Reverse osmosis membrane as well as preparation method and application thereof
By forming a separation layer of three-dimensional network structure and nanotube-like structure on the reverse osmosis membrane, the problems of reverse osmosis membrane pollution and water flux reduction are solved, and efficient water treatment and anti-pollution performance are achieved.
Patent Information
- Application Number
- CN202411087547.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
The reverse osmosis membrane is susceptible to contamination during use, resulting in a decrease in water flux and a shortened service life. The existing anti-pollution layer has insufficient adhesion and denseness, resulting in a decrease in water flux, making it difficult to maintain high flux and high pollution resistance.
The aqueous and oil-phase solution is prepared by metal ionic compounds, cyclodextrins, polyamines and triamlic acid. The separation layer is formed by heat treatment to form a hydrogel and nanotube-shaped structure with a three-dimensional network structure, and the separation layer is improved. Specific surface area and anti-pollution properties.
The reverse osmosis membrane has high pollution resistance while maintaining high water flux and high interception performance, extends the service life of the membrane and improves pollution resistance.
Smart Images

Figure CN118976371A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water treatment, in particular to a reverse osmosis membrane and a preparation method and application thereof. Background Art
[0002] Typically, reverse osmosis membranes are susceptible to contamination during use, resulting in decreased water flux and shortened service life, hindering their application. To improve the anti-fouling properties of reverse osmosis membranes, existing technologies often coat the surface of the membrane with a hydrophilic anti-fouling layer. However, this anti-fouling layer, formed in this manner, has weak adhesion to the membrane surface, making it susceptible to detachment during use. Furthermore, its high density reduces the water flux of the membrane, making it impossible for the membrane to maintain both high flux and high anti-fouling properties. Summary of the Invention
[0003] Based on this, it is necessary to provide a reverse osmosis membrane and its preparation method and application to address the above problems. The reverse osmosis membrane obtained by this preparation method can maintain high water flux and high retention performance while also having high anti-pollution performance when used in water treatment.
[0004] A method for preparing a reverse osmosis membrane comprises the following steps:
[0005] A metal ion compound, cyclodextrin, polyamine and water are prepared into an aqueous solution, wherein the cyclodextrin is selected from β-cyclodextrin and / or γ-cyclodextrin;
[0006] Trimesic acid, a polyphenyl compound, a polyacyl chloride and an isoparaffin solvent are prepared into an oil phase solution, wherein the polyphenyl compound is selected from 1,6-diphenyl-1,3,5-hexatriene and / or 1,4-bis(5-phenyl-2-oxazolyl);
[0007] The aqueous phase solution and the oil phase solution are sequentially placed on the same surface of a support membrane, and are subjected to heat treatment to form a separation layer, thereby obtaining a reverse osmosis membrane.
[0008] In one embodiment, the mass fraction of the metal ion compound in the aqueous solution is 0.1%-0.5%;
[0009] And / or, the metal ion compound is selected from at least one of copper chloride, zinc chloride or ferric chloride.
[0010] In one embodiment, the mass fraction of the cyclodextrin in the aqueous solution is 0.1%-1%.
[0011] In one embodiment, the mass fraction of the trimesic acid in the oil phase solution is 0.05%-0.3%.
[0012] In one embodiment, the mass fraction of the polyphenyl compound in the oil phase solution is 0.02%-0.2%.
[0013] In one embodiment, an acid scavenger is further added to the aqueous solution, and the mass fraction of the acid scavenger in the aqueous solution is 0.5%-3%.
[0014] In one embodiment, the mass fraction of the polyamine in the aqueous solution is 1%-2%;
[0015] And / or, the mass fraction of the polyacyl chloride in the oil phase solution is 0.1%-0.3%.
[0016] In one embodiment, the heat treatment temperature is 80° C.-100° C., and the heat treatment time is 2 min-5 min.
[0017] A reverse osmosis membrane is prepared by the reverse osmosis membrane preparation method as described above.
[0018] An application of the reverse osmosis membrane as described above in a water treatment device.
[0019] In the preparation method of the reverse osmosis membrane of the present invention, when polyamine in an aqueous solution and polyacyl chloride in an oil solution undergo interfacial polymerization to form a polyamide layer, trimesic acid in the oil solution and metal ion compounds in the aqueous solution are complexed at the water-oil interface to form a hydrogel with a three-dimensional network structure. On the one hand, the hydrogel has obvious positive charge due to the action of metal ions. The metal ions in the hydrogel produce electrostatic repulsion with the polyamine, reducing the diffusion rate of the polyamine into the oil-phase solution, which is conducive to forming a relatively dense and relatively flat separation layer, so that the reverse osmosis membrane has high retention performance and high anti-pollution performance. On the other hand, the hydrogel and the formed polyamide layer interpenetrate with each other to jointly constitute the separation layer, which can effectively increase the specific surface area of the separation layer and improve the water flux of the reverse osmosis membrane. At the same time, the polyphenyl compound in the oil phase solution and the cyclodextrin in the aqueous solution form a nanotubular structure at the water-oil interface through self-assembly. The nanotubular structure is distributed in the separation layer, which is conducive to improving the water flux of the reverse osmosis membrane.
[0020] Therefore, the reverse osmosis membrane prepared by the present invention has a relatively flat surface structure, and nanotubular structures are distributed in its separation layer, so that when the reverse osmosis membrane prepared by the present invention is used for water treatment, it can maintain high water flux and high retention performance while also having high anti-pollution performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 This is an electron microscope image of the reverse osmosis membrane prepared in Example 1 of the present invention;
[0023] Figure 2 This is an electron microscope image of the reverse osmosis membrane prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0024] To facilitate understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the technical field of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments or embodiments and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, including any two related listed items, any more related listed items, or the combination of all related listed items.
[0026] The method for preparing a reverse osmosis membrane provided by the present invention comprises the following steps:
[0027] A metal ion compound, cyclodextrin, polyamine and water are prepared into an aqueous solution, wherein the cyclodextrin is selected from β-cyclodextrin and / or γ-cyclodextrin;
[0028] Trimesic acid, a polyphenyl compound, a polyacyl chloride and an isoparaffin solvent are prepared into an oil phase solution, wherein the polyphenyl compound is selected from 1,6-diphenyl-1,3,5-hexatriene and / or 1,4-bis(5-phenyl-2-oxazolyl);
[0029] The aqueous phase solution and the oil phase solution are sequentially placed on the same surface of a support membrane, and are subjected to heat treatment to form a separation layer, thereby obtaining a reverse osmosis membrane.
[0030] In the present invention, when the aqueous solution and the oil solution are sequentially placed on the same surface of a support membrane, the polyamine in the aqueous solution and the polyacyl chloride in the oil solution undergo interfacial polymerization to form a polyamide layer. During this process, trimesic acid in the oil solution and the metal ion compound in the aqueous solution are complexed at the water-oil interface to form a hydrogel having a three-dimensional network structure. On the one hand, the hydrogel has obvious positive charge due to the action of the metal ions, and the polyamine in the aqueous solution also has a slight positive charge. Therefore, when the polyamine passes through the hydrogel, the metal ions in the hydrogel produce an electrostatic repulsion effect with the polyamine, reducing the diffusion rate of the polyamine into the oil solution, which is conducive to forming a denser and smoother separation layer, so that the reverse osmosis membrane has high retention performance and high anti-pollution performance. On the other hand, the hydrogel and the formed polyamide layer interpenetrate with each other to form a separation layer, which can effectively increase the specific surface area of the separation layer and improve the water flux of the reverse osmosis membrane.
[0031] At the same time, the polyphenyl compounds in the oil phase solution (such as 1,6-diphenyl-1,3,5-hexatriene and / or 1,4-bis(5-phenyl-2-oxazolyl)) and the cyclodextrin in the aqueous phase solution self-assemble to form a nanotubular structure at the water-oil interface, and the nanotubular structure is distributed in the hydrogel and then distributed in the separation layer, which is beneficial to improving the water flux of the reverse osmosis membrane.
[0032] Therefore, the reverse osmosis membrane prepared by the present invention has a relatively flat surface structure, and nanotubular structures are distributed in its separation layer, so that when the reverse osmosis membrane prepared by the present invention is used for water treatment, it can maintain high water flux and high retention performance while also having high anti-pollution performance.
[0033] Furthermore, it should be noted that, compared to the peak-and-valley structure of conventional reverse osmosis surfaces, the surface of the reverse osmosis membrane of the present invention is relatively flat, resulting in a reduced surface roughness of the reverse osmosis membrane of the present invention. The smoother the reverse osmosis membrane surface, the fewer binding sites it provides for pollutant deposition, thus increasing the reverse osmosis membrane's anti-fouling ability. Therefore, the reverse osmosis membrane of the present invention exhibits excellent anti-fouling properties.
[0034] Moreover, in the present invention, during interfacial polymerization, since the hydrogel with a three-dimensional network structure and the nanotubular structure are formed at the water-oil interface, both are distributed at the water-oil interface, which is conducive to forming a separation layer with excellent performance and uniformity, and is further conducive to improving the retention performance and water flux of the reverse osmosis membrane, and can ensure the long-term effectiveness of the anti-pollution performance.
[0035] Optionally, the mass fraction of the metal ion compound in the aqueous phase solution is 0.1%-0.5%; such a setting can provide abundant metal ions, which, on the one hand, can be complexed with trimesic acid in the oil phase solution to form a hydrogel with a three-dimensional network structure; on the other hand, the hydrogel with a three-dimensional network structure has obvious positive charge, which can produce electrostatic repulsion with the polyamine, better control the diffusion rate of the polyamine into the oil phase solution, and is conducive to forming a relatively dense separation layer while improving the smoothness of the separation layer surface, thereby making the reverse osmosis membrane have excellent retention performance and anti-fouling performance.
[0036] Furthermore, the metal ion compound is selected from at least one of copper chloride, zinc chloride or ferric chloride.
[0037] Optionally, the mass fraction of the cyclodextrin in the aqueous solution is 0.1%-1%. This configuration allows for better control of the self-assembly of the cyclodextrin with 1,6-diphenyl-1,3,5-hexatriene and / or 1,4-bis(5-phenyl-2-oxazolyl) in the oil phase solution by regulating the amount of cyclodextrin, thereby facilitating the formation of nanotubular structures and further improving the water flux of the reverse osmosis membrane.
[0038] Optionally, the mass fraction of trimesic acid in the oil phase solution is 0.05%-0.3%. This configuration can better form a hydrogel with a three-dimensional network structure, and the three-dimensional network structure of the hydrogel can be better interpenetrated with the polyamide layer to form a separation layer, which is beneficial to further increase the specific surface area of the separation layer and improve the water flux of the reverse osmosis membrane.
[0039] Optionally, the mass fraction of the polyphenyl compound in the oil phase solution is 0.02%-0.2%. This configuration is conducive to forming a better self-assembly with cyclodextrin to obtain a nanotubular structure, thereby facilitating the improvement of the water flux of the reverse osmosis membrane.
[0040] A polyamide layer is formed by interfacial polymerization of a polyamine and a polyacyl chloride. In the present invention, the mass fraction of the polyamine in the aqueous solution is 1%-2%, and the mass fraction of the polyacyl chloride in the oil solution is 0.1%-0.3%. This arrangement allows for more complete cross-linking of the polyamide layer, thereby improving the rejection performance and water flux of the reverse osmosis membrane.
[0041] In one embodiment, the polyamine is selected from at least one of polyethyleneimine, piperazine, m-phenylenediamine, p-phenylenediamine, and tetraethylenepentamine, preferably m-phenylenediamine.
[0042] In one embodiment, the polybasic acid chloride is selected from at least one of trimesoyl chloride, isophthaloyl chloride, and terephthaloyl chloride, preferably trimesoyl chloride.
[0043] In one embodiment, the isoparaffin solvent is selected from at least one of Isopar-E, Isopar-G, and Isopar-L.
[0044] In order to better remove the byproduct hydrochloric acid produced by the interfacial polymerization reaction and ensure the forward polymerization reaction of the polyamine and the polyacyl chloride, the present invention preferably further adds an acid scavenger to the aqueous solution, and the mass fraction of the acid scavenger in the aqueous solution is 0.5%-3%.
[0045] In one embodiment, the acid scavenger is selected from at least one of triethylamine, sodium hydroxide, potassium hydroxide, sodium carbonate, trisodium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, potassium phosphate, dipotassium hydrogen phosphate or potassium dihydrogen phosphate ammonium, preferably triethylamine.
[0046] In one embodiment, the material of the support membrane may include at least one of polysulfone, polypropylene or polyacrylonitrile, among which polysulfone is cheap and easy to obtain, simple to prepare membrane, has good mechanical strength, good pressure resistance, stable chemical properties, is non-toxic, and can resist biodegradation. Therefore, the material of the support membrane is preferably polysulfone.
[0047] In order to increase the strength of the reverse osmosis membrane, in one embodiment, a non-woven fabric layer is further provided. The non-woven fabric layer is stacked with the support membrane, and the aqueous solution and the oily solution are sequentially placed on the surface of the support membrane away from the non-woven fabric layer.
[0048] Optionally, the heat treatment temperature is 80-100° C., and the heat treatment time is 2-5 minutes. This configuration can further ensure the integrity and uniformity of the cross-linking of the polyamide layer, thereby ensuring the retention performance and water flux of the reverse osmosis membrane.
[0049] The present invention also provides a reverse osmosis membrane prepared using the above-described method for preparing a reverse osmosis membrane. The separation layer in the reverse osmosis membrane has a relatively flat surface, lacking peaks and valleys, and contains nanotube-like structures. Therefore, when used in water treatment, the reverse osmosis membrane of the present invention can maintain high water flux and high retention performance while also exhibiting high anti-fouling properties.
[0050] In addition, the present invention also provides a use of the reverse osmosis membrane as described above in a water treatment device.
[0051] In one embodiment, the water treatment device can be a purifier. When the reverse osmosis membrane is used in the water purifier, during the water purification process, the raw water to be purified enters from the separation layer of the reverse osmosis membrane, and the raw water passes through the reverse osmosis membrane under pressure to form pure water.
[0052] In one embodiment, the water treatment device may also be a seawater desalination device.
[0053] The reverse osmosis membrane, its preparation method, and its application will be further described below by the following specific examples. However, those skilled in the art will understand that the following examples are intended only to illustrate the present invention and should not be construed as limiting the scope of the present invention. Where specific conditions are not specified in the examples, the procedures were carried out under conventional conditions or conditions recommended by the manufacturer. Reagents or instruments used, for which the manufacturer is not specified, are all commercially available conventional products.
[0054] Example 1
[0055] Mix m-phenylenediamine, β-cyclodextrin, ferric chloride, triethylamine and water uniformly to obtain an aqueous phase solution, wherein the mass fraction of m-phenylenediamine, the mass fraction of β-cyclodextrin, the mass fraction of ferric chloride and the mass fraction of triethylamine are 1.0%, 0.1% and 0.5% respectively. Mix trimesoyl chloride, trimesic acid, 1,6-diphenyl-1,3,5-hexatriene and Isopar-L uniformly to obtain an oil phase solution, wherein the mass fraction of trimesoyl chloride, the mass fraction of trimesic acid and the mass fraction of 1,6-diphenyl-1,3,5-hexatriene are 0.1%, 0.05% and 0.02% respectively.
[0056] The aqueous solution was applied to the surface of the polysulfone membrane, allowed to stand for 60 seconds, excess aqueous solution was poured out, and the polysulfone membrane surface was blown dry with cold air; then the oily solution was applied to the surface of the polysulfone membrane with the aqueous solution, allowed to stand for 30 seconds, excess oily solution was poured out, and the polysulfone membrane with the oily solution and aqueous solution was placed in an 80°C forced air drying oven for heat treatment for 5 minutes to obtain the following: Figure 1 The reverse osmosis membrane shown.
[0057] Example 2
[0058] Metaphenylenediamine, β-cyclodextrin, ferric chloride, triethylamine and water are uniformly mixed to obtain an aqueous phase solution, wherein the mass fraction of metaphenylenediamine, the mass fraction of β-cyclodextrin, the mass fraction of ferric chloride and the mass fraction of triethylamine are 1.5%; trimesoyl chloride, trimesic acid, 1,6-diphenyl-1,3,5-hexatriene and Isopar-L are uniformly mixed to obtain an oil phase solution, wherein the mass fraction of trimesoyl chloride, the mass fraction of trimesic acid and the mass fraction of 1,6-diphenyl-1,3,5-hexatriene are 0.15%, 0.1% and 0.1% respectively.
[0059] The aqueous solution was applied to the surface of the polysulfone membrane, allowed to stand for 60 seconds, excess aqueous solution was poured out, and the polysulfone membrane surface was blown dry with cold air; then the oily solution was applied to the surface of the polysulfone membrane with the aqueous solution, allowed to stand for 30 seconds, excess oily solution was poured out, and the polysulfone membrane with the oily solution and aqueous solution was placed in a 90° C. forced air drying oven for heat treatment for 3 minutes to obtain a reverse osmosis membrane.
[0060] Example 3
[0061] Metaphenylenediamine, β-cyclodextrin, ferric chloride, triethylamine and water are uniformly mixed to obtain an aqueous phase solution, wherein the mass fraction of metaphenylenediamine, the mass fraction of β-cyclodextrin, the mass fraction of ferric chloride and the mass fraction of triethylamine are 2%, 1%, 0.5% and 3% respectively; trimesoyl chloride, trimesic acid, 1,6-diphenyl-1,3,5-hexatriene and Isopar-L are uniformly mixed to obtain an oil phase solution, wherein the mass fraction of trimesoyl chloride, the mass fraction of trimesic acid and the mass fraction of 1,6-diphenyl-1,3,5-hexatriene are 0.3%, 0.3% and 0.2% respectively in the oil phase solution.
[0062] The aqueous solution was applied to the surface of the polysulfone membrane, allowed to stand for 60 seconds, excess aqueous solution was poured out, and the polysulfone membrane surface was blown dry with cold air; then the oily solution was applied to the surface of the polysulfone membrane with the aqueous solution, allowed to stand for 30 seconds, excess oily solution was poured out, and the polysulfone membrane with the oily and aqueous solutions was placed in a 100° C. forced air drying oven for heat treatment for 2 minutes to obtain a reverse osmosis membrane.
[0063] Example 4
[0064] Compared with Example 1, Example 4 differs only in that, in the step of preparing the aqueous phase solution, γ-cyclodextrin is used instead of β-cyclodextrin, and in the step of preparing the oil phase solution, 1,4-bis(5-phenyl-2-oxazolyl) is used instead of 1,6-diphenyl-1,3,5-hexatriene. The other conditions are the same to obtain a reverse osmosis membrane.
[0065] Example 5
[0066] The only difference between Example 5 and Example 1 is that triethylamine is not added in the step of preparing the aqueous phase solution. Other conditions are the same to obtain a reverse osmosis membrane.
[0067] Example 6
[0068] The only difference between Example 6 and Example 1 is that, in the step of preparing the aqueous phase solution, copper chloride is used instead of ferric chloride. Other conditions are the same to obtain a reverse osmosis membrane.
[0069] Example 7
[0070] The only difference between Example 7 and Example 1 is that the mass fraction of ferric chloride in the aqueous solution is 0.8%. Other conditions are the same, and a reverse osmosis membrane is obtained.
[0071] Example 8
[0072] Compared with Example 1, Example 8 differs only in that the mass fraction of ferric chloride in the aqueous solution is 0.05%, and the other conditions are the same to obtain a reverse osmosis membrane.
[0073] Example 9
[0074] Compared with Example 1, Example 9 differs only in that the mass fraction of β-cyclodextrin in the aqueous solution is 1.5%, and the other conditions are the same to obtain a reverse osmosis membrane.
[0075] Example 10
[0076] Compared with Example 1, Example 10 differs only in that the mass fraction of β-cyclodextrin in the aqueous solution is 0.05%, and other conditions are the same to obtain a reverse osmosis membrane.
[0077] Example 11
[0078] Compared with Example 1, Example 11 differs only in that the mass fraction of trimesic acid in the oil phase solution is 0.4%. Other conditions are the same, and a reverse osmosis membrane is obtained.
[0079] Example 12
[0080] Compared with Example 1, Example 12 differs only in that the mass fraction of trimesic acid in the oil phase solution is 0.01%, and other conditions are the same to obtain a reverse osmosis membrane.
[0081] Example 13
[0082] Compared with Example 1, Example 13 differs only in that the mass fraction of 1,6-diphenyl-1,3,5-hexatriene in the oil phase solution is 0.3%. Other conditions are the same, and a reverse osmosis membrane is obtained.
[0083] Example 14
[0084] Compared with Example 1, Example 14 differs only in that the mass fraction of 1,6-diphenyl-1,3,5-hexatriene in the oil phase solution is 0.01%, and other conditions are the same to obtain a reverse osmosis membrane.
[0085] Comparative Example 1
[0086] Comparative Example 1 differs from Example 1 only in that β-cyclodextrin is not added in the step of preparing the aqueous phase solution, and the other conditions are the same to obtain a reverse osmosis membrane.
[0087] Comparative Example 2
[0088] Comparative Example 2 is different from Example 1 only in that ferric chloride is not added in the step of preparing the aqueous phase solution, and the other conditions are the same, and the following is obtained: Figure 2 The reverse osmosis membrane shown.
[0089] Comparative Example 3
[0090] Comparative Example 3 is different from Example 1 only in that trimesic acid is not added in the step of preparing the oil phase solution. Other conditions are the same to obtain a reverse osmosis membrane.
[0091] Comparative Example 4
[0092] Comparative Example 4 is different from Example 1 only in that 1,6-diphenyl-1,3,5-hexatriene is not added in the step of preparing the oil phase solution. Other conditions are the same to obtain a reverse osmosis membrane.
[0093] Comparative Example 5
[0094] Comparative Example 5 is different from Example 1 only in that α-cyclodextrin is used instead of β-cyclodextrin in the step of preparing the aqueous phase solution, and the other conditions are the same to obtain a reverse osmosis membrane.
[0095] The rejection rate and water flux of the reverse osmosis membranes prepared in Examples 1-14 and Comparative Examples 1-5 were tested. The test conditions were: a test pressure of 1.55 MPa, a concentrate flow rate of 1.0 GPM, an ambient temperature of 25°C, a concentrate pH value of 6.5-7.5, and a 2000 ppm sodium chloride aqueous solution. The test results are shown in Table 1.
[0096] Table 1
[0097] Membrane water flux / LMH Retention rate / % Example 1 85 99.75 Example 2 88 99.76 Example 3 82 99.75 Example 4 83 99.73 Example 5 73 99.58 Example 6 82 99.73 Example 7 61 99.54 Example 8 63 99.57 Example 9 59 99.51 Example 10 56 99.54 Example 11 60 99.61 Example 12 58 99.58 Example 13 55 99.51 Example 14 56 99.61 Comparative Example 1 42 99.32 Comparative Example 2 48 99.48 Comparative Example 3 41 99.36 Comparative Example 4 42 99.41 Comparative Example 5 42 99.25
[0098] The anti-pollution performance of the reverse osmosis membranes prepared in Examples 1-14 and Comparative Examples 1-5 was tested. The test conditions were as follows: the test pressure was 1.55 MPa, the brine flow rate was 1.0 GPM, the ambient temperature was 25 ° C, the brine pH value was 6.5-7.5, and the brine was 2000 ppm sodium chloride + 100 ppm sodium humate + 100 ppm bovine serum albumin as the inlet water condition. The anti-pollution performance test was carried out. After 100 hours of continuous operation, the membrane was cleaned and then the performance test was carried out under the inlet water condition of 2000 ppm sodium chloride. The test results are shown in Table 2.
[0099] Table 2
[0100]
[0101]
[0102] It should be noted that in Table 1-2, the membrane water flux (F) is calculated by the volume of water passing through the reverse osmosis membrane in a certain period of time, and the formula is: F = V / (A×T), where V is the volume of water passing through the reverse osmosis membrane per unit time, A is the effective membrane area, and T is time.
[0103] The rejection rate (R) is calculated by the concentration of the influent and the concentration of the permeate. The calculation formula is: R = (1-C1 / C0) × 100%, where C1 is the concentration of the concentrated water and C0 is the concentration of the permeate.
[0104] The calculation formula of the water flux recovery rate is: (water flux of the reverse osmosis membrane after pollution / water flux of the initial reverse osmosis membrane)×100%.
[0105] from Figure 1-2 It can be seen that the surface of the reverse osmosis membrane prepared in Example 1 of the present invention is relatively flat and contains nanostructures. However, since the aqueous phase solution of Comparative Example 2 does not contain ferric chloride, it is impossible to form a hydrogel with a three-dimensional network structure, and it is even impossible to generate static electricity with the polyamine, thereby failing to reduce the diffusion rate of the polyamine into the oil phase solution. As a result, the surface of the formed reverse osmosis membrane has an obvious concave-convex structure, that is, poor flatness, resulting in poor anti-pollution performance.
[0106] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0107] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.
Claims
1. A method for preparing a reverse osmosis membrane, characterized in that: The following steps are involved: A metal ion compound, cyclodextrin, polyamine and water are prepared into an aqueous solution, wherein the cyclodextrin is selected from β-cyclodextrin and / or γ-cyclodextrin; The oil phase solution is prepared by preparing trimesic acid, a polyphenyl compound, a polyacyl chloride and an isoparaffin solvent, wherein the polyphenyl compound is selected from 1,6-diphenyl-1,3,5-hexatriene and / or 1,4-bis(5-phenyl-2-oxazolyl); The aqueous phase solution and the oil phase solution are sequentially placed on the same surface of a supporting membrane, and a separation layer is formed through heat treatment to obtain a reverse osmosis membrane.
2. The method for preparing a reverse osmosis membrane according to claim 1, characterized in that: The mass fraction of the metal ion compound in the aqueous solution is 0.1%-0.5%; And / or, the metal ion compound is selected from at least one of copper chloride, zinc chloride or ferric chloride.
3. The method for preparing a reverse osmosis membrane according to claim 1, characterized in that: The mass fraction of the cyclodextrin in the aqueous solution is 0.1%-1%.
4. The method for preparing a reverse osmosis membrane according to claim 1, characterized in that: The mass fraction of the trimesic acid in the oil phase solution is 0.05%-0.3%.
5. The method for preparing a reverse osmosis membrane according to claim 1, characterized in that: The mass fraction of the polyphenyl compound in the oil phase solution is 0.02%-0.2%.
6. The method for preparing a reverse osmosis membrane according to any one of claims 1 to 5, characterized in that: An acid absorber is also added to the aqueous phase solution, and the mass fraction of the acid absorber in the aqueous phase solution is 0.5%-3%.
7. The method for preparing a reverse osmosis membrane according to any one of claims 1 to 5, characterized in that: The mass fraction of the polyamine in the aqueous solution is 1%-2%; And / or, the mass fraction of the polyacid chloride in the oil phase solution is 0.1%-0.3%.
8. The method for preparing a reverse osmosis membrane according to any one of claims 1 to 5, characterized in that: The temperature of the heat treatment is 80°C-100°C, and the time of the heat treatment is 2min-5min.
9. A reverse osmosis membrane prepared by the method for preparing a reverse osmosis membrane according to any one of claims 1 to 8.
10. Use of the reverse osmosis membrane according to claim 9 in a water treatment device.
Citation Information
Cited By
Reverse osmosis composite membrane as well as preparation method and application thereof
CN120189828A
Reverse osmosis membrane as well as preparation method and application thereof
CN120204943A
Reverse osmosis membrane as well as preparation method and application thereof
CN121103169A