High-value recovery method of waste sodium vanadium phosphate battery positive electrode material

The liquid phase oxidation method dissolves the used vanadium phosphate battery positive electrode material in acid buffer solution, and synthesizes the layered vanadium phosphate positive electrode material, which solves the problems of low recycling efficiency and high energy consumption in the existing technology, and realizes sodium and vanadium , efficient recovery of phosphorus and improved electrochemical performance.

CN119059505AActive Publication Date: 2024-12-03WUHAN INST OF TECH

Patent Information

Application Number
CN202411182181.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

In the prior art, when recycling waste vanadium phosphate battery positive electrode materials, the recycling efficiency of sodium, vanadium and phosphorus is low and the process is complex, and the energy consumption is high, making it difficult to simplify the recycling process and reduce costs.

Method used

The liquid phase oxidation method is used to dissolve the used vanadium phosphate battery positive electrode material in an acid buffer solution, and the heat reflux reaction is carried out by adding an oxidant and complexing agent to synthesize the layered vanadium phosphate positive electrode material in one step, simplifying the process and improving the recycling efficiency.

Benefits of technology

The comprehensive recycling of sodium, vanadium and phosphorus in waste vanadium phosphate positive electrode materials has been achieved. The product has good electrochemical properties and is suitable for sodium ion batteries, which significantly improves the reuse value of resources and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059505A_ABST
    Figure CN119059505A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium ion battery positive electrode materials, and discloses a high-value recovery method of a waste sodium vanadium phosphate battery positive electrode material, which comprises the following steps: 1) dissolving the waste sodium vanadium phosphate battery positive electrode material in an acidic buffer solution under the protection of an inert atmosphere, and filtering to obtain a filtrate containing Na, V and P; and 2) adding an oxidizing agent and a complexing agent into the filtrate, carrying out a heating reflux reaction under the conditions of stirring and inert atmosphere protection, and washing and drying a precipitate after the reaction is ended to obtain the layered sodium vanadyl phosphate positive electrode material. According to the method, after the waste sodium vanadium phosphate battery positive electrode material is dissolved, the layered sodium vanadyl phosphate positive electrode material is synthesized in one step through a liquid phase oxidation method, the recycled product has good electrochemical performance and can be directly used for a sodium ion battery, and the utilization value is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion battery positive electrode materials, and in particular relates to a high-value recovery method for waste sodium vanadium phosphate battery positive electrode materials. Background Art

[0003] In sodium-ion batteries, the positive electrode material is the key part of sodium-ion batteries. Sodium phosphovanadate positive electrode material has become one of the popular materials for sodium-ion positive electrode materials because of its moderate voltage and relatively ideal capacity, ultra-long cycle life and excellent rate performance. However, after use, it will inevitably lead to the generation of waste batteries. Waste sodium phosphovanadate positive electrode materials contain a large amount of vanadium, which has strong toxicity and carcinogenicity. If vanadium-containing solid waste is not disposed of and randomly piled up, it will not only occupy a large amount of land resources, but also bring harm to the natural environment and people's health. At this time, it is necessary to recycle the waste sodium vanadium phosphate positive electrode materials.

[0004] Patent CN115417392A discloses a method for recovering sodium phosphovanadate positive electrode materials, firstly mixing a solution of the positive electrode material with a strong base to obtain a metal ion solution containing V and P; then 4 3- The vanadium phosphate is complexed with iron ions to obtain an iron phosphate precipitate and a solution containing V; finally, the solution containing V is concentrated and crystallized to obtain a sodium vanadate product. Patent CN115341098A discloses a method for recovering vanadium from waste sodium ion batteries, which firstly roasts the sodium vanadium phosphate positive electrode material, then acid-leaches the roasted product, adjusts the pH of the leaching solution to precipitate vanadium, and finally calcines to obtain vanadium pentoxide.

[0005] The above patents all focus on the recovery of vanadium in sodium vanadium phosphate positive electrode materials. The recovery efficiency of elements such as sodium and phosphorus is low, and the recovery process is complicated and the energy consumption of the recovery process is high. Therefore, how to comprehensively recover sodium, vanadium and phosphorus in waste sodium vanadium phosphate positive electrode materials, simplify the recovery process, and reduce energy consumption and recovery costs are technical challenges faced by researchers in this field. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a high-value recovery method for waste sodium vanadium phosphate battery positive electrode materials in view of the shortcomings of the prior art. After the waste sodium vanadium phosphate battery positive electrode materials are dissolved, a layered sodium vanadium phosphate positive electrode material is synthesized in one step by a liquid phase oxidation method. The recovery method has a simple process and does not involve high energy consumption processes. In addition, sodium, vanadium and phosphorus in the waste sodium vanadium phosphate positive electrode materials can be recovered and utilized. The recovered product has good electrochemical properties and can be directly used in sodium ion batteries, which significantly improves the utilization value.

[0007] In order to solve the technical problem proposed by the present invention, the present invention provides a high-value recovery method for waste sodium vanadium phosphate battery positive electrode materials, comprising the following steps:

[0008] 1) Under inert atmosphere protection conditions, dissolving the waste sodium vanadium phosphate battery positive electrode material in an acidic buffer solution, filtering, and obtaining a filtrate containing Na, V, and P;

[0009] 2) adding an oxidant and a complexing agent to the filtrate, and performing a heating reflux reaction under stirring and inert atmosphere protection conditions, and washing and drying the precipitate after the reaction to obtain a layered sodium vanadate phosphate positive electrode material.

[0010] In the above scheme, the cathode material of the waste sodium vanadium phosphate battery is Na 3 V 2 (PO 4 ) 3 、Na 3 V 2 (PO 4 ) 2 F 3 One or both of the following.

[0011] In the above scheme, the particle size of the waste sodium vanadium phosphate battery positive electrode material is 2 to 30 μm.

[0012] In the above scheme, the acidic buffer solution is an acetic acid-sodium acetate buffer solution with a pH range of 3-4.

[0013] In the above scheme, the volume ratio of the mass of the waste sodium vanadium phosphate battery positive electrode material to the acidic buffer solution is (5-10) g:100 mL.

[0014] In the above scheme, the pH of the filtrate is adjusted to 4-5.5 before the oxidant and the complexing agent are added.

[0015] In the above scheme, the oxidant is sodium persulfate, or a mixture of hydrogen peroxide and sodium sulfate.

[0016] Furthermore, the molar ratio of hydrogen peroxide to sodium sulfate is 1:(1-2).

[0017] In the above scheme, the complexing agent is one or two of ethylenediaminetetraacetic acid (EDTA), citric acid and tartaric acid.

[0018] In the above scheme, the concentration of the oxidant in the filtrate after addition is 0.02-1 mol / L.

[0019] In the above scheme, the concentration of the complexing agent in the filtrate after addition is 0.01-0.5 mol / L.

[0020] In the above scheme, the stirring rate of the stirring is 100 to 300 r / min.

[0021] In the above scheme, the temperature of the heating reflux reaction is 80-100° C. and the time is 2-10 h.

[0022] In the above scheme, the layered sodium vanadium phosphate positive electrode material is Na x VOPO 4 , where 0.4≤x≤0.6.

[0023] In the above scheme, the morphology of the layered sodium vanadium phosphate positive electrode material is spherical particles formed by aggregation of irregular flakes, and the particle size is 10 to 30 μm.

[0024] The technical principle of the present invention is:

[0025] The sodium vanadium phosphate cathode material is dissolved using an acetic acid-sodium acetate buffer solution. After dissolution, other insoluble substances in the cathode material can be separated, and V in the filtrate can be prevented from being directly oxidized to a high-valent state V under weak acid conditions. 5+ , then add oxidant and complexing agent, and synthesize layered sodium vanadium phosphate positive electrode material in one step by liquid phase oxidation method. Oxidant and complexing agent are the preparation of Na x VOPO 4 The key is to make it react under mild conditions and avoid direct oxidation of V in the solution to a high-valent state to generate VO 3 - root.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1) The present invention dissolves the waste sodium vanadium phosphate battery positive electrode material and synthesizes a layered sodium vanadium phosphate positive electrode material in one step through a liquid phase oxidation method. The process is simple, the conditions are mild, and no high energy consumption process is involved. In addition, the sodium, vanadium, and phosphorus in the waste sodium vanadium phosphate positive electrode material can be recycled. The recycled product has good electrochemical properties and can be directly used in sodium ion batteries, showing excellent discharge capacity and cycle performance, significantly improving the reuse value of waste battery resources, and achieving the dual goals of efficient resource reuse and environmental protection.

[0028] 2) Currently, the main preparation methods of sodium vanadyl phosphate are electrochemical deposition method and ion exchange method. The common point of these methods is that they all need to synthesize vanadyl phosphate first and then synthesize sodium vanadyl phosphate. There are problems of cumbersome steps and complicated operations, which are not conducive to industrial production. The present invention can skip the synthesis process of the intermediate product vanadyl phosphate, greatly simplifying the synthesis process of sodium vanadyl phosphate, and facilitating industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1This is the XRD spectrum of the layered sodium vanadium phosphate positive electrode material synthesized in Examples 1 to 3 of the present invention.

[0030] Figure 2 This is a SEM image of the layered sodium vanadium phosphate positive electrode material synthesized in Example 1 of the present invention.

[0031] Figure 3 This is the first cycle charge and discharge curve of a CR2032 button cell assembled with the layered sodium vanadium phosphate positive electrode material synthesized in Example 1 of the present invention.

[0032] Figure 4 This is a cycle performance diagram of a CR2032 button battery assembled with the layered sodium vanadium phosphate positive electrode material synthesized in Examples 1 to 3 of the present invention.

[0033] Figure 5 This is a SEM image of the product obtained in Comparative Example 2 of the present invention.

[0034] Figure 6 The XRD patterns of the products obtained in Comparative Examples 1 to 3 of the present invention are shown in FIG. DETAILED DESCRIPTION

[0035] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0036] Example 1

[0037] The cathode material of the waste sodium vanadium phosphate battery recovered in this embodiment is Na 3 V 2 (PO 4 ) 3 The particle size after crushing and screening is D 50 =10μm, the recovery method comprises the following steps:

[0038] 1) Under the protection of nitrogen atmosphere, the waste sodium vanadium phosphate battery positive electrode material is dissolved in an acetic acid-sodium acetate buffer solution with a pH of 3, and the volume ratio of the waste sodium vanadium phosphate battery positive electrode material to the acidic buffer solution is 5g:100mL, and filtered to obtain a filtrate containing Na, V, and P;

[0039] 2) adjusting the pH value of the filtrate to 4.5, and then adding an oxidant and a complexing agent to the filtrate, wherein the oxidant is a mixture of hydrogen peroxide and sodium sulfate in a molar ratio of 1:1, and the sum of the concentrations of the two in the filtrate after addition is 0.5 mol / L, and the complexing agent is EDTA, and the concentration in the filtrate after addition is 0.1 mol / L, and then heated to 90° C. for reflux reaction for 6 hours under stirring at 100 r / min and nitrogen atmosphere protection, and the precipitate produced after the reaction is washed with deionized water and dried at 80° C. to obtain a layered sodium vanadium phosphate positive electrode material Na 0.45VOPO 4 The V recovery rate in the obtained product is higher than 99.8%.

[0040] Figure 1 The XRD spectrum of the layered sodium vanadium phosphate positive electrode material synthesized in this embodiment and subsequent embodiments, in which PDF#41-0087 is Na 0.45 VOPO 4 According to the standard PDF card, all diffraction peaks in the XRD pattern correspond to the triclinic system P-1, which is consistent with the standard spectrum. No obvious impurity peaks are found, indicating the preparation of pure phase samples.

[0041] Figure 2 This is an SEM image of the layered sodium vanadium phosphate positive electrode material synthesized in this example. It can be seen from the figure that the morphology of the obtained product is spherical particles composed of some irregular thin sheets gathered together, indicating that the obtained sodium vanadium phosphate is a layered structure with a particle size of 10 to 30 μm.

[0042] Example 2

[0043] The cathode material of the waste sodium vanadium phosphate battery recovered in this embodiment is Na 3 V 2 (PO 4 ) 3 The particle size after crushing and screening is 2 to 30 μm, and the recovery method comprises the following steps:

[0044] 1) Under the protection of argon atmosphere, the waste sodium vanadium phosphate battery positive electrode material is dissolved in an acetic acid-sodium acetate buffer solution with a pH of 4.0, and the volume ratio of the waste sodium vanadium phosphate battery positive electrode material to the acidic buffer solution is 10g:100mL, and filtered to obtain a filtrate containing Na, V, and P;

[0045] 2) adjusting the pH value of the filtrate to 5, and then adding an oxidant and a complexing agent to the filtrate, wherein the oxidant is sodium persulfate, and the concentration in the filtrate after addition is 0.3 mol / L, and the complexing agent is citric acid, and the concentration in the filtrate after addition is 0.05 mol / L, and then heating to 85° C. for reflux reaction for 8 hours under stirring at 300 r / min and argon atmosphere protection, and washing the generated precipitate with deionized water after the reaction is completed, and drying at 100° C. to obtain a layered sodium vanadium phosphate positive electrode material Na 0.45 VOPO 4 The V recovery rate in the obtained product was 99.6%.

[0046] Example 3

[0047] The cathode material of the waste sodium vanadium phosphate battery recovered in this embodiment is Na 3 V 2 (PO 4 ) 2F 3 The particle size after crushing and screening is 2 to 30 μm, and the recovery method comprises the following steps:

[0048] 1) Under the protection of nitrogen atmosphere, the waste sodium vanadium phosphate battery positive electrode material is dissolved in an acetic acid-sodium acetate buffer solution with a pH of 3.8, and the volume ratio of the waste sodium vanadium phosphate battery positive electrode material to the acidic buffer solution is 5g:100mL, and filtered to obtain a filtrate containing Na, V, and P;

[0049] 2) The pH value of the filtrate is adjusted to 4.2, and then an oxidant and a complexing agent are added to the filtrate, wherein the oxidant is a mixture of hydrogen peroxide and sodium sulfate in a molar ratio of 1:2, and the sum of the concentrations of the two in the filtrate after addition is 0.2 mol / L, and the complexing agent is tartaric acid, and the concentration in the filtrate after addition is 0.02 mol / L, and then heated to 95° C. for reflux reaction for 4 hours under stirring at 150 r / min and nitrogen atmosphere protection. After the reaction is completed, the precipitate produced is washed with deionized water and dried at 90° C. to obtain a layered sodium vanadium phosphate positive electrode material Na 0.6 VOPO 4 The V recovery rate in the obtained product was 99.8%.

[0050] The electrochemical performance of the layered sodium vanadium phosphate positive electrode materials synthesized in Examples 1 to 3 was tested.

[0051] Test method and conditions: The obtained sodium vanadium phosphate material, carbon black and polyvinylidene fluoride (PVDF) were made into a battery positive electrode at a mass ratio of 8:1:1, and metallic sodium was used as the negative electrode; the mass loading of the active material of the cathode sheet was about 2-4 mg cm -2 ; The electrolyte is 1 mol / L NaClO 4 The ethylene carbonate (EC) / propylene carbonate (PC) (1:1 v / v) solution, the additive is 5% (volume ratio) fluoroethylene carbonate (FEC), the separator is Whatman GF / A, and the CR2032 battery is assembled in a glove box. The charge and discharge test is performed on it. The test step is to stand for 8 hours, set a constant current charge and discharge program with a rate of 0.2C, and the charge and discharge cut-off voltages are 4V and 2V respectively. The test results are shown in Table 1 and Figures 3-4 .

[0052] Table 1

[0053] Experiment number First cycle capacity (mAh / g) Capacity after 20 cycles (mAh / g) Capacity retention rate Example 1 132 131 99.2% Example 2 128 127 99.2% Example 3 129 127 98.5%

[0054] Figure 3The first cycle charge and discharge curve of the CR2032 button battery assembled with the layered sodium vanadium phosphate positive electrode material synthesized in Example 1. As can be seen from the figure, the first cycle discharge specific capacity is 132mAh / g, and the average operating voltage is 3.45V. Both the voltage and specific capacity are higher than sodium vanadium phosphate, indicating that the battery material obtained after recycling has a higher energy density.

[0055] Combination Figure 4 As can be seen from Table 1, the CR2032 button cells assembled in Examples 1, 2, and 3 have a first-cycle discharge capacity of 128 to 132 mAh / g at a rate of 0.2C, and the capacity retention rates after 20 cycles are all higher than 98%, indicating that the synthesized sodium vanadium phosphate positive electrode material has a high discharge specific capacity and capacity retention rate, and exhibits excellent cycle performance.

[0056] Comparative Example 1

[0057] The difference between Comparative Example 1 and Example 1 is that potassium permanganate is used as the oxidant.

[0058] In Comparative Example 1, potassium permanganate was used as an oxidant, and the product obtained an amorphous precipitate, and the recovery rate of V was less than 50%.

[0059] Comparative Example 2

[0060] The difference between Comparative Example 2 and Example 1 is that no complexing agent is added.

[0061] like Figure 5 As shown, in Comparative Example 2, no complexing agent is added, the obtained product has an irregular morphology, and impurity phases exist in the product.

[0062] Comparative Example 3

[0063] The only difference between Comparative Example 3 and Example 1 is that the concentration of the oxidant after addition is 2 mol / L.

[0064] like Figure 6 As shown, the oxidant concentration of ratio 3 is too high, impurity phases exist in the obtained product, and the V recovery rate is less than 50%.

[0065] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. A high-value recovery method for waste sodium vanadium phosphate battery positive electrode materials, characterized in that: The following steps are involved: 1) Under inert atmosphere protection conditions, dissolving the waste sodium vanadium phosphate battery positive electrode material in an acidic buffer solution, filtering, and obtaining a filtrate containing Na, V, and P; 2) adding an oxidant and a complexing agent to the filtrate, and performing a heating reflux reaction under stirring and inert atmosphere protection conditions, and washing and drying the precipitate after the reaction is completed to obtain a layered sodium vanadate phosphate positive electrode material.

2. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 1, characterized in that: The positive electrode material of the waste sodium vanadium phosphate battery is one or two of Na3V2(PO4)3 and Na3V2(PO4)2F3, and the particle size is 2 to 30 μm.

3. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 1, characterized in that: The acidic buffer solution is an acetic acid-sodium acetate buffer solution with a pH range of 3 to 4; the volume ratio of the mass of the waste sodium vanadium phosphate battery positive electrode material to the acidic buffer solution is (5 to 10) g: 100 mL.

4. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 1, characterized in that: The pH of the filtrate is adjusted to 4-5.5 before the oxidant and the complexing agent are added.

5. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 1, characterized in that: The oxidant is sodium persulfate, or a mixture of hydrogen peroxide and sodium sulfate; the concentration of the oxidant in the filtrate after addition is 0.02-1 mol / L.

6. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 5, characterized in that: The molar ratio of hydrogen peroxide to sodium sulfate is 1:(1-2).

7. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 1, characterized in that: The complexing agent is one or two of ethylenediaminetetraacetic acid, citric acid and tartaric acid; the concentration of the complexing agent in the filtrate after being added is 0.01-0.5 mol / L.

8. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 1, characterized in that: The stirring rate of the stirring is 100-300 r / min; the temperature of the heating reflux reaction is 80-100° C., and the time is 2-10 hours.

9. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 1, characterized in that: The layered sodium vanadium phosphate positive electrode material is Na x VOPO4, where 0.4≤x≤0.

6.

10. The high-value recovery method of waste sodium vanadium phosphate battery positive electrode materials according to claim 1, characterized in that: The morphology of the layered sodium vanadium phosphate positive electrode material is spherical particles formed by aggregation of irregular flakes, and the particle size is 10 to 30 μm.

Citation Information

Patent Citations

  • Method for recovering sodium phosphovanadate positive electrode material

    CN115417392A

  • Method for selectively extracting lithium based on synergistic oxidation leaching of waste lithium iron phosphate positive electrode powder

    CN116240384A

  • Preparation method and application of sodium vanadyl phosphate positive electrode material

    CN116395654A

Cited By

  • Method for preparing vanadium electrolyte from waste vanadium-based battery positive electrode material

    CN121790574A