Double-bionic dressing with one-way vertical drainage and reverse drug delivery functions and preparation method of double-bionic dressing

The combination dressing of imitation trunk nanofiber sponge and imitation octopus suction cup nanofiber membrane prepared by electrospinning technology solves the problems of effluent conduction and low drug delivery efficiency, and realizes unidirectional aspiration of effluent and efficient drug delivery , significantly improves the speed and efficiency of wound healing.

CN118976135APending Publication Date: 2024-11-19NORTHWEST UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411077070.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

It is difficult for existing dressings to achieve one-way vertical guidance when absorbing wound ooze, and the drug delivery efficiency is low, so it cannot effectively prevent ooze from reflux and improve wound healing speed.

Method used

Using a double bionic dressing consisting of imitation trunk nanofiber sponge and imitation octopus suction cup nanofiber membrane, an hydrophobic film with a vertically oriented pore structure and a hydrophobic film with a vertically oriented pore structure is prepared to achieve a one-way vertical liquid guide and reverse drug delivery.

Benefits of technology

Efficient one-way aspiration of ooze and efficient delivery of drugs have been achieved, significantly improving the wound healing rate, drug delivery efficiency has been increased by 22%, and wound healing speed has been accelerated by 28.92%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976135A_ABST
    Figure CN118976135A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of medical materials, and particularly relates to a double-bionic dressing with one-way vertical drainage and reverse drug delivery functions and a preparation method of the double-bionic dressing. The method comprises the following steps: firstly, preparing an octopus-sucker-imitated nanofiber membrane by using an electrostatic spinning device by taking a soluble hydrophobic high polymer material and a medicine as raw materials; secondly, a soluble hydrophilic high polymer material is used as a raw material, a nanofiber membrane is obtained through electrostatic spinning equipment, a stabilizer is added after homogenization, and trunk-imitating nanofiber sponge is obtained after freeze drying, heating crosslinking and glutaraldehyde steam crosslinking; and finally, by taking a soluble hydrophobic polymer material as a raw material, bonding the trunk-imitated nanofiber sponge and the octopus-imitated sucker nanofiber membrane through electrospinning to obtain the double-bionic dressing. According to the double-bionic dressing obtained through the method, one-way vertical suction of a large amount of seepage and efficient reverse delivery of an antibacterial agent are achieved, and the promotion effect on severe seepage wound healing is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medical materials, and in particular relates to a double bionic dressing with unidirectional vertical fluid conduction and reverse drug delivery and a preparation method thereof. Background Art

[0002] Common severe exudate wounds include diabetic foot, burn wounds, bacterial infection wounds, etc., which are common and difficult to treat clinically, with the characteristics of slow healing, long treatment cycle, and easy recurrence of the disease, which seriously affect the quality of life of patients. Wound exudate contains a large number of harmful substances, including various enzymes and inflammatory factors that hinder wound healing; in addition, wound exudate is also a culture medium for bacteria, which produce various toxins. Therefore, timely and effective removal of wound exudate can not only reduce the inflammatory response of the wound and prevent the progressive deterioration of the wound, but also create a favorable microenvironment for skin cell proliferation and migration.

[0003] Conventional hydrophilic dressings absorb exudate thanks to the wettability of the material itself and the interconnected capillary channels. The liquid that enters the hydrophilic dressing will be transported along the direction of the channel, and the channel determines the transport height of the liquid in the hydrophilic dressing. Since the pore structure of the hydrophilic dressing is random, after the liquid is absorbed, it will be preferentially transported laterally due to its own gravity. As the amount of absorbed liquid increases, the liquid will accumulate at the bottom of the dressing in large quantities and come into direct contact with the wound surface, causing liquid reverse osmosis. Existing dressings rely on their own hydrophilicity to absorb exudate and cannot prevent reverse osmosis of exudate.

[0004] In addition, wound dressings often need to deliver drugs to the wound to improve the wound microenvironment and accelerate wound healing. Currently common drug delivery dressings include hydrogels, microneedles, micro-nanoparticles, fiber membranes, etc. These drug carriers are difficult to conduct away a large amount of exudate from the wound. The accumulation of a large amount of exudate on the wound will not only cause the sudden release of drugs in these carrier materials, but also lead to the problem of low efficiency of drug delivery to the wound. Therefore, it is of great significance to develop a dual-functional dressing that has both vertical exudate conduction and efficient drug delivery. Summary of the invention

[0005] The object of the present invention is to provide a double bionic dressing with unidirectional vertical fluid conduction and reverse drug delivery and a preparation method thereof.

[0006] The implementation process of the present invention is as follows:

[0007] A double bionic dressing with unidirectional vertical fluid conduction and reverse drug delivery is composed of an upper layer of tree trunk imitation nanofiber sponge and a lower layer of octopus suction cup imitation nanofiber membrane. The upper layer of tree trunk imitation nanofiber sponge is a hydrophilic material with a tree trunk imitation vertical directional pore structure, and the lower layer of octopus suction cup nanofiber membrane is a hydrophobic material with an octopus imitation concave-convex array structure.

[0008] A preparation method of a double bionic dressing with unidirectional vertical fluid conduction and reverse drug delivery comprises the following steps: firstly, using a soluble hydrophobic polymer material and a drug as raw materials, preparing an octopus sucker-like nanofiber membrane by using an electrospinning device; secondly, using a soluble hydrophilic polymer material as raw material, obtaining a nanofiber membrane by using an electrospinning device, adding a stabilizer after homogenization, and obtaining a tree trunk-like nanofiber sponge after freeze-drying, heating cross-linking and glutaraldehyde steam cross-linking; finally, placing the tree trunk-like nanofiber sponge on an octopus sucker-like nanofiber membrane of equal area, and winding nanofibers prepared by using a soluble hydrophobic polymer material as raw material by using an electrospinning device around the tree trunk-like nanofiber sponge and the octopus sucker-like nanofiber membrane to obtain a double bionic dressing.

[0009] The preparation method of the above-mentioned dual bionic dressing comprises the following steps:

[0010] (1) Preparation of octopus suction cup-like nanofiber membrane

[0011] Dispersing or dissolving a soluble hydrophobic polymer material and a drug in a solvent to obtain an electrospinning solution; using a spinning collection device with an array hole structure and an electrospinning device to perform electrospinning to prepare an octopus sucker-like nanofiber membrane;

[0012] (2) Preparation of tree trunk-like nanofiber sponge

[0013] (2.1) Using a soluble hydrophilic polymer material as a raw material, adding a solvent to obtain an electrospinning solution, then using an electrospinning device to electrospin to obtain a nanofiber membrane, and finally placing the nanofiber membrane in glutaraldehyde vapor for cross-linking to obtain a water-insoluble nanofiber membrane;

[0014] (2.2) homogenizing the nanofiber membrane to obtain a short fiber suspension, adding a stabilizer to the short fiber suspension, freezing it with a cold source, and then freeze-drying it to obtain an initial nanofiber sponge;

[0015] (2.3) heating the initial nanofiber sponge for cross-linking, and then placing the initial nanofiber sponge in glutaraldehyde vapor for cross-linking to obtain a tree trunk-mimicking nanofiber sponge;

[0016] (3) Assembly of dual bionic dressing

[0017] A soluble hydrophobic polymer material is dissolved in a solvent to obtain an electrospinning solution; then the octopus suction cup nanofiber membrane is cut into the same size as the bottom surface of the tree trunk nanofiber sponge, and the cut octopus suction cup nanofiber membrane is placed under the tree trunk nanofiber sponge and temporarily fixed with tweezers; during the electrospinning process of the spinning solution, the temporarily fixed octopus suction cup nanofiber membrane and the tree trunk nanofiber sponge are placed between the needle tip and the collecting device, and rotated so that the fibers are evenly wrapped around the surface, and the two are tightly combined to obtain a double bionic dressing.

[0018] Furthermore, in step (1) and step (3), the soluble hydrophobic polymer material is selected from any one or a combination of poly-ε-caprolactone, polyurethane, polylactic acid, poly(lactide-glycol), polysulfone, polymethyl methacrylate, polyvinyl butyral, and polyvinylidene fluoride; in step (2.1), the soluble hydrophilic polymer material is selected from any one or a combination of chitosan, gelatin, collagen, polyacrylonitrile, cellulose acetate, and polyvinyl alcohol.

[0019] Furthermore, in step (1) and step (3), the solvent is selected from any one or a combination of tetrahydrofuran, N,N-dimethylformamide, dichloromethane, chloroform, hexafluoroisopropanol, and ethanol.

[0020] Further, in step (1), the spinning collecting device with an array hole structure is any one or a combination of a spinning collecting device with a circular hole array structure, a spinning collecting device with a triangular hole array structure, a spinning collecting device with a polygonal hole array structure, a spinning collecting device with an irregular hole array structure, and a screen.

[0021] Furthermore, in step (2.1), the solvent is selected from any one or a combination of hexafluoroisopropanol, glacial acetic acid, tetrahydrofuran, N,N-dimethylformamide, N,N-diethylacetamide, and water.

[0022] Furthermore, in step (2.2), the stabilizer is selected from polyvinyl alcohol or graphene oxide.

[0023] Furthermore, in step (1), the mass concentration of the soluble polymer material in the electrospinning solution is 0.1-5.0 g / ml; the electrospinning parameters are a voltage of 5 kv-20 kv, a flow rate of 0.1-2.0 ml / h, and a spinning distance of 5-20 cm; in step (2.1), the mass concentration of the electrospinning solution is 0.02-5 g / ml; in step (2.2), the mass ratio of the stabilizer to the short fibers of the nanofiber membrane in the suspension is (0.15-0.2):1; in step (2.2), the solvent in the homogenization process is water.

[0024] Furthermore, in step (2.2), the degree of freezing is frozen into a solid state; in step (2.3), the heating temperature during the heating cross-linking process is 60-200°C, and the cross-linking time is 1-12 hours; in steps (2.1) and (2.3), the mass percentage of glutaraldehyde vapor is 1%-50%, and the cross-linking time is 12-36 hours; in steps (2.1) and (3), the parameters of the electrospinning equipment are: an aluminum foil wrapped drum is used as a collecting device, the spinning voltage is 5kv-20kv, the flow rate is 0.1-2.0ml / h, and the spinning distance is 5-20cm.

[0025] Design idea of ​​the method of the present invention:

[0026] Inspired by the structure and function of octopus suckers and tree trunks in nature, the present invention proposes a "double bionic" design concept and prepares an "octopus sucker-tree trunk" double bionic dressing to solve the problem of difficulty in efficiently conducting away wound exudate and low drug delivery efficiency. The lower layer of the double bionic dressing is a hydrophobic nanofiber membrane (OS) with a concave-convex array structure imitating an octopus sucker, and the upper layer is a hydrophilic nanofiber sponge (TT) with a vertical directional pore structure imitating a tree trunk. The concave cavity of the nanofiber membrane imitating an octopus sucker can unidirectionally suck the wound exudate, and the nanofiber sponge imitating a tree trunk sucks the exudate vertically for a second time over a long distance to keep the exudate away from the wound; the convex structure of the nanofiber membrane imitating an octopus sucker is in direct contact with the wound, and can reversely deliver the drug to the wound, accelerating the healing of severe exudate wounds.

[0027] Positive effects of the present invention:

[0028] (1) An octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning combined with an array hole collection device. The cavity diameter, cavity spacing, and convex area were regulated by adjusting the collection device structure. The bionic OS fiber membrane can vertically absorb liquid in one direction. The convex area of ​​the bionic OS fiber membrane affects the drug delivery efficiency. The delivery efficiency increases with the increase of the convex area, and the maximum delivery reaches 85.84%. Compared with non-octopus sucker-like nanofiber membranes, the bionic OS fiber membrane can increase the drug delivery efficiency by 22%.

[0029] (2) A tree trunk-like nanofiber membrane sponge (TT) was prepared by electrospinning combined with ice template method. The diameter of the vertical oriented pores was regulated by adjusting the temperature of the cold source. The bionic TT sponge can vertically pump liquid over a long distance, and the pumping speed increases with the increase of the diameter of the vertical oriented pores. Compared with the random pore sponge, the liquid pumping speed of the tree trunk-like nanofiber sponge is increased by 5.25 times.

[0030] (3) The bionic OS fiber membrane and the bionic TT sponge were assembled into a double bionic dressing by electrospinning. The double bionic dressing has two unidirectional vertical liquid suction performances. Compared with the bionic TT sponge, the double bionic dressing increased the suction speed of the liquid in the sponge by 34%. The double bionic dressing can efficiently deliver drugs. Compared with the assembly of non-octopus suction cup nanofiber membrane and bionic TT sponge, the drug delivery efficiency is increased by 22%. The double bionic dressing promotes the healing of bacterial-infected wounds by efficiently delivering drugs. Compared with the un-drug-loaded dressing, the wound healing rate is increased by 28.92%. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The morphology and formation mechanism of the nanofiber membrane imitating the octopus sucker; (a) digital photo; (b) three-dimensional image of the profilometer and (c) cross-sectional height; (d) statistics of the cavity area and convex area; (e) cavity microscope image and (f) fiber area statistics; (g) formation principle of the bionic structure;

[0032] Figure 2 The unidirectional vertical suction behavior of the nanofiber membrane imitating the octopus suction cup on the droplet; (a) 130 μL droplets were dropped from the biomimetic membrane side, (b) 130 μL droplets were dropped from the hydrophilic non-woven fabric side; (c) 5 μL fluorescent droplets were dropped from the biomimetic membrane side; (d) fluorescent droplets were dropped from the hydrophilic non-woven fabric side; a nanofiber membrane without biomimetic structure (NW) was combined with a hydrophilic non-woven fabric as a control group. (e) Fluorescent droplets were dropped from the membrane without biomimetic structure, and (f) fluorescent droplets were dropped from the hydrophilic non-woven fabric side;

[0033] Figure 3 Figure 1 is a graph related to the reverse delivery of drugs by octopus sucker-like nanofiber membranes; (a) Schematic diagram of the reverse delivery process of drugs by octopus sucker-like nanofiber membranes; (b) Schematic diagram of the reverse delivery mechanism of drugs by octopus sucker-like nanofiber membranes; (c) UV characteristic absorption peak of ε-PL; (d) Comparison of drug delivery efficiency between non-biomimetic fiber membrane (NW) and octopus sucker-like nanofiber membrane (OS); (e) Effect of protrusion area on drug delivery efficiency;

[0034] Figure 4 The preparation and morphology characterization diagram of tree trunk-mimicking nanofiber sponge TT; (a) TT preparation process; (b) TT ultralightness; (c) TT resilience; (d) TT top view SEM image; (e) TT magnified SEM image; (f) TT long-range ordered directional pore structure; (g) SEM images of vertical directional pore structures of different TTs; (h) vertical directional pore diameter; (i) TT tortuosity;

[0035] Figure 5The long-distance vertical liquid suction behavior diagram of the tree trunk-mimicking nanofiber sponge; (a) the image of the liquid suction height of different sponges changing with time; (b) the graph of the liquid suction height of different sponges changing with time; (c) the vertical liquid suction rate of different sponges; (d) the schematic diagram of the vertical liquid suction of the tree trunk-mimicking nanofiber sponge, force analysis and the formula of suction height and suction speed;

[0036] Figure 6 Figure 1 is a diagram of the mechanical properties of TT; (a) schematic diagram of compression direction; (b) compression-rebound elasticity of TT-1 under different compression strains in the parallel direction; (c) compression-rebound elasticity of TT-1 under different compression strains in the perpendicular direction; (d) compression-rebound elasticity of TT-1 in different directions; (e) compression-rebound elasticity of different sponges in the parallel direction; (f) compression-rebound elasticity of different sponges in the perpendicular direction;

[0037] Figure 7 Figure 2 is a graph showing the liquid suction performance and reverse drug delivery performance of the dual bionic dressing; (a) schematic diagram of the OS&TT combination; (b) suction image of TT on an absorbent sponge; (c) suction image of OS&TT on an absorbent sponge; (d) change of suction height of TT and OS&TT on an absorbent sponge over time; (e) change of suction speed of TT and OS&TT on an absorbent sponge over time; (f) drug delivery efficiency of NW&TT and OS&TT;

[0038] Figure 8 The experimental diagram of wound healing after bacterial infection, including (a) wound healing photos and wound color simulation diagrams on days 0, 1, 3, 7, and 13, and (b) wound area statistics; (c) exudate colony smear photos on day 3 and (d) colony count statistics;

[0039] Fig. 9 Results of histological staining of bacterially infected wounds; (a) H&E staining of wound tissue sections on the 13th day; (b) Masson staining; (c) statistics of wound length on the 13th day; (d) collagen deposition on the 13th day. DETAILED DESCRIPTION

[0040] The present invention will be further described below by way of examples.

[0041] In the method of the present invention, a spinning collection device with an array hole structure is used in the preparation process of the octopus sucker-like nanofiber membrane. During the electrospinning process, the nanofibers are deposited thickly around the holes, while the nanofibers are deposited thinly inside the holes, thereby forming a concave-convex array structure similar to the octopus sucker.

[0042] It should be noted that the ratio, temperature and dissolution time of the soluble hydrophobic polymer material and the drug in step (1) of the method of the present invention are not limited. In the actual application process, those skilled in the art can select any ratio, temperature and dissolution time according to the actual needs, as long as the obtained electrospinning solution can achieve electrospinning. The ratio of the soluble hydrophobic polymer material to the solvent in step (1) of the method of the present invention is also not limited, as long as the mass concentration of the soluble hydrophobic polymer material in the electrospinning solution is 0.1-5.0g / ml. The type of solvent in step (1) of the method of the present invention is also not limited, as long as it can dissolve the soluble hydrophobic polymer material. The deposition time for electrospinning in step (1) of the method of the present invention is not limited, and those skilled in the art can select the deposition time according to experimental needs. The drug described in step (1) of the method of the present invention can select any one or several drugs according to actual needs, which can be antibacterial agents, anti-inflammatory drugs, antioxidants, angiogenic drugs, anti-tumor drugs, etc., and can be dissolved or dispersed in the solvent. Those skilled in the art can choose to disperse or dissolve according to the characteristics of the drug. In the embodiment of the present invention, ε-polylysine hydrochloride powder is used as a drug, and the effect experiment is verified. It should be noted that the cold source in step (2) of the method of the present invention is not limited. Those skilled in the art can select freezing equipment such as liquid nitrogen, refrigerators, ultra-low temperature refrigerators, etc. that can provide a low-temperature environment below 0°C according to equipment requirements, and can achieve freezing of the sample into a solid state. The ratio of soluble hydrophilic polymer material to solvent in step (2) of the method of the present invention is not limited, as long as the mass concentration of soluble hydrophilic polymer material in the electrospinning solution is 0.02-5 g / ml. The source of graphene oxide in step (2) of the method of the present invention is not limited. Those skilled in the art can purchase it or prepare it according to the existing technology. The deposition time of electrospinning in step (2) of the method of the present invention is not limited. Those skilled in the art can select the deposition time according to experimental needs. It should be noted that the ratio of soluble hydrophobic polymer material to solvent in step (3) of the method of the present invention is not limited, as long as the mass concentration of soluble hydrophobic polymer material in the electrospinning solution is 0.1-5.0 g / ml.

[0043] Example 1 Preparation of Octopus Sucker-like Nanofiber Membrane

[0044] 0.7 g of poly-ε-caprolactone (PCL) particles and 0.14 g of ε-polylysine hydrochloride powder (ε-PL) were added to a mixed solvent of 3 mL DMF and 1 mL THF and stirred at room temperature for 12 h to obtain a spinning solution. The spinning solution was poured into a 5 mL syringe and an octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning technology. The spinning voltage was 6 kV, the spinning speed was 0.5 mL / h, the spinning spacing was 10 cm, the spinning solution volume was 100 μL, the deposition time was 10 min, and a spinning collection device with an array circular hole structure was used.

[0045] By changing the aperture and hole spacing on the spinning collection device, octopus sucker-like nanofiber membranes (OS) with different cavity diameters and cavity spacings were obtained. Octopus sucker-like nanofiber membranes with a cavity diameter of 0.5 mm and cavity spacings of 0.6 mm, 0.8 mm, 1.0 mm, and 1.2 mm were prepared (recorded as: 0.5-0.6, 0.5-0.8, 0.5-1.0, 0.5-1.2). Octopus sucker-like electro-mimetic fiber membranes with a cavity spacing of 1.2 mm and cavity diameters of 0.5 mm, 0.7 mm, and 1.0 mm were prepared (0.5-1.2, 0.7-1.2, 1.0-1.2).

[0046] Comparative Example 1 Non-bionic structure nanofiber membrane (NW)

[0047] The method and parameters are the same as those in Example 1, except that, in Comparative Example 1, a planar collecting device without array holes is selected as the control group, the spinning solution volume is 40 μL, and a non-bionic structure nanofiber membrane (NW) is obtained.

[0048] Example 2 Preparation of Octopus Sucker-like Nanofiber Membrane

[0049] 20 g of polyurethane and 0.5 g of ε-polylysine hydrochloride powder (ε-PL) were added to a mixed solvent of 3 mL DMF and 1 mL THF and stirred at room temperature for 10 h to obtain a spinning solution. The spinning solution was poured into a 5 mL syringe and an octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning technology. The spinning voltage was 5 kV, the spinning speed was 0.5 mL / h, the spinning spacing was 10 cm, the spinning solution volume was 100 μL, the deposition time was 20 min, and a spinning collection device with an array triangular pore structure was used.

[0050] Example 3 Preparation of Octopus Sucker-like Nanofiber Membrane

[0051] 0.4 g of polylactic acid and 0.21 g of ε-polylysine hydrochloride powder (ε-PL) were added to 4 mL of dichloromethane solvent and stirred at room temperature for 15 h to obtain a spinning solution. The spinning solution was poured into a 5 mL syringe and an octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning technology. The spinning voltage was 10 kV, the spinning speed was 0.5 mL / h, the spinning spacing was 10 cm, the spinning solution volume was 100 μL, the deposition time was 15 min, and a spinning collection device with an array rectangular hole structure was used.

[0052] Example 4 Preparation of Octopus Sucker-like Nanofiber Membrane

[0053] 2.8 g of poly(lactide-glycolide) and 0.3 g of ε-polylysine hydrochloride powder (ε-PL) were added to 4 mL of chloroform solvent and stirred at room temperature for 10 h to obtain a spinning solution. The spinning solution was poured into a 5 mL syringe and an octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning technology. The spinning voltage was 6 kV, the spinning speed was 0.5 mL / h, the spinning spacing was 10 cm, the spinning solution volume was 100 μL, the deposition time was 20 min, and a spinning collection device with an array square hole structure was used.

[0054] Example 5 Preparation of Octopus Sucker Imitation Nanofiber Membrane

[0055] 0.7 g of polysulfone and 0.21 g of ε-polylysine hydrochloride powder (ε-PL) were added to a mixed solvent of 2 mL of hexafluoroisopropanol and 2 mL of THF and stirred at room temperature for 15 h to obtain a spinning solution. The spinning solution was poured into a 5 mL syringe and an octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning technology. The spinning voltage was 15 kV, the spinning speed was 1 mL / h, the spinning spacing was 18 cm, the spinning solution volume was 100 μL, the deposition time was 15 min, and a spinning collection device with an array irregular pore structure was used.

[0056] Example 6 Preparation of Octopus Sucker-like Nanofiber Membrane

[0057] 0.7 g of polymethyl methacrylate and 0.07 g of ε-polylysine hydrochloride powder (ε-PL) were added to 4 mL of THF solvent and stirred at room temperature for 10 h to obtain a spinning solution. The spinning solution was poured into a 5 mL syringe and an octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning technology. The spinning voltage was 20 kV, the spinning speed was 0.5 mL / h, the spinning spacing was 15 cm, the spinning solution volume was 100 μL, the deposition time was 20 min, and a mesh was used as a spinning collection device.

[0058] Example 7 Preparation of Octopus Sucker-like Nanofiber Membrane

[0059] 0.7 g of polyvinyl butyral and 0.21 g of ε-polylysine hydrochloride powder (ε-PL) were added to 4 mL of ethanol solvent and stirred at room temperature for 15 h to obtain a spinning solution. The spinning solution was poured into a 5 mL syringe and an octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning technology. The spinning voltage was 6 kV, the spinning speed was 2 mL / h, the spinning spacing was 5 cm, the spinning solution volume was 100 μL, the deposition time was 15 min, and a spinning collection device with an array circular hole structure was used.

[0060] Example 8 Preparation of Octopus Sucker-like Nanofiber Membrane

[0061] 0.7 g of polyvinylidene fluoride and 0.21 g of ε-polylysine hydrochloride powder (ε-PL) were added to 5 mL of DMF solvent and stirred at room temperature for 15 h to obtain a spinning solution. The spinning solution was poured into a 10 mL syringe and an octopus sucker-like nanofiber membrane (OS) was prepared by electrospinning technology. The spinning voltage was 6 kV, the spinning speed was 0.1 mL / h, the spinning spacing was 20 cm, the spinning solution volume was 100 μL, the deposition time was 15 min, and a spinning collection device with an array circular hole structure was used.

[0062] Example 9 Preparation method of tree trunk imitation nanofiber sponge

[0063] (1) Preparation of chitosan nanofiber membrane: 0.3 g chitosan (CS) powder was added to a mixed solvent of 13.5 mL hexafluoroisopropanol and 1.5 mL glacial acetic acid and stirred at room temperature for 24 h to obtain a chitosan spinning solution. Chitosan nanofiber membrane was prepared by electrospinning technology using an aluminum foil wrapped drum as a collection device. The parameters of the electrospinning technology were: spinning voltage 19 kV, flow rate 1.5 mL / h, spinning distance 10 cm, and deposition time 15 min. The chitosan nanofiber membrane was placed in 50% glutaraldehyde vapor for cross-linking for 12 h to obtain a water-insoluble chitosan nanofiber membrane.

[0064] (2) Preparation of tree trunk-like nanofiber sponge: The chitosan nanofiber membrane was cut into polygons with a side length of about 1 mm, placed in a high-speed homogenizer and crushed after adding deionized water, and deionized water was added at a solid content of 1% to obtain a short fiber suspension, and polyvinyl alcohol (PVA) was added to the short fiber suspension and mixed evenly, wherein the mass ratio of PVA to the short fibers of the nanofiber membrane was 0.19:1. The short fiber suspension was added to a container and frozen on a flat cold source (i.e., an iron plate frozen by liquid nitrogen) at a freezing temperature of -30°C. After freezing for 1 h, it was quickly transferred to a freeze dryer for drying for 60 h to obtain an initial nanofiber sponge.

[0065] (3) In order to make the three-dimensional ordered oriented sponge structure more stable, the initial nanofiber sponge was placed in a 120°C oven for thermal crosslinking for 2 h. After the thermal crosslinking, it was placed in 50% glutaraldehyde vapor for crosslinking for 24 h. After oven drying to remove the residual glutaraldehyde vapor, a tree trunk-mimicking nanofiber sponge (TT-1) was obtained.

[0066] Comparative Example: The difference from Example 9 is that the random pore structure sponge (R) directly prepared by cold source liquid nitrogen in step (3) is used as the control group, and no thermal crosslinking and glutaraldehyde vapor crosslinking experiments are performed.

[0067] Example 10

[0068] The raw materials and preparation method are the same as those in Example 9, except that the freezing temperature of -30°C is changed to -70°C to obtain a tree trunk-mimicking nanofiber sponge (TT-2).

[0069] Embodiment 11

[0070] The raw materials and preparation method are the same as those in Example 9, except that the freezing temperature of -30°C is changed to -110°C to obtain a tree trunk-mimicking nanofiber sponge (TT-3).

[0071] Example 12 Preparation method of tree trunk imitation nanofiber sponge

[0072] (1) Preparation of nanofiber membrane: 0.4 g of polyvinyl alcohol was added to 4 mL of water and stirred at room temperature for 24 h to obtain an electrospinning solution. The nanofiber membrane was prepared by electrospinning technology using an aluminum foil wrapped drum as a collection device. The parameters of the electrospinning technology were: spinning voltage 15 kV, flow rate 1.5 mL / h, spinning distance 14 cm, and deposition time 15 min. The nanofiber membrane was placed in 50% glutaraldehyde vapor for crosslinking for 12 h to obtain a water-insoluble nanofiber membrane.

[0073] (2) Preparation of tree trunk-like nanofiber sponge: The nanofiber membrane was cut into polygons with a side length of about 1 mm, placed in a high-speed homogenizer and crushed with deionized water, and deionized water was added at a solid content of 1% to obtain a short fiber suspension. Different amounts of graphene oxide aqueous dispersion were added to the short fiber suspension and mixed evenly, wherein the mass ratio of graphene oxide to fiber membrane was 1:5. The short fiber suspension was added to a container and frozen on a flat cold source (i.e., an iron plate frozen by liquid nitrogen), and the freezing temperature was -30°C. After freezing for 1 h, it was quickly transferred to a freeze dryer for drying for 60 h to obtain the initial nanofiber sponge.

[0074] (3) In order to make the three-dimensional ordered oriented sponge structure more stable, the initial nanofiber sponge was placed in a 120°C oven for thermal crosslinking for 2 h. After the thermal crosslinking, it was placed in 50% by mass glutaraldehyde vapor for crosslinking for 12 h. After oven drying to remove the residual glutaraldehyde vapor, a tree trunk-mimicking nanofiber sponge was obtained.

[0075] Example 13 Preparation method of tree trunk imitation nanofiber sponge

[0076] (1) Preparation of nanofiber membrane: 0.3 g collagen was added to 15 mL hexafluoroisopropanol and stirred at room temperature for 24 h to obtain a spinning solution. The nanofiber membrane was prepared by electrospinning technology using an aluminum foil wrapped drum as a collection device. The parameters of the electrospinning technology were: spinning voltage 5 kV, flow rate 0.1 mL / h, spinning distance 5 cm, and deposition time 15 min. The nanofiber membrane was placed in 1% glutaraldehyde vapor for crosslinking for 36 h to obtain a water-insoluble nanofiber membrane.

[0077] (2) Preparation of tree trunk-like nanofiber sponge: The nanofiber membrane was cut into polygons with a side length of about 1 mm, placed in a high-speed homogenizer and crushed after adding deionized water, and deionized water was added at a solid content of 1% to obtain a short fiber suspension, and polyvinyl alcohol (PVA) was added to the short fiber suspension and mixed evenly, wherein the mass ratio of PVA to the short fibers of the nanofiber membrane was 0.15:1. The short fiber suspension was added to a container and frozen on a flat cold source (i.e., an iron plate frozen by liquid nitrogen) at a freezing temperature of -30°C. After freezing for 1 h, it was quickly transferred to a freeze dryer for drying for 60 h to obtain an initial nanofiber sponge.

[0078] (3) In order to make the three-dimensional ordered oriented sponge structure more stable, the initial nanofiber sponge was placed in a 200°C oven for thermal crosslinking for 1 h. After the thermal crosslinking, it was placed in 1% glutaraldehyde vapor for crosslinking for 36 h. After oven drying to remove the residual glutaraldehyde vapor, a tree trunk-mimicking nanofiber sponge was obtained.

[0079] Example 14 Preparation method of tree trunk imitation nanofiber sponge

[0080] (1) Preparation of nanofiber membrane: 0.4 g of gelatin was added to 15 mL of hexafluoroisopropanol and stirred at room temperature for 24 h to obtain a spinning solution. The nanofiber membrane was prepared by electrospinning technology using an aluminum foil wrapped drum as a collection device. The parameters of the electrospinning technology were: spinning voltage 19 kV, flow rate 1.5 mL / h, spinning distance 10 cm, and deposition time 15 min. The nanofiber membrane was placed in 20% mass fraction glutaraldehyde vapor for crosslinking for 24 h to obtain a water-insoluble nanofiber membrane.

[0081] (2) Preparation of tree trunk-like nanofiber sponge: The nanofiber membrane was cut into polygons with a side length of about 1 mm, placed in a high-speed homogenizer and crushed after adding deionized water, and deionized water was added at a solid content of 1% to obtain a short fiber suspension, and polyvinyl alcohol (PVA) was added to the short fiber suspension and mixed evenly, wherein (the mass ratio of PVA to the short fibers of the nanofiber membrane was 0.2:1). The short fiber suspension was added to a container and frozen on a flat cold source (i.e., an iron plate frozen under liquid nitrogen) at a freezing temperature of -30°C. After freezing for 1 h, it was quickly transferred to a freeze dryer for drying for 60 h to obtain the initial nanofiber sponge.

[0082] (3) In order to make the three-dimensional ordered oriented sponge structure more stable, the initial nanofiber sponge was placed in a 60°C oven for thermal crosslinking for 12 h. After the thermal crosslinking, it was placed in 20% by mass glutaraldehyde vapor for crosslinking for 12 h. After oven drying to remove the residual glutaraldehyde vapor, a tree trunk-mimicking nanofiber sponge was obtained.

[0083] Example 15 Preparation method of tree trunk imitation nanofiber sponge

[0084] (1) Preparation of nanofiber membrane: 3.2 g of polyacrylonitrile (PAN) was added to a mixed solvent of 2 mL of tetrahydrofuran (THF) and 2 mL of N,N-dimethylformamide (DMF) and stirred at room temperature for 24 h to obtain an electrospinning solution. The nanofiber membrane was prepared by electrospinning technology using an aluminum foil wrapped drum as a collection device. The parameters of the electrospinning technology were: spinning voltage 20 kV, flow rate 2 mL / h, spinning distance 20 cm, and deposition time 15 min. The nanofiber membrane was placed in 50% glutaraldehyde vapor for cross-linking for 24 h to obtain a water-insoluble nanofiber membrane.

[0085] (2) Preparation of tree trunk-like nanofiber sponge: The nanofiber membrane was cut into polygons with a side length of about 1 mm, placed in a high-speed homogenizer and crushed after adding deionized water, and deionized water was added at a solid content of 1% to obtain a short fiber suspension, and polyvinyl alcohol (PVA) was added to the short fiber suspension and mixed evenly, wherein the mass ratio of PVA to the fiber membrane was 0.2:1. The short fiber suspension was added to a container and frozen on a flat cold source (i.e., an iron plate frozen under liquid nitrogen) at a freezing temperature of -30°C. After freezing for 1 h, it was quickly transferred to a freeze dryer for drying for 60 h to obtain the initial nanofiber sponge.

[0086] (3) In order to make the three-dimensional ordered oriented sponge structure more stable, the initial nanofiber sponge was placed in an oven at 110°C for thermal crosslinking for 3 h. After the thermal crosslinking, it was placed in 50% by mass glutaraldehyde vapor for crosslinking for 12 h. After oven drying to remove the residual glutaraldehyde vapor, a tree trunk-mimicking nanofiber sponge was obtained.

[0087] Example 16 Preparation method of tree trunk imitation nanofiber sponge

[0088] (1) Preparation of nanofiber membrane: 2.8 g of cellulose acetate (CA) was added to 4 mL of N,N-diethylacetamide and stirred at room temperature for 24 h to obtain an electrospinning solution. The nanofiber membrane was prepared by electrospinning technology using an aluminum foil wrapped drum as a collection device. The parameters of the electrospinning technology were: spinning voltage 15 kV, flow rate 1.5 mL / h, spinning distance 14 cm, and deposition time 15 min. The nanofiber membrane was placed in 50% glutaraldehyde vapor for cross-linking for 24 h to obtain a water-insoluble nanofiber membrane.

[0089] (2) Preparation of tree trunk-like nanofiber sponge: The nanofiber membrane was cut into polygons with a side length of about 1 mm, placed in a high-speed homogenizer and crushed after adding deionized water, and deionized water was added at a solid content of 1% to obtain a short fiber suspension, and polyvinyl alcohol (PVA) was added to the short fiber suspension and mixed evenly, wherein the mass ratio of PVA to the fiber membrane was 0.2:1. The short fiber suspension was added to a container and frozen on a flat cold source (i.e., an iron plate frozen under liquid nitrogen) at a freezing temperature of -30°C. After freezing for 1 h, it was quickly transferred to a freeze dryer for drying for 60 h to obtain the initial nanofiber sponge.

[0090] (3) In order to make the three-dimensional ordered oriented sponge structure more stable, the initial nanofiber sponge was placed in an oven at 110°C for thermal crosslinking for 3 h. After the thermal crosslinking, it was placed in 40% by mass glutaraldehyde vapor for crosslinking for 12 h. After oven drying to remove the residual glutaraldehyde vapor, a tree trunk-mimicking nanofiber sponge was obtained.

[0091] Example 17 Assembly of dual bionic dressing

[0092] (1) 0.7 g of poly-ε-caprolactone (PCL) particles were added to a mixed solvent of 3 mL DMF and 1 mL THF and stirred at room temperature for 12 h to obtain a spinning solution. The spinning solution was poured into a 5 mL syringe for later use.

[0093] (2) The octopus sucker-like nanofiber membrane obtained in Example 1 was cut into the same size as the bottom surface of the tree trunk-like nanofiber sponge obtained in Example 9, and the cut octopus sucker-like nanofiber membrane was placed on top of the tree trunk-like nanofiber sponge and temporarily fixed with tweezers. Figure 7 As shown in a.

[0094] (3) Start the electrospinning equipment. During the electrospinning process of the spinning solution, place the temporarily fixed octopus sucker nanofiber membrane and tree trunk nanofiber sponge between the needle tip and the collection device, and rotate continuously for 10 seconds to make the polycaprolactone fiber evenly wrapped on the surface, so that the octopus sucker nanofiber membrane and the tree trunk nanofiber sponge are tightly combined to obtain a dual bionic dressing. The spinning voltage is 6 kV, the spinning speed is 0.5 mL / h, the spinning distance is 10 cm, the deposition time is 15 min, and the aluminum foil wrapped roller is used as the collection device.

[0095] The lower layer of the double bionic dressing is a hydrophobic nanofiber membrane with a concave-convex array structure imitating an octopus sucker (OS), and the upper layer is a hydrophilic nanofiber sponge with a vertical directional pore structure imitating a tree trunk (TT). The concave cavity of the nanofiber membrane imitating the octopus sucker can unidirectionally suck the exudate from the wound surface, and the nanofiber sponge imitating the tree trunk sucks the exudate vertically for a second time over a long distance to keep the exudate away from the wound surface; the convex structure of the nanofiber membrane imitating the octopus sucker is in direct contact with the wound surface, which can reversely deliver drugs to the wound surface and accelerate the healing of severely exudative wounds.

[0096] Example 18 Assembly of dual bionic dressing

[0097] The preparation method is the same as that of Example 17, except that: in step (1), the raw material is polyurethane, the solvent is a mixed solvent of 3 mL DMF and 1 mL THF, and the concentration of the spinning solution is 0.1 g / ml.

[0098] The parameters of the electrospinning process were spinning voltage of 5 kV, spinning speed of 0.5 mL / h, spinning spacing of 10 cm, deposition time of 15 min, and an aluminum foil-wrapped drum as the collection device.

[0099] Example 19 Assembly of dual bionic dressing

[0100] The preparation method is the same as that of Example 17, except that: in step (1), the raw material is polylactic acid, the solvent is 4 mL of dichloromethane solvent, and the concentration of the spinning solution is 0.5 g / ml.

[0101] The parameters of the electrospinning process were spinning voltage of 10 kV, spinning speed of 0.5 mL / h, spinning spacing of 10 cm, deposition time of 15 min, and an aluminum foil-wrapped drum as the collection device.

[0102] Example 20 Assembly of dual bionic dressing

[0103] The preparation method is the same as that of Example 17, except that: in step (1), the raw material is poly(lactide-glycol), the solvent is 4 mL of chloroform solvent, and the concentration of the spinning solution is 2 g / ml.

[0104] The parameters of the electrospinning process were spinning voltage of 6 kV, spinning speed of 0.5 mL / h, spinning spacing of 10 cm, deposition time of 15 min, and an aluminum foil-wrapped drum as the collection device.

[0105] Example 21 Assembly of dual bionic dressing

[0106] The preparation method is the same as that of Example 17, except that: in step (1), the raw material is polysulfone, the solvent is a mixed solvent of 2 mL hexafluoroisopropanol and 2 mL THF, and the concentration of the spinning solution is 5 g / ml.

[0107] The parameters of the electrospinning process were spinning voltage of 15 kV, spinning speed of 1 mL / h, spinning spacing of 18 cm, deposition time of 15 min, and an aluminum foil-wrapped drum as the collection device.

[0108] Example 22 Assembly of dual bionic dressing

[0109] The preparation method is the same as that of Example 17, except that: in step (1), the raw material is polymethyl methacrylate, the solvent is 4 mL THF solvent, and the concentration of the spinning solution is 3 g / ml.

[0110] The parameters of the electrospinning process were spinning voltage of 20 kV, spinning speed of 0.5 mL / h, spinning spacing of 15 cm, deposition time of 15 min, and an aluminum foil-wrapped drum as the collection device.

[0111] Example 23 Assembly of dual bionic dressing

[0112] The preparation method is the same as that of Example 17, except that: in step (1), the raw material is polyvinyl butyral, the solvent is 4 mL of ethanol solvent, and the concentration of the spinning solution is 1 g / ml.

[0113] The parameters of the electrospinning process were spinning voltage of 6 kV, spinning speed of 2 mL / h, spinning gap of 5 cm, deposition time of 15 min, and an aluminum foil-wrapped drum as the collection device.

[0114] Example 24 Assembly of dual bionic dressing

[0115] The preparation method is the same as that of Example 17, except that: in step (1), the raw material is polyvinylidene fluoride, the solvent is 5 mL DMF solvent, and the concentration of the spinning solution is 0.5 g / ml.

[0116] The parameters of the electrospinning process were spinning voltage of 6 kV, spinning speed of 0.1 mL / h, spinning spacing of 20 cm, deposition time of 15 min, and an aluminum foil-wrapped drum as the collection device.

[0117] Performance characterization:

[0118] 1 Characterization of octopus sucker-like nanofiber membrane

[0119] 1.1 Characterization methods

[0120] (1) Morphological characterization of octopus sucker-like nanofiber membrane

[0121] The macroscopic morphology of the octopus sucker nanofiber membrane (OS) was observed by taking digital photos with a mobile phone (real me X9 pro). The OS morphology was observed using a profilometer, and the cavity diameter, cavity spacing, and protrusion area were measured. The deposition of fibers in the cavity was observed using an optical microscope: different spinning solution volumes (10, 30, 50, 100 μL) were controlled to obtain optical images of the nanofibers in the cavity. The area ratio of nanofibers to the cavity was calculated using Image J software.

[0122] (2) Study on the unidirectional vertical liquid suction performance of octopus suction cup nanofiber membrane

[0123] Study on the performance of unidirectional suction of droplets: Octopus sucker nanofiber membrane (OS) was combined with non-woven fabric to form a double-layer structure of octopus sucker dressing. The octopus sucker dressing was placed on a white A4 paper, and 130 μL of blue methylene blue PBS droplets were dripped onto the dressing surface from the hydrophobic side and the hydrophilic side, respectively. The process of droplet suction was recorded using the video function of a mobile phone. After the suction was completed, the A4 paper was uncovered to observe whether there was a blue dye mark on the A4 paper. Study on the vertical suction performance of a single droplet: The octopus sucker nanofiber membrane (OS) was labeled with curcumin. Drops of Rose Red B were dripped onto the (octopus sucker nanofiber membrane), and the fluorescent camera was used to record the position and process of liquid suction from the hydrophobic side to the hydrophilic side. Drops of Rose Red B were dripped from the hydrophilic side to the hydrophobic side to observe whether dye appeared on the hydrophobic side. A double-layer non-woven dressing (NW dressing) composed of a non-bionic nanofiber membrane (NW) and a hydrophilic material was used as the control group to compare and observe the liquid suction process of droplets on the surfaces of the two dressings.

[0124] (3) Study on the performance of octopus sucker-like nanofiber membrane in efficient drug delivery

[0125] Create a 1 cm2 The wound was simulated by a notch, and 100 μL of phosphate buffer solution was added to the notch. The NW dressing was used as the control group. The octopus sucker nanofiber membrane was placed on the wound for 10 h, and 50 μL of phosphate buffer solution was added every hour. With the help of UV-visible spectrophotometer (UV-vis), the amount of drug that was not released or entered the hydrophilic layer of the octopus sucker nanofiber membrane was determined. Since the drug only exists on the surface of pig skin and in the octopus sucker nanofiber membrane, the amount of drug released into the pig skin can be obtained by subtracting the measured residual amount of drug in the octopus sucker nanofiber membrane from the known total amount of drug.

[0126] 1.2 Experimental Results

[0127] (1) Morphological characterization of octopus sucker-like nanofiber membrane

[0128] By changing the structure of the collecting device, the octopus sucker-like nanofiber membranes with a cavity diameter of 0.5 mm and cavity spacing of 0.6 mm, 0.8 mm, 1.0 mm, and 1.2 mm (denoted as: 0.5-0.6, 0.5-0.8, 0.5-1.0, and 0.5-1.2) and the octopus sucker-like electro-fiber membranes with a cavity spacing of 1.2 mm and cavity diameters of 0.5 mm, 0.7 mm, and 1.0 mm (denoted as: 0.5-1.2, 0.7-1.2, and 1.0-1.2) were prepared. Figure 1 a, b). The surface profile of the bionic OS fiber membrane was observed using a profilometer. The results showed that the surface of the bionic OS fiber membrane was composed of concave cavities (blue) and convexities (red and green). The cross-sectional line graph of the profilometer showed that the height difference between the convexities and the concave cavities exceeded 20 μm ( Figure 1 c). The cavity area can be increased by reducing the cavity spacing and increasing the cavity diameter; conversely, the convex area can be increased by increasing the cavity spacing and reducing the cavity diameter ( Figure 1 d).

[0129] In order to explore the formation mechanism of the octopus sucker-like structure, the distribution of nanofibers in the cavity was observed under a microscope. The density of nanofibers increased with the increase of spinning solution. When the spinning solution amount was 10 μL, the nanofiber area accounted for 21.37%; when the spinning solution amount increased to 100 μL, the nanofiber area accounted for 75.38% ( Figure 1 e,f). This may be due to the fact that when the nanofibers approach the template, the deposition of the fibers is affected by the Coulomb interaction ( Figure 1g). The Coulomb interaction is inversely proportional to the square of the distance between the charges. Because the distance between the fiber and the protrusion of the template is shorter, the stronger Coulomb interaction between the fiber and the protrusion will drive the fiber to deposit on the protrusion, forming a convex structure, and only a small amount of fiber is deposited on the non-protrusion. As the amount of deposition liquid increases, the deposition area of ​​the fiber in the non-protrusion increases. When the fiber is deposited on the template again, the distance between the fiber and the non-protrusion and the protrusion is close, the Coulomb interaction tends to be the same, and the fiber tends to be uniformly deposited on the entire template surface, eventually forming an octopus suction cup-like nanofiber membrane with a concave-convex structure.

[0130] (2) Study on the unidirectional vertical liquid suction performance of octopus suction cup nanofiber membrane

[0131] The suction process of the octopus suction cup nanofiber membrane (OS) on the droplet was observed from the top view and the side view. From the top view, the blue droplet remained in the hydrophobic layer in a spherical shape for 0.88 s, after which the spherical droplet shrank, the blue dye entered the hydrophilic layer, and diffused laterally in the hydrophilic layer ( Figure 2 a). After 3.06 s, no blue liquid remained on the hydrophobic side, and the liquid left the bionic OS fiber membrane. When the dressing was uncovered, dye marks were observed on the white paper and the surface of the hydrophilic layer, indicating that the blue liquid was completely sucked into the hydrophilic layer. On the contrary, Figure 2 As shown in (b), the blue droplet quickly wets the surface of the hydrophilic layer and spreads laterally to form an obvious blue mark. After removing the dressing, no blue dye mark was observed on the white paper and the surface of the hydrophobic layer, indicating that the liquid cannot pass from the hydrophilic side to the hydrophobic side. These results show that the octopus suction cup-like nanofiber membrane has the ability to unidirectionally suck liquid.

[0132] The effect of the concave cavity structure in the bionic OS fiber membrane on the droplet suction process was observed through a side view. The results showed that after the droplet contacted the hydrophobic side of the octopus sucker dressing, the droplet could pass through the octopus sucker nanofiber membrane. The red droplet always remained spherical until the liquid was completely discharged. The liquid suction process of the octopus sucker dressing was vertical ( Figure 2 c). The green color of the convex part is obvious, and there is no red residue, which indicates that the droplet passes through the bionic OS fiber membrane through the cavity during the suction process. When the droplet falls on the hydrophilic side, the droplet spreads laterally in the hydrophilic layer. There is no red mark on the hydrophobic side, indicating that the hydrophobic side is not wetted, and the liquid suction of the droplet on the octopus suction cup dressing is unidirectional ( Figure 2 d). By comparing with the non-bionic structure nanofiber membrane, it was found that when the droplet fell on the surface of the non-bionic structure nanofiber membrane, the non-bionic structure fiber membrane was dyed red, indicating that the fiber membrane was wetted, and the droplet still remained on the hydrophobic side surface after the seepage was diverted away ( Figure 2e). After the liquid contacts the hydrophilic material, the liquid diffuses laterally, and the green non-bionic structure fiber membrane becomes darker and red appears, indicating that the non-bionic structure fiber membrane is wetted and the non-bionic structure fiber membrane has poor unidirectional liquid conduction ( Figure 2 f). In summary, the introduction of the octopus-like structure can make the liquid suction function of the nanofiber membrane both vertical and unidirectional.

[0133] The suction mechanism of the octopus suction cup nanofiber membrane (OS) is as follows:

[0134] The fiber membrane is hydrophobic, with a contact angle greater than 90°, and the cavity is similar to a hydrophobic capillary. When the liquid contacts the cavity, the liquid surface tends to form an upward convex half-moon shape, allowing the liquid to enter the cavity. For the cavity of the octopus suction cup nanofiber membrane, the hydrophobic fiber membrane layer is very thin and fits the hydrophilic layer. The liquid is subjected to a wetting force (f w ) upward, so that the Laplace pressure between the fibers is eliminated, and the liquid can pass through the hydrophobic fibers into the hydrophilic layer. However, for the protrusions of the octopus sucker-like nanofiber membrane, the liquid is subject to gravity (G) and Laplace pressure (f c ), because the hydrophobic fiber layer at the convex part is thicker, liquid can be retained between the fibers. The liquid cannot break through the fiber layer and contact the hydrophilic layer by relying solely on the wetting effect of the fiber surface. The liquid will not be affected by the upward wetting force from the hydrophilic layer (f w ), so the raised part cannot conduct away the liquid. For NW dressings, the thickness of the hydrophobic film is small. After the liquid contacts the hydrophobic fiber, the liquid wets the surface of the hydrophobic fiber. After the fiber is completely wetted, the liquid will break through the hydrophobic fiber and contact the hydrophilic layer, and will be affected by the upward wetting force (f w ) effect, allowing the liquid to pass through the hydrophobic fiber layer and enter the hydrophilic layer.

[0135] When the liquid reaches the hydrophilic material, due to the wetting force (f w ) effect, the liquid diffuses in the hydrophilic layer and is locked in the hydrophilic layer. However, as the amount of liquid gradually increases, the liquid will be affected by the downward gravity (G), forming a downward convex half-moon liquid surface between the hydrophobic fibers, and will be affected by the upward Laplace force (f c ). As the distance between fibers decreases, the Laplace force (f c) becomes larger. The convex part of the octopus suction cup nanofiber membrane has a high fiber density and thickness, and the gravity is smaller than the Laplace force, so it will not reverse osmosis of liquid; the rest of the liquid will contact the fibers in the concave cavity, where the fibers are relatively sparse and fc is small, and the liquid may pass through it. However, when the liquid reaches the concave cavity, the concave cavity structure is similar to a hydrophobic capillary, and the liquid appears a downward convex liquid surface in the capillary. These liquids will be subjected to an upward Laplace pressure (ΔP), which hinders the reverse osmosis of the liquid. The difference is that the NW dressing has only one layer of non-woven fibers. When the gravity of the liquid is greater than the Laplace force (fc), reverse osmosis occurs.

[0136] (3) Study on the reverse delivery performance of antimicrobial agents by octopus suction cup-like nanofiber membrane

[0137] ε-polylysine (ε-PL) with broad-spectrum antibacterial properties was used as a model drug. The drug delivery process was studied to explore the effect of the protrusion area on drug delivery efficiency ( Figure 3 a,b). Figure 3 As shown in Figure c, ε-PL has a maximum absorption peak at 193 nm, and the concentration of ε-PL can be measured using a UV-visible spectrophotometer.

[0138] The delivery efficiency of non-bionic fiber membrane and bionic OS fiber membrane was compared to study the effect of octopus suction cup structure on drug delivery efficiency. Figure 3 As shown in Figure d, the octopus sucker-like nanofiber membranes all have higher drug delivery efficiency. The bionic OS fiber membrane 0.5-1.2 with the highest drug delivery efficiency has a delivery efficiency of 85.84%, which is 22% higher than the drug delivery efficiency of the non-bionic structure nanofiber membrane, indicating that the structure of the octopus sucker can improve the delivery efficiency of ε-PL. Figure 3 e shows that when the protrusion area increases from 45.49% to 86.37%, the drug delivery efficiency increases from 79.45% to 85.84%. The results show that the delivery efficiency increases with the increase of the protrusion area.

[0139] 2 Performance test of TT-1, TT-2 and TT-3 tree trunk imitation nanofiber sponges:

[0140] 2.1 Characterization of tree trunk-mimicking nanofiber sponge

[0141] The trunk-like nanofiber sponge prepared by scanning electron microscopy (SEM) was characterized for morphology. The pore sizes of 100 vertical holes in the SEM image were counted and then the average value was calculated. The tortuosity of the vertical hole was calculated, that is, the ratio of the length of the curve along the pore direction between the two endpoints to the shortest distance (Euclidean distance):

[0142]

[0143] Where L c is the length of the curved line; L r is the linear length of the medium.

[0144] Experimental results and discussion:

[0145] like Figure 4 As shown in a, a tree trunk-like nanofiber sponge (TT-1) with a vertical oriented pore structure was successfully prepared. When the tree trunk-like nanofiber sponge (TT-1) is placed on a branch bud, it will not cause the branch bud to bend, indicating that the tree trunk-like nanofiber sponge (TT-1) is ultra-light ( Figure 4 b). Press the tree trunk imitation nanofiber sponge (TT-1) by hand, compress it by 50% and then remove the external force. The tree trunk imitation nanofiber sponge (TT-1) can rebound to its original shape, indicating that the tree trunk imitation nanofiber sponge (TT-1) has resilience ( Figure 4 c). The vertical oriented pore structure of the tree trunk-like nanofiber sponge (TT-1) was observed from the cross section and longitudinal section using a scanning electron microscope. The results showed that the cross section had a densely arranged macroporous structure ( Figure 4 d); Zooming in on the side wall, it is observed that the fibers overlap each other to form the side wall, and there are small holes between the fibers ( Figure 4 e); The longitudinal section shows that TT-1 has a long-range ordered structure ( Figure 4 f).

[0146] Comparing the longitudinal sections of the three tree trunk-like nanofiber sponges, the results show that the pore sizes of the vertically oriented pores decrease in sequence. However, the pores of the random pore sponge R are irregular ( Figure 4 g). The statistical results of the vertical oriented pore size of the tree trunk-like nanofiber sponge show that the vertical oriented pore sizes of the tree trunk-like nanofiber sponge TT-1, tree trunk-like nanofiber sponge TT-2 and tree trunk-like nanofiber sponge TT-3, which were frozen at -30, -70 and -110°C, are 38, 29 and 12 μm respectively. Figure 4 h). This indicates that the pore size decreases as the freezing temperature decreases.

[0147] The formation mechanism of vertical directional holes is speculated. The vertical directional holes may be caused by the sublimation of ice crystals that grow directionally during the freezing process. The plane cold source forms a temperature gradient from bottom to top, and the ice crystals grow from bottom to top, causing the short fiber suspension to freeze directionally. The chitosan fibers are squeezed between the ice crystals to form the pore wall. After the ice crystals sublimate into gas, a vertical directional pore structure will be left. The freezing speed affects the size of the vertical directional pores. The lower the cold source temperature, the faster the freezing speed, the smaller the ice crystals, and the smaller the pore size of the vertical directional holes.

[0148] The tortuosity of the three tree trunk-like nanofiber sponges (TT-1, TT-2, and TT-3) is between 1.018 and 1.022, all close to 1, indicating that the vertical oriented pore structure of the tree trunk-like nanofiber sponges has low tortuosity and high orientation ( Figure 4 i).

[0149] 2.2 Long-distance vertical liquid suction performance of tree trunk-mimicking nanofiber sponge

[0150] Add 2 mL of PBS solution containing blue methylene blue to the crystallization dish to simulate the infiltration, put a semi-cylindrical sponge with a diameter of 1 cm and a height of 3 cm into the crystallization dish (the directional hole direction is perpendicular to the liquid surface), use the mobile phone video function to shoot the liquid suction process of the tree trunk nanofiber sponge, measure the liquid transmission height, and record the corresponding suction time. Place sponges with different pore sizes in the crystallization dish to compare the effect of the pore size of the vertical directional pores on the liquid suction performance. With the help of the capillary model, analyze the force of the liquid in the vertical directional pores, and study the vertical suction mechanism of the liquid in the tree trunk nanofiber sponge. The random pore sponge R prepared in the comparative example was used as the control group.

[0151] Experimental results and discussion:

[0152] By studying the vertical suction process of tree trunk-like nanofiber sponge, the effect of the vertical oriented pore diameter on the vertical suction speed is explored. Figure 5 As shown in a and b, at 16 s, the liquid transmission height of the TT-1 tree trunk nanofiber sponge with the largest pore size reached 3 cm; in comparison, the transmission height of the random pore sponge R was only 1.17 cm at 16 s, which was only 39% of the height of TT-1. The tree trunk nanofiber sponge took less time to transmit to a height of 3 cm than the random pore sponge R. This shows that the tree trunk nanofiber sponge can transmit liquid upward to a higher distance in the same time.

[0153] Liquid can be vertically sucked in the tree trunk-like nanofiber sponge. This may be because after the liquid contacts the tree trunk-like nanofiber sponge, the chitosan sponge is hydrophilic, and the liquid forms a concave liquid column inside the vertical oriented hole ( Figure 5 d). The pressure of the liquid is different from that of the gas above the liquid surface. This pressure difference between the internal and external gas-liquid pressures due to the surface curvature is called the Laplace pressure (F S ), which can be described by the Young-Laplace formula. According to the definition of curvature, the curvature of the concave liquid surface is negative, so the Laplace pressure is less than zero. In other words, the liquid pressure near the concave liquid surface is less than the gas pressure. However, since the pressure inside and outside the channel must be kept equal, that is, the absolute pressure is equal to the atmospheric pressure, the pressure inside the capillary is less than the atmospheric pressure. This allows the liquid to overcome its own gravity (G) and be forced to spontaneously transport along the channel until F SEqual to G. The channel direction in the random pore sponge is random. Under the action of gravity, the liquid in the random pore sponge tends to be transmitted horizontally first. The tree trunk-like nanofiber sponge has a vertical oriented pore structure. The liquid will spontaneously transmit upward along the vertical pore structure. Therefore, the tree trunk-like nanofiber sponge can make the liquid transmit vertically upward. The vertical oriented pore structure can transmit the liquid higher in the same time.

[0154] All tree trunk-like nanofiber sponges have faster suction speeds than the random pore sponge R ( Figure 5 c), the liquid suction speed of TT-1 is 0.21 cm / s, and the liquid suction speed of R is 0.04 cm / s. The liquid suction speed of TT-1 is 5.25 times that of R. This shows that the tree trunk-like nanofiber sponge can quickly transfer liquid from the bottom to the top. According to the Washburn equation, ignoring air resistance, the rate equation corresponding to capillary conduction is:

[0155]

[0156] h is the transport height of the liquid, r is the radius of the capillary, γ is the surface tension of the liquid, θ is the interfacial contact angle, η is the viscosity of the liquid, t is the transport time, and l is the length filled by the liquid.

[0157] The rate of liquid under its own capillary pressure is directly proportional to the radius of the capillary, the cosine of the contact angle, the ratio of surface tension to liquid viscosity, and inversely proportional to the length that the liquid has filled. This formula is consistent with the experimental results. The trunk sponge TT-1 with the largest vertical oriented pore size has the fastest liquid suction speed. The suction speed of the trunk-like nanofiber sponge can be adjusted by the vertical oriented pore size. As the pore size increases, the trunk-like nanofiber sponge exhibits a faster liquid suction speed.

[0158] 2.3 Compression resilience of tree trunk-mimicking nanofiber sponge

[0159] By studying the compression-rebound process in the direction parallel to the pores and perpendicular to the pores, the anisotropic compression-rebound elasticity of the tree trunk-mimicking nanofiber sponge was explored. Figure 6 As shown in a, when the tree trunk-like nanofiber sponge deforms parallel to the directional pore direction, the stress of the tree trunk-like nanofiber sponge increases rapidly until the compression deformation exceeds 30%, and then the increase in stress begins to slow down ( Figure 6 b). As the compression deformation increases from 10% to 50%, the compression resilience gradually decreases. When compressed below 30%, the tree trunk nanofiber sponge can rebound to more than 95% of its original shape. When compressed to 50%, the tree trunk nanofiber sponge can only rebound to 90% of its original shape. After deformation perpendicular to the pore direction, the tree trunk nanofiber sponge has good resilience and can still recover to its original shape when the compression deformation reaches 50% ( Figure 6 c) If Figure 6 As shown in (d), the deformation stress parallel to the directional pores is 1.97-3.75 times that perpendicular to the directional pores. The results show that the mechanical strength and elastic modulus of the trunk-mimicking nanofiber sponge are anisotropic.

[0160] Comparing the compression resilience of tree trunk-like nanofiber sponge and random pore sponge, the results show that when the compression deformation is 50%, the compression stress of TT-3 is 32.84 kPa in the parallel direction, and the compression stress of R is 10.9 kPa. The compression stress of TT-3 is 3.01 times that of R ( Figure 6 e). In the vertical direction, the compressive stress of TT-3 is 23.64 kPa, and the compressive stress of R is 7.11 kPa. The compressive stress of TT-3 is 3.32 times that of R ( Figure 6 f).

[0161] It is speculated that the excellent compression resilience of the tree trunk-like nanofiber sponge is due to the unique vertical oriented pore structure of the tree trunk-like nanofiber sponge. From the SEM image, it can be seen that the pore wall is formed by the overlap of fibers and fibers. When pressure is applied in the direction parallel to the oriented pores, the pore wall supports the sponge. The sponge is difficult to be compressed in the direction parallel to the pores, so the deformation stress is large. The size of the pore size will also affect the mechanical properties of the tree trunk-like nanofiber sponge. By comparing the compression-resilience of different pore sizes and taking the sponge with random pore structure as the control group, a comparison is made. Compared with the random pore sponge, the tree trunk-like nanofiber sponge has better mechanical strength and compression resilience. The random pore sponge has isotropic mechanical properties, uniformly distributed pores and fibers, which makes the sponge have less mechanical strength when it is compressed.

[0162] The compression-rebound results of tree trunk nanofiber sponges with different vertical oriented pore sizes were compared to study the effect of the vertical oriented pore size on the compression rebound elasticity. The results showed that when the compression direction was parallel to the vertical oriented pore, TT-3 with the smallest pore size had the greatest mechanical strength and elastic modulus, and also showed the best rebound elasticity during rebound. When the compression direction was parallel to the vertical oriented pore direction, TT-1 with the largest pore size had the smallest compressive stress, but had the best compression rebound elasticity, and could rebound to its original state after being compressed by 50%.

[0163] 3 Characterization of the double bionic dressing

[0164] 3.1 Characterization methods

[0165] (1) Study on the performance of the double-bionic dressing obtained in Example 17 for two vertical liquid suctions

[0166] A sponge filled with water was used to simulate edema tissue to explore the suction performance of OS&TT on exudate in edema tissue. A commercial gelatin sponge was filled with Rose Red B solution to simulate edema tissue, and a semi-cylindrical OS&TT with a diameter of 1 cm and a height of 2 cm was placed on the "edema tissue". The OS side was in contact with the "edema tissue" and the directional hole of the TT was perpendicular to the liquid surface. The video was taken using the video recording function of a mobile phone to measure the liquid transmission height and record the suction time. Using TT as the control group, the suction height and suction speed were compared, and the mechanism of OS&TT's two vertical suctions was explored.

[0167] (2) Study on the high efficiency delivery performance of antibacterial agent of dual bionic dressing obtained in Example 17

[0168] The double bionic dressing was cut into a cylinder with a diameter of 1 cm and a height of 0.5 cm. The control group was a combination of non-bionic nanofiber membrane (NW) and tree trunk-like nanofiber sponge (TT). The antimicrobial delivery efficiency of the double bionic dressing (OS&TT) was measured to explore the relationship between the double bionic structure and the antimicrobial delivery efficiency.

[0169] (3) Study on the effect of the dual bionic dressing obtained in Example 17 on the healing of bacterially infected wounds

[0170] (3.1) Research on establishment and healing promotion of bacterial infection wounds

[0171] The preparation process of the dual bionic dressing without antibacterial agent (OS&TT(N)) is the same as that of Example 17, except that the drug ε-polylysine hydrochloride powder is not added during the preparation of the octopus suction cup nanofiber membrane.

[0172] Forty ICR mice were selected and anesthetized with sodium pentobarbital (50 mg / kg). The hair was shaved and depilatory cream was used to remove the hair. A full-thickness wound with a diameter of 8 mm was cut on the front chest of the mouse. 100 μL of 1×10 8 CFU / mL Staphylococcus aureus, apply 3M transparent dressing, wrap and fix with elastic bandage, record as day 0 after 24 hours, randomly divide mice into 4 groups, place the double bionic dressing (OS&TT) obtained in Example 17, the octopus suction cup nanofiber membrane dressing (OS) obtained in Example 1, the double bionic dressing without antibacterial agent (OS&TT(N)), and the blank group (Blank) without dressing, place the dressing on the wound, fix it with 3M transparent airtight dressing, wrap and fix it with elastic bandage, and change the dressing every 24 hours. Take pictures and measure the wound area on days 1, 3, 7, and 13, and measure the wound closure rate according to the following formula:

[0173] Wound closure rate = (S x -S 0 ) / S x ×100%(3)

[0174] Where S x is the wound area on day x (1, 3, 8, 15), S 0 It is the initial size of the wound.

[0175] (3.2) In vivo antibacterial activity study

[0176] The exudate from the wound on the third day was collected with a sterile cotton swab and placed in 1 mL of PBS solution. The bacterial solution was diluted and smeared on the agar plate, and the number of colonies was counted.

[0177] (3.3) Histochemical staining analysis

[0178] The wound tissues were collected on the 13th day for H&E staining and Masson staining. Images were collected by scanning machine, and the wound length and collagen fiber density were statistically analyzed using Image J software.

[0179] (3.4) Statistical analysis

[0180] In all experiments, each group of experiments was repeated at least three times, and the results of three times were used for statistical analysis. Statistical analysis was performed using GraphPad Prism 8 software, and the results were expressed as mean ± standard deviation. The differences between the groups were analyzed using a two-sample t-test, and when p ≤ 0.05, it was considered statistically significant and marked with *; when p was less than or equal to 0.01, it was marked with **; when p ≤ 0.001, it was marked with ***.

[0181] 3.2 Experimental Results

[0182] (1) Study on the performance of double-bionic dressing in vertically aspirating liquid

[0183] like Figure 7 As shown in a, OS and tree trunk-like nanofiber sponge TT were combined into a dual bionic dressing OS&TT by electrospinning technology. Comparing the process of water suction in the sponge by the dual bionic dressing (OS&TT) and the tree trunk-like dressing (TT), it was found that the liquid suction height of OS&TT reached 2 cm in 50s, which was about 13% higher than the liquid suction height of TT (1.77 cm). Figure 7 b,c). Figure 7 d. Before 20 s, the liquid suction heights of the dual bionic dressing and the tree trunk nanofiber sponge were basically the same, both reaching half the sponge height in 20 s. After 20 s, the liquid suction height of the dual bionic dressing gradually widened the gap with the tree trunk nanofiber sponge, and the suction height exceeded the tree trunk nanofiber sponge in the same time. The mechanism of the two vertical liquid suctions of OS&TT and TT is capillary action. The height and time are calculated by the formula h=at b Fitting, R of the fitting result2 Greater than 0.99, the fitting curve fits the actual process of liquid suction. The b value of TT is 0.59, which is close to the theoretical value of vertical liquid suction of 0.5, while the b value of OS&TT reaches 0.70, which deviates greatly from 0.5, indicating that the first vertical liquid suction of the bionic OS fiber membrane can change the vertical liquid suction behavior of the bionic TT sponge. The fitting curve is derived to obtain the speed change curves of OS&TT and TT during the vertical liquid suction process. The speeds of OS&TT and TT both show a gradually decreasing trend, which is consistent with the speed formula of the Washburn equation. The liquid suction speed is inversely proportional to the length that the liquid has filled. However, the change trend of OS&TT is smaller than that of TT. At 50 s, the liquid suction speed of OS&TT is 1.34 times that of TT ( Figure 7 e). This shows that the double vertical suction of OS&TT can increase the suction speed of liquid.

[0184] (2) Study on the performance of dual bionic dressing in delivering antimicrobial agents

[0185] like Figure 7 f. The delivery efficiency of the double bionic dressing (OS&TT) reached 88.27%, which was 22% higher than that of the combination of non-bionic structure nanofiber membrane and trunk-like nanofiber sponge (NW&TT), effectively realizing the efficient delivery of ε-PL by the double bionic dressing. It is worth noting that compared with the ordinary hydrophilic layer, the presence of TT increased the delivery efficiency of both OS&TT and NW&TT by more than 2%. This is because TT allows the liquid to be directly transferred upward to the top of the sponge, avoiding a large amount of liquid residue at the hydrophilic-hydrophobic junction, reducing the loss of ε-PL, and thus improving the ε-PL delivery efficiency. This shows that OS&TT can efficiently deliver ε-PL to the wound surface.

[0186] (3) Study on promoting healing of bacterially infected wounds using dual bionic dressings

[0187] (3.1) Research on establishment and healing promotion of bacterial infection wounds

[0188] The repair effect of double bionic dressing on bacterial infection wounds was studied. Figure 8 As shown in a, the photos of the wound healing process show that the wound area decreases with the increase of healing days. In the first 3 days, the wounds of the four groups appeared yellow, indicating that the wounds were infected and pus was produced in the wounds. On the 3rd day, there was still yellow in the wounds of the three control groups. In contrast, the yellow color disappeared in the OS&TT group, exposing the red wound tissue. This shows that the bacterial infection at the wound of the OS&TT group was controlled. On the 7th day, there was no pus in OS&TT, OS, and OS&TT (N), and the wound area decreased. On the 13th day, the wounds of the three control groups had not yet closed. In contrast, the wounds of the experimental group OS&TT group were completely closed.

[0189] The wound area color simulation results showed that the wound area of ​​the OS&TT group continued to shrink during the wound healing process. Figure 8 As shown in b, on the 13th day, the wound closure rate of the blank control group was 58.7%; the wound closure rates of OS and OS&TT (N) were between 81% and 83%; in comparison, the wound closure rate of OS&TT was as high as 87.6%, indicating that OS&TT has the best performance in promoting the healing of bacterially infected wounds.

[0190] (3.2) In vivo antibacterial activity study

[0191] The antibacterial effect of the double bionic dressing on the wound surface was evaluated by counting the exudate smear plate. Figure 8 As shown in c and d, the plate was smeared and found that there were no colonies in the OS&TT treatment group, while there were a small number of colonies in the OS treatment group, indicating that the antibacterial effect of the wound treated by the OS&TT group was the best, which was mainly because the OS&TT group had the best antibacterial agent delivery efficiency.

[0192] (3.3) Histological staining analysis

[0193] H&E staining was used to evaluate the effect of the double bionic dressing on wound tissue healing. Fig. 9 As shown in a and c, the H&E results showed that the dermis of the control group had a loose structure and a large number of inflammatory cells and fibroblasts, indicating that the wound surface had not yet healed. In contrast, in the OS&TT group, only a small number of inflammatory cells were present, the skin structure of each layer was dense and orderly, and the squamous epithelial cells were intact and uniform; at the same time, new skin appendages could be observed in the regenerated skin tissue. This shows that the wound surface of the OS&TT group was basically healed.

[0194] Masson staining was used to study the deposition of collagen fibers in the wound. Fig. 9 As shown in b, the results of Masson staining showed that there were very few blue collagen fibers in the blank group, and most of them were red muscle fibers. In contrast, the blue collagen fibers in the OS&TT group were complete in structure, evenly arranged, and denser than those in other groups, with only a small amount of red muscle fibers. This indicates that the dermis healed well in the OS&TT group. This may be due to the fact that the infection on the wound was not effectively controlled in a timely manner. Comparison of the deposition of collagen fibers ( Fig. 9 d), it was found that the collagen fiber deposition in the OS&TT group was the largest, reaching about 81.16%, indicating that the OS&TT group had the best effect on the healing of bacterial infection wounds.

[0195] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and the specific implementation of the present invention cannot be limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A dual bionic dressing with unidirectional vertical fluid conduction and reverse drug delivery, characterized in that: The invention is composed of an upper layer of tree trunk-imitating nanofiber sponge and a lower layer of octopus suction cup-imitating nanofiber membrane. The upper layer of tree trunk-imitating nanofiber sponge is a hydrophilic material with a tree trunk-imitating vertical directional pore structure, and the lower layer of octopus suction cup-imitating nanofiber membrane is a hydrophobic material with an octopus-imitating concave-convex array structure.

2. A method for preparing a dual bionic dressing with unidirectional vertical fluid conduction and reverse drug delivery, characterized in that: Firstly, octopus sucker-like nanofiber membranes were prepared by electrospinning equipment using soluble hydrophobic polymer materials and drugs as raw materials. Secondly, nanofiber membranes were obtained by electrospinning equipment using soluble hydrophilic polymer materials as raw materials, stabilizers were added after homogenization, and tree trunk-like nanofiber sponges were obtained after freeze-drying, heat cross-linking and glutaraldehyde steam cross-linking. Finally, the tree trunk-like nanofiber sponges were placed on octopus sucker-like nanofiber membranes of equal areas, and nanofibers prepared by electrospinning equipment using soluble hydrophobic polymer materials as raw materials were wrapped around the tree trunk-like nanofiber sponges and the octopus sucker-like nanofiber membranes to obtain a double bionic dressing.

3. The method for preparing the dual bionic dressing according to claim 2, characterized in that: The steps include: (1) Preparation of octopus suction cup-like nanofiber membrane Dispersing or dissolving a soluble hydrophobic polymer material and a drug in a solvent to obtain an electrospinning solution; using a spinning collection device with an array hole structure and an electrospinning device to perform electrospinning to prepare an octopus sucker-like nanofiber membrane; (2) Preparation of tree trunk-like nanofiber sponge (2.1) Using a soluble hydrophilic polymer material as a raw material, adding a solvent to obtain an electrospinning solution, then using an electrospinning device to electrospin to obtain a nanofiber membrane, and finally placing the nanofiber membrane in glutaraldehyde vapor for cross-linking to obtain a water-insoluble nanofiber membrane; (2.2) homogenizing the nanofiber membrane to obtain a short fiber suspension, adding a stabilizer to the short fiber suspension, freezing it with a cold source, and then freeze-drying it to obtain an initial nanofiber sponge; (2.3) heating the initial nanofiber sponge for cross-linking, and then placing the initial nanofiber sponge in glutaraldehyde vapor for cross-linking to obtain a tree trunk-mimicking nanofiber sponge; (3) Assembly of dual bionic dressing A soluble hydrophobic polymer material is dissolved in a solvent to obtain an electrospinning solution; then the octopus suction cup nanofiber membrane is cut into the same size as the bottom surface of the tree trunk nanofiber sponge, and the cut octopus suction cup nanofiber membrane is placed under the tree trunk nanofiber sponge and temporarily fixed with tweezers; during the electrospinning process of the spinning solution, the temporarily fixed octopus suction cup nanofiber membrane and the tree trunk nanofiber sponge are placed between the needle tip and the collecting device, and rotated so that the fibers are evenly wrapped around the surface, and the two are tightly combined to obtain a double bionic dressing.

4. The method for preparing the dual bionic dressing according to claim 3, characterized in that: In step (1) and step (3), the soluble hydrophobic polymer material is selected from any one or a combination of poly-ε-caprolactone, polyurethane, polylactic acid, poly(lactide-glycol), polysulfone, polymethyl methacrylate, polyvinyl butyral, and polyvinylidene fluoride; in step (2.1), the soluble hydrophilic polymer material is selected from any one or a combination of chitosan, gelatin, collagen, polyacrylonitrile, cellulose acetate, and polyvinyl alcohol.

5. The method for preparing the dual bionic dressing according to claim 3, characterized in that: In step (1) and step (3), the solvent is selected from any one or a combination of tetrahydrofuran, N,N-dimethylformamide, dichloromethane, chloroform, hexafluoroisopropanol, and ethanol.

6. The method for preparing the dual bionic dressing according to claim 3, characterized in that: In step (1), the spinning collecting device with an array hole structure is any one or a combination of a spinning collecting device with a circular hole array structure, a spinning collecting device with a triangular hole array structure, a spinning collecting device with a polygonal hole array structure, a spinning collecting device with an irregular hole array structure, and a screen.

7. The method for preparing the dual bionic dressing according to claim 3, characterized in that: In step (2.1), the solvent is selected from any one or a combination of hexafluoroisopropanol, glacial acetic acid, tetrahydrofuran, N,N-dimethylformamide, N,N-diethylacetamide, and water.

8. The method for preparing the dual bionic dressing according to claim 3, characterized in that: In step (2.2), the stabilizer is selected from polyvinyl alcohol or graphene oxide.

9. The method for preparing the dual bionic dressing according to claim 3, characterized in that: In step (1), the mass concentration of the soluble polymer material in the electrospinning solution is 0.1-5.0 g / ml; the electrospinning parameters are voltage of 5 kv-20 kv, flow rate of 0.1-2.0 ml / h, and spinning distance of 5-20 cm; in step (2.1), the mass concentration of the electrospinning solution is 0.02-5 g / ml; in step (2.2), the mass ratio of the stabilizer to the short fibers of the nanofiber membrane in the suspension is (0.15-0.2):1; in step (2.2), the solvent in the homogenization process is water.

10. The method for preparing the dual bionic dressing according to claim 3, characterized in that: In step (2.2), the degree of freezing is frozen into a solid state; in step (2.3), the heating temperature during the heating cross-linking process is 60-200°C, and the cross-linking time is 1-12 hours; in steps (2.1) and (2.3), the mass percentage of glutaraldehyde vapor is 1%-50%, and the cross-linking time is 12-36 hours; in steps (2.1) and (3), the parameters of the electrospinning equipment are: an aluminum foil wrapped drum is used as a collecting device, a spinning voltage is 5kv-20kv, a flow rate is 0.1-2.0ml / h, and a spinning distance is 5-20cm.

Citation Information

Cited By

  • Skin wound bionic dressing and preparation method thereof

    CN121130136A