layer of the anode slurry onto a current collector material to provide an anode composition layer on the current collector material; and (iii) optionally coating the anode composition, wherein the microsilicon active material particles have a BET surface area measured by (a) between about 0.1 m 2 / g and about 10m 2 / g, and (b) D 50 The particle size is between about 0.1 μm and about 10 μm, or (c) D 50 The ratio of the BET surface area is between about 0.1 and about 10.

[0231] In some embodiments or examples, the method may further comprise step (iii) curing the wet anode layer by solvent evaporation to provide a dry anode composition layer on the current collector material.

[0232] In some embodiments or examples, the coating layer may be selected from the group consisting of carbon, graphene, graphite, metal oxides, polymers, and combinations thereof to form coated micro silicon active material particles or coated anode compositions.

[0233] In some embodiments or examples, the coating may be a coating of micro-silicon active material particles. In other embodiments or examples, the coating may be a coating of the anode composition. In other words, the coating may be present on at least a portion of the surface of the anode composition.

[0234] In some embodiments, the coating layer may be selected from the group consisting of carbon, graphene, graphite, metal oxides, polymers, and combinations thereof to form coated micro silicon active material particles or coated anode compositions.

[0235] The coating may be from materials and prepared by methods as described in any of the foregoing embodiments relating to coatings of the disclosure and / or silicon particles of the disclosure having such applied coatings.

[0236] In some embodiments or examples, the solvent may be an organic solvent selected from the following: aromatic compounds, halogenated aromatic compounds, halogenated aliphatic hydrocarbons, aliphatic hydrocarbons, glycols, ethers, glycol ethers, esters, alcohols, ketones, or combinations thereof. In some embodiments or examples, the solvent may be present in an amount between about 40wt.% and 90wt.%, between about 40wt.% and 70wt.%, or between about 40wt.% and 60wt.% (by weight % of the total anode composition). The solvent may be a low boiling point organic solvent, or a mixture of one or more of such solvents. In some embodiments or examples, the solvent may be selected from the group comprising: water, methanol, ethanol, n-propanol, isopropanol, tetrahydrofuran, dichloromethane, chloroform, diethyl ether, room temperature ionic liquids, ethylene glycol, glycerol, formamide, N-methylformamide, dimethylformamide, N-methylsterone, an aqueous solution thereof, and any mixture thereof. For example, the solvent may be water, ethanol, N,N'dimethylformamide, or a combination thereof.

[0237] In some embodiments or examples, the ratio of the binder to the micro-silicon active material particles may be about 1:40, 1:35, 1:32, 1:30, 1:25, 1:23, 1:20, 1:15, 1:10, 1:9, 1:6 or 1:4. The ratio of the binder to the micro-silicon active material particles or the coated micro-silicon active material particles may be in the range of about 1:4 to about 1:32. The ratio of the binder to the micro-silicon active material particles or the coated micro-silicon active material particles may be in the range of about 1:8 to about 1:23. The ratio of the binder to the micro-silicon active material particles or the coated micro-silicon active material particles may be in the range of about 1:9 to about 1:15.

[0238] In some embodiments or examples, the binder (in wt.%) may be present in the anode composition in a range of about 2.5 to 15. The binder (in wt.%) may be present in the anode composition in an amount less than about 15, 12, 10, 8, 5, or 2.5. The binder (in wt.%) may be present in the anode composition in an amount of at least about 2.5%, 5%, 8%, 10%, 12%, or 15%. The amount of binder (in wt.%) present in the anode composition may be within the range provided by any two of these upper and / or lower limits. For example, the binder (in wt.%) may be present in the anode composition in a range of about 3 to about 8 or about 4 to about 8.

[0239] In some embodiments or examples, the viscosity of the anode slurry may be in the range of about 10 mPas to 100,000 mPas. At a given shear rate, the viscosity (mPas) may be less than about 100,000, 90,000, 80,000, 70,000, 60,000, 50,000, 40,000, 30,000, 20,000, 10,000, 8000, 6000, 4000, 2000, 1000, 800, 600, 400, 200, 100, 50 or 10. At a given shear rate, the viscosity may be at least about 10, 20, 40, 60, 80, 100, 300, 500, 700, 900, 1000, 3000, 5000, 7000, 9000, 10,000, 20,000, 30,000, 40,000, 50,000, 60,000, 70,000, 80,000, 90,000 or 100,000. The viscosity (mPas) of the anode slurry may be in the range provided by any two of these upper and / or lower limits. For example, at a given shear rate, the viscosity (mPas) of the anode slurry may be in the range of about 2500mPas to about 8000mPas. All viscosity values ​​described herein may be at a given shear rate. In an embodiment, the shear rate may be the shear rate used in any recognized standard test method in the art.

[0240] In some embodiments or examples, the thickness of the dry anode composition may be substantially uniform and in the range of about 5 μm to about 70 μm. The thickness (μm) of the dry anode composition may be less than about 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10 or 5. The thickness (μm) of the dry anode composition may be at least about 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 or 65. The thickness of the dry anode composition may be within the range provided by any two of these upper and / or lower limits.

[0241] In some embodiments or examples, in step (iii)(a), the wet anode composition layer may be maintained at a temperature of about 40°C to about 60°C for about 30 seconds to about 5 minutes. The wet anode composition may be maintained at a temperature (°C) of less than about 60, 55, 50, 45 or 40. The wet anode composition may be maintained at a temperature (°C) of at least about 40, 45, 50, 55 or 60. The wet anode composition may be maintained at a temperature (°C) within the range provided by any two of these upper and / or lower limits. The wet anode composition may be maintained at a temperature as described herein for less than about 24 hours, 12 hours, 8 hours, 4 hours, 2 hours, 1 hour, 30 minutes, 5 minutes, 4 minutes, 3 minutes, 2 minutes, 1 minute or 30 seconds. The wet anode composition may be maintained at a temperature as described herein for at least about 30 seconds, 1 minute, 2 minutes, 3 minutes, 4 minutes, 5 minutes, 30 minutes, 1 hour, 2 hours, 4 hours, 10 hours, 12 hours or 24 hours. The wet anode composition can be maintained at a temperature as described herein for a time within a range provided by any two of these upper and / or lower limits.

[0242] In some embodiments or examples, in step (iii)(b), the wet anode composition may be maintained at a temperature between about 90° C. and about 180° C. for about 30 seconds to about 5 minutes. The wet anode composition may be maintained at a temperature (° C.) of less than about 180, 170, 160, 150, 140, 130, 120, 115, 110, 105, 100, 95, or 90. The wet anode composition may be maintained at a temperature (° C.) of at least about 90, 95, 100, 105, 110, 115, 120, 130, 140, 150, 160, or 170. The wet anode composition may be maintained at a temperature (° C.) within the range provided by any two of these upper and / or lower limits. The wet anode composition may be maintained at a temperature as described herein for less than about 24 hours, 12 hours, 8 hours, 4 hours, 2 hours, 1 hour, 30 minutes, 5 minutes, 4 minutes, 3 minutes, 2 minutes, 1 minute, or 30 seconds. The wet anode composition can be maintained at a temperature as described herein for at least about 30 seconds, 1 minute, 2 minutes, 3 minutes, 4 minutes, 5 minutes, 30 minutes, 1 hour, 2 hours, 4 hours, 10 hours, 12 hours, or 24 hours. The wet anode composition can be maintained at a temperature as described herein for a time within the range provided by any two of these upper and / or lower limits.

[0243] In some embodiments or examples, the anode slurry may be made homogenous to provide additional advantages / improvements.

[0244] In some embodiments or examples, the present disclosure relates to a method for assembling an electrochemical cell, wherein the method may include the following steps: preparing an anode as defined by at least the method according to any one of the examples described herein, wherein the anode may include an anode composition, the anode composition including microsilicon active material particles; and assembling the anode into an electrochemical cell. In some other embodiments or examples, the present disclosure relates to a method for assembling an electrochemical cell, wherein the method may include the following steps: preparing an anode as defined by at least the method according to any one of the examples described herein, wherein the anode may include or consist of an anode composition according to at least any one of the examples described herein, the anode composition including microsilicon active material particles or coated microsilicon active material particles, optionally one or more additional active materials, optionally one or more binders, and optionally one or more conductive materials, at least according to any one of the examples described herein; and assembling the anode into an electrochemical cell.

[0245] When forming the anode slurry, some or all of the solvent may be removed (eg, by natural evaporation, forced evaporation, or under vacuum) to produce a solid or viscous anode slurry.The anode slurry may be formed or molded into any desired shape, such as an anode.

[0246] In some embodiments or examples, the anode slurry may also be deposited on a current collector material as defined herein to produce an anode. It should be understood that the anode is a combination of a current collector material and an anode composition, also referred to as an anode composition applied to a current collector material. The current collector material may be selected from any current collector material mentioned herein.

[0247] During the preparation of the anode, the anode composition can be applied to only a portion of the surface of the current collector material. In some embodiments or examples, the portion (%) may be less than about 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10 or 5. In some embodiments or examples, the anode composition can be applied to the current collector material by casting (e.g., roll-to-roll processing).

[0248] The coating may be prepared by dissolving or dispersing the coating in a suitable solvent and then optionally mixing it with one or more reagents or dissolving the coating in a suitable solvent under suitable processing conditions.

[0249] The coating can be applied in different physical forms, such as solutions, dispersions, suspensions, mixtures, aerosols, emulsions, pastes or combinations thereof.

[0250] In one example, a method for preparing a coated anode comprises:

[0251] a. applying a coating as described herein to the anode composition; and

[0252] b. Optionally applying one or more post-coatings to the coating present on the anode composition.

[0253] In some embodiments, the coated anode composition can be provided by pyrolysis of a coating or by chemical vapor deposition, physical vapor deposition, sputtering, or mechanical deposition.

[0254] In some embodiments or examples, the coating may be in the form of a single layer. In another embodiment, the coating may be in the form of two or more layers (e.g., multiple layers). The coating may include about 1 to 5 layers. The coating may include less than 5 layers, 4 layers, 3 layers, or less than 2 layers. The coating may include at least about 1 layer, 2 layers, 3 layers, 4 layers, or at least about 5 layers. The coating may be included in a layer within the range provided by any lower limit and / or upper limit as previously described. It should be understood that each layer may be provided by a different coating. For example, a coated micro-silicon active material particle or a coated anode composition may include a coating, wherein one coating includes a carbon material, another coating includes a metal oxide (e.g., aluminum oxide), and another layer includes a polymer coating applied to the micro-silicon in any order. Alternatively, the coating may be a carbon material coating and a metal oxide coating applied to the micro-silicon in any order. In addition, the coating may be a carbon material coating and a polymer coating applied to the micro-silicon in any order.

[0255] In some embodiments or examples, the thickness of the coating may be between about 0.1 nm and about 200 nm, or between about 0.2 nm and about 150 nm, or between about 0.3 nm and about 100 nm, or between about 0.3 nm and about 75 nm, or between about 0.3 nm and about 50 nm, or between about 0.3 nm and about 25 nm, or between about 0.3 nm and about 20 nm, or between about 0.3 nm and about 10 nm. The thickness of the coating (in nm) may be less than about 200, 175, 150, 125, 100, 90, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 8, 6, 5, 4, 3, 2, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, or 0.1. The thickness (in nm) of the coating can be at least about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 12, 14, 16, 18, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, or 80. The thickness (in nm) of the coating can be within a range provided by any two of these upper and / or lower amounts.

[0256] In some embodiments, the ratio of the coating thickness to the uncoated silicon particle diameter (t / d, in the form of X:1) may be between about 0.0001:1 and about 0.2:1, or between about 0.0001:1 and about 0.15:1, or between about 0.0001:1 and about 0.12:1, or between about 0.0001:1 and about 0.1:1, or between about 0.0001:1 and about 0.09:1, or between about 0.0001:1 and about 0.085:1. Viewed from another perspective, in some embodiments, the ratio of silicon particle diameter to coating thickness (d / t, in the form of 1:X) may be between about 1:100,000 and about 1:5, or between about 1:100,000 and about 1:8, or between about 1:100,000 and about 1:10, or between about 1:100,000 and about 1:12.

[0257] It is believed that the coating on the micro silicon active material particles or anode composition, as described herein, can improve the cycling stability and reduce the electrolyte decomposition due to the electrochemical protection of the anode surface. It should be understood that the coating can provide a variety of properties to the micro silicon active particles or anode composition, including, for example, structural strength, lower surface area, reduced pulverization, electronic conductivity, Li ion conductivity, passivation and / or insulation, and ultimately improve the silicon anode capacity retention rate.

[0258] It will be appreciated by those skilled in the art that many changes and / or modifications may be made to the above-described embodiments without departing from the broad general scope of the present disclosure. Therefore, the embodiments of the present invention should be considered in all aspects as illustrative and not restrictive.

[0259] Example

[0260] The present disclosure is further described by the following embodiments.It should be understood that the following description is only for the purpose of describing specific embodiments, and is not intended to limit the above description.

[0261] Example 1: General procedure for preparing anodes

[0262] To prepare the anode slurry, the binder solution and the conductive material are combined using a planetary centrifugal mixer. The mixture is then incorporated at 2000 rpm for 2 minutes, manually mixed with a spatula, and then mixed for another 2 minutes. Microsilicon active material particles and the required amount of additional water are added and the mixing step is repeated. Active graphite is added and the mixing step is repeated. Unless otherwise specified, a predetermined amount of anode slurry is transferred to a container compatible with the Dispermat and mixed for 5 minutes at 6000 rpm using an overhead mixer (e.g., VMA-Getzmann Dispermat).

[0263] In the full cell assembly, the slurry was cast onto copper foil and dried at 60°C and then cut for button cell assemblies. The electrodes (coated anode and commercially available NCM 523 cathode) were further dried at 110°C under vacuum for 12 hours. 150 μL of FEC / DEC (2:8) vol.% containing 1M LiPF6 was used as the electrolyte for the button cell (CR 20232 type) assembly, and Whatman glass fiber was used as the separator. For the charge / discharge cycle test, the button cell was activated at 0.05C for 1 cycle and then cycled at 0.5C for long-term stability testing. The C rate is based on the mass of the active material (Si particles, graphite) in the electrode. The voltage range of the charge / discharge test was 4.2-2.5V during formation and 4.2-3V during cycling. The charge / discharge test was performed on a Neware multi-channel battery tester controlled by a computer. Four replicate batteries were prepared and tested for each condition.

[0264] Table 1: Full cell formation test procedure

[0265] name magnification Cut-off(V) Notes still 1 hour Tap Charging C / 3 3 still 12 hours Constant current and constant voltage charging C / 20 4.2 Cut-off current (C / 100) Constant current discharge C / 20 2.5 Final loop

[0266] Note that the current density used for the cycling tests was based on the electrode capacity obtained from the final delithiation step of the formation procedure.

[0267] Table 2: Cycling test procedure for full cells

[0268] name magnification Cut-off(V) Notes Constant current and constant voltage charging C / 2 4.2 Cut-off current (C / 20) Constant current discharge C / 2 3 Repeat from step 1 Repeat until battery fails or capacity < 80% Final loop

[0269] It should be understood that if the surface area of ​​the particles before coating, the weight of the coating contribution to the microsilicon particle powder, and the density of the corresponding coating material are known, the thickness of the coating applied to the microsilicon particles can be estimated. The following general formula is used to estimate the coating thickness of the coating applied to the microsilicon particles disclosed in any of the following embodiments and in all discussions of coating thickness within this disclosure, where the true density of the coating material is used as an approximation of the resulting coating density:

[0270] Calculated coating thickness on micro-silicon particles = (weight of coating material added to micro-silicon particles / true density of coating material) / surface of uncoated micro-silicon particles.

[0271] It will be appreciated that the actual coating thickness on the microsilicon particles may be slightly higher or lower depending on the characteristics and actual density of the coating, which will vary depending on the coating material and application method.

[0272] Example 2: Al2O3 coated microsilicon

[0273] D of uncoated micro-silicon and Al2O3 coated micro-silicon 50The particle size and BET surface area values ​​are as follows.

[0274] Table 3: Particle size and surface area characteristics

[0275]

[0276] Example 2 (a) Electrode composition

[0277] Anode compositions containing either uncoated micro-silicon or Al2O3 coated micro-silicon were manufactured. Table 4 below shows the specific electrode and slurry compositions used for all experiments.

[0278] Table 4: Electrode and slurry composition

[0279]

[0280] The slurries were prepared using the compositions in Table 4. The procedure described in Example 1 was used for the preparation method.

[0281] Example 2 (b) Slurry preparation

[0282] The slurries were prepared using the compositions in Table 4. The procedure described in Example 1 was used for the preparation method.

[0283] Example 2 (c) Electrochemical Testing Procedure

[0284] Full cells were assembled using the procedure described in Example 1. See Tables 1 and 2 for the cycling procedure.

[0285] Example 2(d) Cyclic Testing - Summary of Key Findings

[0286] Table 5: Summary of electrochemical data for limited capacity full cells

[0287]

[0288]

[0289] When compared to uncoated and equal starting capacities, Al2O3 coated at different ratios showed equal increases in ICE (0.8%) (Table 5). At cycle 90, there was no significant difference in capacity retention between samples coated with 0.2wt% and 0.3wt% Al2O3 (about 96%) ( Figure 1b ), and the capacity retention was only 1% different compared to the uncoated sample. Whereas a higher amount of Al2O3 (0.6wt%) showed a rapid decrease in capacity retention at cycle 90, and the tested cell lost 6% of its capacity.

[0290] Example 3: Phenolic resin precursor carbon-coated micro-silicon

[0291] Example 3 (a) Microsilicon Particle Coating

[0292] Example 3.1: 6.6 wt% carbon-coated microsilicon

[0293] 30g of phenol resin was added to 150g of anhydrous ethanol, and the solution was mixed using a magnetic stirrer at room temperature until the resin was completely dissolved. Next, 104g of microsilicon was added to the ethanol-resin solution, and the suspension was continued to be stirred for 1 hour. The mixture was then heated at 70°C for 12 hours until the ethanol was completely evaporated. 61.5g of resin-coated microsilicon was transferred to a ceramic crucible and placed in a furnace tube. Before starting the calcination process, the furnace was purged with high-purity nitrogen at a flow rate of 2L / min for 30 minutes at room temperature and maintained throughout the process. The sample was heated to 900°C at a heating rate of 4°C / min and calcined for 1 hour. The furnace was then cooled to room temperature while maintaining a nitrogen flow at least until the furnace temperature reached 100°C. The calcined microsilicon sample was ground using a mortar and pestle for approximately 5 minutes to decompose any larger silicon chunks. The product was then ball milled at 520 rpm with 6 minute grinding intervals and 3 minute rest intervals for a total of 3 hours using a grinding ratio of 30 wt% silicon and 70 wt% grinding media (ie, 1 cm diameter ceramic balls).

[0294] Example 3.2: 7.93 wt% carbon-coated microsilicon

[0295] The coating procedure in Example 3.1 was repeated using 40 g of phenol resin and 104 g of microsilicon. 65 g of the resin-coated microsilicon was transferred to a ceramic crucible and placed in a furnace tube. Before starting the calcination process, the furnace was purged with high-purity nitrogen at a flow rate of 2 L / min for 30 minutes at room temperature and maintained throughout the process. The sample was heated to 900°C and calcined for 2 hours at a heating rate of 4°C / min. The furnace was then cooled to room temperature while maintaining a nitrogen flow at least until the furnace temperature reached 100°C. The calcined microsilicon sample was ground using a mortar and pestle for approximately 5 minutes to break down any larger silicon chunks. The product was then ball milled at 520 rpm with a grinding interval of 6 minutes and a standing interval of 3 minutes for a total of 3 hours using a grinding ratio of 30 wt% silicon and 70 wt% grinding media (i.e., ceramic balls of 1 cm diameter).

[0296] Carbon-coated micro-silicon 50 The particle size and BET surface area values ​​are as follows.

[0297] Table 6: Particle size and surface area characteristics

[0298]

[0299] Example 3 (b) Electrode composition

[0300] Anode compositions consisting of carbon-coated micro-silicon were manufactured. Table 7 below shows the specific slurry and electrode compositions used for all experiments.

[0301] Table 7: Electrode composition

[0302]

[0303] Example 3 (c) Slurry preparation

[0304] The amounts of materials specified in Table 7 were used in the slurry preparation process. The same procedure as in Example 1 was followed.

[0305] Example 3(d) Electrochemical Testing Procedure

[0306] Full cells were assembled using the procedure described in Example 1. See Tables 1 and 2 for the cycling procedure.

[0307] Example 3(e) Cyclic Testing - Summary of Key Findings

[0308] Table 8: Summary of electrochemical data for limited capacity full cells

[0309]

[0310]

[0311] Table 8 shows that increasing the amount of phenolic resin (PR) in the coating affects the ICE. The 8 wt.% PR coating showed a 3.7% reduction in ICE compared to the control, and the 6.6 wt.% PR coating showed a 2.4% reduction. At cycle 50, the capacity retention of the uncoated cell was 99.4%, while the capacity retention of the 8 wt.% PR coated cell was 96.2%, and the capacity retention of the 6.6 wt.% PR cell was 97% ( Figure 2b ).

[0312] Example 4: PVP Precursor Carbon-Coated Micro-Silicon

[0313] Example 4 (a) Microsilicon Particle Coating

[0314] Example 4.1-6.03wt% Carbon-coated Microsilicon

[0315] 22.5 g of PVP (55,000 MW) was added to 250 ml of anhydrous ethanol, and the solution was mixed using a magnetic stirrer at 40 ° C until the polymer was completely dissolved. Next, 22.5 g of microsilicon was added to the ethanol-PVP solution, and the suspension was continued to be stirred. Another 30 ml of anhydrous ethanol was added to the mixture to promote uniform dispersion of the ingredients. Next, the mixture was dried at 40 ° C for 12 hours under ambient conditions, followed by an additional drying step at 40 ° C for 3 hours under vacuum. 31.6 g of PVP-coated microsilicon was transferred to a ceramic crucible and placed in a furnace tube. Before starting the calcination process, the furnace was purged with high-purity nitrogen at a flow rate of 2 L / min at room temperature for 30 minutes and maintained throughout the process. The sample was heated to 700 ° C at a heating rate of 4 ° C / min and calcined for 2 hours. The furnace was then cooled to room temperature while maintaining a nitrogen flow at least until the furnace temperature reached 100 ° C. The calcined micro-silicon sample was ground using a mortar and pestle to break down any larger silicon chunks. The product was then ball milled at 520 rpm with a grinding interval of 6 minutes and a rest interval of 3 minutes for a total of 3 hours using a grinding ratio of 30 wt % silicon and 70 wt % grinding media (i.e., 0.7 cm diameter ceramic balls).

[0316] Example 4.2-3.12 wt% Carbon-coated Microsilicon

[0317] 45 g of PVP (55,000 MW) was added to a mixture of 3 L of deionized water and 5 ml of anhydrous ethanol. The solution was mixed using a magnetic stirrer at room temperature until the polymer was completely dissolved. Next, 90.0 g of microsilicon was added to the PVP solution and the suspension was continued to be stirred. This suspension was further ultrasonicated for 30 minutes to promote uniform dispersion of the microsilicon powder. The suspension was then dried using a micro spray dryer B-290 The prepared 5wt% suspension was spray dried at 220°C inlet temperature, 30L / min air flow, 100% suction and 40% solution feed rate. 37.0g of PVP coated microsilicon was transferred to a ceramic crucible and placed in a furnace tube. Before starting the calcination process, the furnace was purged with high purity nitrogen at a flow rate of 2L / min for 30 minutes at room temperature and maintained throughout the process. The sample was heated to 700°C at a heating rate of 4°C / min and calcined for 1 hour. The furnace was then cooled to room temperature while maintaining a nitrogen flow at least until the furnace temperature reached 100°C. The coated microsilicon sample was first ground using a mortar and pestle to break down larger silicon chunks, followed by grinding in a laboratory sample mill for 30 minutes.

[0318] Example 4.3-6.92wt% Carbon-coated Microsilicon

[0319] 90 g of PVP (55,000 MW) was added to 6 L of deionized water, and the solution was mixed using a magnetic stirrer at 30 °C until the polymer was completely dissolved. Next, 91.0 g of microsilicon was added to the PVP solution cooled to room temperature, and stirring was continued. This suspension was further ultrasonicated for 30 minutes to promote uniform dispersion of the microsilicon powder. The suspension was then dried using a micro spray dryer B-290 The prepared 3wt% suspension was spray dried at 220°C inlet temperature, 30L / min air flow, 100% suction and 40% solution feed rate. 27.0g of PVP-coated microsilicon was transferred to a ceramic crucible and placed in a furnace tube. Before starting the calcination process, the furnace was purged with high-purity nitrogen at a flow rate of 2L / min for 30 minutes at room temperature and maintained throughout the process. The sample was heated to 700°C and calcined for 2 hours at a heating rate of 4°C / min. The furnace was then cooled to room temperature while maintaining a nitrogen flow at least until the furnace temperature reached 100°C. The calcined microsilicon sample was ground using a mortar and pestle to break down any larger silicon chunks. The product was then ball milled at 520rpm with a grinding interval of 6 minutes and a standing interval of 3 minutes for a total of 3 hours using a grinding ratio of 30wt% silicon and 70wt% grinding media (i.e., ceramic balls of 0.7cm diameter).

[0320] Carbon-coated micro-silicon 50 The particle size and BET surface area values ​​are as follows.

[0321] Table 9: Particle size and surface area characteristics

[0322]

[0323] Example 4 (b) Electrode composition

[0324] Anode compositions consisting of carbon coated micro-silicon were manufactured. The specific electrode compositions used for all experiments are shown in Table 10 below.

[0325] Table 10: Electrode composition

[0326]

[0327]

[0328] Example 4 (c) Slurry preparation

[0329] The amounts of materials specified in Table 10 were used in the slurry preparation process. The same procedure as in Example 1 was followed.

[0330] Example 4(d) Electrochemical Testing Procedure

[0331] Full cells were assembled using the procedure described in Example 1. See Tables 1 and 2 for the cycling procedure.

[0332] Example 4(e) Cyclic Testing - Summary of Key Findings

[0333] Table 11: Summary of electrochemical data for limited capacity full cells

[0334]

[0335] Table 11 shows that increasing the amount of PVP coating adversely affects ICE: the 3.12wt% PVP sample shows a slight decrease in ICE of 0.6% compared to the control, while the 6.92wt% PVP sample loses about 3% of its ICE. At cycle 100, the uncoated sample loses about 3% of its capacity, while the 3.1wt% PVP loses 5% in the same cycle.

[0336] Example 5: PAN Precursor Carbon-Coated Micro-Si

[0337] Example 5 (a) - 14.5 wt% carbon-coated microsilicon

[0338] 45 g of PAN (150,000 MW) was added to 500 mL of DMF while stirring at 70 ° C using a shear mixer. After the polymer was completely dissolved, 90.0 g of microsilicon was added to the polymer solution, and the suspension was continued to be mixed using a shear mixer. During this process, the solution temperature was raised to 120 ° C, thereby promoting the evaporation of the DMF solvent. After the solution consistency became difficult to mix mechanically, the resulting product was transferred to 3 ceramic crucibles and further dried under any of the following conditions: (i) dried at 200 ° C for 2 hours under N2 gas flow; (ii) dried at 200 ° C for 2 hours under atmospheric conditions; or (iii) dried at 110 ° C for 2 hours under vacuum. 60 g of the resulting dried product was placed in a furnace tube, and before starting the calcination process, the furnace was purged with high purity nitrogen at a flow rate of 2 L / min for 30 minutes at room temperature. The sample was heated to 900 ° C at a heating rate of 4 ° C / min and calcined for 2 hours. The furnace was then cooled to room temperature while maintaining a nitrogen flow at least until the furnace temperature reached 100° C. The calcined microsilicon sample was ground using a mortar and pestle for approximately 5 minutes to break down any larger silicon chunks. The product was then ball milled at 520 rpm with a grinding interval of 6 minutes and a rest interval of 3 minutes for a total of 3 hours using a grinding ratio of 30 wt % silicon and 70 wt % grinding media (i.e., 0.7 cm diameter ceramic balls).

[0339] Carbon-coated micro-silicon 50 The particle size and BET surface area values ​​are as follows.

[0340] Table 12: Particle size and surface area characteristics

[0341]

[0342] Example 5 (b) Electrode composition

[0343] Anode compositions consisting of carbon coated micro-silicon were manufactured. The specific electrode compositions used for all experiments are shown in Table 13 below.

[0344] Table 13: Electrode composition

[0345] Material describe Content [wt%] Mass(g) Active Materials Silicon (coated with 14.5wt% PAN(C)) 82.20 37.4 Conductive filler Timrex KS6L Flake Graphite 7.80 2.73 Conductive additives Timcal Super C65 2.00 0.91 Adhesives PAA, 25%, neutralized with LiOH 8.00 18.2 water _ _ 19.76

[0346] Example 5 (c) Slurry preparation

[0347] The amounts of materials specified in Table 13 were used in the slurry preparation process. The same procedure as in Example 1 was followed.

[0348] Example 5(d) Electrochemical Testing Procedure

[0349] Full cells were assembled using the procedure described in Example 1. See Tables 1 and 2 for the cycling procedure.

[0350] Example 5(e) Cyclic Testing - Summary of Key Findings

[0351] Table 14: Summary of electrochemical data for limited capacity full cells

[0352]

[0353]

[0354] 14.5wt% PAN coated micro-Si has an ICE of 82.1%, while uncoated mSi has an ICE of 89% (Table 14). Figure 4b ), the PAN coated sample lost 4.4% of its capacity.

[0355] Example 6: Pre-lithiation of coated micro-silicon

[0356] Example 6 (a) Electrode composition

[0357] All silicon material samples were incorporated into electrodes using the specific electrode compositions shown in Table 15 below.

[0358] Table 15: Electrode composition

[0359]

[0360] Example 6 (b) Slurry preparation

[0361] The amounts of materials specified in Table 15 were used in the slurry preparation process. The same procedure as in Example 1 was followed.

[0362] Example 6 (c) Electrochemical Testing Procedure

[0363] Table 16: Half-cell formation test procedure (with pre-lithiation)

[0364]

[0365] Example 6 (d) Pre-lithiation step

[0366] The slurry was cast onto copper foil and dried at 60°C and then cut for button cell assembly. The electrodes were further dried at 110°C under vacuum for 12 hours. Lithium (Li) metal was used as the counter electrode and Celgard separator was used. 150 μL of FEC / DEC (2:8) vol.% containing 1M LiPF6 was used as the electrolyte for the button cell assembly. Based on the expected capacity of the anode, the button cell was subjected to partial formation cycles at 0.05C until a certain degree of lithiation (Table 16).

[0367] The C rate is based on the mass of active material (Si particles, graphite) in the electrode. The first lithiation is limited by capacity (mAh / g) accounting for 20% of the expected capacity of the anode with about 10% lithium loss in the first cycle.

[0368] Example 6 (e) Post-prelithiation step

[0369] The button cell was taken out and introduced into a glove box (under Ar atmosphere) and disassembled to prepare a full cell. Prior to assembly, the anode was washed with DMC and dried. The full cell was assembled using the procedure described in Example 1. For the cycling procedure, see Tables 1 and 2.

[0370] Example 6(f) Cyclic Testing—Summary of Key Findings.

[0371] Table 17: Summary of electrochemical data for limited capacity full cells

[0372]

[0373] The data for the unlithiated samples were taken from Example 2 (for 0.6 wt% Al2O3) and Example 4 (for 3.12 wt% PVP). Electrochemical pre-lithiation of the coated samples significantly increased the ICE (by about 1%) compared to the unlithiated samples, which resulted in cycling at higher capacity (Table 17). The cycling capacity and average coulombic efficiency increased significantly. For both pre-lithiated (3.12 wt% PVP cells and 0.6 wt% Al2O3) cells, negligible capacity loss was observed in the first 50 cycles (Figure 5).

Claims

1. An anode composition comprising micro-silicon active material particles, The microsilicon active material particles have one or more of the following: (i) a BET surface area of ​​about 0.1 m 2 / g and about 10m 2 / g; (ii) D 50 The particle size is between about 0.1 μm and about 10 μm; and (iii) D 50 :BET surface area ratio is between about 0.1 and about 10, wherein the amount of the micro-silicon active material particles present in the anode composition is between about 60 wt. % and about 95 wt. % based on the total weight % of the anode composition, and wherein the anode composition comprises a coating. 2 . The anode composition according to claim 1 , wherein the coating is a coating of the microsilicon active material particles.

3. The anode composition according to claim 1, wherein the coating is a coating of the anode composition.

4. The anode composition according to any one of claims 1 to 3, wherein the D of the micro-silicon active material particles is 50 The ratio of the BET surface area is between about 0.1 and about 6.

5. The anode composition according to any one of claims 1 to 4, wherein the coating is selected from the group comprising carbon, graphene, graphite, metal oxides, polymers and combinations thereof to form coated micro silicon active material particles.

6. The anode composition according to any one of claims 1 to 5, wherein the measured BET surface area of ​​the microsilicon active material particles is between about 1 m 2 / g and about 5m 2 / g.

7. The anode composition according to any one of claims 1 to 6, wherein the amount of the micro-silicon active material particles or coated micro-silicon active material particles present in the anode composition is between about 70 wt.% and about 95 wt.%, based on the total weight % of the anode composition.

8. The anode composition according to any one of claims 1 to 7, wherein the density of the micro-silicon active material particles or the coated micro-silicon active material particles is between about 0.5 g / cm 2 About 1.2g / cm 2 between.

9. The anode composition according to any one of claims 1 to 8, wherein the microsilicon active material particles have a purity of at least 95 wt.% (free of oxygen).

10. The anode composition according to any one of claims 1 to 9, wherein the D of the micro-silicon active material particles is 50 The particle size is between about 2 μm and about 8 μm.

11. The anode composition of any one of claims 2 to 10, wherein the measured BET surface area of ​​the coated microsilicon active material particles is between about 1 μm and about 100 μm.

12. The anode composition of any one of claims 1 to 11, wherein the coating has a thickness between about 0.1 nm and about 200 nm.

13. The anode composition of any one of claims 1 to 12, wherein the ratio of the coating thickness to the uncoated silicon particle diameter (t / d, in the form of X:1) is between about 0.0001:1 and about 0.2:

1.

14. The anode composition of any one of claims 1 to 13, wherein the anode composition further comprises one or more binders.

15. The anode composition of claim 14, wherein the binder is present in the anode composition in an amount ranging from about 2.5 wt.% to about 15 wt.%, based on the total weight of the anode composition.

16. The anode composition of any one of claims 1 to 15, wherein the anode composition further comprises one or more conductive materials.

17. The anode composition of claim 16, wherein the amount of conductive material present in the anode composition is between about 2.5 wt.% and about 40 wt.%, based on the total weight of the anode composition.

18. The anode composition according to any one of claims 1 to 17, wherein the micro-silicon active material particles or coated micro-silicon active material particles are pre-lithiated.

19. The anode composition of claim 18, wherein the micro-silicon active material particles or coated micro-silicon active material particles are pre-lithiated prior to incorporation into the anode composition.

20. The anode composition of claim 18 or claim 19, wherein the pre-lithiation level of the micro-silicon active material particles or coated micro-silicon active material particles is between about 1% and about 30%.

21. The anode composition of any one of claims 18 to 20, wherein the pre-lithiation level of the micro-silicon active material particles or coated micro-silicon active material particles is between about 10% and about 30%.

22. The anode composition of any one of claims 1 to 21, wherein the anode composition is a coating or film applied to the surface of a current collector material.

23. The anode composition of claim 22, wherein the current collector material for the anode is selected from the group comprising copper, aluminum, stainless steel, titanium, carbon, perforated metal foils, metal foams, and porous and non-porous films based on metal-coated polymers.

24. The anode composition according to any one of claims 1 to 23, wherein the micro-silicon active material particles or the anode composition comprises one or more layers of the coating.

25. The anode composition of any one of claims 1 to 24, wherein the anode composition is an anode of an electrochemical cell.

26. The anode composition of any one of claims 1 to 25, wherein the anode composition is an anode of a primary or secondary battery.

27. The anode composition of any one of claims 1 to 26, wherein the anode composition is an anode of a lithium ion battery.

28. An electrochemical cell comprising: an anode; a cathode; an electrolyte; and a separator, wherein the anode comprises the anode composition according to any one of claims 1 to 27, The lithium uptake capacity of the anode is greater than the lithium release capacity of the cathode.

29. The electrochemical cell of claim 28, wherein the capacity of the lithium uptake capacity of the anode is not fully utilized during charging of the lithium ion battery.

30. An electrochemical cell according to claim 28 or claim 29, wherein the anode is only partially lithiated in a fully charged state.

31. The electrochemical cell of any one of claims 28 to 29, wherein the degree of silicon lithiation is limited to about 20% to about 80%.

32. The full cell assembly of any one of claims 28 to 31, wherein the capacity ratio of the anode to the cathode (N / P ratio) is between about 1.05 and about 7.

33. The electrochemical cell of any one of claims 28 to 32, wherein the capacity ratio of the anode to the cathode (N / P ratio) is between about 1.5 and about 4.

34. The electrochemical cell of any one of claims 28 to 33, wherein the capacity ratio of the anode to the cathode (N / P ratio) is between about 1.8 and about 3.

5.

35. The electrochemical cell of any one of claims 28 to 34, wherein the lower cutoff voltage is between about 2.5V and 3.0V.

36. The electrochemical cell of any one of claims 28 to 35, wherein the anode is pre-lithiated.

37. The electrochemical cell of claim 36, wherein the pre-lithiation level of the anode is between about 1% and about 30%.

38. An electrochemical cell according to any one of claims 28 to 37, wherein the cathode is selected from the group comprising lithium nickel cobalt manganese oxide (NCM), lithium iron phosphate (LFP), lithium nickel manganese spinel (LNMO), lithium nickel cobalt aluminum oxide (NCA), lithium manganese oxide (LMO), lithium cobalt oxide (LCO) and sulfur or a sulfur composite.

39. The electrochemical cell according to any one of claims 28 to 38, wherein the electrolyte is selected from a non-aqueous electrolyte solution comprising one or more lithium salts.

40. The electrochemical cell of any one of claims 28 to 39, wherein the electrochemical cell is an energy storage device.

41. The electrochemical cell of claim 40, wherein the energy storage device is a battery, preferably a secondary battery.

42. The electrochemical cell of claim 41, wherein the battery is a lithium ion battery.

43. A method for improving the cycling stability of a lithium ion battery having an anode and a cathode, at least one electrolyte and optionally a separator, wherein the anode composition is as defined in any one of claims 1 to 27.

44. The method of claim 43, wherein the anode within the battery delivers a specific capacity of at least about 450 mAh / g, 500 mAh / g, 600 mAh / g, 800 mAh / g, 1000 mAh / g, 1200 mAh / g, or 1500 mAh / g, and retains at least about 80% of its initial capacity after 100, 200, 400, 600, 800, 1000, or 1500 cycles of the battery.

45. Use of an anode composition in an electrochemical cell, wherein the anode composition is at least partially applied to a current collector material, and wherein the anode composition is as defined in any one of claims 1 to 27.

46. ​​A method for preparing coated microsilicon active material particles, the method comprising: (i) providing a plurality of micro-silicon active material particles, wherein the micro-silicon active material particles have one or more of the following: (i) a BET surface area of ​​about 0.1 m 2 / g and about 10m 2 / g, (ii)D 50 The particle size is between about 0.1 μm and about 10 μm, and (iii) D 50 :BET surface area ratio is between about 0.1 to about 10; and (ii) applying a coating layer onto the surface of the microsilica active material particles.

47. The method of claim 46, wherein the coating is selected from the group consisting of carbon, graphene, graphite, metal oxides, polymers, and combinations thereof.

48. A method for preparing an anode of an electrochemical cell, the method comprising the steps of: (i) preparing an anode slurry, the anode slurry comprising micro-silicon active material particles or coated micro-silicon active material particles, optionally one or more additional active materials, optionally one or more binders, optionally one or more conductive materials, optionally one or more additives and a solvent system; (ii) casting a layer of the anode slurry onto a current collector material to provide a layer of an anode composition on the current collector material, and (iii) optionally coating the anode composition, The microsilicon active material particles have one or more of the following: (a) a BET surface area of ​​about 0.1 m 2 / g and about 10m 2 / g, (b)D 50 The particle size is between about 0.1 μm and about 10 μm, (c) D 50 The ratio of the BET surface area is between about 0.1 and 10.

49. The method of claim 48, wherein the method further comprises the step of (iii) curing the anode layer by (a) solvent evaporation and / or (b) heat treatment to provide a dry anode composition layer coated on the current collector material.

50. The method of claim 48 or claim 49, wherein the coating is selected from the group comprising carbon, graphene, graphite, metal oxides, polymers, and combinations thereof.

51. The method of any one of claims 48 or 50, wherein the binder content in the anode slurry is between about 2.5 wt.% and about 15 wt.%, based on the total weight of the anode composition.

52. The method of any one of claims 48 to 51, wherein the content of conductive material in the anode slurry is between about 2.5 wt.% and about 40 wt.%, based on the total weight of the anode composition.

53. The method of any one of claims 48 to 52, wherein the viscosity of the anode slurry at a given shear rate is in the range between 500 mPas and 100,000 mPas.

54. The method of any one of claims 48 to 53, wherein the thickness of the dry anode composition layer ranges between about 5 μm and about 70 μm.

55. The method of any one of claims 49 to 54, wherein the temperature of step (iii)(a) is between about 40°C and 60°C.

56. The method of any one of claims 49 to 55, wherein the temperature of step (iii)(b) is between about 90°C and 180°C.

57. The method of any one of claims 48 to 56, wherein the coating is applied to at least a portion of a surface of the anode composition.

58. An anode comprising the anode composition according to any one of claims 1 to 27, the anode being prepared according to the method according to any one of claims 48 to 57.

59. A method for assembling an electrochemical cell, wherein the method comprises the steps of: An anode prepared according to the method of any one of claims 48 to 57, wherein the anode comprises an anode composition according to any one of claims 1 to 27; and The anode is assembled into an electrochemical cell.