Positive electrode material for lithium-sulfur battery and lithium-sulfur battery comprising same
By inducing lithium sulfide deposition on the surface of the electrode of the lithium-sulfur battery, the porous carbon substrate and needle-shaped metal particles combined with highly dissolved electrolyte are used to solve the passivation problem caused by lithium sulfide accumulation and improve the discharge capacity and life of the battery.
Patent Information
- Application Number
- CN202380032172.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-27
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-15
AI Technical Summary
The accumulation of lithium sulfide in lithium-sulfur batteries causes electrode passivation, affecting the discharge capacity and life of the battery.
By inducing the deposition of lithium sulfide on the electrode surface, needle-like metal particles are formed on the porous carbon substrate, and combined with highly solubility electrolytes such as LiBr, the deposition position of lithium sulfide is controlled to improve sulfur utilization.
It effectively inhibits the overall accumulation of lithium sulfide on the electrode surface, improves the discharge capacity and life characteristics of lithium-sulfur batteries, and enhances the electrochemical reactivity of sulfur.
Smart Images

Figure CN118974969A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a positive electrode material for a lithium-sulfur battery and a lithium-sulfur battery comprising the positive electrode material.
[0002] This application claims priority to Korean Patent Application No. 10-2022-0186344 filed in Korea on December 27, 2022, the disclosure of which is incorporated herein by reference. Background Art
[0003] Lithium-sulfur batteries are battery systems that use sulfur-sulfur (SS) bonds as positive electrode active materials and lithium metal as negative electrode active materials. Sulfur, the main component of positive electrode active materials, is abundant in nature and widely available worldwide, non-toxic and low in atomic weight.
[0004] Because secondary batteries are widely used in applications including electric vehicles (EVs) and energy storage systems (ESSs), lithium-sulfur battery technology that theoretically achieves higher energy storage density per unit weight (~2,600 Wh / kg) than lithium-ion secondary batteries with a lower energy storage density per unit weight (~250 Wh / kg) has attracted attention.
[0005] During the discharge process, the lithium-sulfur battery undergoes oxidation at the negative electrode active material lithium by releasing electrons into the lithium cations, and undergoes reduction at the positive electrode active material sulfur material by accepting electrons. Through the reduction reaction, the sulfur material is converted into sulfur anions through the SS bond that accepts two electrons. The lithium cations generated by the oxidation reaction of lithium migrate to the positive electrode via the electrolyte and combine with the sulfur anions generated by the reduction reaction of the sulfur compound to form a salt. Specifically, the sulfur before discharge has a cyclic S8 structure, and it is converted into lithium polysulfide (Li2S x ) and is completely reduced to lithium sulfide (Li2S).
[0006] In this case, because lithium sulfide accumulates on the electrode surface of the lithium-sulfur battery, the discharge capacity of the lithium-sulfur battery is lower than the theoretical capacity. In recent years, the automobile market has required vehicles to travel long distances on a single charge, and in order to meet this demand, the battery industry is trying to develop batteries that allow vehicles to travel farther on a single charge. In order to keep up with this trend, it is necessary to develop lithium-sulfur batteries that meet energy density standards so that vehicles can travel farther on a single charge.
[0007] To commercialize lithium-sulfur batteries, technology development is needed to overcome the passivation caused by the accumulation of lithium sulfide on the electrodes. Summary of the invention
[0008] Technical issues
[0009] The present invention aims to overcome the passivation caused by the accumulation of lithium sulfide on electrodes used in lithium-sulfur batteries.
[0010] To this end, one aspect of the present invention is to provide an electrode for a lithium-sulfur battery, wherein the deposition of lithium sulfide is induced at a specific position on the surface of the electrode to effectively control the deposition of lithium sulfide.
[0011] In addition, another aspect of the present invention is to provide a lithium-sulfur battery comprising a three-dimensionally shaped electrode for locally inducing the deposition of lithium sulfide, and an electrolyte having high solubility for lithium sulfide to effectively control the deposition of lithium sulfide.
[0012] Therefore, the present invention aims to provide a lithium-sulfur battery having high sulfur utilization by improving the electron supply to lithium sulfide and lithium polysulfide by inducing the deposition of lithium sulfide at specific locations.
[0013] Technical Solution
[0014] In order to solve the above problems, according to one aspect of the present invention, a carbon composite material according to the following embodiments is provided.
[0015] A carbon composite material according to a first embodiment includes:
[0016] a porous carbon substrate; and
[0017] metal particles on at least a portion of the surface of the porous carbon substrate,
[0018] The metal particles are in a needle-like shape.
[0019] According to the second embodiment, in the first embodiment, the position near the surface of the porous carbon substrate where the metal particles are formed is referred to as the lower part, and the position in the direction extending outward from the surface of the porous carbon substrate is referred to as the upper part, then the needle-shaped metal particles can have a morphology in which the upper radius is smaller than the lower radius and L / D is greater than 1, wherein L / D is the ratio of the total length to the lower radius.
[0020] According to the third embodiment, in the first or second embodiment, L / D of the needle-shaped metal particles may be 5 or more.
[0021] According to a fourth embodiment, in any one of the first to third embodiments, the upper radius (D 50 ) can be less than 100 nm.
[0022] According to a fifth embodiment, in any one of the first to fourth embodiments, the lower radius (D 50 ) can be from 100 nm to 1,000 nm.
[0023] According to a sixth embodiment, in any one of the first to fifth embodiments, the total length (D 50 ) can be from 1 µm to 10 µm.
[0024] According to the seventh embodiment, in any one of the first to sixth embodiments, the porous carbon substrate may include carbon fiber cloth, carbon nanotubes (CNTs), graphene, graphene oxide (GO), reduced graphene oxide (rGO), carbon black, graphite, graphite nanofibers (GNF), carbon nanofibers (CNF), activated carbon fibers (ACF), activated carbon, fullerenes, or two or more of these materials.
[0025] According to an eighth embodiment, in any one of the first to seventh embodiments, the metal particles may include transition metal particles.
[0026] According to another aspect of the present invention, an electrode and a battery according to the following embodiments are provided.
[0027] An electrode according to a ninth embodiment comprises:
[0028] The carbon composite material according to any one of the first to eighth embodiments; and
[0029] Sulfur materials.
[0030] According to a tenth embodiment, in the ninth embodiment, the sulfur-based material may be coated on all or a part of the surface of the carbon composite material.
[0031] A lithium secondary battery according to an eleventh embodiment includes:
[0032] an electrode assembly, the electrode assembly comprising a positive electrode, a negative electrode, and a separator between the positive electrode and the negative electrode; and
[0033] Electrolytes,
[0034] Here, the positive electrode is the electrode according to the ninth or tenth embodiment.
[0035] In the lithium secondary battery according to the twelfth embodiment, in the eleventh embodiment, the electrolyte may contain LiBr, LiCl, LiI, LiTf, or a mixture thereof as the lithium salt.
[0036] In the lithium secondary battery according to the thirteenth embodiment, in the eleventh or twelfth embodiment, the lithium secondary battery may be a lithium sulfur battery.
[0037] According to still another aspect of the present invention, a method for manufacturing a carbon composite material according to the following embodiment is provided.
[0038] A method for producing a carbon composite material according to a fourteenth embodiment is a method for producing the carbon composite material according to any one of the first to eighth embodiments, and the method includes the steps of:
[0039] mixing a metal chloride hydrate, ammonium fluoride, and urea to prepare a metal particle precursor solution; and
[0040] While the porous carbon substrate is in contact with the metal particle precursor solution, needle-shaped metal particles are formed on at least a portion of the surface of the porous carbon substrate by a hydrothermal reaction.
[0041] According to a fifteenth embodiment, in the fourteenth embodiment, the metal chloride hydrate may be a chloride hydrate of a transition metal.
[0042] Beneficial Effects
[0043] The carbon composite material according to one embodiment of the present invention can realize a lithium-sulfur battery having a high discharge capacity by inducing the deposition of lithium sulfide at a specific location during battery operation.
[0044] Specifically, lithium-sulfur batteries using cathode active materials containing sulfur (S)-sulfur (S) bonds can inhibit the accumulation of lithium sulfide on the entire surface of the cathode by inducing the accumulation of lithium sulfide (Li2S) at specific locations on the cathode surface, thereby preventing electrode passivation, leading to high sulfur utilization in cathodes for lithium-sulfur batteries and lithium-sulfur batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] The accompanying drawings show an exemplary embodiment of the present invention and, together with the foregoing description, serve to provide a further understanding of the technical aspects of the present invention, whereby the present invention should not be construed as being limited to the accompanying drawings.
[0046] Figure 1 The life characteristic evaluation results of the battery according to Experimental Example 1 of the present invention are shown.
[0047] Figure 2 The discharge capacity evaluation results of the battery according to Experimental Example 1 of the present invention are shown.
[0048] Figure 3 The resistance curve evaluation results of the battery according to Experimental Example 2 of the present invention are shown. Figure 3 , the graph of Comparative Example 4 shows 2 Hz.
[0049] Figure 4 The results of observation of the lithium sulfide deposition morphology on the electrodes of Example 2 and Example 3 according to the experiment of the present invention are shown.
[0050] Figure 5Shows the observation results of the deposition morphology of lithium sulfide on the electrodes of Example 2 and Example 3 in the experiments according to the present invention.
[0051] Figure 6 Shows the X-ray photoelectron spectroscopy (XPS) analysis results of metal particles after the deposition of lithium sulfide on the electrodes of Comparative Example 5 in the experiments according to the present invention.
[0052] Figure 7 Is the observation image of the scanning electron microscope on the electrode surface of Comparative Example 5 in the experiments according to the present invention.
[0053] Figure 8 Shows the observation results of the deposition morphology of lithium sulfide on the electrode of Comparative Example 5 in the experiments according to the present invention. Detailed Description
[0054] Hereinafter, the present invention will be described in more detail.
[0055] It should be understood that the terms or words used in the specification and the appended claims should not be construed as limited to the general meaning and the meaning in the dictionary, but should be interpreted based on the principle that allows the inventor to appropriately define the terms for the best explanation according to the meaning and concept corresponding to the technical aspect of the present invention.
[0056] Unless otherwise clearly indicated in the context, the term "comprising" or "including" when used in this specification specifies the presence of the stated element, but does not exclude the presence or addition of one or more other elements.
[0057] In addition, when specifying the inherent manufacturing and material tolerances in the stated case, the terms "about" and "substantially" as used herein are used in the sense of being equal to or close to the value, and are used to prevent unscrupulous infringers from improperly using the exact numerical value or absolute numerical value stated for the purpose of helping to understand the present invention.
[0058] Throughout the specification, "A and / or B" means A or B or both.
[0059] In the present invention, the "specific surface area" is measured by the Brunauer-Emmett-Teller (BET) method. Specifically, it can be calculated based on the nitrogen adsorption amount at liquid nitrogen temperature (77 K) using BELSORP mini II of BEL Japan.
[0060] As the term "polysulfide" used herein encompasses "polysulfide ion (S x 2- , 1 < x ≤ 8)" and "lithium polysulfide (Li2S x or LiS x- the concept of "1 < x ≤ 8)".
[0061] As used herein, the term "composite material" refers to a material formed by combining two or more materials and having physically and chemically different phases and more effective functions.
[0062] As used herein, the term "porosity" refers to the ratio of the pore volume to the total volume of the structure, expressed as a volume percentage, and can be used interchangeably with terms such as pore ratio and void fraction.
[0063] In the present invention, "particle size D n " refers to the particle size at the n% of the cumulative volume particle size distribution of the particles. That is, "particle size D 50 " refers to the particle size at the 50% of the cumulative volume particle size distribution of the particles. The particle size D n can be measured by the laser diffraction method. For example, by dispersing the target particle powder in a dispersion medium, supplying it to a commercially available laser diffraction particle size measuring instrument (e.g., Microtrac MT 3000), irradiating ultrasonic waves of about 28 kHz with an output of 60 W to obtain a cumulative volume particle size distribution curve, and determining the particle size corresponding to 50% of the cumulative volume distribution, the particle size D 50 can be measured.
[0064] The present invention relates to a carbon composite material for an electrochemical device, a positive electrode active material containing the same, a positive electrode, and a secondary battery containing the positive electrode. The secondary battery can be a lithium-ion secondary battery. In particular, the positive electrode active material according to one aspect of the present invention contains a sulfur-based material, and the lithium-ion secondary battery is a lithium-sulfur secondary battery.
[0065] The carbon composite material for the positive electrode in a lithium-sulfur battery is characterized in that needle-shaped metal particles are formed on a porous carbon material.
[0066] Carbon composite material
[0067] Specifically, the carbon composite material according to one aspect of the present invention contains
[0068] a porous carbon substrate, and
[0069] metal particles on at least a part of the surface of the porous carbon substrate, and
[0070] the metal particles are in a needle shape.
[0071] In one embodiment of the present invention, the "needle shape" of the metal particles can be defined as follows by way of example.
[0072] For example, when a position near the surface of a porous carbon substrate on which metal particles are formed is referred to as the "lower part" and a position in a direction extending outward from the surface of the porous carbon substrate is referred to as the "upper part", the needle-shaped metal particles may have a morphology in which the upper radius is smaller than the lower radius and the ratio of the total length to the lower radius (L / D) is greater than 1.
[0073] Specifically, the L / D of the needle-shaped metal particles may be 1 or more. For example, the L / D of the needle-shaped metal particles may be 5 or more. The lower limit of the L / D ratio is the ratio of the metal particles in the needle-shaped morphology, and when L / D has a lower limit smaller than the above value, the electric field may be less strongly concentrated on the needle-shaped end (top) of the metal particle, and the initial nucleus of lithium sulfide may not be formed at the needle-shaped end (top), or the nucleation effect may not be obvious. In order to achieve the purpose of the present invention, L / D may preferably be 1 or more.
[0074] In addition, the upper limit of the L / D ratio is not limited to a specific range, and may be within any range for achieving the above-mentioned purpose. However, when the needle-shaped metal particles are too long, the particles may be easily broken and become brittle, and accordingly, for example, the upper limit of the L / D ratio may be preferably 50 or less, such as 25 or less, 20 or less, or 15 or less.
[0075] In one embodiment of the present invention, the L / D ratio of the needle-shaped metal particles may be 10, for example.
[0076] The size of the needle-shaped metal particles at each position can be measured by a method generally used to determine the size of metal fine particles, such as laser diffraction, electron microscopy, etc., and the measuring method is not particularly limited.
[0077] In one embodiment of the present invention, the size of the needle-shaped metal particles at each position may refer to, for example, a size at 50% in the cumulative particle size distribution.
[0078] In one embodiment of the present invention, the upper radius D of the needle-shaped metal particle 50 It can be less than 100 nm.
[0079] In one embodiment of the present invention, the lower radius D of the needle-shaped metal particle 50 It may be 100 nm to 1,000 nm.
[0080] In one embodiment of the present invention, the total length D of the needle-shaped metal particles is 50 It can be 1 μm to 10 μm.
[0081] In one embodiment of the present invention, the metal particles are characterized in that they have a controlled morphology as described above, and they are not limited to a specific material and may comprise any material having catalytic activity for enhanced kinetic activity in the oxidation / reduction reaction of sulfur-based materials as positive electrode active materials.
[0082] For example, the metal particles are not limited to a specific type, and may include transition metal particles that can be used in the positive electrode of a lithium-sulfur battery. The transition metal may include, for example, zinc (Zn), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), niobium (Nb), molybdenum (Mo), technetium (Tc), rubidium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), lanthanum (La), hafnium (Hf), tantalum (Ta), tungsten (W), osmium (Os), iridium (Ir), cerium (Ce), gallium (Gd), scandium (Sc), titanium (Ti), gallium (Ga), indium (In), or two or more thereof.
[0083] In one embodiment of the present invention, the transition metal included in the catalyst may include cobalt (Co).
[0084] In the present invention, because the carbon composite material contains needle-like metal particles, when used in an electrode, the electric field is concentrated at the top end of the needle-like metal particles. During the operation of a lithium-sulfur battery using the same, the initial nucleation of lithium sulfide can be spatially controlled. Therefore, the deposition of lithium sulfide can be induced to occur at the top end of the needle-like metal particles.
[0085] In one embodiment of the present invention, the porous carbon substrate is a substrate for growing metal particles and supporting a sulfur-based material, and may include a substrate used in a positive electrode of a lithium secondary battery without limitation.
[0086] For example, the porous carbon substrate may include carbon fiber cloth, carbon nanotubes (CNTs), graphene, graphene oxide (GO), reduced graphene oxide (rGO), carbon black, graphite, graphite nanofibers (GNFs), carbon nanofibers (CNFs), activated carbon fibers (ACFs), activated carbon, fullerenes, or mixtures thereof.
[0087] In one embodiment of the present invention, the porous carbon substrate may include carbon fibers.
[0088] In one embodiment of the present invention, the porous carbon substrate may include carbon cloth (also referred to as carbon fiber cloth).
[0089] The carbon composite material according to one embodiment of the present invention provides an electrode frame, and the carbon composite material for supporting an active material without including a current collector may be provided as an electrode, but the use of the carbon composite material is not limited thereto.
[0090] In one embodiment of the present invention, a porous carbon substrate is used as a host to provide a skeleton for uniformly and stably fixing a sulfur-based material used as a positive active material of a lithium-sulfur battery, thereby compensating for low conductivity of sulfur to enhance electrochemical reactions.
[0091] Thus, the porous carbon substrate may include a plurality of pores on the surface and inside thereof. In one embodiment of the present invention, the porous carbon substrate may have a diameter of 1,500 m 2 / g or more Brewer-Emmett-Teller (BET) specific surface area.
[0092] The carbon composite material according to the present invention can achieve high loading, low irreversible capacity and high energy density of sulfur-based materials due to the large BET specific surface area of the porous carbon substrate used as the main body of the sulfur-based material in the positive electrode. That is, an electrode having a structure for improving sulfur utilization in an electrochemical reaction and a lithium secondary battery including the same can be realized.
[0093] In another embodiment of the present invention, the porous carbon substrate can be produced by carbonizing a variety of carbon precursors.
[0094] electrode
[0095] According to another aspect of the present invention, there is provided an electrode comprising the carbon composite material as described above and a sulfur-based material.
[0096] In one embodiment of the present invention, an electrode including a sulfur-based material as an active material may be preferably used as a positive electrode.
[0097] The electrode may have a coating structure of the sulfur-based material on the entire or a portion of the surface of the carbon composite material.
[0098] In this case, in one embodiment of the present invention, the sulfur-based material may be supported in the pores of the porous carbon substrate in the carbon composite material and in the whole or at least a part of the surface of the porous carbon substrate in the carbon composite material.
[0099] In one embodiment of the present invention, the sulfur-based material may be deposited on at least a portion of the surface of the carbon composite material.
[0100] In one embodiment of the present invention, the sulfur-based material is not limited to a specific type and may include any type of sulfur-based material that contains a sulfur (S)-sulfur (S) bond in at least one of an oxidized state or a discharged state and can be used as a positive electrode active material for a lithium-sulfur battery.
[0101] The sulfur-based material may include, for example, at least one selected from the following: inorganic sulfur (S8); lithium sulfide (Li2S); lithium polysulfide (Li2S n, where \(1 < n\leq8\)); disulfide compounds such as 2,5-dimercapto-1,3,4-thiadiazole, 1,3,5-trithiocyanic acid; organic sulfur compounds; and carbon-sulfur polymers \((C_2S\) x ) n , where \(x = 2.5\) to \(50\) and \(n\geq2\).
[0102] In one embodiment of the present invention, the sulfur-based material may preferably comprise sulfur \((S_8)\), lithium sulfide \((Li_2S)\), polysulfide lithium \((Li_2S\) n , where \(1 < n\leq8)\) or a mixture thereof.
[0103] In one embodiment of the present invention, the sulfur-based material may comprise sulfur \((S_8)\), lithium sulfide \((Li_2S)\) or a mixture thereof.
[0104] In another embodiment of the present invention, the sulfur-based material may comprise polysulfide lithium \((Li_2S\) n , where \(1 < n\leq8)\) or a mixture thereof.
[0105] In one embodiment of the present invention, in order to achieve a high-capacity battery, based on 100% by weight of the electrode, the content of the sulfur-based material in the electrode may be more than 30% by weight, for example, more than 40% by weight, more than 50% by weight or more than 60% by weight, for example, more than 70% by weight. For example, based on 100% by weight of the electrode, the content of the sulfur-based material may be 40% to 80% by weight, 40% to 60% by weight or 40% to 50% by weight, but the present invention is not limited thereto.
[0106] In one embodiment of the present invention, the electrode may comprise a carbon composite material containing needle-shaped metal particles on a 3 cm × 4 cm porous carbon substrate, and may comprise a sulfur-based material, such as polysulfide lithium deposited on a part of the surface of the carbon composite material.
[0107] In the positive electrode active material according to the present invention, the sulfur-based material may be located on at least one surface of the pores of the porous carbon substrate or on the outer surface of the porous carbon substrate, and in this case, the sulfur-based material may be present in an area less than 100%, preferably 1% to 95%, more preferably 60% to 90% of the entire inner and outer surfaces of the porous carbon substrate. When the sulfur-based material is present on the surface of the porous carbon substrate within the above range, the maximum effect can be exhibited in terms of electron transport area and electrolyte wetting. Specifically, within the above range, since the sulfur-based material is thinly and uniformly impregnated into the surface of the porous carbon substrate, the electron transport contact area can be increased during charge and discharge.
[0108] The electrode can be made by simply mixing the sulfur material with the carbon composite to form a composite material or coating or loading it into a core-shell structure. The coating of the core-shell structure can include coating any of the sulfur material or the carbon composite on another material, such as covering the surface of the carbon composite with the sulfur material, or vice versa. In addition, the load can include filling the sulfur material in a porous carbon substrate of the carbon composite, especially filling it in the pores. The electrode can be in any form that satisfies the content ratio of the above-mentioned sulfur material to the carbon composite, and is not limited in the present invention.
[0109] As described above, according to one embodiment of the present invention, the sulfur-based material may preferably be deposited on at least a portion of the surface of the carbon composite material. More specifically, the carbon composite material comprises needle-shaped metal particles on a porous carbon substrate, in which case the sulfur-based material may be deposited on at least a portion of the surface of the needle-shaped metal particles. More preferably, the sulfur-based material may be deposited on the upper portion of the needle-shaped metal particles in a spatially specific manner (in this case, the area near the porous carbon substrate is referred to as the lower portion, and the position in the direction of the needle-shaped morphology growth is referred to as the upper portion).
[0110] An electrode using the sulfur-carbon composite material according to one embodiment of the present invention has a structure that increases sulfur loading and sulfur utilization, thereby enhancing the electrochemical reactivity of sulfur and improving accessibility and contact with an electrolyte, resulting in improvements in capacity and life characteristics of lithium-sulfur batteries.
[0111] In one embodiment of the present invention, the above-mentioned electrode may be a positive electrode, and in this case, the positive electrode may further include a positive electrode current collector.
[0112] However, as described above, according to one embodiment of the present invention, the electrode may include only the porous carbon substrate without including a current collector, and preferably, may not include a current collector.
[0113] According to one embodiment of the present invention, the positive electrode may not include a current collector, for example, a positive electrode active material including a carbon composite material and a sulfur-based material itself may be used as the positive electrode.
[0114] In addition, in addition to the above-mentioned sulfur-based materials, the positive electrode may further include at least one additive selected from the following: transition metal elements, group IIIA elements, group IVA elements, compounds of these elements with sulfur, and alloys of these elements with sulfur as a positive electrode active material. In a specific embodiment of the present invention, the positive electrode active material layer may include a lithium transition metal composite oxide represented by the following [Chemical Formula 1].
[0115] [Chemical formula 1]
[0116] Li a Ni b Co c M1 d M 2 e O2
[0117] In the above chemical formula 1, M 1 It may be Mn, Al or a combination thereof, preferably Mn or Mn and Al.
[0118] M 2 It may be at least one selected from Zr, W, Y, Ba, Ca, Ti, Mg, Ta and Nb, preferably at least one selected from Zr, Y, Mg and Ti, more preferably Zr, Y or a combination thereof. 2 It is not essential, but when it is included in an optimum amount, it may play a role in promoting the growth of grains during sintering or improving the stability of the crystal structure.
[0119] On the other hand, in one embodiment of the present invention, when the positive electrode includes a current collector, the positive electrode current collector may include various positive electrode current collectors used in the corresponding technical field. For example, the positive electrode current collector may include: stainless steel, aluminum, nickel, titanium, sintered carbon; aluminum or stainless steel treated with carbon, nickel, titanium or silver on the surface, etc. The thickness of the positive electrode current collector may generally be 3 μm to 500 μm, and may have fine concavoconvexities on the surface to increase the adhesion strength of the positive electrode active material. The positive electrode current collector may have various forms, such as films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc.
[0120] In one embodiment of the present invention, the electrode may further comprise a binder and / or a conductive material in addition to the carbon composite material.
[0121] The binder plays a role in improving the adhesion between the porous carbon substrate and the metal particles, and specific examples may include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene rubber (EPDM rubber), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber or its various copolymers, used alone or in combination. Based on the gross weight of the electrode, the content of the binder may be 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight.
[0122] When a conductive material is included, it is used to provide conductive properties to the electrode, and may include but is not limited to any conductive material having the ability to conduct electrons without causing any chemical changes in the corresponding battery. Specific examples may include the following substances used alone or in combination: graphite such as natural graphite or artificial graphite; carbon materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, carbon nanotubes, etc.; metal powders or metal fibers such as copper, nickel, aluminum, silver, etc.; conductive whiskers such as zinc oxide, potassium titanate, etc.; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. When a conductive material is included, the content of the conductive material may generally be 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the electrode.
[0123] Lithium secondary battery
[0124] The present invention provides a lithium-sulfur battery, the lithium-sulfur battery comprising:
[0125] An electrode assembly, the electrode assembly comprising a positive electrode comprising the carbon composite material; and
[0126] Electrolytes.
[0127] The electrode assembly includes a positive electrode, a negative electrode, and a separator between the positive electrode and the negative electrode.
[0128] The electrode assembly may have, for example, a stacked or stacked / folded structure including a negative electrode and a positive electrode stacked with a separator interposed therebetween, or a jelly-roll structure including a negative electrode and a positive electrode wound together with a separator. In addition, in the jelly-roll structure, an additional separator may be placed outside to prevent contact between the negative electrode and the positive electrode.
[0129] The negative electrode includes a negative electrode current collector and a negative electrode active material layer on at least one surface of the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, a conductive material, and a binder.
[0130] negative electrode
[0131] The negative electrode will be described in more detail below.
[0132] The negative electrode may include a long sheet-shaped negative electrode current collector and a negative electrode active material layer on one or both surfaces of the negative electrode current collector, and the negative electrode active material layer may include a negative electrode active material, a binder, and optionally a conductive material.
[0133] Specifically, the negative electrode can be manufactured by coating a negative electrode slurry on one or both surfaces of a long sheet of negative electrode current collector, then removing the solvent from the negative electrode slurry by drying, and rolling. The negative electrode slurry is prepared by dispersing a negative electrode active material, a binder, and an optional conductive material in a solvent such as dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone, and water. On the other hand, a negative electrode including an uncoated portion can be manufactured by not coating a portion of the negative electrode current collector, such as an end portion of the negative electrode current collector, with the negative electrode slurry when coating the negative electrode slurry.
[0134] The negative electrode active material may include: a material capable of reversibly inserting or deinserting lithium (Li + ) material; a material capable of reversibly forming a lithium-containing compound by reacting with lithium ions; lithium metal; or a lithium alloy. The material capable of reversibly inserting or extracting lithium ions may include, for example, crystalline carbon, amorphous carbon, or a mixture thereof, specifically, may include, for example, artificial graphite, natural graphite, graphitizable carbon fiber, amorphous carbon, soft carbon, hard carbon, etc., but is not limited thereto. The material capable of reversibly forming a lithium-containing compound by reacting with lithium ions may include, for example, tin oxide, titanium nitrate, or a silicon compound. The lithium alloy may include, for example, an alloy of lithium (Li) and a metal selected from sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al), and tin (Sn). Preferably, the negative electrode active material may be lithium metal, specifically, in the form of lithium metal foil or lithium metal powder. The silicon-based negative electrode active material may include Si, Si-Me alloy (wherein Me is at least one selected from Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti and Ni), SiO y (wherein 0<y<2), Si-C composite material or a combination thereof, preferably SiO y (where 0<y<2) Since the silicon-based negative electrode active material has a high theoretical capacity, when the silicon-based negative electrode active material is included, the capacity characteristics can be improved.
[0135] In one embodiment of the present invention, the negative electrode may include lithium metal or lithium alloy, and specifically may be lithium metal foil or lithium alloy foil.
[0136] In one embodiment of the present invention, when a lithium metal foil or a lithium alloy foil is used as the negative electrode, the negative electrode may be a self-standing lithium metal foil or lithium alloy foil without a current collector.
[0137] The negative electrode current collector may include a negative electrode current collector commonly used in the corresponding technical field, and may include, for example: copper, stainless steel, aluminum, nickel, titanium, sintered carbon; copper or stainless steel treated with carbon, nickel, titanium or silver on the surface; aluminum-cadmium alloy, etc. The thickness of the negative electrode current collector may generally be 3 to 500 μm, and in the same manner as the positive electrode current collector, may have fine concave-convex on the surface to enhance the bonding strength of the negative electrode active material. For example, the negative electrode current collector may have various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam, a non-woven fabric, etc.
[0138] The binder serves to attach the negative electrode active material particles to each other and improve the bonding strength between the negative electrode active material and the negative electrode current collector. Specific examples may include the following substances used alone or in combination: polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene rubber (EPDM rubber), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber or its various copolymers. Based on the gross weight of the negative electrode active material layer, the content of the binder may be 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight.
[0139] The conductive material is used to provide conductive properties to the negative electrode, and may include, but is not limited to, any conductive material that has the ability to conduct electrons without causing any chemical changes in the corresponding battery. Specific examples may include the following substances used alone or in combination: graphite such as natural graphite or artificial graphite; carbon materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, carbon nanotubes, etc.; metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive whiskers such as zinc oxide, potassium titanate, etc.; conductive metal oxides such as titanium oxide, etc.; or conductive polymers such as polyphenylene derivatives, etc. When a conductive material is used, the content of the conductive material can generally be 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.
[0140] Diaphragm
[0141] On the other hand, the electrode assembly also includes a diaphragm, which is between the negative electrode and the positive electrode in the electrode assembly. The diaphragm can separate the negative electrode from the positive electrode and provide a mobile channel for lithium ions, and can include but is not limited to any type of diaphragm commonly used in lithium secondary batteries. Specifically, the diaphragm can include: a porous polymer film, such as a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a stacked structure of more than two layers thereof. In addition, commonly used porous non-woven fabrics can be used, such as non-woven fabrics made of high melting point glass fibers, polyethylene terephthalate fibers, etc. In addition, a coated diaphragm comprising a ceramic or polymer material can be used to ensure heat resistance or mechanical strength.
[0142] Another aspect of the present invention relates to an electrochemical device including an electrode assembly. The electrochemical device includes a battery case containing the electrode assembly and an electrolyte, and the battery case is not limited to a specific type and can be appropriately selected from any type of battery case commonly used in the corresponding technical field, such as a bag type, a metal can type, etc.
[0143] Electrolytes
[0144] According to one aspect of the present invention, the electrolyte used in the lithium secondary battery can include various electrolytes that can be used in the lithium secondary battery. The electrolyte is not limited to a specific type, and can include, for example, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel polymer electrolyte, a solid inorganic electrolyte, and a molten inorganic electrolyte.
[0145] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0146] The organic solvent may include, but is not limited to, any type of organic solvent that can act as a medium for the movement of ions involved in the electrochemical reaction of the battery. Specifically, the organic solvent may include: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; ether solvents such as dibutyl ether, tetrahydrofuran, etc.; ketone solvents such as cyclohexanone, etc.; aromatic hydrocarbon solvents such as benzene, fluorobenzene, etc.; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), etc.; alcohol solvents such as ethanol, isopropanol, etc.; R-CN nitrile (R is a C2-C20 straight chain, branched or cyclic hydrocarbon, and may contain a double bond, an aromatic ring or an ether bond); amides such as dimethylformamide, etc.; dioxolanes such as 1,3-dioxolanes, etc.; or cyclopentane sulfone.
[0147] On the other hand, in one embodiment of the present invention, it is desirable to include a heterocyclic compound containing an oxygen atom or a sulfur atom to form a polymer protective layer so as to inhibit the generation of lithium dendrites and prevent electrolyte decomposition and side reactions on the surface of the lithium metal. The heterocyclic compound may include a 3- to 15-membered, preferably a 3- to 7-membered, more preferably a 5- and 6-membered heterocyclic compound.
[0148] The heterocyclic compound may include: a substituted or unsubstituted heterocyclic compound having at least one selected from a C1-C4 alkyl group, a C3-C8 cycloalkyl group, a C6-C10 aryl group, a halogen group, a nitro group (-NO2), an amine group (-NH2) and a sulfonyl group (-SO2); or a polycyclic compound of a heterocyclic compound and at least one selected from a C3-C8 cycloalkyl group and a C6-C10 aryl group.
[0149] When the heterocyclic compound is a substituted heterocyclic compound having a C1-C4 alkyl group, the free radical is preferably stable, thereby suppressing the side reaction between the additive and the electrolyte. In addition, when the heterocyclic compound is a substituted heterocyclic compound having a halogen group or a nitro group, preferably, a functional protective layer can be formed on the surface of the lithium metal. The functional protective layer can be a stable and dense protective layer, and can make the lithium metal uniformly deposited and suppress the side reaction between the polysulfide and the lithium metal.
[0150] Specifically, the heterocyclic compound may, for example, contain at least one selected from the following: furan, 2-methylfuran, 3-methylfuran, 2-ethylfuran, 2-propylfuran, 2-butylfuran, 2,3-dimethylfuran, 2,4-dimethylfuran, 2,5-dimethylfuran, pyran, 2-methylpyran, 3-methylpyran, 4-methylpyran, benzofuran, 2-(2-nitrovinyl)furan, thiophene, 2-methylthiophene, 2-ethylthiophene, 2-propylthiophene, 2-butylthiophene, 2,3-dimethylthiophene, 2,4-dimethylthiophene and 2,5-dimethylthiophene, preferably at least one selected from 2-methylfuran and 2-methylthiophene.
[0151] The lithium salt may include, but is not limited to, any compound that provides lithium ions used in lithium secondary batteries. Specifically, the lithium salt may include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiBr, LiCl, LiI, LiTf or LiB(C2O4)2. The concentration of the lithium salt may preferably be in the range of 0.1 to 5.0 M and preferably 0.1 to 3.0 M. When the concentration of the lithium salt is included in the above range, the electrolyte may have appropriate conductivity and viscosity and exhibit excellent electrolyte performance, which contributes to the effective movement of lithium ions.
[0152] In one embodiment of the present invention, preferably, the lithium salt may include LiBr, LiCl, LiI, LiTf or a mixture thereof. When the lithium salt includes the above lithium salt, it may have a favorable effect on the solubility of lithium sulfide, thereby preventing the deposition of lithium sulfide in the electrode of the lithium-sulfur battery.
[0153] In particular, the lithium secondary battery can have a synergistic effect of improving the performance of the lithium-sulfur battery by inducing the deposition of lithium sulfide at a specific location and inhibiting the deposition through a combination of a carbon composite material containing needle-shaped metal particles in the positive electrode and LiBr, LiCl, LiI, LiTf or a mixture thereof in the electrolyte, but the present invention is not limited thereto.
[0154] For example, even if a positive electrode including the above-described carbon composite material is used, when a composition having high solubility for lithium sulfide is used in an electrolyte, the spatial control effect of the carbon composite material on lithium sulfide deposition may be low.
[0155] From this perspective, according to one embodiment of the present invention, the lithium salt may include LiBr.
[0156] In addition to the above-mentioned electrolyte constituents, the electrolyte may also contain additives to improve the life characteristics of the battery, prevent the capacity decay of the battery and improve the discharge capacity of the battery. For example, the additives may include the following substances used alone or in combination: LiNO3, halogenated alkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, (condensed) glycol dimethyl ethers, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted The additive may be present in an amount of 0.1 to 10 wt %, preferably 0.1 to 5 wt %, based on the total weight of the electrolyte.
[0157] As described above, the lithium secondary battery according to the present invention may be a lithium-sulfur battery.
[0158] The lithium-sulfur battery is not limited to a specific shape and may have various shapes such as a cylindrical type, a stacked type, a coin type, and the like.
[0159] In addition, the present invention provides a battery module including a lithium-sulfur battery as a unit cell. The battery module can be used as a power source for medium and large-sized devices requiring high temperature stability, long cycle characteristics, and high capacity characteristics.
[0160] Examples of medium and large devices may include devices that work using power generated by electric motors, such as: power tools; electric vehicles, including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc.; electric two-wheeled vehicles, including electric bicycles and electric scooters; electric golf carts; energy storage systems, etc., but are not limited to these.
[0161] In the following, examples are given to help understand the present invention, but the following examples are provided for describing the present invention in an illustrative manner, and it is obvious to those skilled in the art that various variations and changes can be made without departing from the scope and technical aspects of the present invention, and such variations and changes fall within the scope of the appended claims.
[0162] [Manufacturing of carbon composite materials]
[0163] Comparative Example 1. Preparation of bare CC carbon composite material
[0164] A commercially available carbon fiber cloth (Cetech, WOS1011) made of carbon fibers having a diameter of several µm was washed with ethanol and distilled water.
[0165] Example 1. Preparation of CC@CoP1 carbon composite material
[0166] A carbon composite material containing needle-shaped metal particles was synthesized on a 3 cm×4 cm area of the carbon fiber cloth prepared in Comparative Example 1 by dissolving 0.595 g of cobalt chloride hydrate, 0.13 g of ammonium fluoride and 0.27 g of urea (mass ratio of cobalt chloride hydrate: ammonium fluoride: urea = 4.6:1:2) in 40 mL of distilled water and causing a hydrothermal reaction at 100°C for 12 hours using water as a solvent.
[0167] The carbon composite material includes needle-shaped cobalt metal particles, the cobalt metal particles having a lower radius of 500 nm, an upper radius of 100 nm, a total length of 5 µm, and a total length / lower radius ratio (L / D) of 10.
[0168] Comparative Example 2. Preparation of CC@CoP2 carbon composite material
[0169] A carbon composite material was manufactured in the same manner as in Example 1, except that hydrated cobalt chloride was not used as the cobalt precursor and was replaced with cobalt acetate, and a solvothermal reaction was performed using methanol at 170° C. for 6 hours.
[0170] It was confirmed that the carbon composite material contained metal cobalt particles on the surface of the carbon fiber cloth, but the metal cobalt particles were not in a needle-like form but in a particle form.
[0171] [Manufacturing of electrodes]
[0172] Sulfur was loaded on the carbon composite material according to Example 1, Comparative Example 1 or Comparative Example 2 by dropwise addition of 0.2 M Li2S8 solution (Li2S:S8 molar ratio of 1:0.875 in DME) to produce a positive electrode (sulfur (S8) content: 45 wt % based on the total weight of the positive electrode).
[0173] For the negative electrode, a 35 µm thick lithium metal foil was used. For the separator, porous polyethylene was used. The electrolyte was prepared by adding 3 wt% LiNO3 to a mixed organic solvent of 2-methylfuran and dimethoxyethanol (volume ratio 33 / 77). In the experiments, as the lithium salt, 1M LiBr or 1M LiTFSI was used.
[0174] The positive electrode and the negative electrode prepared as described above were placed with a separator interposed therebetween, and the prepared electrolyte was injected to manufacture a pouch-shaped battery.
[0175] Table 1 below summarizes the types of carbon composites and lithium salts used to make batteries.
[0176]
[0177] Experimental Example 1. Evaluation of discharge capacity and life characteristics
[0178] The prepared lithium-sulfur batteries were discharged in CC mode at 0.5C at 25°C to 1.8 V and then charged at a constant current of 0.3C to 2.5 V, and their discharge capacities were measured / compared. The discharge capacity (mAh / g (sulfur weight)) was measured based on the sulfur content.
[0179] The measurement results are shown in Figure 1 and Figure 2 middle.
[0180] according to Figure 1 and Figure 2Compared with the batteries of Comparative Examples 3 and 4 having the same electrolyte composition, the batteries of Examples 2 and 3 using a carbon composite material containing needle-shaped cobalt metal particles as the sulfur main body in the positive electrode have more excellent discharge capacity and life characteristics.
[0181] This indicates that according to one embodiment of the present invention, when an active material such as lithium sulfide (Li2S) is supported on a porous carbon substrate containing grown needle-like metal particles, the deposition of lithium sulfide on the electrode is spatially controlled, resulting in improved discharge capacity and life characteristics compared to the uncontrolled deposition of lithium sulfide (Comparative Example 3, Comparative Example 4).
[0182] Lithium sulfide is electrically insulating and acts as a resistor on the electrode, and the deposition of lithium sulfide on the electrode surface is spatially controlled so that the lower portion of the electrode having a needle-like structure is not covered by lithium sulfide, thereby making the lower portion of the electrode a continuous electron supply source. Therefore, the sulfur utilization in the electrode can be increased, thereby improving the discharge capacity and life characteristics.
[0183] On the other hand, refer to Figure 1 and Figure 2 It was confirmed that the batteries of Example 2 and Comparative Example 3 using LiBr as the lithium salt in the electrolyte had more excellent discharge capacity and life characteristics than those of Example 3 and Comparative Example 4 using LiTFSI as the lithium salt, respectively.
[0184] It is inferred that the LiBr-containing electrolyte has a higher solubility for LiS than the LiTFSI-containing electrolyte, thus providing a higher spatial control over the deposition of LiS.
[0185] Experimental Example 2. Evaluation of resistance characteristics
[0186] The prepared lithium-sulfur battery was discharged to the same amount and the impedance curve was measured. The results are shown in Figure 3 middle.
[0187] Reference Figure 3 , resistance component analysis confirmed that the increase in discharge capacity was due to the effective deposition control of electrically insulating lithium sulfide. Figure 3 As a result, the needle-structured electrode exhibits the lowest resistance component when used with an electrolyte that has a high solubility for lithium sulfide.
[0188] It was confirmed that through effective control of lithium sulfide deposition, the resistance layer of lithium sulfide was significantly reduced, thereby alleviating the overvoltage during battery operation and significantly improving the discharge capacity.
[0189] Experimental Example 3. Observation of Lithium Sulfide Deposition Morphology
[0190] In the batteries according to Example 2 and Example 3, after lithium polysulfide was deposited on the electrode, the morphology was observed by electron microscopy (FEI Company, Magellan 400, ×3500 magnification). The observation results are shown in Figure 4 and 5 middle.
[0191] Reference Figure 4 and 5 First, it was confirmed that the positive electrodes used in Examples 2 and 3 contained a needle-shaped carbon composite material. However, by looking at the deposition morphology of lithium sulfide on the carbon composite material, it was confirmed that, in Example 2, lithium sulfide was deposited only on the upper part of the electrode and the lower part of the electrode in the needle-shaped form was not covered with lithium sulfide, while in Example 3, the entire area of the needle-shaped electrode from top to bottom was covered with lithium sulfide.
[0192] According to Example 2, the surface of the electrode as the electron supply source is not covered with non-conductive lithium sulfide, and thus the electrode passivation suppressing effect of lithium sulfide can be expected.
[0193] also, Figure 7 The electron microscope observation result of the shape of the carbon composite material according to Comparative Example 5 is shown in FIG. Figure 8 Observations of lithium sulfide deposition are shown in .
[0194] according to Figure 7 and Figure 8 It was confirmed that the carbon composite material used in Comparative Example 5 contained cobalt metal particles on a porous carbon substrate, but the morphology was not needle-shaped and was a predetermined grain morphology. In addition, it was confirmed that LiBr was used as a lithium salt in the electrolyte, but since the initial deposition position of lithium sulfide could not be controlled, lithium sulfide was deposited on the entire surface of the carbon composite material.
[0195] Experimental Example 4. Surface observation of metal particles after lithium sulfide deposition
[0196] After a series of experiments in which lithium sulfide was deposited on metal particles of carbon composites, the surface characteristics of the metal particles were analyzed by X-ray photoelectron spectroscopy (XPS). The results are shown in Figure 6 middle.
[0197] As previously passed Figure 4 and Figure 5 It was confirmed that cobalt particles formed in a needle-like morphology were found in the electrodes according to Examples 2 and 3 after lithium sulfide deposition.
[0198] In contrast, reference Figure 6, all Co-P and Co-O peaks of cobalt metal particles (CoP) showing needle-like morphology after lithium sulfide deposition were not observed in Example 3, while these two peaks were clearly observed in Example 2.
[0199] Thus, as shown in the deposition morphology of lithium sulfide Figure 4 and Figure 5 It can be seen that it is confirmed that the surface of the electrode according to Example 3 is covered with lithium sulfide, while the surface of the electrode according to Example 2 has some areas that are not covered with lithium sulfide.
[0200] Therefore, both surface image observation and surface analysis confirmed that the deposition of lithium sulfide can be effectively controlled.
Claims
1. A carbon composite material, comprising: a porous carbon substrate; and metal particles on at least a portion of the surface of the porous carbon substrate, in, The metal particles are in needle-like form.
2. The carbon composite material according to claim 1, wherein The position near the surface of the porous carbon substrate where the metal particles are formed is designated as the lower part, and the position in the direction extending outward from the surface of the porous carbon substrate is designated as the upper part, then the needle-shaped metal particles have a morphology in which the upper radius is smaller than the lower radius and L / D is greater than 1, wherein L / D is the ratio of the total length to the lower radius.
3. The carbon composite material according to claim 2, wherein: The L / D of the needle-shaped metal particles is 5 or more.
4. The carbon composite material according to claim 2, wherein: The upper radius (D 50 ) is less than 100nm.
5. The carbon composite material according to claim 2, wherein: The lower radius (D 50 ) is 100nm to 1,000nm.
6. The carbon composite material according to claim 2, wherein: The total length (D 50 ) is 1 µm to 10 µm.
7. The carbon composite material according to claim 1, wherein The metal particles include transition metal particles.
8. The carbon composite material according to claim 1, wherein The porous carbon substrate comprises carbon fiber cloth, carbon nanotubes (CNTs), graphene, graphene oxide (GO), reduced graphene oxide (rGO), carbon black, graphite, graphite nanofibers (GNF), carbon nanofibers (CNF), activated carbon fibers (ACF), activated carbon, fullerene, or two or more of these materials.
9. An electrode, comprising: The carbon composite material according to any one of claims 1 to 8; and Sulfur materials.
10. The electrode according to claim 9, wherein The sulfur-based material covers all or part of the surface of the carbon composite material.
11. A lithium secondary battery, comprising: an electrode assembly, the electrode assembly comprising a positive electrode, a negative electrode, and a separator between the positive electrode and the negative electrode; and Electrolytes, in, The positive electrode is the electrode according to claim 9.
12. The lithium secondary battery according to claim 11, wherein The electrolyte includes LiBr, LiCl, LiI, LiTf or a mixture thereof as a lithium salt.
13. The lithium secondary battery according to claim 11, wherein The lithium secondary battery is a lithium-sulfur battery.
14. A method for producing the carbon composite material according to any one of claims 1 to 8, the method comprising the following steps: mixing a metal chloride hydrate, ammonium fluoride, and urea to prepare a metal particle precursor solution; and While the porous carbon substrate is in contact with the metal particle precursor solution, needle-shaped metal particles are formed on at least a portion of the surface of the porous carbon substrate by a hydrothermal reaction.
15. The method for producing a carbon composite material according to claim 14, wherein: The metal chloride hydrate is a transition metal chloride hydrate.