Positive electrode material and preparation method thereof

In the preparation of sodium ion battery positive electrode material, the coordinated method of water medium mixing and spray drying and sintering was used to solve the problem of uneven mixing between Na, M and PO4, and a positive electrode material with high purity and high electrochemical performance was prepared. , improves the performance of sodium ion batteries and reduces production costs.

CN118993013AActive Publication Date: 2024-11-22MICRO-NANO (NINGBO) ELECTRONIC MATERIALS CO LTD

Patent Information

Application Number
CN202411143626.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

In the existing preparation method of polyanionic cathode materials for sodium ion batteries, uniform mixing between Na, M and PO4 is difficult to achieve, resulting in the generation of a large number of heterogeneous phases, affecting the electrochemical performance of the material.

Method used

Through the special design of the raw materials, the coordinated combination of mixing, spray drying and sintering was used to prepare a high-purity positive electrode material Na4M3-3δN6δ/m(PO4)2P2O7, where N is a doped metal element and M is a transition metal element. Water is used as a medium for mixing and stirring, spray drying and sintering steps to ensure uniform distribution of sodium ions and stable presence of transition metal elements.

Benefits of technology

It has achieved the preparation of positive electrode materials with high purity and excellent electrochemical performance, which has significantly improved the discharge capacity and circulation performance of sodium ion batteries, reduced production costs, and has the prospect of large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993013A_ABST
    Figure CN118993013A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sodium ion batteries, in particular to a positive electrode material and a preparation method thereof. The preparation method comprises the following steps: a mixing step: weighing a certain amount of raw material X and a certain amount of raw material Y, placing the raw material X and the raw material Y in a container filled with water, mixing and stirring to obtain slurry A, and grinding to obtain precursor slurry B; a spray drying step: placing the precursor slurry B in spray drying equipment for spray drying treatment to obtain precursor powder C; and a sintering step: putting the precursor powder C into sintering equipment for sintering treatment to obtain the positive electrode material. Through special design of the raw materials and synergistic cooperation of mixing, spray drying and sintering, the positive electrode material with relatively high purity and relatively good electrochemical performance can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a positive electrode material and a preparation method thereof. Background Art

[0002] Lithium-ion batteries with high energy density and long cycle life have been widely used in the two major fields of energy storage and power batteries. With the rapid development of the two major fields, lithium resources have gradually become scarce, becoming a "bottleneck" problem in the development of lithium-ion batteries in my country. Sodium, which has a high abundance (2.3%), is in the same main group as lithium, and the two have similar electrochemical properties, so sodium-ion batteries can be developed to replace lithium-ion batteries. With the soaring price of lithium resources and the increasing scarcity of resources, the research and development and industrialization of sodium-ion batteries will have great social significance and commercial value.

[0003] Sodium-ion batteries have the advantage of low cost and strong competitive advantages in certain market segments. Its industrialization can alleviate the shortage of lithium resources to a certain extent. Therefore, the research and development of sodium-ion battery electrode materials has become a hot spot in the research of new energy materials. Polyanion cathode materials have attracted much attention due to their low cost, good cycle stability and high safety.

[0004] At present, the commonly used methods for preparing polyanion positive electrode materials for sodium ion batteries are solid phase ball milling and liquid phase process. However, the solid phase ball milling process cannot ensure the uniform mixing of Na, M and PO4, resulting in the generation of a large number of impurities in the final product, which affects the electrochemical performance of the material; the liquid phase process is accompanied by the generation of a variety of phosphate metal salt precipitates during the mixing process, which will also cause uneven mixing between Na, M and PO4, resulting in the generation of a large number of impurities in the final product, affecting the electrochemical performance of the material.

[0005] Therefore, providing a new method for preparing a positive electrode material for a sodium ion battery to solve the above-mentioned defects is an urgent problem to be solved. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a positive electrode material and a method for preparing the same. The present application can prepare a positive electrode material with higher purity and better electrochemical performance through special design of raw materials, and coordinated coordination of mixing, spray drying and sintering.

[0007] To achieve the above-mentioned object, the first aspect of the present application provides a method for preparing a positive electrode material, wherein the molecular formula of the positive electrode material is Na4M 3-3δ N 6δ / m (PO4)2P2O7, where N is a doping metal element and the valence state of N is m +, M is a transition metal element, and 0≤δ≤0.3, the preparation method of the positive electrode material comprises the following steps:

[0008] Mixing step: weigh a certain amount of raw material X and raw material Y, place them in a container filled with water, mix and stir to obtain slurry A, and then grind to obtain precursor slurry B;

[0009] Spray drying step: placing the precursor slurry B in a spray drying device for spray drying to obtain a precursor powder C;

[0010] Sintering step: placing the precursor powder C in a sintering device for sintering to obtain a positive electrode material;

[0011] The X raw material is a substance that is not easily soluble in water and contains a transition metal element M, the Y raw material is a substance that is easily soluble in water and contains an element Na, and at least one of the X raw material and the Y raw material contains an element P.

[0012] In the above preparation method, especially in the mixing step, the raw materials are mixed and stirred with water as a medium. In the design of the raw materials, the X raw material is a substance that is not easily soluble in water and contains the transition metal element M. Therefore, the X raw material is added to the aqueous solution to form dispersed tiny particles, and the Y raw material is a substance that is easily soluble in water and contains the element Na. The Y raw material is added to the aqueous solution to form sodium ions. Under the action of external force, the uniform distribution of sodium ions on the surface of the X raw material can be accelerated; further, after the mixing step, through the coordinated cooperation between the spray drying step, the pretreatment step, and the sintering step, a positive electrode material product with higher purity can be obtained.

[0013] In some embodiments, the X raw material is one or more compounds containing transition metal M and element P, and the solubility product K of the corresponding anhydrous compound is sp ≤1.0×10 -25 .

[0014] In some embodiments, the Y raw material is a compound containing one or more of the element Na and the element P, and the solubility of the corresponding anhydrous compound is ≥3 g / 100 g water.

[0015] In some embodiments, both the X raw material and the Y raw material contain the element P.

[0016] In some embodiments, in the X raw material, the stoichiometric ratio of the transition metal element M to the element P is 3:2.

[0017] Furthermore, the molecular formula of the anhydrous compound of the X raw material is M3(PO4)2.

[0018] Further preferably, the X raw material is selected from one or more of Mn3(PO4)2.yH2O (0≤y≤7), Fe3(PO4)2.z1H2O (0≤z1≤8), Ni3(PO4)2.z2H2O (0≤z2≤8), and Co3(PO4)2.z3H2O (0≤z3≤8).

[0019] Further preferably, the X raw material is selected from Mn3(PO4)2.yH2O (0≤y≤7) and / or Fe3(PO4)2.z1H2O (0≤z1≤8).

[0020] Further preferably, the X raw material is selected from Mn3(PO4)2·3H2O and Fe3(PO4)2·8H2O.

[0021] In some embodiments, in the Y raw material, the stoichiometric ratio of element Na to element P is 2:1.

[0022] In some embodiments, the Y raw material is selected from one or more of NaOH, Na2C2O4, CH3COONa, Na2CO3, NaHCO3, Na4P2O7, Na3HP2O7, Na2H2P2O7, NaH3P2O7, H4P2O7, Na2HPO4, NaH2PO4, Na3PO4, H3PO4, NH4H2PO4, (NH4)2HPO4 and (NH4)3PO4.

[0023] Further preferably, the Y raw material is selected from Na4P2O7 and / or Na2HPO4.

[0024] In some embodiments, in the mixing step, the mass proportion of raw material X is ≥ 15%.

[0025] More preferably, the mass proportion of raw material X is ≤80%.

[0026] In some embodiments, in the mixing step, the mass proportion of raw material Y is ≥ 20%.

[0027] More preferably, the mass proportion of raw material Y is ≤70%.

[0028] In some embodiments, the mixing step further includes: one or more of a modifying additive, a phosphorus source supplement, a carbon source, a dispersant, and a viscosity reducer.

[0029] In some embodiments, the mixing step further includes adding a modifying additive, wherein the modifying additive includes the doping metal element N, wherein the doping metal element N is another metal element different from the transition metal element M.

[0030] Preferably, the doping metal element N is selected from one or more of Mg, Al, Ti, V, Zn, Zr, Cr and Cu.

[0031] More preferably, the molecular formula of the modifying additive is N 6 / m m+ (PO4)2.

[0032] More preferably, in the mixing step, the weight proportion of the modifying additive is ≥ 1%. Even more preferably, the weight proportion of the modifying additive is ≤ 20%.

[0033] In some embodiments, in the mixing step, a phosphorus source supplement is also included. The phosphorus source supplement is one or more of a single substance, a compound or a solution containing element P.

[0034] Preferably, the phosphorus source supplement is selected from one or more of H3PO4, NH4H2PO4, (NH4)2HPO4.

[0035] More preferably, in the mixing step, the mass proportion of the phosphorus source supplement is ≥ 1%. Even more preferably, the mass proportion of the phosphorus source supplement is ≤ 20%.

[0036] In some embodiments, the particle size D50 of the precursor slurry B after grinding is 300-800 nm.

[0037] Preferably, the particle size D50 of the precursor slurry B is 300-600 nm; more preferably 300-450 nm.

[0038] In some embodiments, a pretreatment step is further included. The pretreatment step is located before the sintering step. The pretreatment step includes: placing the precursor powder C in an ammonia solution for treatment.

[0039] In some embodiments, in the pretreatment step, the mass percentage concentration of the aqueous ammonia solution is 2-10%.

[0040] In some embodiments, in the pretreatment step, the pretreatment time is 2-15 hours.

[0041] In some embodiments, in the spray drying step, the inlet temperature of the spray drying equipment is 180-300°C, preferably 190-220°C.

[0042] In some embodiments, in the spray drying step, the outlet temperature of the spray drying equipment is 80-130°C, preferably 90-110°C.

[0043] In some embodiments, in the sintering step, the temperature range of the sintering treatment is 300-800°C; preferably, the temperature range is 450-800°C; more preferably, 450-750°C.

[0044] In some embodiments, in the sintering step, the sintering treatment time is 3-20 hours, preferably 10-20 hours.

[0045] In some embodiments, in the sintering step, the heating rate of the sintering equipment is 5-10° C. / min.

[0046] The second aspect of the present application provides a positive electrode material, which is prepared according to the preparation method of the positive electrode material.

[0047] The third aspect of the present application provides a sodium ion battery, which includes the positive electrode material provided by the second aspect of the present application.

[0048] A fourth aspect of the present application provides a battery module, which includes the sodium ion battery provided by the third aspect of the present application.

[0049] The fifth aspect of the present application provides an electrical device, which includes at least one selected from the positive electrode material of the second aspect of the present application, the sodium ion battery of the third aspect of the present application, or the battery module of the fourth aspect of the present application.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] 1. This application can prepare positive electrode materials with high purity and good electrochemical performance through special design of raw materials, as well as coordinated coordination of mixing, spray drying and sintering;

[0052] 2. The preparation method provided in this application is simple to operate, has low production cost, and has prospects for large-scale production.

[0053] 3. The sodium ion battery provided in this application can significantly improve the discharge capacity and cycle performance of the battery due to the high purity of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 This is a process flow chart for preparing the positive electrode material of the present invention;

[0055] Figure 2 XRD diagram of the positive electrode material Na4Fe3(PO4)2P2O7 prepared in Example 1 of the present invention;

[0056] Figure 3 This is a SEM image of the positive electrode material Na4Fe3(PO4)2P2O7 prepared in Example 1 of the present invention;

[0057] Figure 4 The charge and discharge curves of the sodium ion battery prepared in Example 1 of the present invention at different rates;

[0058] Figure 5 This is a cycle curve diagram of the sodium ion battery prepared in Example 1 of the present invention at a current density of 10C. DETAILED DESCRIPTION

[0059] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0061] In the description of the present application, the terms "(1)", "(2)", "first", and "second" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "(1)", "(2)", "first", and "second" may explicitly or implicitly include at least one of the features. In the description of the present application, "plurality" means at least two, for example, two, three, etc., unless otherwise clearly and specifically defined.

[0062] In the description of the present application, unless otherwise specified, the term "or" is inclusive. That is, the phrase "A or (or) B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or A and B are both true (or exist).

[0063] The weight of the relevant components mentioned in the specification of the examples of this application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the specification of the examples of this application, it is within the scope disclosed in the specification of the examples of this application. Specifically, the weight described in the specification of the examples of this application can be mass units known in the chemical industry such as μg, mg, g, and kg.

[0064] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0065] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0066] The following is a detailed description of the implementation of the present application.

[0067] The first embodiment of the present application provides a positive electrode material. The molecular formula of the positive electrode material is Na4M 3-3δ N 6δ / m (PO4)2P2O7 (or expressed as Na4(M3(PO4)2) 1-δ (N 6δ / m m+ (PO4) 2δ )P2O7), where N is a doping metal element and the valence state of N is m + , M is a transition metal element, and 0≤δ≤0.3. Specifically, M can be selected from one or more transition metal elements such as Fe, Mn, etc. N is a doping metal element. It can be understood that the doping metal element N is another metal element different from the transition metal element M. Specifically, N can be selected from one or more of Mg, Al, Ti, V, Zn, Zr, Cr, and Cu.

[0068] In any embodiment of the present application, when δ=0, no doping metal element N is added. It can be understood that when M is only one element; for example, when it is selected from Mn, the molecular formula of the positive electrode material is Na4Mn3(PO4)2P2O7; when M is selected from Fe, the molecular formula of the positive electrode material is Na4Fe3(PO4)2P2O7; when M is selected from Ni, the molecular formula of the positive electrode material is Na4Ni3(PO4)2P2O7; when M is selected from Co, the molecular formula of the positive electrode material is Na4Co3(PO4)2P2O7. When M is selected from two or more of Mn, Fe, Ni and Co, the molecular formula of the positive electrode material is Na4Mn α Fe β Ni γ Co 3-α-β-γ (PO4)2P2O7, where 0≤α≤3, 0≤β≤3, 0≤γ≤3, and 0≤α+β+γ≤3.

[0069] It is further understood that when the positive electrode material is doped with a metal element N, the doped metal element N is a metal element other than the transition metal element M (Mn, Fe, Ni and Co). The doped metal element N may be one or more of Mg, Al, Ti, V, Zn, Zr, Cr and Cu.

[0070] The first aspect of the present application provides a method for preparing a positive electrode material, comprising the following steps:

[0071] Mixing step: weigh a certain amount of raw material X and raw material Y, place them in a container filled with water, mix and stir to obtain slurry A, and then grind to obtain precursor slurry B;

[0072] Spray drying step: placing the precursor slurry B in a spray drying device for spray drying to obtain a precursor powder C;

[0073] Sintering step: placing the precursor powder C in a sintering device for sintering to obtain a positive electrode material;

[0074] The X raw material is a water-insoluble substance containing a transition metal element M, the Y raw material is a water-soluble substance containing an element Na, and at least one of the X raw material and the Y raw material contains an element P.

[0075] In the above preparation method, first, in the mixing step, the raw materials are mixed and stirred with water as a medium. In the design of the raw materials, the X raw material is a substance that is not easily soluble in water and contains the transition metal element M. Therefore, the X raw material is added to the aqueous solution to form dispersed tiny particles, and the Y raw material is a substance that is easily soluble in water and contains the element Na. The Y raw material is added to the aqueous solution to form sodium ions. Under the action of external force, the uniform distribution of sodium ions on the surface of the X raw material can be accelerated; further, after the mixing step, through the coordinated cooperation between the spray drying step, the pretreatment step, and the sintering step, a positive electrode material product with higher purity can be obtained.

[0076] In addition, the above preparation method is simple to operate, has low production cost, and has the prospect of large-scale production.

[0077] After in-depth research, the applicant found that when the raw materials of the present application meet the aforementioned design conditions and can also meet one or more of the following conditions, the purity of the positive electrode material can be further improved and the performance of the battery can be further improved.

[0078] In any embodiment of the present application, the X raw material is one or more compounds containing transition metal M and element P, and the solubility product K of the corresponding anhydrous compound is sp ≤1.0×10 -25 It can be understood that the X raw material with a smaller solubility product can stably exist during the grinding process in the mixing step, which is helpful for preparing the precursor slurry B with higher purity.

[0079] In any embodiment of the present application, the Y raw material is a compound containing one or more of the element Na and the element P, and the solubility of the corresponding anhydrous compound is ≥3g / 100g water. It can be understood that the Y raw material with a solubility product ≥3g / 100g water has better solubility in an aqueous solution, and it is easy to produce sodium ions, pyrophosphate, phosphate (monohydrogen / dihydrogen), etc., which helps the above ions to be evenly dispersed on the particle surface of the X raw material.

[0080] In any embodiment of the present application, both the X raw material and the Y raw material contain the element P. It can be understood that, since the positive electrode material is fitted to contain M3(PO4)2, in which the element P is an important component, the inventors of the present application have found that the element P will be lost during the synthesis and preparation of the material, which will lead to the generation of various types of impurities, so increasing the content of the element P is helpful to reduce the generation of impurities; therefore, the selected X raw material and Y raw material both contain the element P, which can increase the percentage of the element P in the synthesis environment and help reduce the generation of impurities.

[0081] In any embodiment of the present application, the X raw material also includes element P. In the X raw material, the stoichiometric ratio of the transition metal element M to the element P is 3:2, that is, in the X raw material, the sum of the stoichiometric ratios of the transition metal element M: the stoichiometric ratio of the element P = 3:2. It can be understood that the X raw material can be a compound or a mixture of multiple compounds. As long as the sum of the stoichiometric ratios of the transition metal element M and the stoichiometric ratio of the element P is 3:2, it belongs to the category of X raw material. It can be understood that since it is fitted into the positive electrode material Na4(M3(PO4)2) 1-δ (N 6δ / m m+ (PO4) 2δ )P2O7, which contains (1-δ) stoichiometric M3(PO4)2. When the sum of the stoichiometric ratios of the transition metal elements and the sum of the stoichiometric ratios of element P meet the requirement of 3:2, the X raw material just provides the transition metal element M and element P in M3(PO4)2, which is helpful to synthesize the positive electrode material with higher purity.

[0082] In any embodiment of the present application, the molecular formula of the anhydrous compound of the X raw material is M3(PO4)2. The X raw material not only provides the synthetic positive electrode material Na4(M3(PO4)2) 1-δ (N 6δ / m m+ (PO4) 2δ)M3(PO4)2 required for P2O7; and M3(PO4)2 with a smaller solubility product is stable during the grinding process and is evenly mixed with the element Na and element P in the Y raw material; in addition, during the sintering step, the presence of M3(PO4)2 also helps to synthesize the positive electrode material Na4(M3(PO4)2) with higher purity 1-δ (N 6δ / m m+ (PO4) 2δ )P2O7.

[0083] Since it is fitted into the positive electrode material Na4M 3-3δ N 6δ / m (PO4)2P2O7 (where N is in a valence state of m + ), also known as Na4(M3(PO4)2) 1-δ (N 6δ / m m+ (PO4) 2δ )P2O7, which contains (1-δ) stoichiometric M3(PO4)2. When the sum of the stoichiometric ratios of the transition metal element M and the sum of the stoichiometric ratios of the element P meet the requirement of 3:2, the X raw material just provides the transition metal element M and the element P in M3(PO4)2, which is helpful to synthesize the positive electrode material with higher purity.

[0084] In any embodiment of the present application, the X raw material is selected from one or more of Mn3(PO4)2.yH2O (0≤y≤7), Fe3(PO4)2.z1H2O (0≤z1≤8), Ni3(PO4)2.z2H2O (0≤z2≤8), and Co3(PO4)2.z3H2O (0≤z3≤8). Since Mn3(PO4)2.yH2O (0≤y≤7), Fe3(PO4)2.z1H2O (0≤z1≤8), Ni3(PO4)2.z2H2O (0≤z2≤8), and Co3(PO4)2.z3H2O (0≤z3≤8) are easy to industrialize, it is beneficial to the industrialization promotion and application of the positive electrode material provided in the present application.

[0085] Furthermore, the solubility product Ksp of Mn3(PO4)2 is 1.0×10 -27 , the solubility product Ksp of Fe3(PO4)2 is 1.0×10 -36 , the solubility product Ksp of Ni3(PO4)2 is 5.0×10 -31 , the solubility product Ksp of Co3(PO4)2 is 2.04×10 -35 .

[0086] In any embodiment of the present application, the X raw material is selected from at least two or more of Mn3(PO4)2.yH2O (0≤y≤7), Fe3(PO4)2.z1H2O (0≤z1≤8), Ni3(PO4)2.z2H2O (0≤z2≤8) and Co3(PO4)2.z3H2O (0≤z3≤8). Polyanion sodium cathode materials are similar to lithium ion olivine materials. Fe-based materials have good electrochemical properties, but the low platform voltage leads to low energy density; Mn-based materials have high platform voltage and high energy density, but low electronic conductivity leads to poor electrochemical performance, and poor cycle stability due to the Jahn-Teller effect; Ni-based and Co-based materials have high voltage platforms, but high costs. When two or more of Mn, Fe, Ni, and Co are mixed under the synergistic effect, a material with good energy density, electrochemical performance, and cycle life and moderate cost is obtained to meet the needs of practical applications.

[0087] Furthermore, Mn3(PO4)2.yH2O (0≤y≤7) is selected from Mn3(PO4)2·3H2O. Since Mn3(PO4)2·3H2O can be directly prepared by co-precipitation of manganese salt and phosphate in a solution, it is simple and easy, which is conducive to reducing production difficulty, improving the efficiency of industrial production, and reducing the cost of purchasing raw materials.

[0088] Furthermore, Fe3(PO4)2.z1H2O (0≤z1≤8) is selected from Fe3(PO4)2·8H2O. Since Fe3(PO4)2·8H2O can be directly prepared by co-precipitation of ferrous salt and phosphate in a solution, it is simple and easy, which is conducive to reducing the difficulty of production, improving the efficiency of industrial production, and reducing the cost of purchasing raw materials.

[0089] Furthermore, Ni3(PO4)2.z2H2O (0≤z2≤8) is selected from Ni3(PO4)2·8H2O. Since Ni3(PO4)2·8H2O can be directly prepared by co-precipitation of nickel salt and phosphate in a solution, it is simple and easy, which is conducive to reducing the difficulty of production, improving the efficiency of industrial production, and reducing the cost of purchasing raw materials.

[0090] Furthermore, Co3(PO4)2.z3H2O (0≤z3≤8) is selected from Co3(PO4)2·8H2O. Since Co3(PO4)2·8H2O can be directly prepared by coprecipitation of cobalt salt and phosphate in solution, it is simple and easy, which is conducive to reducing production difficulty, improving the efficiency of industrial production, and reducing the cost of purchasing raw materials.

[0091] Furthermore, the X raw material is selected from one or more of Mn3(PO4)2·3H2O, Fe3(PO4)2·8H2O, Ni3(PO4)2·8H2O, and Co3(PO4)2·8H2O.

[0092] Furthermore, the X raw material is selected from Mn3(PO4)2·3H2O and Fe3(PO4)2·8H2O. Similar to lithium manganese iron phosphate, composite sodium manganese phosphate combines the low cost of iron and manganese with the high voltage platform of manganese to synergistically provide the most cost-effective positive electrode material.

[0093] In any embodiment of the present application, in the Y raw material, the stoichiometric ratio of the element Na to the element P is 2:1, that is, the sum of the stoichiometric ratios of the element Na in the Y raw material: the sum of the stoichiometric ratios of the element P = 2:1. It can be understood that the Y raw material can be a compound or a mixture of multiple compounds. As long as the sum of the stoichiometric ratios of the element Na: the sum of the stoichiometric ratios of the element P = 2:1, it belongs to the category of the Y raw material. It can be understood that since it is fitted into the positive electrode material Na4M 3-3δ N 6δ / m (PO4)2P2O7 contains an equal stoichiometric amount of Na4P2O7. When the sum of the stoichiometric ratios of element Na: the sum of the stoichiometric ratios of element P = 2:1, the Y raw material just provides the sodium and phosphorus elements in Na4P2O7, which helps to synthesize a positive electrode material with higher purity.

[0094] In any embodiment of the present application, the Y raw material is selected from one or more of NaOH, Na2C2O4, CH3COONa, Na2CO3, NaHCO3, Na4P2O7, Na3HP2O7, Na2H2P2O7, NaH3P2O7, H4P2O7, Na2HPO4, NaH2PO4, Na3PO4, H3PO4, NH4H2PO4, (NH4)2HPO4 and (NH4)3PO4. It can be understood that the above compounds include both their corresponding anhydrous compounds and their compounds containing different crystal waters.

[0095] Furthermore, the Y raw material is selected from one or more of Na4P2O7 and Na2HPO4. The applicant has found that Na4P2O7 and Na2HPO4 are not only soluble in water, but also have strong complexing ability with transition metal elements, which helps to mix evenly with the X raw material when using water as a medium, and helps to generate a positive electrode material with higher purity.

[0096] In any embodiment of the present application, in the mixing step, the mass proportion of raw material X is ≥15%.

[0097] Furthermore, the mass proportion of raw material X is ≤80%.

[0098] The applicant has found that if the mass proportion of raw material X is too low, more side reactions will be produced, and if the mass proportion of raw material X is too high, serious agglomeration will occur during the mixing step. Therefore, it is recommended that the mass proportion of raw material X be preferably 15% to 80%.

[0099] In any embodiment of the present application, in the mixing step, the mass proportion of the Y raw material is ≥20%.

[0100] Furthermore, the mass proportion of Y raw material is ≤70%.

[0101] The applicant found that when the mass proportion of raw material Y is too low, it cannot be evenly dispersed on the surface of raw material X, resulting in the generation of more impurities; while when the mass proportion of raw material Y is too high, the pH value of the solution will be too high, requiring the addition of additional pH regulators, increasing the difficulty of preparation. Therefore, it is recommended that the mass proportion of raw material Y be preferably 20% to 70%.

[0102] In any embodiment of the present application, in the mixing step: the raw materials at least include raw materials X and Y. It can be understood that the raw materials also include other raw materials besides raw materials X and Y.

[0103] In any embodiment of the present application, in the mixing step, the raw material further includes: one or more of a modifying additive, a phosphorus source supplement, a carbon source, a dispersant, and a viscosity reducer.

[0104] In any embodiment of the present application, in the mixing step, the raw material further includes: a modifying additive, wherein the modifying additive includes a doping metal element N.

[0105] The main purpose of the modified additive is to dope the synthesized positive electrode material with cations. Generally, the ionic conductivity and electronic conductivity of polyanionic materials are low, and appropriate cation doping can greatly improve their ionic conductivity and electronic conductivity, thereby improving the electrochemical performance of the resulting positive electrode material.

[0106] It can be understood that the molecular formula of the positive electrode material obtained by adding the modifying additive is Na4(M3(PO4)2) 1-δ (N 6δ / m m+ (PO4) 2δ )P2O7. The doping metal element N is another metal element different from the transition metal element M. Specifically, N can be selected from one or more of Mg, Al, Ti, V, Zn, Zr, Cr, and Cu.

[0107] Furthermore, the modifying additive may be selected from simple substances, compounds or solutions containing the above elements.

[0108] Furthermore, the modifying additive may be soluble in water or insoluble in water.

[0109] Furthermore, the molecular formula of the modifying additive is N 6 / m m+ (PO4)2, wherein N is selected from one or more of Mg, Al, Ti, V, Zn, Zr, Cr, Cu, m + is the valence of N. This is because the molecular formula N 6 / m m+ (PO4)2 and Na4(M3(PO4)2) 1-δ (N 6δ / m m+ (PO4) 2δ ) The N in the delta chemical bond contained in the P2O7 molecular formula 6 / m m+ (PO4)2, in the mixing step, the required modified doping metal element N is introduced, but no other new impurity elements are introduced, and due to the similar structure, it is easier to mix evenly during the mixing process, which is beneficial to the embedding of the doping metal element N in the subsequent reaction process.

[0110] Furthermore, the mass proportion of the modifying additive is ≥ 1%.

[0111] Furthermore, the mass proportion of the modifying additive is ≤20%.

[0112] In any embodiment of the present application, in the mixing step, the raw material may also include: a phosphorus source supplement. Appropriate addition of a phosphorus source supplement can increase the phosphorus content of the raw material, and help to replenish the phosphorus lost during the preparation process, for example, during the mixing process, the phosphorus element is not fully attached to the X raw material due to a short mixing time or other factors. In particular, when the above-mentioned modifying additive is not selected from N 6 / m m+ (PO4)2, but N in the form of a single substance or other compound (such as oxide, carbonate, oxalate, nitrate), add a phosphorus source supplement to the raw material, and the stoichiometric sum of phosphorus in the phosphorus source supplement is 2:3 / m of the stoichiometric sum of the added N. This ensures that the chemical formula of the final material meets

[0113] Na4(M3(PO4)2) 1-δ (N 6δ / m m+ (PO4) 2δ )P2O7, thereby improving the purity of the prepared positive electrode material.

[0114] It is understood that the phosphorus source supplement is a simple substance or compound containing phosphorus. The phosphorus source supplement may be soluble in water or insoluble in water.

[0115] Furthermore, the phosphorus source supplement is a solvent containing phosphorus element. The solvent can be more easily mixed with other materials during the stirring and grinding process.

[0116] Furthermore, the phosphorus source supplement is selected from one or more of H3PO4, NH4H2PO4, (NH4)2HPO4. The above phosphorus source is soluble in water, easy to mix with M3(PO4)2 and N compound, and it is not easy to leave any impurities after high-temperature sintering.

[0117] Furthermore, the mass proportion of phosphorus source supplement is ≥1%.

[0118] Furthermore, the mass proportion of phosphorus source supplement is ≤20%.

[0119] In any embodiment of the present application, in the mixing step, the raw material further includes: a carbon source.

[0120] Specifically, the carbon source may be selected from one or more of inorganic carbon materials and / or organic carbon materials.

[0121] Furthermore, the organic carbon material is selected from one or more of citric acid, glucose, sucrose, polyethylene glycol, starch, lignin, and asphalt.

[0122] Furthermore, the inorganic carbon material is selected from one or more of graphite, activated carbon, carbon nanotubes, and graphene.

[0123] In any embodiment of the present application, in the mixing step, the raw material further includes: a dispersant.

[0124] Furthermore, the dispersant is selected from one or more of polyethylene oxide, polytetrafluoroethylene, polyacrylic acid, polymethyl acrylate, carboxymethyl cellulose, methyl cellulose, ethyl cellulose, carboxyethyl cellulose, carboxypropyl methyl cellulose and carboxyethyl methyl cellulose.

[0125] In a specific embodiment, in the mixing step, the raw material further includes: a viscosity reducing agent.

[0126] Furthermore, the viscosity reducing agent is selected from one or more of polyvinyl alcohol, polyethylene glycol, and polypropylene glycol.

[0127] In any embodiment of the present application, the particle size D50 of the precursor slurry B after grinding is 300-800nm. Controlling the particle size of the precursor slurry B within an appropriate range helps to evenly mix the sodium and phosphorus elements in the X raw material and the Y raw material, and is conducive to the preparation of a positive electrode material with higher purity. When the particle size of the precursor slurry B is less than 300nm, it is easy to agglomerate, which may lead to incomplete reaction in the spray drying step and the sintering step, so that the generated positive electrode material contains more impurities. When the particle size of the precursor slurry B is greater than 800nm, during the sintering process, Na + and P2O7 4- , especially P2O7 4-, it is difficult to diffuse all to the correct site, resulting in the easy appearance of impurities, such as Na2MP2O7.

[0128] Furthermore, the particle size D50 of the precursor slurry B is 300-600 nm. Furthermore, the particle size D50 of the precursor slurry B is 300-450 nm.

[0129] In any embodiment of the present application, in the spray drying step, the inlet temperature of the spray drying device is 180-300° C. Controlling the inlet temperature of the spray drying device within an appropriate range can improve the average particle size and bulk density of the precursor powder C, which helps the precursor powder C to react more fully in the sintering step; it can also reduce the occurrence of other side reactions that may generate impurities during the spray drying process, thereby improving the purity of the positive electrode material.

[0130] Furthermore, the inlet temperature of the spray drying equipment is 190-220°C.

[0131] In any embodiment of the present application, in the spray drying step, the outlet temperature of the spray drying device is 80-130° C. Controlling the outlet temperature of the spray drying device within an appropriate range can maintain the material activity of the precursor powder C, which is beneficial to the sintering of the precursor powder C in the subsequent steps; thereby improving the purity of the positive electrode material.

[0132] Furthermore, the outlet temperature of the spray drying equipment is 90-110°C.

[0133] In any embodiment of the present application, a pretreatment step is further included. The pretreatment step is located before the sintering step. The pretreatment step includes: placing the precursor powder C in an ammonia solution for treatment.

[0134] Ammonia can further react with the precursor powder C to affect the grain growth rate and morphology of the precursor powder C by controlling the concentration of free ions, and make the corresponding ions such as Na + and P2O7 4- During the calcination step, it diffuses to the correct site to the greatest extent possible, reduces the occurrence of other side reactions that may generate impurities during the subsequent calcination process, avoids the generation of impurities, and promotes the reaction to produce pure phase products, thereby improving the purity of the positive electrode material.

[0135] Furthermore, in the pretreatment step, the mass percentage concentration of the ammonia solution is 2-10%.

[0136] Further, in the pretreatment step, the pretreatment time is 2-15 hours. Preferably, the pretreatment time is 3-8 hours.

[0137] In any embodiment of the present application, in the pretreatment step, the precursor powder C is placed in an aqueous ammonia solution for a treatment time of 3-4 hours.

[0138] In any embodiment of the present application, in the sintering step, the atmosphere of the sintering process is air or an inert atmosphere.

[0139] Further, preferably, the sintering may be performed once or multiple times.

[0140] Further, preferably, when the sintering process is performed in an inert atmosphere, nitrogen is preferred. Ammonia atmosphere can reduce the occurrence of other side reactions that may generate impurities during the calcination process, control the grain size of the precursor powder C, and the free ion concentration, thereby improving the purity of the positive electrode material.

[0141] In any embodiment of the present application, in the sintering step, the temperature range of the sintering treatment is 300-800° C. Specifically, the temperature may be 450° C., 500° C., 550° C., 600° C., 650° C., 700° C., 750° C. or 800° C. When the temperature is as high as 800° C., the particle size of the particles in the precursor powder C is too large, and the specific surface area is reduced, so that the electrochemical performance of the battery made of the positive electrode material is reduced.

[0142] Furthermore, preferably, the temperature range of the sintering treatment is 450-800°C.

[0143] Furthermore, preferably, the temperature range of the sintering treatment is 450-750°C.

[0144] In any embodiment of the present application, in the sintering step, the sintering treatment time is 3-20 hours.

[0145] Furthermore, preferably, the sintering treatment time is 10-20 hours.

[0146] In any embodiment of the present application, in the sintering step, the heating rate of the sintering equipment is 5-10° C. / min.

[0147] The present application also provides a sodium ion battery, comprising the positive electrode of the positive electrode material or the positive electrode material prepared by the above-mentioned preparation method. Specifically, the positive electrode comprises a current collector and a positive electrode active material disposed on the current collector, and the positive electrode active material comprises the positive electrode material of the present application or the positive electrode material prepared by the preparation method of the present application.

[0148] The present application also provides a battery module, including the above-mentioned sodium ion battery. Specifically, the battery module includes a housing, a cover plate and a sodium ion battery. The housing has a receiving cavity and an opening; the sodium ion battery is received in the receiving cavity; and the cover plate is used to close the opening of the housing.

[0149] The present application also provides an electrical device, including the above-mentioned sodium ion battery. The electrical device can be a device using a sodium ion battery as a power supply device. Exemplarily, the electrical device can be a small electronic device (such as a mobile phone, a tablet computer, a laptop computer, etc.), or a large transportation device such as a vehicle (such as a hybrid vehicle, an electric vehicle, etc.), or an electric tool (such as an electric drill, an electric saw, etc.).

[0150] Example

[0151] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0152] Example 1

[0153] 1. Preparation method of positive electrode material:

[0154] Weigh 100.32g Fe3(PO4)2·8H2O of X raw material, 53.18g Na4P2O7 of Y raw material, 20g sucrose of carbon source, and 15.74g PEG (molecular weight 1675) of dispersant respectively. Mix at 500r / min for 30min in water medium to obtain slurry A. The obtained slurry A is grinded by sand mill to obtain slurry B, and its particle size D50 is 512nm. After spray drying of slurry B, precursor powder C is obtained. Then, precursor C is placed in nitrogen atmosphere and calcined at 500℃ for 10h to obtain Na4Fe3(PO4)2P2O7 / C (in this embodiment, M is Fe, d=0).

[0155] Figure 2-3 The synthesized Na4Fe3(PO4)2P2O7 / C was characterized and tested in detail. XRD showed that the obtained product was pure phase with almost no impurity peaks ( Figure 2 ). SEM shows that the particle size of the obtained material is 2-4mm ( Figure 3 ).

[0156] 2. Preparation of button cells

[0157] Take 0.8 grams of the above Na4Fe3(PO4)2P2O7 / C material, mix it with 0.1 grams of conductive carbon black and 0.1 grams of PVDF, grind it with NMP as the medium, apply the obtained slurry to the aluminum foil current collector, and obtain the positive electrode after drying. The obtained electrode is cut into a square electrode with a side length of 1 cm as the working electrode, and the metal sodium sheet is used as the counter electrode. 1M NaPF6 is dissolved in EC:DEC (50:50vol / vol) as the electrolyte, and a button cell (2032) is assembled under an inert atmosphere. The button half-cell test results show that the discharge capacity of the material is 117mAh / g at 0.1C, 102mAh / g at 1C, and 90mAh / g at 10C ( Figure 4 ). 10C first cycle 88.6mAh / g, 2000 cycles 80.1mAh / g; capacity retention rate 90.4% ( Figure 5 ).

[0158] Example 2

[0159] The preparation method of the positive electrode material is similar to that of Example 1, except that a pretreatment step is provided before the sintering step. Specifically, the precursor C is placed in an ammonia solution with a mass percentage concentration of 2% for 3 hours and then calcined in a nitrogen atmosphere.

[0160] Example 3

[0161] The preparation method of the positive electrode material is similar to that of Example 1, except that in the mixing step, the mixing is carried out at 800 r / min for 30 min in the water medium.

[0162] Example 4

[0163] The preparation method of the positive electrode material is similar to that of Example 1, except that in the mixing step, the particle size of the slurry B is adjusted by adjusting the grinding parameters, and the particle size D50 of the slurry B is measured to be 400 nm.

[0164] Example 5

[0165] The preparation method of the positive electrode material is similar to that of Example 1, except that the X raw material weighed is 81.2 g Mn3(PO4)2·3H2O; and the Y raw material weighed is 56.38 g Na2HPO4.

[0166] Example 6

[0167] The preparation method of the positive electrode material is similar to that of Example 1, except that the X raw material weighed is 31.95 g Mn3(PO4)2 and 35.46 g Fe3(PO4)2·2H2O; and the Y raw material is 37.87 g Na2HPO4.

[0168] Example 7

[0169] The preparation method of the positive electrode material is similar to that of Example 1, except that the X raw material weighed is 97.01 g Fe3(PO4)2·8H2O; the Y raw material weighed is 53.18 g Na4P2O7 and 1.52 g NH4H2PO4.

[0170] Example 8

[0171] The preparation method of the positive electrode material is similar to that of Example 1, except that the weighed X raw material is 76.03 g Mn3(PO4)2·3H2O, and the Y raw material is 53.18 g Na4P2O7.

[0172] Example 9

[0173] The preparation method of the positive electrode material is similar to that of Example 8, except that 2.62 g of Zn powder is added as a modifying additive in the mixing step.

[0174] Example 10

[0175] The preparation method of the positive electrode material is similar to that of Example 1, except that the X raw material weighed is 38.18g Mn3(PO4)2·3H2O, 46.85g Fe3(PO4)2·8H2O, 1.70g Ni3(PO4)2·8H2O, and 1.71g Co3(PO4)2·8H2O; the Y raw material is 53.18g Na4P2O7, 1.50g NH4H2PO4.

[0176] Embodiment 11

[0177] The preparation method of the positive electrode material is similar to that of Example 11, except that 37.88 g of Zn(NO3)3 10% solution as a modifying additive is added in the mixing step.

[0178] The positive electrode material products prepared in Examples 1-11 were subjected to charge and discharge tests, and the test results are shown in Table 1:

[0179] Table 1. Charge and discharge test results of positive electrode material products prepared in Examples 1-11

[0180]

[0181] It can be seen from the data in the table that the positive electrode materials synthesized by this method all show high initial discharge capacity and coulombic efficiency, and also show excellent cycle performance under large current. This strongly proves that the present invention can prepare positive electrode materials with high purity and good electrochemical performance through special design of raw materials, and coordinated coordination of mixing, spray drying and sintering.

[0182] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a positive electrode material, wherein the molecular formula of the positive electrode material is Na4M 3-3δ N 6δ / m (PO4)2P2O7, where N is a doping metal element and the valence state of N is m + , M is a transition metal element, and 0≤δ≤0.3, characterized in that, The preparation method comprises the following steps: Mixing step: weigh a certain amount of raw material X and raw material Y, place them in a container filled with water, mix and stir to obtain slurry A, and then grind to obtain precursor slurry B; Spray drying step: placing the precursor slurry B in a spray drying device for spray drying to obtain a precursor powder C; Sintering step: placing the precursor powder C in a sintering device for sintering to obtain the positive electrode material; The X raw material is a substance that is not easily soluble in water and contains a transition metal element M, the Y raw material is a substance that is easily soluble in water and contains an element Na, and at least one of the X raw material and the Y raw material contains an element P.

2. The method for preparing the positive electrode material according to claim 1, characterized in that: The X raw material is one or more compounds containing transition metal elements M and elements P, and the solubility product K of the corresponding anhydrous compound is sp ≤1.0×10 -25 ; and / or The Y raw material is a compound containing one or more of the elements Na and P, and the solubility of the corresponding anhydrous compound is ≥3g / 100g water.

3. The method for preparing the positive electrode material according to any one of claims 1 to 2, characterized in that: In the X raw material, the stoichiometric ratio of the transition metal element M to the element P is 3:2; and / or In the Y raw material, the stoichiometric ratio of the element Na to the element P is 2:

1.

4. The method for preparing a positive electrode material according to any one of claims 1 to 3, characterized in that: The X raw material is selected from one or more of Mn3(PO4)2.yH2O (0≤y≤7), Fe3(PO4)2.z1H2O (0≤z1≤8), Ni3(PO4)2.z2H2O (0≤z2≤8), and Co3(PO4)2.z3H2O (0≤z3≤8); and / or The Y raw material is selected from one or more of NaOH, Na2C2O4, CH3COONa, Na2CO3, NaHCO3, Na4P2O7, Na3HP2O7, Na2H2P2O7, NaH3P2O7, H4P2O7, Na2HPO4, NaH2PO4, Na3PO4, H3PO4, NH4H2PO4, (NH4)2HPO4 and (NH4)3PO4.

5. The method for preparing the positive electrode material according to claim 1, characterized in that: In the mixing step, a modifying additive is further added, wherein the modifying additive includes the doping metal element N, wherein N is selected from one or more of Mg, Al, Ti, V, Zn, Zr, Cr, and Cu; preferably, the molecular formula of the modifying additive is N 6 / m m+ (PO4)2.

6. The method for preparing the positive electrode material according to claim 1, characterized in that: In the mixing step, a phosphorus source supplement is also included; the phosphorus source supplement is selected from one or more of H3PO4, NH4H2PO4, (NH4)2HPO4.

7. The method for preparing the positive electrode material according to claim 1, characterized in that: The particle size D50 of the precursor slurry B is 300-800 nm; preferably, 300-600 nm; more preferably, 300-450 nm.

8. The method for preparing the positive electrode material according to claim 1, characterized in that: The method further comprises a pretreatment step, which is located before the sintering step. The pretreatment step comprises: placing the precursor powder C in an ammonia solution for treatment.

9. The method for preparing the positive electrode material according to claim 1, characterized in that: In the spray drying step, the inlet temperature of the spray drying equipment is 180-300° C., and the outlet temperature of the spray drying equipment is 80-130° C.; and / or In the sintering step, the sintering temperature range is 300-800° C., the sintering time is 3-20 hours, and the heating rate of the sintering equipment is 5-10° C. / min.

10. A positive electrode material, characterized in that: The positive electrode material is prepared according to the method for preparing the positive electrode material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Carbon-coated ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof

    CN116230923A

  • Polyanionic sodium-ion battery positive electrode material as well as preparation method and application thereof

    CN116504940A

  • Iron-based phosphate-based polyanion positive electrode material as well as preparation and application thereof

    CN116553505A

  • Vanadium-doped ferric sodium pyrophosphate / carbon composite material as well as preparation method and application thereof

    CN117080392A

  • Preparation method and application of sodium ion positive electrode material

    CN117486186A

Cited By

  • Positive electrode material and preparation method thereof

    CN121990545A