Nonaqueous electrolyte secondary battery

By adding organic phosphorus compounds to the positive electrode active material layer of the nonaqueous electrolyte secondary battery and adding corresponding materials to the nonaqueous electrolyte to form a protective film and repair material, the problem of metal ions dissolution in the nonaqueous electrolyte secondary battery is solved. Improves battery stability and life.

CN118974994APending Publication Date: 2024-11-15PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380031355.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-03-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Under high voltage conditions, metal ions dissolution from the positive electrode leads to a slight short circuit, affecting battery performance, and the prior art is difficult to effectively suppress this problem.

Method used

The positive electrode active material layer of the nonaqueous electrolyte secondary battery contains 0.1% to 5% of the first organophosphorus compound, and 0.1% to 3% of the second organophosphorus compound is added to the nonaqueous electrolyte to form a protective film and Repair materials to inhibit the dissolution of metal ions.

Benefits of technology

It significantly reduces the amount of metal ions dissolution, improves the stability and life of the battery, avoids increasing resistance, and ensures the performance of the battery in high voltage environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974994A_ABST
    Figure CN118974994A_ABST
Patent Text Reader

Abstract

This nonaqueous electrolyte secondary battery is provided with a positive electrode, a negative electrode, and a nonaqueous electrolyte, and is characterized in that: the positive electrode is provided with a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector, and the positive electrode active material layer contains active material particles, a binder, and a first organic phosphorus compound; the content (Cpn) of the first organophosphorus compound contained in the positive electrode active material layer is from 0.1% by mass to 5% by mass (inclusive), and the non-aqueous electrolyte contains a non-aqueous solvent, an electrolyte salt, and a second organophosphorus compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a nonaqueous electrolyte secondary battery. Background Art

[0002] Patent Document 1 describes that generation of gas accompanying charge and discharge can be suppressed by using a positive electrode active material having a coating formed of at least one compound selected from a specific phosphonic acid ester and a specific phosphite triester.

[0003] Patent Document 2 describes that by using an electrolyte solution containing a solvent containing a specific phosphonic acid compound, the chemical stability of the electrolyte solution is improved, and thus the decomposition reaction of the electrolyte solution can be suppressed during charge and discharge.

[0004] Patent document 3 proposes a battery comprising a positive electrode containing a positive electrode active material, a negative electrode, and an electrolyte containing a solvent and an electrolyte salt, wherein the negative electrode contains a lithium transition metal compound having a spinel structure as the negative electrode active material, and at least one of the above-mentioned positive electrode and the above-mentioned electrolyte contains a phosphorus compound having a P-OH structure.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2017 / 126276

[0008] Patent Document 2: Japanese Patent Application Publication No. 2009-224258

[0009] Patent Document 3: Japanese Patent Application Publication No. 2013-152825 Summary of the invention

[0010] Problems to be solved by the invention

[0011] The positive electrode of a non-aqueous electrolyte secondary battery mostly contains particles of metal compounds as active material particles. Sometimes metal ions dissolve from such a positive electrode into the non-aqueous electrolyte. The metal ions dissolved from the positive electrode precipitate at the negative electrode, causing a micro short circuit. The higher the upper limit voltage of the secondary battery (for example, when it is greater than 4.3V), the more significant the dissolution of metal ions from the positive electrode becomes. The upper limit voltage is usually the battery voltage in the fully charged state (charge termination voltage), corresponding to a 100% state of charge (SOC).

[0012] Means for solving problems

[0013] One aspect of the present disclosure relates to a nonaqueous electrolyte secondary battery, comprising a positive electrode, a negative electrode and a nonaqueous electrolyte, wherein the positive electrode comprises a positive electrode collector and a positive electrode active material layer supported on the positive electrode collector, the positive electrode active material layer comprises active material particles, a binder and a first organic phosphorus compound, the content Cpn of the first organic phosphorus compound contained in the positive electrode active material layer is greater than or equal to 0.1% by mass and less than or equal to 5% by mass, and the nonaqueous electrolyte comprises a nonaqueous solvent, an electrolyte salt and a second organic phosphorus compound.

[0014] Another aspect of the present disclosure relates to a nonaqueous electrolyte secondary battery comprising a positive electrode, a negative electrode and a nonaqueous electrolyte, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector, the positive electrode active material layer comprises active material particles, a binder and a first organic phosphorus compound, the content of the first organic phosphorus compound contained in the positive electrode active material layer is 0.1 mass % or more and 5 mass % or less, the nonaqueous electrolyte comprises a nonaqueous solvent, an electrolyte salt and a second organic phosphorus compound, the first organic phosphorus compound and the second organic phosphorus compound are each independently represented by general formula (1),

[0015]

[0016] In the general formula (1), R 1 and R 2 Each independently represents the surface of the active material particle, -H, -CH2X, -CH2CH2X or -Si((CH2) n CH3)3,R 3 -(CH2) m CH2X or -O-Si((CH2) n CH3)3, X is -H, -NH2, -COOH, -CN or -F, for R 1 , R 2 and R 3 The integer n for defining is independently 0 or 1, for R 3 The integer m for definition is 0 to 16, and when there are a plurality of Xs, the plurality of Xs are independent of each other.

[0017] Another aspect of the present disclosure relates to a non-aqueous electrolyte secondary battery, which comprises a positive electrode, a negative electrode and a non-aqueous electrolyte, the positive electrode comprising a positive electrode collector and a positive electrode active material layer supported on the positive electrode collector, the positive electrode active material layer comprising active material particles, a binder and phosphorus element, the content of the phosphorus element contained in the positive electrode active material layer is greater than 100 ppm and less than 4000 ppm on a mass basis, the non-aqueous electrolyte comprises a non-aqueous solvent, an electrolyte salt and phosphorus element, and the ratio (Cpn / Cen) of the content Cpn (mass %) of the phosphorus element contained in the positive electrode active material layer to the content Cen (mass %) of the phosphorus element contained in the non-aqueous electrolyte is greater than 0.1 / 4.0 and less than 4.0 / 3.0.

[0018] Effects of the Invention

[0019] According to the present disclosure, for example, the elution of metal ions from the positive electrode of a nonaqueous electrolyte secondary battery in a charged state can be suppressed.

[0020] The novel features of the present invention are described in the appended claims, but the present invention relates to both the configuration and the content, and can be better understood through the following detailed description together with other objects and features of the present invention and with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] [ Figure 1 ] is a longitudinal cross-sectional view schematically showing the internal structure of a non-aqueous electrolyte secondary battery involved in an embodiment of the present disclosure. DETAILED DESCRIPTION

[0022] Hereinafter, the embodiments of the non-aqueous electrolyte secondary battery involved in the present disclosure are illustrated, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials are sometimes illustrated, but other numerical values ​​and materials may also be applied as long as the effects of the present disclosure can be obtained. In this specification, the description of "numerical value A to numerical value B" includes numerical value A and numerical value B, which can be replaced by "numerical value A or more and numerical value B or less". In the following description, when the lower limit and upper limit of numerical values ​​related to specific physical properties, conditions, etc. are illustrated, as long as the lower limit is not above the upper limit, any lower limit illustrated can be arbitrarily combined with any upper limit illustrated. When multiple materials are illustrated, one of them can be selected and used alone, or two or more can be combined and used.

[0023] The nonaqueous electrolyte secondary battery widely includes secondary batteries containing a nonaqueous electrolyte, but hereinafter, as an example of the nonaqueous electrolyte secondary battery, a lithium ion secondary battery, a lithium secondary battery (lithium metal secondary battery), etc. are mainly described. The nonaqueous electrolyte may be in a state of liquid, gel, or the like.

[0024] The non-aqueous electrolyte secondary battery has a positive electrode, a negative electrode, and a non-aqueous electrolyte. A separator may also be sandwiched between the positive electrode and the negative electrode. The positive electrode, the negative electrode, and the separator can form an electrode group of various forms. For example, the positive electrode and the negative electrode can be wound across the separator to form a columnar electrode group (wound electrode group). The non-aqueous electrolyte secondary battery may also have a battery case that accommodates the electrode group and the non-aqueous electrolyte.

[0025] The positive electrode includes a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector. The positive electrode active material layer is formed, for example, directly or indirectly (via other materials) on the surface of the sheet-like positive electrode current collector.

[0026] The positive electrode current collector is made of a sheet-like conductive material and can be a non-porous conductive substrate (metal foil, etc.) or a porous conductive substrate (mesh, net, punched sheet, etc.).

[0027] The positive electrode active material layer is carried on one or both surfaces of the positive electrode current collector. The positive electrode active material layer is usually a positive electrode mixture layer composed of a positive electrode mixture, and is in a layer or film form.

[0028] The positive electrode mixture (i.e., the positive electrode active material layer) includes active material particles (particles of the positive electrode active material), a binder, and a first organic phosphorus compound. The active material particles include a metal compound. The metal compound may include, for example, a transition metal oxide containing lithium. In the binder, a resin material may be used. The resin material may include, for example, a fluororesin.

[0029] The first organophosphorus compound is an organic compound containing phosphorus. Examples of the organic compound containing phosphorus include phosphoric acid, phosphonic acid, phosphoric acid esters, and phosphonic acid esters. Among them, in the present disclosure, at least the first organophosphorus compound represented by the following formula (1) is used. The first organophosphorus compound may be a liquid or a solid at room temperature. In this specification, room temperature refers to a temperature of 20°C or more and 30°C or less.

[0030] The content of the first organic phosphorus compound contained in the positive electrode active material layer is, for example, 0.1 mass % to 5 mass %, or 0.2 mass % to 3 mass %, or 0.5 mass % to 2 mass %. When the first organic phosphorus compound is contained in the positive electrode active material layer at such a content, a state different from that in the case where the organic phosphorus compound is only dissolved in the non-aqueous electrolyte is formed.

[0031] Specifically, a film containing the first organic phosphorus compound (or a film derived from the first organic phosphorus compound) is formed in a manner that covers at least a portion of the surface of the particles of the positive electrode active material. The thickness of such a film is sufficiently thicker than the molecular layer corresponding to the molecular size of the first organic phosphorus compound, and plays a strong protective role in suppressing side reactions that the positive electrode active material may participate in. The thick film obtained from the first organic phosphorus compound may not cover the entire surface of the particles of the positive electrode active material, but may be attached to the surface of the particles of the positive electrode active material in a dotted manner (in other words, in an island shape).

[0032] In order to include the first organophosphorus compound in a high content in the positive electrode active material layer, it is important to mix a considerable amount of the first organophosphorus compound itself in the positive electrode mixture constituting the positive electrode active material layer. In the case where the first organophosphorus compound is included in a high content in the positive electrode active material layer, one of the effective means is to mix a sufficient amount of the first organophosphorus compound itself in the positive electrode mixture slurry.

[0033] In the past, attempts have been made to dissolve an organic phosphorus compound in a predetermined solvent to prepare a solution and to impregnate the solution into the positive electrode active material or the positive electrode. In this case, in order to improve the impregnation and further improve the uniformity of the distribution of the organic phosphorus compound, an attempt can be made to limit the amount of the organic phosphorus compound dissolved in the solution so that the viscosity of the solution is quite low. Even with such a solution, only a thin film corresponding to the molecular size of the organic phosphorus compound can be formed.

[0034] In addition, in the past, attempts have been made to dissolve an organophosphorus compound in a non-aqueous electrolyte. However, when only dissolving an organophosphorus compound in a non-aqueous electrolyte, it is still difficult to include an organophosphorus compound at a high content in the positive electrode active material layer. Considering the viscosity, ion conductivity, influence on the negative electrode, suppression of side reactions, etc. of the non-aqueous electrolyte, the content of the soluble organophosphorus compound in the non-aqueous electrolyte naturally has an upper limit. According to the content below such an upper limit, it is difficult to include an organophosphorus compound at a high content in the positive electrode active material layer.

[0035] At least part of the side reactions in which the positive electrode active material participates is a reaction accompanied by the dissolution of metal ions. Such side reactions are accompanied by the decomposition of the non-aqueous electrolyte. In addition, part of the side reactions may be reactions that disrupt the order of the crystal structure of the positive electrode active material. The disorder of the order of the crystal structure refers to a change in the configuration of the constituent elements of the positive electrode active material. For example, in the case where the positive electrode active material is a transition metal oxide containing lithium, the configuration of lithium atoms and transition metal atoms will partially replace. Such disorder (or mixed arrangement of atoms) is accompanied by an increase in the resistance of the positive electrode, a decrease in the capacity of the positive electrode, etc. In addition, it will promote the dissolution of metal ions.

[0036] At least a portion of the first organic phosphorus compound contained in the positive electrode active material layer will be oxidized or decomposed in the positive electrode active material layer, or react with the surface of the positive electrode active material or the components attached to the surface. In this case, the residue containing the phosphorus atom (P) of the first organic phosphorus compound is contained in the positive electrode active material layer. Therefore, "the content of the first organic phosphorus compound contained in the positive electrode active material layer" can also be said to be "the content of the phosphorus element contained in the positive electrode active material layer". In this case, the content of the phosphorus element contained in the positive electrode active material layer is, for example, 100 ppm or more and 4000 ppm or less on a mass basis, or 500 ppm to 3000 ppm, or 1000 ppm to 2000 ppm.

[0037] The content of the first organic phosphorus compound or phosphorus element contained in the positive electrode active material layer can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron beam microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), infrared absorption spectroscopy (FT-IR), gas chromatography-mass spectrometry (GC-MS), or other analytical methods.

[0038] The positive electrode to be measured is taken out from a non-aqueous electrolyte secondary battery with a depth of discharge (DOD) of more than 90%. The so-called depth of discharge (DOD) is the ratio of the discharged amount of electricity to the rated amount of electricity of the battery in the fully charged state. It should be noted that the charging amount (i.e. the full charge amount) when charging a battery in a fully discharged state (DOD=100%) to a fully charged state (SOC=100%, DOD=0%) is equivalent to the rated capacity. The voltage of a battery in a fully charged state corresponds to the charge termination voltage. The voltage of a battery in a fully discharged state corresponds to the discharge termination voltage.

[0039] When the positive electrode active material layer contains the first organic phosphorus compound or phosphorus element at the above content, it is considered that a thick film containing phosphorus element is easily formed. Such a film is formed in an island shape, for example, to cover at least a part of the surface of the positive electrode active material particles.

[0040] On the other hand, the nonaqueous electrolyte contains a nonaqueous solvent, an electrolyte salt, and a second organic phosphorus compound. That is, a major feature of the nonaqueous electrolyte secondary battery of the present disclosure is that the organic phosphorus compound is contained not only in the positive electrode active material layer but also in the nonaqueous electrolyte.

[0041] The first organic phosphorus compound contained in the positive electrode active material layer can form a thick film that protects the particles of the positive electrode active material from side reactions, but on the other hand, it is difficult to protect the entire surface of the active material particles by attaching to the surface of the particles of the positive electrode active material in an island shape. It is better to say that protecting the entire surface of the active material particles with a thick film will lead to an increase in resistance, so it cannot be said to be ideal. In this regard, the second organic phosphorus compound has the effect of covering the surface of the active material particles that are not covered by the thick film of the first organic phosphorus compound with a thin film. That is, it can be said that the second organic phosphorus compound functions as a coating repair material that increases the coating rate of the active material particles based on the film. As a result, it is possible to protect substantially the entire surface of the active material particles without significantly increasing the resistance. In other words, the second organic phosphorus compound is attached to the surface of the active material particles in a manner that fills the gaps (exposed surfaces of the active material particles) that are not covered by the thick film formed by the first organic phosphorus compound. As a result, the effect of inhibiting the dissolution of metal ions can be significantly improved.

[0042] The content of the second organic phosphorus compound contained in the non-aqueous electrolyte is, for example, 0.1 mass % or more and 3 mass % or less, and may be 0.2 mass % to 2 mass % or 0.5 mass % to 1.5 mass %. When the second organic phosphorus compound is included in the non-aqueous electrolyte at such a content, the film can be formed sufficiently thinly in a manner that the gaps on the surface of the active material particles not covered by the thick film are repaired and the resistance is not increased. In addition, the viscosity of the non-aqueous electrolyte can be maintained sufficiently low, and the influence of the side reaction in the negative electrode can be limited to a minimum.

[0043] In the above case, the ratio (Cpn / Cen) of the content Cpn (mass %) of the first organic phosphorus compound contained in the positive electrode active material layer to the content Cen (mass %) of the second organic phosphorus compound contained in the non-aqueous electrolyte can be, for example, greater than 0.1 / 4.0 and less than 4.0 / 3.0 (preferably 0.5 / 4.0 to 3.0 / 3.0).

[0044] The content of the second organic phosphorus compound contained in the non-aqueous electrolyte can also be evaluated based on the content of phosphorus atoms (P) contained in the second organic phosphorus compound. Therefore, the "content of the second organic phosphorus compound contained in the non-aqueous electrolyte" can also be expressed as "the content of phosphorus element contained in the non-aqueous electrolyte". The content of phosphorus element contained in the non-aqueous electrolyte is, for example, 100 ppm or more and 3000 ppm or less on a mass basis, or 500 ppm to 2500 ppm, or 750 ppm to 1500 ppm.

[0045] The nonaqueous electrolyte secondary battery involved in the present disclosure can also be stated as "a nonaqueous electrolyte secondary battery, which comprises a positive electrode, a negative electrode and a nonaqueous electrolyte, the positive electrode comprises a positive electrode collector and a positive electrode active material layer supported on the positive electrode collector, the positive electrode active material layer comprises active material particles, a binder and phosphorus element, the content of phosphorus element contained in the positive electrode active material layer is greater than 100 ppm and less than 4000 ppm on a mass basis, the nonaqueous electrolyte comprises a nonaqueous solvent, an electrolyte salt and phosphorus element, and the ratio (Cpn / Cen) of the content Cpn (mass %) of phosphorus element contained in the positive electrode active material layer to the content Cen (mass %) of phosphorus element contained in the nonaqueous electrolyte is greater than 0.1 / 4.0 and less than 4.0 / 3.0".

[0046] The content of the second organic phosphorus compound or phosphorus element contained in the non-aqueous electrolyte can be measured by inductively coupled plasma atomic emission spectrometry (ICP-AES), gas chromatography-mass spectrometry (GC-MS), infrared absorption spectroscopy (FT-IR), or other analytical methods. The positive electrode to be measured is taken out from a secondary battery with a depth of discharge (DOD) of 90% or more.

[0047] As described above, the thickness of at least a portion of the film covering the surface of the active material particles is not uniform. The thickness of at least a portion of the film may be 0.2 nm or more, or may be 200 nm or more. The thickness of the film may be determined, for example, by the following method. However, the determination method is not particularly limited, and the method for inferring the approximate thickness of the film may be applied to the determination of the thickness of the film without limitation.

[0048] (1) Photographing of a cross section of a positive electrode using a scanning electron microscope (SEM)

[0049] First, a positive electrode to be measured is prepared. The positive electrode to be measured is taken out from a secondary battery having a depth of discharge (DOD) of 90% or more.

[0050] Next, the positive electrode active material layer and the positive electrode current collector are simultaneously cut along the thickness direction of the positive electrode to form a cross section. At this time, a thermosetting resin may also be filled in the positive electrode active material layer and cured. A cross-sectional sample of the positive electrode is obtained by, for example, a CP (cross-section polisher) method, a FIB (focused ion beam) method, or the like. The cross-sectional sample is observed using an SEM. The magnification of the observation using an SEM may be, for example, 500 to 5000 times. For the SEM image, a 40 μm 2 ~400μm 2 Shoot in the field of view.

[0051] (2) Elemental analysis using energy dispersive X-ray spectroscopy (EDX)

[0052] Using a SEM image of a cross-sectional sample of the positive electrode, elemental analysis was performed using EDX.

[0053] (3) Preparation of phosphorus spectrum

[0054] A phosphorus element spectrum is obtained by extracting a phosphorus-derived component (P component) from the EDX analysis data of the cross-section sample of the positive electrode. This makes it possible to count all phosphorus-derived components within the field of view.

[0055] (4) Measurement of film thickness

[0056] The obtained phosphorus element spectrum can be presented as a two-dimensional image. In the two-dimensional image, it is possible to distinguish the P component that constitutes the film (for example, the component concentrated near the surface of the active material particles) and the P component that does not constitute the film (for example, the component floating in the non-aqueous electrolyte between the active material particles). Select any five active material particles, find the maximum thickness of the film based on the P component concentrated near its surface, and calculate the average of the five measured values.

[0057] The first organophosphorus compound and the second organophosphorus compound are each independently represented by the general formula (1).

[0058]

[0059] That is, the first organophosphorus compound and the second organophosphorus compound may be the same compound or different compounds. In addition, the first organophosphorus compound and the second organophosphorus compound may be products derived from the same compound or different compounds.

[0060] In the general formula (1), R 1 ~R 3 The definitions are as follows: Hereinafter, the organophosphorus compound defined by the general formula (1) (the first organophosphorus compound and the second organophosphorus compound) is also collectively referred to as an organophosphorus compound (P).

[0061] Therefore, the non-aqueous electrolyte secondary battery involved in the present disclosure can be stated as "a non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, the positive electrode comprising a positive electrode collector and a positive electrode active material layer supported on the positive electrode collector, the positive electrode active material layer comprising active material particles, a binder and a first organic phosphorus compound (P), the content of the first organic phosphorus compound (P) contained in the positive electrode active material layer is greater than 0.1% by mass and less than 5% by mass, and the non-aqueous electrolyte comprises a non-aqueous solvent, an electrolyte salt and a second organic phosphorus compound (P)".

[0062] Similarly, the non-aqueous electrolyte secondary battery involved in the present disclosure can also be expressed as "a non-aqueous electrolyte secondary battery, which comprises a positive electrode, a negative electrode and a non-aqueous electrolyte, the positive electrode comprises a positive electrode collector and a positive electrode active material layer supported on the positive electrode collector, the positive electrode active material layer comprises active material particles, a binder and phosphorus element, the content of phosphorus element contained in the positive electrode active material layer is greater than 100 ppm and less than 4000 ppm on a mass basis, and the non-aqueous electrolyte comprises a non-aqueous solvent, an electrolyte salt and an organic phosphorus compound (P) (a second organic phosphorus compound)".

[0063] Here, R 1 and R 2 Each independently represents the surface of an active material particle, -H, -CH2X, -CH2CH2X or -Si((CH2) n CH3)3 (hereinafter also referred to as "organosilyl group (EM)").

[0064] In addition, R 3 -(CH2) m CH2X or -O-Si((CH2) n CH3))3(organosilyloxy). Organosilyloxy(-O-Si((CH2) n CH3)3) contains an organosilyl group (EM).

[0065] R 1 , R 2 and R 3 The integer n used for definition is independently 0 or 1. 1 , R 2 and R 3 The organosilyl groups (EM) may all be the same group, three may all be different groups, or any two may be the same group and one may be a different group.

[0066] R 3 The integer m used for definition is 0 to 16, and may be 4 to 16, or 9 to 14. 3 (-(CH2) m The organic phosphorus compound (P) containing CH2X group or the film derived therefrom has high stability and remains in the positive electrode active material layer for a long time, and has a great effect of suppressing the side reactions in which the positive electrode active material participates. 3 The organic phosphorus compound (P) which is an alkyl group having 5 to 17 carbon atoms is mostly solid at room temperature and has a sufficiently slow dissolution rate in the solvent in the non-aqueous electrolyte, and can exert the effect of replenishing the surface of the active material particle with a film derived from the organic phosphorus compound (P).

[0067] The organosilyl group (EM) may be any of -Si(CH3)3, -Si(CH2CH3)3, -SiCH3(CH2CH3)2 and -SiCH2CH3(CH3)2.

[0068] The surface of the positive electrode active material that can bond with the PO-group is R 1 or R 2 The so-called surface refers specifically to the components constituting the surface or adhering to the surface, for example, each of which can be a metal atom or cation, oxygen atom or anion, etc. that can constitute a positive electrode active material.

[0069] X is -H, -NH2, -COOH, -CN or -F. When the organophosphorus compound (P) has a plurality of Xs, the plurality of Xs are independent of each other. That is, the plurality of Xs may be the same, or all three may be different, or any two may be the same and one may be different.

[0070] You can also 1 and R 2 Each is independently -Si((CH2) n CH3)3,R 3 -O-Si((CH2) n CH3)3. In this case, the organic phosphorus compound (P) is a trialkylsilyl phosphate (O=P(OSiR3), R=alkyl). The trialkylsilyl phosphate may be, for example, tris(trimethylsilyl) phosphate (trimethylsilyl phosphate (TMSP) (O=P(OSi(CH3)3))), triethylsilyl phosphate (O=P(OSi(CH2CH3)3)), or the like.

[0071] You can also 1 and R 2 Each is -H, R 3 -(CH2) m In this case, the organic phosphorus compound (P) is an alkyl phosphonate (O=P(OH)2R, R=alkyl). Examples of the alkyl phosphonate include hexyl phosphonate, heptyl phosphonate, octyl phosphonate, nonyl phosphonate, and decyl phosphonate.

[0072] The organophosphorus compound (P) contained in the positive electrode active material layer is stable even under a high voltage environment. In addition, the organophosphorus compound (P) contained in the positive electrode active material layer has many opportunities to contact the active material particles, and therefore has an excellent effect of inhibiting the oxidative decomposition of the non-aqueous electrolyte. In addition, in the case where at least a portion of the organophosphorus compound (P) is solid at room temperature, or the organophosphorus compound (P) can undergo a condensation reaction on the surface of the active material particles, a tendency to form a film with a higher protective effect can be observed.

[0073] It is believed that when the organic phosphorus compound (P) can undergo a condensation reaction on the surface of the active material particles, a film having a thickness of multiple molecular layers can be formed on the surface of the active material particles, which has a high protective effect and is stable even in a high voltage atmosphere (for example, greater than 4.3 V).

[0074] On the other hand, it is believed that when the organic phosphorus compound (P) is solid at room temperature, in the positive electrode slurry for forming the positive electrode or in the non-aqueous electrolyte secondary battery, the particulate organic phosphorus compound (P) is partially dissolved in the dispersion medium (e.g., N-methyl-2-pyrrolidone) and the non-aqueous electrolyte, and adheres to at least a portion of the surface of the active material particles to form a high protective film. Moreover, in the non-aqueous electrolyte secondary battery, the dissolution rate in the non-aqueous solvent (e.g., carbonate) is slow, and there is a tendency to dissolve slowly for a long time. Therefore, even in the case of damage to the film from the organic phosphorus compound (P) covering the surface of the active material particles in the early stage, the film can be repaired at any time. Therefore, even when the upper limit voltage of the non-aqueous electrolyte secondary battery is high (e.g., greater than 4.3V), it is possible to continuously obtain a sufficient effect of protecting the active material particles and suppressing the decomposition reaction of the non-aqueous electrolyte.

[0075] At least a portion of the organophosphorus compound (P) may exist in the positive electrode active material layer in the form of particles having a particle size of 0.1 μm or more and 5 μm or less. In the case where the organophosphorus compound (P) has such a particle size, it can be said that the organophosphorus compound (P) is excessively contained in the positive electrode active material layer. Since the particulate organophosphorus compound (P) slowly dissolves over a long period of time, and the film from the organophosphorus compound (P) is replenished on the surface of the active material particles at any time, the effect of suppressing side reactions for a longer period of time can be obtained. The particle size of the organophosphorus compound (P) may be greater than 0.3 μm, or may be greater than 1 μm. In addition, the maximum value of the particle size of the organophosphorus compound (P) may be less than 3 μm, or may be less than 2 μm. If the maximum value of the particle size is within the above range, the effect on battery performance can be sufficiently reduced. The particle size of the organophosphorus compound (P) can be measured, for example, according to the following points.

[0076] (1) Preparation of positive electrode cross-sectional sample

[0077] First, prepare the positive electrode to be measured. The positive electrode to be measured is taken out from a secondary battery with a depth of discharge (DOD) of 90% or more. Next, the positive electrode active material layer and the positive electrode collector are cut simultaneously along the thickness direction of the positive electrode to form a cross section. At this time, a thermosetting resin can also be filled in the positive electrode active material layer and cured. The cross-sectional sample of the positive electrode is obtained by, for example, the CP (cross-section polisher) method, the FIB (focused ion beam) method, etc.

[0078] (2) Photographing of a cross-sectional sample of a positive electrode using a scanning electron microscope (SEM)

[0079] Next, the cross-section sample is observed using SEM. The observation using SEM is performed at a low magnification (e.g., 200 to 1000 times). The SEM image is taken so as to observe a region with a length of 300 μm or more (preferably 400 μm or more) in the surface direction of the positive electrode active material layer.

[0080] (3) Elemental analysis using energy dispersive X-ray spectroscopy (EDX)

[0081] Using the SEM image of the cross-sectional sample, elemental analysis is performed using EDX. A component (P component) derived from the organophosphorus compound (P) is extracted from the EDX analysis data of the cross-sectional sample, thereby obtaining a spectrum of the organophosphorus compound (P). The particles of the organophosphorus compound (P) are determined from the obtained spectrum. The diameter of an equivalent circle having the same area as the determined particle is taken as the particle size of the organophosphorus compound (P).

[0082] The particle size of the organic phosphorus compound (P) is 0.1 μm or more and the particle size of the organic phosphorus compound (P) is 400 μm. 2 It is sufficient to observe one or more particles in the observation field (for example, a rectangle of 20 μm×20 μm), it is desirable to observe three or more particles, and it is further desirable to observe six or more particles. The more particles of the organic phosphorus compound (P) with a particle size of 0.1 μm or more observed in the above-mentioned observation field, the greater the effect of suppressing the decomposition of the electrolyte under a high voltage environment. The upper limit of the number of particles of the organic phosphorus compound (P) with a particle size of 0.1 μm or more observed in the above-mentioned observation field is, for example, 16 or less. The above-mentioned numbers may also be the average of the number of particles of the organic phosphorus compound (P) with a particle size of 0.1 μm or more counted in multiple (for example, three or more) observation fields. It is desirable to set the observation field near the center of the positive electrode active material layer in the cross-sectional sample.

[0083] <Method for manufacturing positive electrode>

[0084] Next, an example of a method for manufacturing a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure will be described.

[0085] The manufacturing method comprises the following steps: a step of preparing a positive electrode having a positive electrode active material layer containing a first organic phosphorus compound; a step of preparing a negative electrode; a step of preparing a non-aqueous electrolyte containing a second organic phosphorus compound; and a step of assembling a secondary battery using the obtained positive electrode, negative electrode and non-aqueous electrolyte.

[0086] The process for preparing the positive electrode includes the following processes: a process (I) of preparing a positive electrode paste containing active material particles (particles of the positive electrode active material), a binder, a first organic phosphorus compound (organic phosphorus compound (P)), and a dispersion medium; a process (II) of preparing a positive electrode current collector; a process (III) of coating the positive electrode current collector with the positive electrode paste to form a coating film; a process (IV) of drying the coating film to form an unrolled layer; and a process (V) of rolling the unrolled layer to form a positive electrode active material layer.

[0087] (I) Paste preparation process

[0088] The positive electrode paste can be prepared by mixing a positive electrode mixture containing active material particles, a binder, and the first organic phosphorus compound with a liquid dispersion medium and dispersing it in the dispersion medium. The positive electrode mixture may further contain other components (for example, a conductive material). As the liquid dispersion medium, an organic solvent having excellent affinity with both the binder and the first organic phosphorus compound is used.

[0089] As the organic solvent, N-methyl-2-pyrrolidone (NMP) is preferably used, but alcohols such as ethanol, ethers such as tetrahydrofuran, amides such as dimethylformamide, and ketones such as cyclohexanone can also be used.

[0090] The first organic phosphorus compound can be pre-mixed with the dispersion medium to dissolve at least a part thereof. For example, a particulate first organic phosphorus compound having an average particle size of D1 can be mixed with the dispersion medium to prepare a dispersion of a particulate first organic phosphorus compound having an average particle size of d1 (d1 < D1 or d1 < 0.8D1). Thereby, it is easy to coat at least a part of the surface of the active material particles with the first organic phosphorus compound or a film derived therefrom. Here, the average particle size is the median particle size (D 50 ) at which the cumulative volume is 50% in the volume-based particle size distribution obtained by a laser diffraction particle size distribution measuring device.

[0091] The binder is not particularly limited, and for example, a fluororesin, a hydrogenated nitrile butadiene rubber, etc. can be used. As the fluororesin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), perfluoroalkoxy alkane (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), vinylidene fluoride-hexafluoropropylene copolymer, etc. can be cited.

[0092] (II) Process of preparing a positive electrode current collector

[0093] As the positive electrode collector, a sheet-like conductive material (metal foil, mesh, net, punching sheet, etc.) is used. Among them, metal foil is preferred. As the material of the positive electrode collector, stainless steel, aluminum, aluminum alloy, titanium, etc. can be exemplified. The thickness of the positive electrode collector is not particularly limited, for example, 1 to 50 μm, and can also be 5 to 30 μm.

[0094] (III) Step of forming a coating film of positive electrode slurry

[0095] The positive electrode slurry is applied to the surface of the positive electrode collector to form a coating film. As a coating device for the positive electrode slurry, for example, a bar coater, a gravure coater, a knife coater, a roll coater, a comma coater, a die coater, a lip coater, etc. can be used.

[0096] In the positive electrode slurry applied to the surface of the positive electrode current collector, at least a portion of the first organic phosphorus compound may be in the form of particles having a particle size of 0.1 μm to 5 μm. Thus, a positive electrode active material layer containing the first organic phosphorus compound having a particle size of 0.1 μm to 5 μm can be easily obtained.

[0097] (IV) Coating Drying Step

[0098] Next, the coating is dried to volatilize the dispersion medium to form an unrolled coating. It is also possible to appropriately control the conditions during drying so that the first organophosphorus compound migrates from the positive electrode collector side to the outermost side (i.e., the diaphragm side) together with the dispersion medium. As a result, the first organophosphorus compound becomes a state that is biased toward the outermost side compared to the positive electrode collector side of the positive electrode active material layer. The closer the region is to the outermost side of the positive electrode active material layer, the easier it is to carry out the oxidative decomposition reaction of the electrolyte. This is because, in such a region, the flow rate of the electrolyte is large. By making the first organophosphorus compound biased toward the outermost side, the effect of suppressing the oxidative decomposition reaction of the electrolyte becomes more significant.

[0099] (V) Rolling process of unrolled layer

[0100] Next, the unrolled layer is rolled to form a positive electrode active material layer. The rolling conditions are not particularly limited, and the density of the active material particles (positive electrode active material) in the positive electrode active material layer after rolling is, for example, 3.3 g / cm 3 Above and 4.0g / cm 3 Below, can also be 3.5g / cm 3 Above and 4.0g / cm 3 the following.

[0101] When the first organic phosphorus compound is biased towards the outermost surface side of the positive electrode active material layer, and the thickness of the positive electrode active material layer is denoted as T, the existence probability Pb ​​of the first organic phosphorus compound in the region from the surface of the positive electrode collector to 0.5T of the positive electrode active material layer (hereinafter also referred to as the "lower layer region"), and the existence probability Pt of the first organic phosphorus compound in the region from the position 0.5T away from the surface of the positive electrode collector to the outermost surface of the positive electrode active material layer (hereinafter also referred to as the "upper layer region") can satisfy, for example, 1.2≤Pt / Pb.

[0102] Pb and Pt can be determined by analyzing the cross-sectional sample of the positive electrode obtained by the above method using SEM and EDX. Specifically, in the spectrum of the first organophosphorus compound obtained from the EDX analysis data of the cross-sectional sample, the area occupied by the first organophosphorus compound in the lower region and the upper region is measured. At this time, regardless of the particle size of the first organophosphorus compound, all the first organophosphorus compounds are counted. Then, the proportion of the area of ​​the first organophosphorus compound in the area of ​​the lower region and the upper region is regarded as Pb and Pt, respectively. At 400μm 2 Pb and Pt are measured in an observation field (e.g., a rectangle of 20 μm×20 μm). Pb and Pt may also be average values ​​of Pb and Pt obtained in multiple (e.g., more than 3) observation fields. It is desirable to set the observation field near the center of each of the lower and upper regions in the cross-sectional sample.

[0103] The process of preparing the negative electrode, for example, includes the following steps: a step (I) of preparing a negative electrode slurry containing active material particles (particles of negative electrode active material), a binder and a dispersion medium; a step (II) of preparing a negative electrode collector; a step (III) of applying the negative electrode slurry on the surface of the negative electrode collector to form a coating film; a step (IV) of drying the coating film to form an unrolled layer; and a step (V) of rolling the unrolled layer to form a negative electrode active material layer.

[0104] Each step can be carried out according to the step of preparing the positive electrode. However, the negative electrode does not necessarily need a negative electrode active material layer. For example, the negative electrode of a lithium (metal) secondary battery can have at least a negative electrode collector. In this case, the steps other than step (II) of preparing the negative electrode collector can be omitted.

[0105] In the process of preparing the non-aqueous electrolyte, for example, the electrolyte salt can be dissolved in the non-aqueous solvent and the second organic phosphorus compound can be dissolved. It is desirable to dissolve the second organic phosphorus compound in the non-aqueous electrolyte. However, the non-aqueous electrolyte is not limited to a liquid and can be in any form of a gel or a solid.

[0106] The process of assembling a nonaqueous electrolyte secondary battery includes, for example, the following steps: a step of preparing an electrode group including a positive electrode, a negative electrode, and a separator sandwiched between the positive electrode and the negative electrode; a step of accommodating the electrode group together with the nonaqueous electrolyte in a battery case; and a step of sealing the battery case.

[0107] Hereinafter, the configuration of the nonaqueous electrolyte secondary battery will be further described by taking a lithium ion secondary battery as an example.

[0108] [positive electrode]

[0109] As the positive electrode, a positive electrode having the above-mentioned characteristics is used. The positive electrode active material layer is composed of a positive electrode mixture. The positive electrode mixture contains active material particles (particles of positive electrode active material), a binder and a first organic phosphorus compound as essential components, and may also contain optional components. As optional components, a conductive material, a thickener, etc. may be included.

[0110] The thickness of the positive electrode active material layer is not particularly limited, and may be, for example, 20 μm or more and 120 μm or less, or 40 μm or more and 80 μm or less. A positive electrode active material layer may also be formed using a plurality of layers having different morphologies. For example, two or more layers containing active material particles having different average particle diameters may be stacked, or two or more layers having different types or compositions of positive electrode active materials may be stacked.

[0111] The average particle size of the active material particles (particles of the positive electrode active material) is, for example, 3 μm or more and 30 μm or less, or 5 μm or more and 25 μm or less. The average particle size is the median particle size (D) at which the cumulative volume is 50% in the volume-based particle size distribution obtained by a laser diffraction particle size distribution measuring device. 50 ). The active material particles may be separated and recovered from the positive electrode. As a measuring apparatus, for example, "LA-750" manufactured by HORIBA, Ltd. may be used.

[0112] It should be noted that the average particle size of the active material particles can be measured by the cross-sectional sample of the above-mentioned positive electrode. The cross-sectional SEM image can be taken in a manner where 10 or more active material particles are observed, and the diameter of the equivalent circle having the same area as the cross-sectional area of ​​10 or more active material particles is obtained by image processing, and their average value is used as the average particle size.

[0113] The positive electrode active material constituting the active material particles may include a lithium-containing transition metal oxide. From the viewpoint of increasing the capacity, the lithium-containing transition metal oxide preferably includes a lithium nickel oxide (composite oxide N), which contains lithium and Ni and has a layered rock salt-type crystal structure. The proportion of the composite oxide N in the positive electrode active material is, for example, 70% by mass or more, may be 90% by mass or more, or may be 95% by mass or more. The proportion of Ni contained in the composite oxide N among the metal elements other than Li may be 50 atomic% or more.

[0114] The lithium nickel oxide (composite oxide N) is represented, for example, by the formula: Li α Ni x1 Mn x2 M (1-x1-x2) O 2+β Here, the element M is at least one selected from V, Co, Mn, Mg, Al, Ca, Ti, Cu, Zn, and Nb. In addition, 0.9 ≤ α ≤ 1.10, -0.05 ≤ β ≤ 0.05, 0.5 ≤ x1 < 1, 0 < x2 ≤ 0.5, 0 < 1 - x1 - x2 ≤ 0.1. α increases or decreases during charge and discharge.

[0115] The composite oxide N may also contain Ni and Mn, and contain at least one element selected from Co and Al as the element M. Co, Mn, and Al contribute to the stabilization of the crystal structure of the composite oxide N.

[0116] The proportion of Mn among the metal elements other than Li may be 50 atomic% or less, or may be 30 atomic% or less. The proportion of Mn among the metal elements other than Li may be 1 atomic% or more, may be 3 atomic% or more, or may be 5 atomic% or more. By using Mn as a main component together with Ni, a high-capacity positive electrode active material can be obtained at low cost.

[0117] From the viewpoints of cost reduction and high capacity, it is desirable that the proportion of Co contained in the composite oxide N among the metal elements other than Li is 0 atomic% or more and 10 atomic% or less, and more desirably 0 atomic% or more and 5 atomic% or less.

[0118] The proportion of Al among the metal elements other than Li may be 10 atomic% or less, or may be 5 atomic% or less. The proportion of Al among the metal elements other than Li may be 1 atomic% or more, may be 3 atomic% or more, or may be 5 atomic% or more.

[0119] The composite oxide N in which the proportion of Ni and Mn in the metal elements other than Li is greater than 90 atomic % has high surface activity and tends to easily cause side reactions. Therefore, it is important to take measures to suppress the dissolution of metal ions into the non-aqueous electrolyte. In other words, in the composite oxide N in which the proportion of Ni and Mn in the metal elements other than Li is greater than 90 atomic %, the effect obtained by including the first organic phosphorus compound in the positive electrode active material layer and the second organic phosphorus compound in the non-aqueous electrolyte is particularly significant.

[0120] Examples of the conductive material that may be included as an optional component in the positive electrode active material layer include carbon nanotubes (CNTs), carbon fibers other than CNTs, and conductive particles (eg, carbon black and graphite).

[0121] [negative electrode]

[0122] The negative electrode includes at least a negative electrode current collector, for example, a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is supported on one or both surfaces of the negative electrode current collector.

[0123] As the negative electrode current collector, a nonporous conductive substrate (metal foil, etc.) or a porous conductive substrate (mesh, net, punched sheet, etc.) is used. Examples of the material of the negative electrode current collector include stainless steel, nickel, nickel alloy, copper, copper alloy, and the like.

[0124] The negative electrode active material layer may also be a negative electrode mixture layer composed of a negative electrode mixture. The negative electrode mixture layer is in the form of a film or a film sheet. The negative electrode mixture contains particles of the negative electrode active material as an essential component and may contain a binder, a conductive agent, a thickener, etc. as optional components. In addition, lithium metal foil or lithium alloy foil may be attached to the negative electrode collector as the negative electrode active material layer.

[0125] The negative electrode mixture layer can be formed, for example, by dispersing a negative electrode mixture including particles of a negative electrode active material, a binder, etc. in a dispersion medium to obtain a negative electrode slurry, applying the negative electrode slurry to the surface of the negative electrode collector, and drying the negative electrode slurry. The dried coating can also be rolled as needed.

[0126] The negative electrode active material includes materials that electrochemically absorb and release lithium ions, lithium metal, lithium alloys, etc. As materials that electrochemically absorb and release lithium ions, carbon materials, alloy materials, etc. can be used. As carbon materials, examples include graphite, easily graphitized carbon (soft carbon), and difficultly graphitized carbon (hard carbon). Among them, graphite with excellent charge and discharge stability and low irreversible capacity is preferred. As alloy materials, materials containing at least one metal that can form an alloy with lithium can be cited, specifically, silicon, tin, silicon alloys, tin alloys, silicon compounds, etc. Silicon oxide, tin oxide, etc. can also be used.

[0127] As alloy materials containing silicon, for example, a lithium ion conductive phase and a composite material obtained by dispersing silicon particles in the lithium ion conductive phase can be used. As a lithium ion conductive phase, for example, a silicon oxide phase, a silicate phase, a carbon phase, etc. can be used. The main component (for example, 95 to 100% by mass) of the silicon oxide phase can be silicon dioxide. Among them, a composite material consisting of a silicate phase and silicon particles dispersed in the silicate phase is preferred from the perspective of high capacity and low irreversible capacity. In addition, as a silicate phase, a lithium silicate phase (a silicate phase containing lithium) having a small irreversible capacity and high initial charge and discharge efficiency is preferred.

[0128] As the binder, for example, a resin material can be used. As the binder, for example, polyacrylic acid and polyacrylates and their derivatives, fluororesins, polyolefin resins, polyamide resins, polyimide resins, acrylic resins, vinyl resins, rubber particles, etc. can be mentioned. The binder can be used alone or in combination of two or more.

[0129] Examples of the conductive material include carbon nanotubes (CNTs), carbon fibers other than CNTs, and conductive particles (for example, carbon black and graphite).

[0130] Examples of thickeners include carboxymethyl cellulose (CMC) and modified products thereof (including salts such as Na salt), cellulose derivatives such as methyl cellulose (cellulose ethers, etc.); saponified products of polymers having vinyl acetate units such as polyvinyl alcohol; polyethers (polyoxyalkylenes such as polyethylene oxide); and the like.

[0131] [Diaphragm]

[0132] The separator is sandwiched between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation. As the separator, microporous films, fabrics, non-woven fabrics, etc. can be cited. As the material of the separator, polyolefins such as polypropylene and polyethylene can be used. The separator can have a heat-resistant insulating layer on at least one surface layer. The heat-resistant insulating layer can contain an inorganic oxide filler as a main component (for example, 80% by mass or more), and can also contain a heat-resistant resin as a main component (for example, 40% by mass or more). Among the heat-resistant resins, polyamide resins such as aromatic polyamide (aramid), polyimide resins, polyamide-imide resins, etc. can be used.

[0133] [Non-aqueous electrolyte]

[0134] The nonaqueous electrolyte includes a nonaqueous solvent, an electrolyte salt dissolved in the nonaqueous solvent, and a second organic phosphorus compound. The electrolyte salt includes at least a lithium salt. The concentration of the lithium salt in the nonaqueous electrolyte is, for example, 0.5 mol / L or more and 2 mol / L or less.

[0135] As the non-aqueous solvent, for example, cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, etc. can be used. As cyclic carbonates, propylene carbonate (PC), ethylene carbonate (EC), etc. can be mentioned. As chain carbonates, diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), etc. can be mentioned. As cyclic carboxylic acid esters, γ-butyrolactone (GBL), γ-valerolactone (GVL), etc. can be mentioned. The non-aqueous solvent can be used alone or in combination of two or more.

[0136] Examples of lithium salts include lithium salts containing chloric acid (LiClO4, LiAlCl4, LiB 10 Cl 10 etc.), lithium salts of fluorinated acids (LiPF6, LiBF4, LiSbF6, LiAsF6, LiCF3SO3, LiCF3CO2, etc.), lithium salts of fluorinated acid imides (LiN(SO2F)2, LiN(CF3SO2)2, LiN(CF3SO2)(C4F9SO2), LiN(C2F5SO2)2, etc.), lithium halides (LiCl, LiBr, LiI, etc.), etc. The lithium salt can be used alone or in combination of two or more. It should be noted that when a salt containing phosphorus such as LiPF6 is used as a lithium salt, a small amount of phosphorus from the lithium salt may be contained in the positive electrode active material layer, but it is a trace amount compared to the amount of the first organic phosphorus compound contained in the positive electrode active material layer and can be ignored. In addition, the correlation between the lithium salt concentration in the non-aqueous electrolyte and the content of phosphorus in the non-aqueous electrolyte from the lithium salt can be obtained, for example, by preparing a standard curve. The lithium salt concentration can be determined by the lithium ion concentration. Therefore, even if the lithium salt is a salt containing phosphorus, the content of phosphorus derived from the second organic phosphorus compound in the non-aqueous electrolyte can be calculated.

[0137] As an example of the structure of a nonaqueous electrolyte secondary battery, an electrode group formed by winding a positive electrode and a negative electrode across a separator and being contained in a battery case or an outer body together with a nonaqueous electrolyte can be cited. However, it is not limited to this, and other forms of electrode groups can also be applied. For example, a stacked electrode group obtained by stacking a positive electrode and a negative electrode across a separator can also be used. The form of the nonaqueous electrolyte secondary battery is also not limited, and can be, for example, cylindrical, square, coin-shaped, button-shaped, laminated, etc.

[0138] Below, refer to Figure 1 The structure of the nonaqueous electrolyte secondary battery will be described. Figure 1 1 is a longitudinal cross-sectional view of a cylindrical nonaqueous electrolyte secondary battery (hereinafter also referred to as “secondary battery 10 ”) as an example of the present embodiment. However, the present disclosure is not limited to the following configuration.

[0139] The secondary battery 10 includes an electrode group 18, a non-aqueous electrolyte (not shown) and a bottomed cylindrical battery case 22 for accommodating them. A sealing body 11 is fixed to the opening of the battery case 22 by caulking via a sealing gasket 21. As a result, the interior of the battery is sealed. The sealing body 11 includes a valve body 12, a metal plate 13 and an annular insulating member 14 sandwiched between the valve body 12 and the metal plate 13. The valve body 12 and the metal plate 13 are connected to each other at their respective center portions. The positive electrode lead 15a derived from the positive electrode 15 is connected to the metal plate 13. Therefore, the valve body 12 functions as an external terminal of the positive electrode. The negative electrode lead 16a derived from the negative electrode 16 is connected to the bottom inner surface of the battery case 22. An annular groove portion 22a is formed near the opening end of the battery case 22. A first insulating plate 23 is arranged between one end surface of the electrode group 18 and the annular groove portion 22a. A second insulating plate 24 is disposed between the other end surface of the electrode group 18 and the bottom of the battery case 22. The electrode group 18 is formed by winding the positive electrode 15 and the negative electrode 16 with the separator 17 interposed therebetween.

[0140] Example

[0141] Hereinafter, the present disclosure will be specifically described based on Examples and Comparative Examples, but the present disclosure is not limited to the following Examples.

[0142] Comparative Example 1

[0143] A test battery cell of a lithium ion secondary battery was produced by the following procedure and evaluated.

[0144] (1) Preparation of positive electrode

[0145] (I) Slurry Preparation Step

[0146] The active material particles (LiNi 0.8 Mn 0.2 A positive electrode mixture of 95 parts by mass of aluminum oxide (O2), 2.5 parts by mass of polyvinylidene fluoride (PVDF) as a binder and 2.5 parts by mass of acetylene black as a conductive material is mixed with NMP as a liquid dispersion medium, and the positive electrode mixture is dispersed in NMP to prepare a positive electrode slurry.

[0147] (II) Step of Preparing Positive Electrode Collector

[0148] As a positive electrode current collector, an aluminum foil (thickness: 15 μm) was prepared.

[0149] (III) Step of forming a coating film of positive electrode slurry

[0150] The positive electrode slurry is applied to one surface of the positive electrode current collector using a predetermined coating machine, thereby forming a coating film.

[0151] (IV) Coating Drying Step

[0152] Next, the coating film was dried at 80° C. to volatilize the dispersion medium, thereby forming an unrolled layer.

[0153] (V) Rolling process of unrolled layer

[0154] Next, the unrolled layer was rolled to form a positive electrode active material layer (thickness 95 μm, density 3.6 g / cm 3 ) to obtain the positive electrode.

[0155] The positive electrode was cut into a predetermined shape, and the positive electrode active material layer was partially peeled off to obtain a positive electrode for evaluation. The positive electrode had a 60 mm × 40 mm power generation area with a positive electrode active material layer and a 10 mm × 10 mm connection area without a positive electrode active material layer. The positive electrode tab was connected to the connection area.

[0156] (2) Preparation of negative electrode

[0157] The negative electrode was prepared by attaching lithium metal foil to one side of electrolytic copper foil (current collector). The negative electrode was cut into the same shape as the positive electrode, and the lithium metal foil on the connection area was peeled off, and the negative electrode tab was connected to the connection area.

[0158] (3) Preparation of non-aqueous electrolyte

[0159] LiPF6 was dissolved at a concentration of 1 mol / L in a mixed solvent of fluoroethylene carbonate (FEC) and dimethyl carbonate (DMC) in a volume ratio of 20:80 to prepare a non-aqueous electrolyte.

[0160] (4) Preparation of battery cells for evaluation

[0161] The above-mentioned positive electrode and negative electrode for evaluation were used to prepare a battery cell with a negative electrode design capacity of 114 mAh. The positive electrode and the negative electrode were stacked with a polyethylene separator (thickness 15 μm) between the positive electrode active material layer and the lithium metal foil to obtain a flat electrode group. The electrode group was placed on a 1.2 cm 3 The non-aqueous electrolyte is contained in a cylindrical shell with openings at both ends made of a laminated film, and each pole ear is led out from an opening, and the opening is sealed. Then, the operation of standing for 3 minutes under a reduced pressure of 0.02MPa and then returning to atmospheric pressure is performed twice to impregnate the positive electrode active material layer with the non-aqueous electrolyte. Finally, the other opening is sealed to obtain the evaluation battery cell B1 of Comparative Example 1. The evaluation battery cell is made in a dry air atmosphere with a dew point of less than -60°C.

[0162] (5) Battery evaluation

[0163] The evaluation battery cell was clamped by a pair of 10×5cm stainless steel (6mm thick) clamps and fixed with 3.2MPa pressure. In a 25°C constant temperature chamber, the battery was charged to a voltage of 4.5V at a constant current of 0.3It, and then discharged to 2.5V at a constant current of 0.3It. The above charge and discharge were repeated twice. Next, the voltage was 4.5V at a constant current of 0.3It. Then, the temperature of the constant temperature chamber was changed to 55°C, and a trickle charge was performed at a constant voltage of 4.5V for 3 days.

[0164] After trickle charge, the battery cells were disassembled, the negative electrode was washed with dimethyl carbonate, and the amount of transition metal precipitated at the negative electrode (total amount of Ni+Mn) was measured using an inductively coupled plasma emission spectrometer (ICP-AES) as the amount of metal ions dissolved from the positive electrode into the non-aqueous electrolyte.

[0165] Furthermore, after the positive electrode was washed with dimethyl carbonate, the amount of phosphorus (P) contained in the positive electrode active material layer was measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), but no phosphorus was detected.

[0166] Comparative Example 2

[0167] In the preparation of the non-aqueous electrolyte (3), in the non-aqueous electrolyte, as an organic phosphorus compound (P), the following formula:

[0168]

[0169] Except that tris(trimethylsilyl) phosphate (TMSP) was contained at a content of 2 mass %, an evaluation cell B2 was prepared in the same manner as in Comparative Example 1 and evaluated in the same manner. TMSP in the nonaqueous electrolyte was completely dissolved.

[0170] 《Comparative Example 3》

[0171] In the slurry preparation step (I) of the preparation (1) of the positive electrode, the positive electrode mixture contains an organic phosphorus compound (P) of the formula:

[0172]

[0173] The decylphosphonic acid (DP) (average particle size D1 = 3 μm) which is solid at room temperature is contained in the positive electrode active material layer at a content of 1 mass %, and the evaluation cell B3 is prepared in the same manner as in Comparative Example 1, and the evaluation is performed in the same manner. It should be noted that the decylphosphonic acid in the positive electrode slurry is not completely dissolved, but a part of it is present in the positive electrode slurry in the form of particles having a particle size of 0.1 μm or more and 5 μm or less (average particle size d1 <3 μm).

[0174] 《Comparative Example 4》

[0175] In the slurry preparation step (I) of the preparation of the positive electrode (1), TMSP was contained in the positive electrode mixture as the organic phosphorus compound (P) so that the content in the positive electrode active material layer was 1 mass %, and the evaluation cell B4 was prepared and evaluated in the same manner as in Comparative Example 1. It should be noted that TMSP in the positive electrode slurry was completely dissolved.

[0176] 《Comparative Example 5》

[0177] In the slurry preparation step (I) of the preparation of the positive electrode (1), LiNi 0.8 Co 0.15 Al 0.05 O2 to replace LiNi 0.8 Mn 0.2 An evaluation battery cell B5 was prepared in the same manner as in Comparative Example 1 except for the above-mentioned conditions and was evaluated in the same manner.

[0178] 《Example 1》

[0179] In the slurry preparation step (I) of the preparation of the positive electrode (1), decylphosphonic acid (DP) (average particle size D1 = 3 μm) was included in the positive electrode mixture as an organic phosphorus compound (P) at a content of 1% by mass in the positive electrode active material layer, and in the preparation of the non-aqueous electrolyte (3), TMSP was included in the non-aqueous electrolyte at a content of 2% by mass as an organic phosphorus compound (P). The evaluation cell A1 was prepared in the same manner as in Comparative Example 1 and was evaluated in the same manner. It should be noted that the decylphosphonic acid in the positive electrode slurry was not completely dissolved, but a part of it was present in the positive electrode slurry in the form of particles having a particle size of 0.1 μm or more and 5 μm or less (average particle size d1 < 3 μm). The TMSP in the non-aqueous electrolyte was completely dissolved.

[0180] 《Example 2》

[0181] Evaluation cell A2 was prepared and evaluated in the same manner as in Comparative Example 1, except that in the slurry preparation step (I) of the preparation of the positive electrode (1), TSMP was included in the positive electrode mixture as the organic phosphorus compound (P) at a content of 1% by mass in the positive electrode active material layer, and in the preparation of the nonaqueous electrolyte (3), TMSP was included in the nonaqueous electrolyte at a content of 2% by mass as the organic phosphorus compound (P). It should be noted that TSMP in the positive electrode slurry and TMSP in the nonaqueous electrolyte were completely dissolved.

[0182] 《Example 3》

[0183] In the slurry preparation step (I) of the preparation of the positive electrode (1), LiNi 0.8 Co 0.15 Al 0.05 O2 to replace LiNi 0.8 Mn 0.2 A battery cell A3 for evaluation was prepared in the same manner as in Example 1 except for the above-mentioned conditions and was evaluated in the same manner.

[0184] <Quantification of Phosphorus (P) Element in Positive Electrode Active Material Layer>

[0185] Using the positive electrode used in battery cells B2 to B4, A1, and A2, and a non-aqueous electrolyte obtained by dissolving lithium bis(fluorosulfonyl)imide (LiN(SO2F)2) at a concentration of 1 mol / L in a mixed solvent of ethylene fluorocarbonate (FEC) and dimethyl carbonate (DMC) in a volume ratio of 20:80, a battery cell for quantitative measurement of phosphorus (P) element was prepared in the same manner as described above. 2% by mass of TMSP was dissolved in the non-aqueous electrolyte of the battery cells containing B2, A1, and A2. After charging and discharging between 4.2V and 2.5V, the positive electrode was taken out at DOD 100%, and the positive electrode was washed with DMC to obtain the positive electrode after charging and discharging. The amount of phosphorus element (P) contained in the positive electrode active material layer of the obtained positive electrode was measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES).

[0186] The results are shown in Table 1. The values ​​in Table 1 are relative values ​​when the amount of eluted metal ions in the battery cell B1 of Comparative Example 1 is taken as 100%.

[0187] [Table 1]

[0188]

[0189] As can be seen from Table 1, in batteries A1 and A2, the amount of dissolved metal ions is significantly reduced. On the other hand, when only the organic phosphorus compound (P) is dissolved in the non-aqueous electrolyte, the reduction rate of the amount of dissolved metal ions is about 40%. In addition, when only the organic phosphorus compound (P) is included in the positive electrode active material layer, the reduction rate of the amount of dissolved metal ions is about 18 to 40%. In contrast, when the organic phosphorus compound (P) is included in the positive electrode active material layer and the non-aqueous electrolyte respectively, the reduction rate of the amount of dissolved metal ions increases to 83% to 88%.

[0190] Here, regarding the reduction in the amount of dissolved metal ions, it is assumed that additivity exists between the effect of adding the organic phosphorus compound (P) only to the positive electrode active material layer and the effect of adding only to the non-aqueous electrolyte. If only the organic phosphorus compound (P) is included in the positive electrode active material layer, the amount of dissolved metal ions is reduced to 60-82. If only the organic phosphorus compound (P) is dissolved in the non-aqueous electrolyte, the amount of dissolved metal ions is reduced to 60%. That is, when additivity exists, it can be expected that the amount of dissolved metal ions is reduced to (60-88)×0.6=36%-52%. On the other hand, the amount of dissolved metal ions in A1 and A2 is reduced to 12-17%, and it can be understood that a synergistic effect above the additive effect is obtained.

[0191] In addition, compared with the case (B2) in which the organic phosphorus compound (P) is included only in the non-aqueous electrolyte, when the organic phosphorus compound (P) is directly included in the positive electrode mixture (B3, B4, A1, A2), a very large amount of phosphorus element is detected from the positive electrode active material layer. This makes it possible to understand the importance of including the organic phosphorus compound (P) in both the positive electrode active material layer and the non-aqueous electrolyte.

[0192] In addition, when Example 1, Example 3 and Comparative Example 5 are compared, it can be seen that when the positive electrode active material containing Ni and Mn as main components is used, a particularly large effect of reducing the amount of eluted metal ions can be obtained.

[0193] Industrial Applicability

[0194] The nonaqueous electrolyte secondary battery according to the present disclosure is useful as a main power source for mobile communication devices, portable electronic devices, electric vehicles, and the like.

[0195] The present invention has been described with respect to the currently preferred embodiments, but such disclosure is not to be construed as limiting. A person skilled in the art in the art to which the present invention belongs can accurately know various modifications and changes by reading the above disclosure. Therefore, the attached claims should be interpreted as including all modifications and changes in a manner that does not depart from the true spirit and scope of the present invention.

[0196] Description of Reference Numerals

[0197] 10: Secondary battery, 11: Sealing body, 12: Valve body, 13: Metal plate, 14: Insulating member, 15: Positive electrode, 15a: Positive electrode lead, 16: Negative electrode, 16a: Negative electrode lead, 17: Separator, 18: Electrode group, 21: Sealing gasket, 22: Battery case, 22a: Groove, 23: First insulating plate, 24: Second insulating plate

Claims

1. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, The positive electrode comprises a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector. The positive electrode active material layer comprises active material particles, a binder and a first organic phosphorus compound. The content Cpn of the first organic phosphorus compound contained in the positive electrode active material layer is 0.1 mass % or more and 5 mass % or less, The nonaqueous electrolyte includes a nonaqueous solvent, an electrolyte salt, and a second organic phosphorus compound.

2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the ratio of the content Cpn of the first organic phosphorus compound contained in the positive electrode active material layer to the content Cen of the second organic phosphorus compound contained in the nonaqueous electrolyte, i.e., Cpn / Cen, is greater than 0.1 / 4.0 and less than 4.0 / 3.0, and the units of the content Cpn and the content Cen are mass %.

3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the first organic phosphorus compound and the second organic phosphorus compound are each independently represented by the general formula (1): In the general formula (1), R 1 and R 2 Each independently represents the surface of the active material particle, -H, -CH2X, -CH2CH2X or -Si((CH2) n CH3)3, R 3 -(CH2) m CH2X or -O-Si((CH2) n CH3)3, X is -H, -NH2, -COOH, -CN or -F, R 1 , R 2 and R 3 The integers n are each independently 0 or 1, R 3 The integer m used for definition is 0 to 16. When there are multiple Xs, the multiple Xs are independent of each other.

4. The nonaqueous electrolyte secondary battery according to claim 2, wherein R 1 and R 2 Each is independently -Si((CH2) n CH3)3, R 3 -O-Si((CH2) n CH3)3.

5. The nonaqueous electrolyte secondary battery according to claim 2, wherein R 1 and R 2 Each is -H, R 3 -(CH2) m CH3. 6 . The nonaqueous electrolyte secondary battery according to claim 1 , wherein a content of the second organic phosphorus compound contained in the nonaqueous electrolyte is 0.1% by mass or more and 3% by mass or less. 7 . The nonaqueous electrolyte secondary battery according to claim 1 , wherein at least a portion of the surface of the active material particle is covered with a coating, and the coating contains phosphorus. 8 . The nonaqueous electrolyte secondary battery according to claim 7 , wherein at least a portion of the coating has a thickness of 0.2 nm or more.

9. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 5, wherein the active material particles include a transition metal oxide containing lithium. The lithium-containing transition metal oxide includes a lithium nickel oxide, the lithium nickel oxide includes lithium and Ni and has a layered rock salt type crystal structure, The ratio of Ni contained in the lithium nickel oxide to the metal elements other than Li is 50 atomic % or more.

10. The non-aqueous electrolyte secondary battery according to claim 9, wherein the lithium nickel oxide is of the formula: Li α Ni x1 Mn x2 M (1-x1-x2) O 2+β express, The element M is at least one selected from V, Co, Mn, Mg, Al, Ca, Ti, Cu, Zn and Nb, The lithium nickel oxide satisfies: 0.9≤α≤1.10, -0.05≤β≤0.05, 0.5≤x1<1, 0<x2≤0.5, 0<1-x1-x2≤0.

1.

11. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, The positive electrode comprises a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector. The positive electrode active material layer comprises active material particles, a binder and phosphorus element. The content of the phosphorus element contained in the positive electrode active material layer is 100 ppm or more and 4000 ppm or less on a mass basis, The non-aqueous electrolyte comprises a non-aqueous solvent, an electrolyte salt and phosphorus element, A ratio of a content Cpn of the phosphorus element contained in the positive electrode active material layer to a content Cen of the phosphorus element contained in the non-aqueous electrolyte, i.e., Cpn / Cen, is 0.1 / 4.0 or more and 4.0 / 3.0 or less, and the units of the content Cpn and the content Cen are mass %.

Citation Information

Patent Citations

  • Battery, battery pack, electronic device, electrically-powered vehicle, power storage device and electric power system

    JP2013152825A

  • Positive electrode active material for lithium secondary cell, positive electrode for lithium secondary cell, lithium secondary cell, and methods for manufacturing same

    WO2017126276A1