MXene bipolar membrane, preparation method thereof and electrodialysis device

By using MXene material as the intermediate interface layer and the membrane layer forming a semi-interpenetrating network structure in the bipolar membrane, the problems of low hydrolysis efficiency and poor structural stability of traditional bipolar membranes are solved, and efficient electrodialysis performance is achieved.

CN118976382AActive Publication Date: 2024-11-19JIANGSU HELPER FUNCTIONAL MATERIALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411195694.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-19
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Traditional bipolar membranes have problems such as low hydrolysis efficiency, low electrochemical performance and poor structural stability, which limits its development.

Method used

Using MXene material as the intermediate interface layer, by spraying the suspension containing MXene material onto the cation exchange layer and forming an anion exchange layer thereon, polyvinylidene fluoride and corresponding monomers are used for blending and crosslinking with crosslinking agent. Reactions to form a film layer with a semi-interpenetrating network structure, enhancing the interaction and stability of the film layer.

Benefits of technology

It improves the hydrolysis efficiency, electrochemical performance and structural stability of the bipolar membrane, achieves efficient electrodialysis performance, and has a wide range of application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976382A_ABST
    Figure CN118976382A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrodialysis, in particular to an MXene bipolar membrane, a preparation method thereof and an electrodialysis device. The preparation method of the MXene bipolar membrane comprises the following steps: carrying out first membrane forming treatment on a first membrane casting solution containing polyvinylidene fluoride, a cationic monomer and a first cross-linking agent to form a cation exchange layer; spraying a suspension containing an MXene material on the cation exchange layer to form a middle interface layer; and carrying out second membrane forming treatment on a second membrane casting solution containing polyvinylidene fluoride, an anionic monomer and a second cross-linking agent, and forming an anion exchange layer on the middle interface layer. The MXene bipolar membrane prepared by the invention has the advantages of high water dissociation efficiency, excellent electrochemical performance and good structural stability, and has a wide application prospect in the field of electrodialysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrodialysis technology, and in particular to a MXene bipolar membrane, a preparation method thereof, and an electrodialysis device. Background Art

[0002] Bipolar membrane is a new type of ion exchange membrane, which is a layered polymer membrane composed of a cation exchange layer, an intermediate interface layer and an anion exchange layer stacked in sequence. Under the action of an external electric field, water molecules dissociate into H + and OH - , and migrate to the solutions on both sides of the bipolar membrane through the charged groups on the cation exchange layer and the anion exchange layer, thereby producing acid and alkali.

[0003] An efficient bipolar membrane should have the characteristics of high selectivity, high water dissociation efficiency, good structural stability and low energy consumption. However, most traditional bipolar membranes have problems such as low water dissociation efficiency, low electrochemical performance and poor structural stability, which restricts the development of bipolar membranes. Summary of the invention

[0004] Based on this, there is a need for a MXene bipolar membrane and its preparation method and electrodialysis device to solve the problems of low water dissociation efficiency, low electrochemical performance and poor structural stability existing in traditional bipolar membranes.

[0005] The above-mentioned purpose of the present application is achieved through the following technical solutions:

[0006] In a first aspect of the present application, a method for preparing a MXene bipolar membrane is provided, comprising the following steps:

[0007] Subjecting a first casting solution containing polyvinylidene fluoride, a cationic monomer and a first cross-linking agent to a first film-forming treatment to form a cation exchange layer;

[0008] Spraying a suspension containing MXene material onto the cation exchange layer to form an intermediate interface layer;

[0009] The second casting solution containing polyvinylidene fluoride, anionic monomer and a second crosslinking agent is subjected to a second film-forming treatment to form an anion exchange layer on the intermediate interface layer.

[0010] In one embodiment, the cationic monomer includes one or more of sodium styrene sulfonate and sodium allyl sulfonate.

[0011] In one embodiment, the anionic monomer includes one or more of vinyl imidazole and vinyl pyridine.

[0012] In one of the embodiments, in the first casting solution, the mass ratio of the polyvinylidene fluoride to the cationic monomer is 1:(0.5~1.5).

[0013] In one of the embodiments, in the second casting solution, the mass ratio of the polyvinylidene fluoride to the anion monomer is 1:(0.5-1.5).

[0014] In one embodiment, the first cross-linking agent includes divinylbenzene.

[0015] In one embodiment, the second cross-linking agent includes 1,6-dibromohexane.

[0016] In one embodiment, the mass ratio of the cationic monomer to the first cross-linking agent is 100:(3-15).

[0017] In one embodiment, the mass ratio of the anionic monomer to the second cross-linking agent is 100:(3-15).

[0018] In one embodiment, the first casting solution further contains a first initiator, and the second casting solution further contains a second initiator.

[0019] In one embodiment, the first initiator and the second initiator independently include one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, azobiscyanovaleric acid, benzoyl peroxide and 2,2-azobis(2-methylpropylimidazole) dihydrochloride.

[0020] In one embodiment, the mass ratio of the cationic monomer to the first initiator is 100:(0.5~5).

[0021] In one embodiment, the mass ratio of the anionic monomer to the second initiator is 100:(0.5~5).

[0022] In one embodiment, the solid content of the first casting solution and the second casting solution is independently 10% to 30%.

[0023] In one embodiment, the method for preparing the MXene material comprises the following steps:

[0024] The MAX precursor is placed in an etching solution containing hydrogen ions and fluorine ions to perform an etching reaction, and is purified to prepare the MXene material.

[0025] In one embodiment, the MAX precursor includes one or more of Ti3AlC2, Ti2AlC, Ti3AlCN, Ta4AlC3, V2AlC, V3AlC2, Mo2AlC and Mo2TiAlC2.

[0026] In one embodiment, the etching solution contains one or more of HF, HCl and fluoride salt.

[0027] In one embodiment, the etching reaction comprises the following steps: etching at 20° C. to 50° C. for 12 h to 48 h.

[0028] In one of the embodiments, the mass fraction of the MXene material in the suspension is 0.1%~5%.

[0029] In one embodiment, the thickness of the cation exchange layer and the anion exchange layer are independently 100 μm to 300 μm.

[0030] In a second aspect of the present application, a MXene bipolar membrane is provided, which is prepared by the method for preparing a MXene bipolar membrane as described above.

[0031] In one embodiment, the transmembrane voltage of the MXene bipolar membrane is 0.9 V~3 V.

[0032] In one embodiment, the current efficiency of the MXene bipolar membrane is 80% to 95%.

[0033] In one embodiment, the energy consumption of the MXene bipolar membrane is 1.1 kWh / kg~5.3 kWh / kg.

[0034] In a third aspect of the present application, an electrodialysis device is provided, comprising the MXene bipolar membrane as described above.

[0035] This application has at least the following beneficial effects:

[0036] The present application uses polyvinylidene fluoride (PVDF), cationic monomers and a first crosslinking agent to perform a co-mixing crosslinking reaction to form a cationic exchange membrane with a semi-interpenetrating network structure, and uses PVDF, anionic monomers and a second crosslinking agent to perform a co-mixing crosslinking reaction to form an anionic exchange membrane with a semi-interpenetrating network structure, which can not only allow the bipolar membrane to maintain a high ion exchange capacity, but also limit the water absorption rate of the bipolar membrane, avoid the bipolar membrane from swelling due to excessive water absorption, and give it good mechanical properties and structural strength. At the same time, the intermediate interface layer uses MXene material as a water dissociation catalyst; MXene material has high hydrophilicity and can effectively improve the water dissociation efficiency of the bipolar membrane; the surface of the MXene material contains rich active groups, which can form intermolecular hydrogen bonds with the functional groups on the surface of the ion exchange layer on both sides, enhance the interaction between the membrane layers, and improve the structural stability of the bipolar membrane. Therefore, the MXene bipolar membrane prepared in the present application has the advantages of high water dissociation efficiency, excellent electrochemical performance and good structural stability, and has broad application prospects in the field of electrodialysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0038] Figure 1 Schematic diagram of a process for preparing a MXene bipolar membrane in one embodiment;

[0039] Figure 2 This is a Raman characterization image of the MXene material prepared in Example 1;

[0040] Figure 3 XRD spectrum of the MXene material prepared in Example 1;

[0041] Figure 4 CV curves of the MXene bipolar membranes of Examples 1 to 3 and the bipolar membranes of Comparative Examples 1 to 2;

[0042] Figure 5 It is a comparison chart of current efficiency and energy consumption of the MXene bipolar membranes of Examples 1 to 3 and the bipolar membranes of Comparative Examples 1 to 2. DETAILED DESCRIPTION

[0043] In order to facilitate the understanding of the present application, the present application is further described in detail below in conjunction with specific embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0045] In the present application, the meaning of "and / or" includes any and all combinations of one or more related listed items. "At least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layer" means at least two layers, such as two layers, three layers, etc., unless otherwise clearly and specifically defined. In the description of the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0046] When a numerical range is disclosed in this application, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed in this application should be understood to include any and all subranges included therein.

[0047] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0048] In this application, "above" or "below" includes the number itself. For example, "1 below" includes 1.

[0049] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0050] In the present application, room temperature refers to indoor temperature, normal temperature or general temperature. Generally speaking, the range of room temperature can be any one of the following temperature intervals: 23°C ± 2°C, 25°C ± 5°C or 20°C ± 5°C.

[0051] For bipolar membranes, the water dissociation process occurs in the middle interface layer, so the performance of the middle interface layer largely determines the performance of the bipolar membrane. By selecting a suitable water dissociation catalyst as the middle interface layer and adopting a suitable preparation process and molding material, a bipolar membrane with excellent performance can be obtained. An efficient bipolar membrane should have the characteristics of high selectivity, high water dissociation efficiency, good structural stability and low energy consumption. However, most traditional bipolar membranes have the disadvantages of high production cost and low water dissociation efficiency, and the bonding between the middle interface layer and the cation exchange layer and anion exchange layer on both sides is not tight enough, resulting in reduced electrochemical performance of the bipolar membrane, poor structural stability, and shortened service life, which limits the development of bipolar membranes.

[0052] Based on this, in the first aspect of the present application, a method for preparing a MXene bipolar membrane is provided.

[0053] See also Figure 1 , which is a schematic diagram of a process for preparing a MXene bipolar membrane in one embodiment. Figure 1 As shown, the method for preparing the MXene bipolar membrane includes the following steps:

[0054] S100: performing a first film-forming treatment on a first casting solution containing polyvinylidene fluoride, a cationic monomer and a first cross-linking agent to form a cation exchange layer;

[0055] S200: spraying a suspension containing MXene material onto the cation exchange layer to form an intermediate interface layer;

[0056] S300: subjecting a second casting solution containing polyvinylidene fluoride, anionic monomers and a second cross-linking agent to a second film-forming treatment to form an anion exchange layer on the intermediate interface layer.

[0057] The present application uses polyvinylidene fluoride (PVDF), cationic monomers and a first crosslinking agent to perform a co-mixing crosslinking reaction to form a cationic exchange membrane with a semi-interpenetrating network structure, and uses PVDF, anionic monomers and a second crosslinking agent to perform a co-mixing crosslinking reaction to form an anionic exchange membrane with a semi-interpenetrating network structure, which can not only allow the bipolar membrane to maintain a high ion exchange capacity, but also limit the water absorption rate of the bipolar membrane, avoid the bipolar membrane from swelling due to excessive water absorption, and give it good mechanical properties and structural strength. At the same time, the intermediate interface layer uses MXene material as a water dissociation catalyst; MXene material has high hydrophilicity and can effectively improve the water dissociation efficiency of the bipolar membrane; the surface of the MXene material contains rich active groups, which can form intermolecular hydrogen bonds with the functional groups on the surface of the ion exchange layer on both sides, enhance the interaction between the membrane layers, and improve the structural stability of the bipolar membrane. Therefore, the MXene bipolar membrane prepared in the present application has the advantages of high water dissociation efficiency, excellent electrochemical performance and good structural stability, and has broad application prospects in the field of electrodialysis.

[0058] The following is a detailed description of the preparation method of MXene bipolar membrane in a step-by-step manner.

[0059] S100: subjecting a first casting solution containing polyvinylidene fluoride, a cationic monomer and a first cross-linking agent to a first film-forming treatment to form a cation exchange layer.

[0060] It can be understood that the ion exchange capacity of the cation exchange layer is related to the grafting rate of the cationic monomer. The higher the content of the cationic monomer in the first casting solution, the ion exchange capacity of the resulting cation exchange layer will be increased accordingly. The appropriate water content in the bipolar membrane can promote the migration of ions, but the excessive water absorption of the bipolar membrane will cause the bipolar membrane to swell, reducing its mechanical properties and structural strength. The present application utilizes PVDF, cationic monomers and a first cross-linking agent for co-modification, so that the cross-linked polymer and the non-cross-linked polymer are interlaced to form a semi-interpenetrating network structure, which can limit the water absorption of the bipolar membrane while maintaining the high ion exchange capacity of the bipolar membrane, thereby giving the bipolar membrane good mechanical properties. The role of the anion exchange layer is also the same, which will not be repeated.

[0061] Optionally, the cationic monomer includes one or more of sodium styrene sulfonate and sodium allyl sulfonate, and further may be one or more of sodium styrene sulfonate and sodium allyl sulfonate.

[0062] Optionally, in the first casting solution, the mass ratio of polyvinylidene fluoride to the cationic monomer is 1:(0.5-1.5). As an example, the mass ratio of PVDF to the cationic monomer can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5, and can further be 1:(0.8-1.2).

[0063] Optionally, the first cross-linking agent comprises divinylbenzene.

[0064] Optionally, the mass ratio of the cationic monomer to the first crosslinking agent is 100:(3-15). As an example, the mass ratio of the cationic monomer to the first crosslinking agent may be 100:3, 100:4, 100:5, 100:6, 100:7, 100:8, 100:9, 100:10, 100:11, 100:12, 100:13, 100:14 or 100:15, and may further be 100:(8-12).

[0065] Optionally, the first casting solution further contains a first initiator.

[0066] Optionally, the first cross-linking agent includes one or more of azobisisobutyronitrile (AIBN), azobisisovaleronitrile (AMBN), azobisisoheptylnitrile (ADVN), azobiscyanovaleric acid (ACVA), benzoyl peroxide (BPO) and 2,2-azobis(2-methylpropylimidazole) dihydrochloride (AAPH), and may further be azobisisobutyronitrile (AIBN).

[0067] Optionally, the mass ratio of the cationic monomer to the first initiator is 100:(0.5-5). As an example, the mass ratio of the cationic monomer to the first initiator can be 100:0.5, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, 100:3.5, 100:4, 100:4.5 or 100:0.5, and can further be 100:(1-3).

[0068] Optionally, the first casting solution further contains a first organic solvent.

[0069] Optionally, the first organic solvent includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP) and dimethyl sulfoxide (DMSO), and may further be DMF.

[0070] Optionally, the solid content of the first casting solution is 10% to 30%. It can be understood that the solid content in the first casting solution refers to the sum of the mass fractions of PVDF, cationic monomer, first crosslinking agent and first initiator in the first casting solution. As an example, the solid content of the first casting solution can be 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28% or 30%, and can further be 10% to 20%.

[0071] Optionally, the method for preparing the first casting solution comprises the following steps: dissolving PVDF, a cationic monomer, a first cross-linking agent and a first initiator in a first organic solvent, stirring the mixture evenly and then heating the mixture to react, thereby preparing the first casting solution.

[0072] Optionally, the temperature of the temperature-raising reaction is 40°C to 80°C, and the time is 6h to 24h. As an example, the temperature of the temperature-raising reaction can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, and the time can be 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24h.

[0073] Optionally, the first film forming process includes one or more of a film casting process, a film forming process by blade coating, a film forming process by spin coating and a film forming process by spray coating, and further optionally a film forming process by blade coating.

[0074] Optionally, after the first film-forming treatment, the step of drying the first liquid film obtained by the first film-forming treatment at 60°C to 120°C for 1h to 12h is further included. As an example, the drying temperature of the first liquid film may be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, and the drying time may be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h or 12h.

[0075] Optionally, the thickness of the cation exchange layer is 100 μm to 300 μm. As an example, the thickness of the cation exchange layer can be 100 μm, 120 μm, 140 μm, 160 μm, 180 μm, 200 μm, 220 μm, 240 μm, 260 μm, 280 μm or 300 μm.

[0076] S200: Spraying a suspension containing MXene material onto the cation exchange layer to form an intermediate interface layer.

[0077] Among two-dimensional (2D) nanomaterials, MXene materials are a new type of two-dimensional nano-layered materials with good flexibility, high specific surface area, high mechanical strength and excellent conductivity. Its hydrophilicity and adjustable interlayer space improve the water dissociation efficiency of the prepared bipolar membrane, effectively reducing the transmembrane voltage and the energy consumption of water dissociation. The surface of MXene materials contains a large number of active functional groups, such as -OH, -F or -O, which can produce intermolecular hydrogen bonds with the functional groups of the ion exchange layers on both sides, making the bipolar membrane have excellent structural stability.

[0078] Optionally, the molecular formula of the MXene material is M n+1 X n T x ;

[0079] Wherein, n=1, 2, 3; M represents a transition metal element, M includes one or more of Ti, Ta, Mo, V, Sr and Zr; X represents one or more of carbon and nitrogen; T represents a surface active functional group, T includes one or more of -OH, -F and -O, x represents the number of T, x>0.

[0080] Optionally, the MXene material includes Ti3C2T x 、Ti2CT x 、Ti3CNT x 、Ta4C3T x 、V2CT x 、V3C2T x 、Mo2CT x and Mo2TiC2T x One or more of .

[0081] Optionally, the MXene material includes one or more of a multilayer MXene material and a single-layer MXene material. The thickness of the multilayer MXene material is 5 μm to 50 μm, and the thickness of the single-layer MXene material is 0.5 nm to 5 nm.

[0082] Optionally, the preparation method of MXene material comprises the following steps: placing a MAX precursor in a liquid containing hydrogen ions (H + ) and fluoride ions (F - ) in an etching solution for etching reaction and purification treatment to prepare MXene materials.

[0083] Optionally, the MAX precursor includes one or more of Ti3AlC2, Ti2AlC, Ti3AlCN, Ta4AlC3, V2AlC, V3AlC2, Mo2AlC and Mo2TiAlC2.

[0084] Optionally, the etching solution contains one or more of HF, HCl and fluoride salts, wherein the fluoride salts include one or more of lithium fluoride (LiF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), and ammonium fluoride (NH4F).

[0085] Optionally, the etching solution is an HF solution, and the concentration of HF is 6 mol / L to 12 mol / L.

[0086] Optionally, the etching solution is a mixed solution containing HCl and a fluoride salt, and the molar ratio of HCl to the fluoride salt is 1:(0.1-0.5).

[0087] Optionally, the mass volume ratio of the MAX precursor to the etching solution is 1 g / 10 mL to 1 g / 20 mL.

[0088] Optionally, the etching reaction comprises the following steps: etching at 20° C. to 50° C. for 12 h to 48 h. As an example, the temperature of the etching reaction may be 20° C., 25° C., 30° C., 35° C., 40° C., 45° C. or 50° C., and the etching reaction time may be 12 h, 16 h, 20 h, 24 h, 28 h, 32 h, 36 h, 40 h, 44 h or 48 h.

[0089] Optionally, the purification treatment includes the following steps: repeatedly centrifuging and washing the reaction liquid after the etching reaction with HCl solution and deionized water until the pH value of the upper liquid after centrifugation is ≥6 to obtain a washed product; dispersing the washed product in deionized water and ultrasonicating it under an inert gas atmosphere to obtain a dispersion; and then high-speed centrifuging and freeze-drying the dispersion to obtain a MXene material.

[0090] Optionally, the method for preparing a suspension containing a MXene material comprises the following steps: dispersing the MXene material in a second organic solvent to obtain a suspension.

[0091] Optionally, the second organic solvent includes one or more of DMF, DMAc, NMP and DMSO, and may further be DMF.

[0092] Optionally, the mass fraction of the MXene material in the suspension is 0.1% to 5%. As an example, the mass fraction of the MXene material in the suspension can be 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, and further optionally 0.5% to 1.5%.

[0093] Optionally, after the step of spraying the suspension containing MXene material on the cation exchange layer, the step of drying the sprayed second liquid film at 50°C to 80°C for 0.5h to 2h is further included. As an example, the drying temperature of the second liquid film can be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, and the drying time can be 0.5h, 0.8h, 1h, 1.2h, 1.5h, 1.8h or 2h.

[0094] S300: subjecting a second casting solution containing polyvinylidene fluoride, anionic monomers and a second cross-linking agent to a second film-forming treatment to form an anion exchange layer on the intermediate interface layer.

[0095] Optionally, the anionic monomer includes one or more of vinyl imidazole and vinyl pyridine, and may further be vinyl imidazole.

[0096] Optionally, in the second casting solution, the mass ratio of polyvinylidene fluoride to the anionic monomer is 1:(0.5-1.5). As an example, the mass ratio of PVDF to the anionic monomer can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5, and can further be 1:(0.8-1.2).

[0097] Optionally, the second cross-linking agent includes one or more of 1,6-dibromohexane and 1-bromo-n-hexane, and may further be 1,6-dibromohexane.

[0098] Optionally, the mass ratio of the anionic monomer to the second crosslinking agent is 100:(3-15). As an example, the mass ratio of the anionic monomer to the second crosslinking agent can be 100:3, 100:4, 100:5, 100:6, 100:7, 100:8, 100:9, 100:10, 100:11, 100:12, 100:13, 100:14 or 100:15, and can further be 100:(8-12).

[0099] Optionally, the second casting solution further contains a second initiator.

[0100] Optionally, the second initiator includes one or more of azobisisobutyronitrile (AIBN), azobisisovaleronitrile (AMBN), azobisisoheptylnitrile (ADVN), azobiscyanovaleric acid (ACVA), benzoyl peroxide (BPO) and 2,2-azobis(2-methylpropylimidazole) dihydrochloride (AAPH), and may further be azobisisobutyronitrile (AIBN).

[0101] Optionally, the mass ratio of the anionic monomer to the second initiator is 100:(0.5-5). As an example, the mass ratio of the anionic monomer to the second initiator can be 100:0.5, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, 100:3.5, 100:4, 100:4.5 or 100:0.5, and can further be 100:(1-3).

[0102] Optionally, the second casting solution further contains a third organic solvent.

[0103] Optionally, the second organic solvent includes one or more of DMF, DMAc, NMP and DMSO, and may further be DMF.

[0104] Optionally, the solid content of the second casting solution is 10% to 30%. It can be understood that the solid content in the second casting solution refers to the sum of the mass fractions of PVDF, anionic monomer, second crosslinking agent and second initiator in the second casting solution. As an example, the solid content of the second casting solution can be 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28% or 30%, and can further be 10% to 20%.

[0105] Optionally, the method for preparing the second casting solution comprises the following steps: dissolving PVDF, anionic monomer, second crosslinking agent and second initiator in a third organic solvent, stirring evenly and then heating to react, so as to prepare the second casting solution.

[0106] Optionally, the temperature of the temperature-raising reaction is 40°C to 80°C, and the time is 6h to 24h. As an example, the temperature of the temperature-raising reaction can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, and the time can be 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24h.

[0107] Optionally, the second film forming process includes one or more of a film casting process, a film forming process by scraping, a film forming process by spin coating and a film forming process by spraying, and may further be a film forming process by scraping.

[0108] Optionally, after the second film-forming treatment, the following step is further included: drying the third liquid film obtained by the second film-forming treatment at 60° C. to 120° C. for 1 h to 12 h. As an example, the drying temperature of the third liquid film may be 60° C., 70° C., 80° C., 90° C., 100° C., 110° C. or 120° C., and the drying time may be 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h.

[0109] Optionally, the thickness of the anion exchange layer is 100 μm to 300 μm. As an example, the thickness of the anion exchange layer can be 100 μm, 120 μm, 140 μm, 160 μm, 180 μm, 200 μm, 220 μm, 240 μm, 260 μm, 280 μm or 300 μm.

[0110] In a second aspect of the present application, a MXene bipolar membrane is provided, which is prepared by the method for preparing a MXene bipolar membrane as described above.

[0111] Optionally, the MXene bipolar membrane includes a cation exchange layer, an intermediate interface layer and an anion exchange layer stacked in sequence.

[0112] Optionally, the transmembrane voltage of the MXene bipolar membrane is 0.9 V to 3 V. As an example, the transmembrane voltage of the MXene bipolar membrane can be 0.9 V, 1 V, 1.2 V, 1.4 V, 1.6 V, 1.8 V, 2 V, 2.2 V, 2.4 V, 2.6 V, 2.8 V or 3 V.

[0113] Optionally, the current efficiency of the MXene bipolar membrane is 80% to 95%. As an example, the current efficiency of the MXene bipolar membrane can be 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94% or 95%.

[0114] Optionally, the energy consumption of the MXene bipolar membrane is 1.1 kWh / kg to 5.3 kWh / kg. As an example, the energy consumption of the MXene bipolar membrane can be 1.1 kWh / kg, 1.5 kWh / kg, 2 kWh / kg, 2.5 kWh / kg, 3 kWh / kg, 3.5 kWh / kg, 4 kWh / kg, 4.5 kWh / kg, 5 kWh / kg or 5.3 kWh / kg.

[0115] Understandably, the energy consumption of the MXene bipolar membrane is also one of the indicators of water dissociation efficiency. The higher the water dissociation efficiency, the smaller the transmembrane voltage, and the lower the energy consumption of water dissociation. The MXene bipolar membrane prepared in this application uses MXene material as a water dissociation catalyst, and its high hydrophilicity can greatly promote the dissociation of water, reduce the transmembrane voltage, and thus reduce energy consumption.

[0116] In a third aspect of the present application, an electrodialysis device is provided, comprising the MXene bipolar membrane as described above.

[0117] Optionally, the electrodialysis device includes a positive electrode, a MXene bipolar membrane, an anion exchange membrane, a cation exchange membrane, a MXene bipolar membrane and a negative electrode arranged in sequence.

[0118] Optionally, the electrodialysis device includes an electrode chamber and an acid-base chamber, wherein the circulating liquid of the electrode chamber is a Na2SO4 solution with a concentration of 0.3M, and the circulating liquid of the acid-base chamber is a NaCl solution with a concentration of 0.5M.

[0119] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0120] Example 1

[0121] This embodiment provides a method for preparing a MXene bipolar membrane, and the specific steps are as follows:

[0122] (1) Preparation of cation exchange layer: 3 g of polyvinylidene fluoride, 2.5 g of sodium styrene sulfonate, 0.25 g of divinylbenzene and 25 mL of N,N-dimethylformamide were added to a 100 mL round-bottom flask, stirred thoroughly to dissolve, and then 0.05 g of initiator benzoyl peroxide was added. The temperature was raised to 70°C for reaction for 8 h. After cooling, the mixture was allowed to stand for degassing to obtain a first casting solution. The first casting solution was cast on a clean glass plate and coated with a 300 µm scraper to form a film. The film was then placed in a 60°C oven and dried for 5 h to obtain a cation exchange layer with a thickness of 300 µm.

[0123] (2) Preparation of MXene materials: 3 g of LiF was added to 60 mL of 9 M HCl solution and stirred until fully dissolved to obtain an etching solution; then 3 g of MAX precursor was slowly added to the etching solution and reacted at 35 °C for 24 h to obtain a reaction solution; the reaction solution was centrifuged and the supernatant was poured out, the centrifuged product was washed with 1 M HCl solution, and then centrifuged and washed repeatedly with deionized water until the pH of the supernatant after centrifugation was ≥ 6 to obtain a washed product; the washed product was dispersed in 30 mL of deionized water and ultrasonicated for 1 h in a N2 atmosphere to obtain a dispersion; the dispersion was high-speed centrifuged at a speed of 3500 rpm, and the centrifuged product was freeze-dried to obtain a MXene material; wherein the MAX precursor is Ti3AlC2, and the MXene material obtained by etching is Ti3C2T x Nanomaterials.

[0124] (3) Preparation of the intermediate interface layer: The MXene material was ultrasonically dispersed in N,N-dimethylformamide to prepare a suspension with a mass fraction of 0.5%. The suspension was evenly sprayed on the cation exchange layer using a spray gun and dried at 60 °C for 30 min to obtain the intermediate interface layer.

[0125] (4) Preparation of anion exchange layer: 3 g of polyvinylidene fluoride, 3 g of vinyl imidazole, 0.3 g of 1,6-dibromohexane and 25 mL of N,N-dimethylformamide were added to a 100 mL round-bottom flask, stirred thoroughly to dissolve, and then 0.05 g of initiator benzoyl peroxide was added. The temperature was raised to 70 °C for reaction for 8 h. After cooling, the mixture was allowed to stand for degassing to obtain a second casting solution. The second casting solution was cast on the middle interface layer and coated with a 300 µm scraper. The membrane was then placed in a 60 °C oven and dried for 5 h to obtain an anion exchange layer with a thickness of 300 µm, i.e., a MXene bipolar membrane.

[0126] Example 2

[0127] This embodiment provides a method for preparing a MXene bipolar membrane, and the specific steps are as follows:

[0128] (1) Preparation of cation exchange layer: 2.5 g of polyvinylidene fluoride, 2.5 g of sodium styrene sulfonate, 0.25 g of divinylbenzene and 25 mL of N,N-dimethylformamide were added to a 100 mL round-bottom flask, stirred thoroughly to dissolve, and then 0.05 g of initiator benzoyl peroxide was added. The temperature was raised to 70°C for reaction for 8 h. After cooling, the mixture was allowed to stand for degassing to obtain a first casting solution. The first casting solution was cast on a clean glass plate and coated with a 200 µm scraper to form a film. The film was then placed in a 60°C oven and dried for 5 h to obtain a cation exchange layer with a thickness of 200 µm.

[0129] (2) Preparation of MXene materials: the same as step (2) of Example 1.

[0130] (3) Preparation of the intermediate interface layer: the same as step (3) of Example 1.

[0131] (4) Preparation of anion exchange layer: 2.5 g of polyvinylidene fluoride, 3 g of vinyl imidazole, 0.3 g of 1,6-dibromohexane and 25 mL of N,N-dimethylformamide were added to a 100 mL round-bottom flask, stirred thoroughly to dissolve, and then 0.05 g of initiator benzoyl peroxide was added. The temperature was raised to 70 °C for reaction for 8 h. After cooling, the mixture was allowed to stand for degassing to obtain a second casting solution. The second casting solution was cast on the middle interface layer and coated with a 200 µm scraper. The membrane was then placed in a 60 °C oven and dried for 5 h to obtain an anion exchange layer with a thickness of 200 µm, i.e., a MXene bipolar membrane.

[0132] Example 3

[0133] This embodiment provides a method for preparing a MXene bipolar membrane, and the specific steps are as follows:

[0134] (1) Preparation of cation exchange layer: 2.5 g of polyvinylidene fluoride, 2.5 g of sodium allyl sulfonate, 0.25 g of divinylbenzene and 25 mL of N,N-dimethylformamide were added to a 100 mL round-bottom flask, stirred thoroughly to dissolve, and then 0.05 g of initiator benzoyl peroxide was added. The temperature was raised to 70°C for reaction for 8 h. After cooling, the mixture was allowed to stand for degassing to obtain a first casting solution. The first casting solution was cast on a clean glass plate and coated with a 100 µm scraper to form a film. The film was then placed in a 60°C oven and dried for 5 h to obtain a cation exchange layer with a thickness of 100 µm.

[0135] (2) Preparation of MXene materials: the same as step (2) of Example 1.

[0136] (3) Preparation of the intermediate interface layer: The MXene material was ultrasonically dispersed in N,N-dimethylformamide to prepare a suspension with a mass fraction of 1%. The suspension was evenly sprayed on the cation exchange layer using a spray gun and dried at 60 °C for 30 min to obtain the intermediate interface layer.

[0137] (4) Preparation of anion exchange layer: 2.5 g of polyvinylidene fluoride, 3 g of vinyl imidazole, 0.3 g of 1,6-dibromohexane and 25 mL of N,N-dimethylformamide were added to a 100 mL round-bottom flask, stirred thoroughly to dissolve, and then 0.05 g of initiator benzoyl peroxide was added. The temperature was raised to 70 °C for reaction for 8 h. After cooling, the mixture was allowed to stand for degassing to obtain a second casting solution. The second casting solution was cast on the middle interface layer and coated with a 100 µm scraper to form a film. The membrane was then placed in a 60 °C oven and dried for 5 h to obtain an anion exchange layer with a thickness of 100 µm, i.e., a MXene bipolar membrane.

[0138] Comparative Example 1

[0139] This comparative example provides a method for preparing a bipolar membrane, and the specific steps are as follows:

[0140] (1) Preparation of cation exchange layer: the same as step (1) of Example 1.

[0141] (2) Preparation of anion exchange layer: the same as step (4) of Example 1.

[0142] The bipolar membrane of this comparative example is composed of a cation exchange layer and an anion exchange layer stacked in sequence, and does not contain an intermediate interface layer made of MXene material.

[0143] Comparative Example 2

[0144] This comparative example provides a method for preparing a MXene bipolar membrane, and the specific steps are as follows:

[0145] (1) Preparation of cation exchange layer: the same as step (1) of Example 1.

[0146] (2) Preparation of the intermediate interface layer: Polyvinyl alcohol was dissolved in deionized water to prepare a solution with a mass fraction of 4%, which was evenly sprayed on the cation exchange layer using a spray gun and dried at 60°C for 30 min to obtain the intermediate interface layer.

[0147] (3) Preparation of anion exchange layer: the same as step (4) of Example 1.

[0148] Test Case

[0149] The MXene bipolar membranes of Examples 1 to 3 and the bipolar membranes of Comparative Examples 1 to 2 were tested as follows.

[0150] (1) MXene material: Raman spectroscopy and XRD tests were performed on the MAX precursor and MXene material of Example 1. The results are as follows: Figure 2 and Figure 3 As shown. Figure 2~Figure 3 It can be seen that Example 1 successfully produced MXene material.

[0151] (2) Current-voltage (CV) curve test: Before the test, the bipolar membrane was immersed in a 1M NaCl solution for 24 hours, and then the membrane was placed in a four-compartment electrodialysis device for testing; the electrode compartment used a 0.3M Na2SO4 solution as the circulating fluid, and the acid-base compartment used a 0.5M NaCl solution as the circulating fluid. During the test, the applied current was increased every 20 seconds, and the transmembrane voltage was recorded using a multimeter. The resulting CV curve is shown in the figure below. Figure 4 The transmembrane voltage of water dissociation process is shown in Table 1. Figure 4 As can be seen from Table 1, the MXene bipolar membranes prepared in Examples 1 to 3 have lower transmembrane voltage and higher water dissociation efficiency.

[0152] (3) Electrodialysis test: The water dissociation performance of the bipolar membrane was tested by electrodialysis. Before the test, the membrane was immersed in a 1 M NaCl solution for 24 h, and then the membrane was installed in the electrodialysis device in the order of "positive electrode-bipolar membrane-commercial anion exchange membrane-commercial cation exchange membrane-bipolar membrane-negative electrode". The electrode chamber used a 0.3 M Na2SO4 solution as the circulating fluid, and the acid-base chamber used a 0.5 M NaCl solution. A constant current was applied for testing. The current efficiency and energy consumption were shown in Figure 2. Figure 5 The relevant data are shown in Table 1. Figure 5As can be seen from Table 1, the MXene bipolar membranes prepared in Examples 1 to 3 have higher current efficiency and lower energy consumption, which means that the MXene bipolar membrane has the advantages of high water dissociation efficiency and excellent electrochemical performance, and has broad application prospects in the field of electrodialysis.

[0153] Table 1. Performance comparison of bipolar membranes

[0154]

[0155] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0156] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of protection of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the scope of protection of the present application. Therefore, the scope of protection of the present application shall be subject to the attached claims.

Claims

1. A method for preparing a MXene bipolar membrane, characterized in that: The following steps are involved: Subjecting a first casting solution containing polyvinylidene fluoride, a cationic monomer and a first cross-linking agent to a first film-forming treatment to form a cation exchange layer; Spraying a suspension containing MXene material onto the cation exchange layer to form an intermediate interface layer; The second casting solution containing polyvinylidene fluoride, anionic monomer and a second crosslinking agent is subjected to a second film-forming treatment to form an anion exchange layer on the intermediate interface layer.

2. The method for preparing a MXene bipolar membrane according to claim 1, characterized in that: The cationic monomer includes one or more of sodium styrene sulfonate and sodium allyl sulfonate.

3. The method for preparing a MXene bipolar membrane according to claim 1, characterized in that: The anionic monomer includes one or more of vinyl imidazole and vinyl pyridine.

4. The method for preparing a MXene bipolar membrane according to any one of claims 1 to 3, characterized in that: One or more of the following conditions are met: (1) In the first casting solution, the mass ratio of the polyvinylidene fluoride to the cationic monomer is 1:(0.5-1.5); (2) In the second casting solution, the mass ratio of the polyvinylidene fluoride to the anionic monomer is 1:(0.5-1.5); (3) the first cross-linking agent includes divinylbenzene; (4) the second cross-linking agent includes one or more of 1,6-dibromohexane and 1-bromohexane; (5) The mass ratio of the cationic monomer to the first cross-linking agent is 100:(3-15); (6) The mass ratio of the anionic monomer to the second cross-linking agent is 100:(3-15).

5. The method for preparing a MXene bipolar membrane according to claim 4, characterized in that: The first casting solution further contains a first initiator, and the second casting solution further contains a second initiator.

6. The method for preparing a MXene bipolar membrane according to claim 5, characterized in that: One or more of the following conditions are met: (1) The first initiator and the second initiator each independently include one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, azobiscyanovaleric acid, benzoyl peroxide and 2,2-azobis(2-methylpropylimidamide) dihydrochloride; (2) The mass ratio of the cationic monomer to the first initiator is 100:(0.5-5); (3) The mass ratio of the anionic monomer to the second initiator is 100:(0.5-5); (4) The solid content of the first casting solution and the second casting solution are each independently 10% to 30%.

7. The method for preparing a MXene bipolar membrane according to any one of claims 1 to 3, characterized in that: The preparation method of the MXene material comprises the following steps: The MAX precursor is placed in an etching solution containing hydrogen ions and fluorine ions to perform an etching reaction, and is purified to prepare the MXene material.

8. The method for preparing a MXene bipolar membrane according to claim 7, characterized in that: One or more of the following conditions are met: (1) The MAX precursor includes one or more of Ti3AlC2, Ti2AlC, Ti3AlCN, Ta4AlC3, V2AlC, V3AlC2, Mo2AlC and Mo2TiAlC2; (2) The etching solution contains one or more of HF, HCl and fluoride salt; (3) The etching reaction comprises the following steps: etching at 20°C to 50°C for 12h to 48h; (4) The mass fraction of the MXene material in the suspension is 0.1%~5%.

9. The method for preparing a MXene bipolar membrane according to any one of claims 1 to 3, characterized in that: The thickness of the cation exchange layer and the anion exchange layer are each independently 100 μm to 300 μm.

10. A MXene bipolar membrane, characterized in that: The MXene bipolar membrane is prepared by the preparation method of any one of claims 1 to 9.

11. The MXene bipolar membrane according to claim 10, characterized in that One or more of the following conditions are met: (1) The transmembrane voltage of the MXene bipolar membrane is 0.9V~3V; (2) The current efficiency of the MXene bipolar membrane is 80% to 95%; (3) The energy consumption of the MXene bipolar membrane is 1.1 kWh / kg~5.3 kWh / kg.

12. An electrodialysis device, characterized in that: Comprising the MXene bipolar membrane as claimed in claim 10 or 11.

Citation Information

Patent Citations

  • Solution grafting preparation method of PVDF cation exchange membrane

    CN104629068A

  • Preparation method of MBR membrane and application of MBR membrane to treatment on rural sewage

    CN107899439A

  • PVDF-PVIm blend membrane material and anion exchange membrane

    CN114044930A

  • Preparation method and application of copolymer membrane material

    CN114426643A

  • Two-dimensional titanium-carbon-based bipolar membrane and preparation method thereof

    CN116351255A