Cellulose and polyvinyl alcohol composite magnetic porous aerogel as well as preparation method and application thereof
By preparing cellulose polyvinyl alcohol composite magnetic porous aerogel, the problems of small adsorption capacity and high cost of existing adsorbents are solved, and efficient adsorption and recycling of oil-containing wastewater is achieved, which is suitable for power plant wastewater treatment.
Patent Information
- Application Number
- CN202411067294.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
Existing adsorbents such as activated carbon and single-component aerogels have limited adsorption capacity, high cost and difficult to recover when treating oily wastewater, which limits their application.
Using cellulose polyvinyl alcohol composite magnetic porous aerogel, heat the iron tetraoxide nanoparticles with cellulose, polyvinyl alcohol and crosslinking agent in water to form a glue, and in a long-chain alkyl silane coupling agent solution Immerse in the medium to form a material with magnetic properties and high adsorption properties.
It realizes effective adsorption and recovery of oil, has good magnetic properties and cyclic adsorption properties, and is suitable for the treatment of oil-containing wastewater in power plants, reducing costs and improving adsorption efficiency.
Smart Images

Figure HDA0004981383790000011 
Figure HDA0004981383790000012 
Figure HDA0004981383790000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material technology, and in particular relates to a cellulose polyvinyl alcohol composite magnetic porous aerogel, a preparation method and application thereof. Background Art
[0002] As the environmental protection requirements of the power industry continue to increase, the treatment of oily wastewater has attracted more and more attention. The main methods for treating oily wastewater include: sedimentation separation, coarse granulation, filtration, membrane separation, flotation, adsorption, coagulation, salting out, electrolysis and biochemical methods.
[0003] Among them, the adsorption method uses porous solid adsorbents to adsorb dissolved oil and other soluble organic matter in oily wastewater on the surface. It is simple and easy to operate and can be used to treat oily wastewater. Commonly used adsorbents include activated carbon, which not only has good adsorption properties for oil, but can also effectively adsorb other organic matter in wastewater at the same time. However, its adsorption capacity is limited (generally 30-80 mg / g for oil), and its cost is high and regeneration is difficult, which limits its application.
[0004] Aerogel has become a potential adsorption material due to its high specific surface area and high adsorption efficiency. However, the single-component aerogel is difficult to recycle as an adsorbent and has a small adsorption capacity, which hinders its application as an adsorbent. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a cellulose polyvinyl alcohol composite magnetic porous aerogel with high adsorption performance and cycle performance, and a preparation method and application thereof.
[0006] The present invention provides a method for preparing a cellulose polyvinyl alcohol composite magnetic porous aerogel, comprising the following steps:
[0007] S1) mixing ferroferric oxide nanoparticles, cellulose, polyvinyl alcohol and a cross-linking agent in water and heating them, then forming a gel under low temperature conditions, and freeze-drying them to obtain a magnetic aerogel;
[0008] S2) immersing the magnetic aerogel in a solution containing a long-chain alkyl silane coupling agent to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel.
[0009] Preferably, the cellulose is selected from one or more of cellulose nanocrystals, cellulose nanofibers and microcrystalline cellulose;
[0010] The molecular weight of the polyvinyl alcohol is 9000 to 50000;
[0011] The cross-linking agent is selected from tannic acid;
[0012] The long-chain alkylsilane coupling agent is selected from octadecyltrimethoxysilane.
[0013] Preferably, in the step S1), the ferrosoferric oxide nanoparticles are first dispersed in water, and then mixed with cellulose, polyvinyl alcohol and a cross-linking agent and heated; the dispersion method is ultrasound; and the dispersion time is 5 to 20 minutes.
[0014] Preferably, the mass ratio of the ferrosoferric oxide nanoparticles to water is 1:100 to 15:100.
[0015] Preferably, the mass ratio of the total mass of the ferrosoferric oxide nanoparticles and water to the polyvinyl alcohol is 100:10 to 100:25.
[0016] Preferably, the mass ratio of the cellulose to the polyvinyl alcohol is 1:3 to 1:10.
[0017] Preferably, the mass ratio of the cross-linking agent to polyvinyl alcohol is 1:3 to 1:10.
[0018] Preferably, the temperature of the mixed heating is 90°C to 120°C; the time of the mixed heating is 2 to 3 hours;
[0019] The volume ratio of the long-chain alkyl silane coupling agent to the solution containing the long-chain alkyl silane coupling agent is 0.5:100 to 1.5:100;
[0020] The cellulose polyvinyl alcohol composite magnetic porous aerogel has loose 3D pores; the pore size of the 3D pores is 10-80 nm.
[0021] The present invention also provides a cellulose polyvinyl alcohol composite magnetic porous aerogel prepared by the above-mentioned preparation method, wherein the cellulose polyvinyl alcohol composite magnetic porous aerogel comprises ferrosoferric oxide nanoparticles; the ferrosoferric oxide nanoparticles are dispersed inside and on the surface of the cellulose polyvinyl alcohol composite magnetic porous aerogel; and the surface of the cellulose polyvinyl alcohol composite magnetic porous aerogel and the surface of the pores are coated with a long-chain alkyl silane coupling agent.
[0022] The present invention also provides an application of the cellulose polyvinyl alcohol composite magnetic porous aerogel as an adsorbent for oil-water separation.
[0023] The present invention provides a method for preparing a cellulose polyvinyl alcohol composite magnetic porous aerogel, comprising the following steps: S1) mixing ferroferric oxide nanoparticles, cellulose, polyvinyl alcohol and a crosslinking agent in water and heating them, then forming gel under low temperature conditions, freeze drying, and obtaining a magnetic aerogel; S2) impregnating the magnetic aerogel in a solution containing a long-chain alkyl silane coupling agent to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel. Compared with the prior art, the present invention prepares a gel by adding ferroferric oxide nanoparticles to deionized water, ultrasonically dispersing the mixture, and then forming a gel with cellulose, polyvinyl alcohol and a crosslinking agent, and then freeze drying the gel to form an aerogel. The ferrosoferric oxide nanoparticles do not agglomerate, and the addition of the ferrosoferric oxide nanoparticles does not affect the synthesis of the aerogel, which is beneficial to the processing of the material molding. The advantages of the ferrosoferric oxide nanoparticles, such as small particle size, large specific surface area, excellent magnetic properties, low cost and non-toxicity, are utilized to impart magnetism to the cellulose polyvinyl alcohol composite porous aerogel, thereby achieving effective adsorption and recycling of oil. Then, a long-chain alkyl silane coupling agent is utilized to impart oil absorption capacity to the aerogel through a simple surface dip coating method, thereby adsorbing oil in the water body, thereby enabling the prepared cellulose polyvinyl alcohol composite magnetic porous aerogel to have good adsorption in the oily wastewater solution of the power plant, and the aerogel has good magnetic properties and good cyclic adsorption performance, and can be used as a treatment material for oily wastewater in the power plant. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope (SEM) photograph of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 of the present invention;
[0025] Figure 2 is a magnetization curve diagram of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 of the present invention;
[0026] Figure 3 is a cyclic compression curve diagram of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 of the present invention;
[0027] Figure 4 This is an optical photograph of the water contact angle of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 of the present invention;
[0028] Figure 5 This is a graph showing the adsorption efficiency of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 of the present invention at different pH values;
[0029] Figure 6 is a cyclic adsorption diagram of the cellulose / polyvinyl alcohol magnetic porous aerogel obtained in Example 4 of the present invention;
[0030] Figure 7The photographs are of the process of adsorbing oil on the surface and underwater in water by the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 of the present invention;
[0031] Figure 8 The photographs are of the magnetic adsorption process of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 of the present invention and the cellulose polyvinyl alcohol composite porous aerogel obtained in Comparative Example 1;
[0032] Fig. 9 The photos are of the oil adsorption effect of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 of the present invention and the cellulose polyvinyl alcohol magnetic porous aerogel obtained in Comparative Example 2 in water. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0034] The invention provides a method for preparing a cellulose polyvinyl alcohol composite magnetic porous aerogel, comprising the following steps: S1) mixing ferroferric oxide nanoparticles, cellulose, polyvinyl alcohol and a cross-linking agent in water and heating them, then gelling them under low temperature conditions, and freeze-drying them to obtain a magnetic aerogel; S2) immersing the magnetic aerogel in a solution containing a long-chain alkyl silane coupling agent to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel.
[0035] The present invention has no particular limitation on the sources of all raw materials, and any raw materials available on the market can be used.
[0036] Mix ferroferric oxide nanoparticles, cellulose, polyvinyl alcohol and a crosslinking agent in water and heat them; wherein the cellulose can be any cellulose known to those skilled in the art without any special limitation, and in the present invention, it is preferably one or more of cellulose nanocrystals, cellulose nanofibers and microcrystalline cellulose; the diameter of the cellulose is preferably 1-50 nm, more preferably 4-10 nm; the molecular weight of the polyvinyl alcohol is preferably 9000-50000, specifically, the polyvinyl alcohol is selected from one or more of the molecular weight type 9000-10000, the molecular weight type 13000-23000 and the molecular weight type 31000-50000; the crosslinking agent is preferably tannic acid; in a specific embodiment provided by the present invention, the ferroferric oxide nanoparticles are first dispersed in water, and then mixed with the cellulose, polyvinyl alcohol and the crosslinking agent and heated; the dispersion method is preferably ultrasound; the ultrasound preferably uses an ultrasonic cell crusher; the power of the ultrasound is preferably 10-20 W; the dispersion time is preferably 5-20 min. The mass ratio of the ferrosoferric oxide nanoparticles to water is preferably 1:100-15:100, more preferably 1:100-10:100, and more preferably 3:100-7:100; in some embodiments provided by the present invention, the mass ratio of the ferrosoferric oxide nanoparticles to water is specifically 1:100, 3:100, 5:100, 7:100, 10:100 or 15:100; the mass ratio of the total mass of the ferrosoferric oxide nanoparticles and water to polyvinyl alcohol is preferably 1:1-5:1, more preferably 1:1-4:1, more preferably 2:1-3:1, and most preferably 2:1; the mass ratio of cellulose to polyvinyl alcohol is preferably 1:3-1:10, more preferably 1:3-1 :8, and more preferably 1:3.3~1:7.5; in some embodiments provided by the present invention, the mass ratio of cellulose to polyvinyl alcohol is specifically 1:5, 1:7.5, 3:10 or 3:20; the mass ratio of the cross-linking agent to polyvinyl alcohol is preferably 1:3~1:10, more preferably 1:3~1:8, and more preferably 1:3.3~1:7.5; in some embodiments provided by the present invention, the mass ratio of the cross-linking agent to polyvinyl alcohol is specifically 3:10, 1:5, 3:20 or 1:7.5; the mixed heating temperature is preferably 90℃~120℃, more preferably 90℃~110℃, and more preferably 90℃; the mixed heating time is preferably 1~3h, more preferably 1~2h.
[0037] After mixing and heating, the mixture is gelled under low temperature conditions and freeze-dried to obtain a magnetic aerogel; the temperature of the low temperature conditions is preferably -50°C to -10°C, more preferably -40°C to -20°C, more preferably -35°C to -25°C, and most preferably -30°C; the freeze-drying temperature is preferably -120°C to -80°C, more preferably -110°C to -90°C, and more preferably -100°C; the freeze-drying pressure is preferably 20 to 30 Pa, more preferably 25 Pa; the freeze-drying time is preferably 8 to 15 h, more preferably 10 to 14 h, and more preferably 12 h.
[0038] The magnetic aerogel is immersed in a solution containing a long-chain alkyl silane coupling agent to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel; the long-chain alkyl silane coupling agent can be a long-chain alkyl silane coupling agent well known to those skilled in the art, without any special restrictions, and is preferably octadecyltrimethoxysilane in the present invention; the solvent of the solution containing the long-chain alkyl silane coupling agent is preferably water and / or an alcohol solvent, more preferably water and an alcohol solvent; the alcohol solvent can be an alcohol solvent well known to those skilled in the art, without any special restrictions, and is preferably ethanol in the present invention; the volume ratio of water to alcohol solvent is preferably (10-30):1, more preferably (15-25):1 , and preferably 20:1; the volume ratio of the long-chain alkyl silane coupling agent to the solution in the solution containing the long-chain alkyl silane coupling agent is 0.5:100 to 1.5:100; the immersion temperature is preferably 20°C to 30°C, and more preferably 25°C; the immersion time is preferably 30 to 90 min, more preferably 40 to 70 min, and more preferably 1 h; after immersion, it is preferably dried to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel; the drying temperature is preferably 50°C to 80°C, more preferably 50°C to 70°C, and more preferably 60°C; the drying time is preferably 1 to 3 h, more preferably 1 to 2 h, and more preferably 1.5 h.
[0039] According to the present invention, the cellulose polyvinyl alcohol composite magnetic porous aerogel preferably has loose 3D pores; the pore size of the 3D pores is preferably 10 to 80 nm.
[0040] Cellulose is a biomass renewable resource, which has attracted much attention due to its abundant reserves and excellent performance. Its polyhydroxy structure between chains and molecular chains with high polymerization degree give it a natural advantage as a gel material. Polyvinyl alcohol, as a natural water-soluble polymer, has the characteristics of non-toxicity and good mechanical properties. The widely existing hydrogen between its chains is conducive to combining with cellulose to form a gel with stable mechanical properties. The present invention prepares a gel by adding ferrosoferric oxide nanoparticles to deionized water, ultrasonically dispersing them, and then preparing a gel with cellulose, polyvinyl alcohol, and a crosslinking agent, and then freeze-drying the gel to form an aerogel. The ferrosoferric oxide nanoparticles do not agglomerate, and the addition of the ferrosoferric oxide nanoparticles does not affect the synthesis of the aerogel, which is beneficial to the processing of the material molding. The advantages of the ferrosoferric oxide nanoparticles, such as small particle size, large specific surface area, excellent magnetic properties, low cost and non-toxicity, are utilized to impart magnetism to the cellulose polyvinyl alcohol composite porous aerogel, thereby achieving effective adsorption and recycling of oil. Then, a long-chain alkyl silane coupling agent is utilized to impart oil absorption capacity to the aerogel through a simple surface dip coating method, thereby adsorbing oil in the water body, thereby enabling the prepared cellulose polyvinyl alcohol composite magnetic porous aerogel to have good adsorption in the oily wastewater solution of the power plant, and the aerogel has good magnetic properties and good cyclic adsorption performance, and can be used as a treatment material for oily wastewater in the power plant.
[0041] The present invention also provides a cellulose polyvinyl alcohol composite magnetic porous aerogel prepared by the above-mentioned preparation method, wherein the cellulose polyvinyl alcohol composite magnetic porous aerogel comprises ferroferric oxide nanoparticles; the ferroferric oxide nanoparticles are dispersed in the interior and surface of the cellulose polyvinyl alcohol composite magnetic porous aerogel; the surface and pore surfaces of the cellulose polyvinyl alcohol composite magnetic porous aerogel are coated with a long-chain alkyl silane coupling agent; the long-chain alkyl silane coupling agent is the same as described above and will not be repeated here.
[0042] The present invention also provides an application of the cellulose polyvinyl alcohol composite magnetic porous aerogel as an adsorbent for oil-water separation.
[0043] More specifically, the cellulose polyvinyl alcohol composite magnetic porous aerogel is used as an adsorbent for oil-water separation in oily wastewater from power plants.
[0044] In order to further illustrate the present invention, a cellulose polyvinyl alcohol composite magnetic porous aerogel, a preparation method and an application thereof provided by the present invention are described in detail below in conjunction with embodiments.
[0045] The reagents used in the following examples are all commercially available; the particle size of the ferroferric oxide nanoparticles is 100 nm to 1 μm; and the cellulose is McLean nanocellulose with a diameter of 4 to 10 nm.
[0046] Example 1
[0047] Take ferroferric oxide nanoparticles and water in a mass ratio of 3:100 respectively, disperse them for 20 minutes using an ultrasonic cell crusher with a power of 10 W to obtain a mixed solution.
[0048] 20g of the mixed solution, 2g of cellulose, 10g of polyvinyl alcohol with a molecular weight of 9000-10000 and 3g of tannic acid were stirred and heated at 90°C for 1h. After heating, the solution was poured into a mold and frozen into gel at a low temperature of minus 30 degrees Celsius. After gelation, it was freeze-dried at a temperature of -100°C and a pressure of 25Pa for 12h to obtain magnetic aerogel.
[0049] Octadecyltrimethoxysilane was added to a mixed solution of ethanol / deionized water in a volume ratio of 1:20 so that the volume concentration of octadecyltrimethoxysilane in the final solution was 1%. The prepared magnetic aerogel was immersed in the above solution to react for 1 hour. The sample was taken out, cleaned, and dried at 60°C for 1.5 hours to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel.
[0050] Example 2
[0051] Take ferroferric oxide nanoparticles and water in a mass ratio of 5:100 respectively, and disperse them for 20 minutes using an ultrasonic cell crusher with a power of 10 W to obtain a mixed solution.
[0052] 20g of the mixed solution, 2g of cellulose, 10g of polyvinyl alcohol with a molecular weight of 9000-10000 and 3g of tannic acid were stirred and heated at 90°C for 1h. After heating, the solution was poured into a mold and frozen into gel at a low temperature of minus 30 degrees Celsius. After gelation, it was freeze-dried at a temperature of -100°C and a pressure of 25Pa for 12h to obtain magnetic aerogel.
[0053] Octadecyltrimethoxysilane was added to a mixed solution of ethanol / deionized water in a volume ratio of 1:20 so that the volume concentration of octadecyltrimethoxysilane in the final solution was 1%. The prepared magnetic aerogel was immersed in the above solution to react for 1 hour. The sample was taken out, cleaned, and dried at 60°C for 1.5 hours to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel.
[0054] Example 3
[0055] Take ferroferric oxide nanoparticles and water in a mass ratio of 7:100 respectively, and disperse them for 20 minutes using an ultrasonic cell crusher with a power of 10 W to obtain a mixed solution.
[0056] 20g of the mixed solution, 2g of cellulose, 10g of polyvinyl alcohol with a molecular weight of 9000-10000 and 3g of tannic acid were stirred and heated at 90°C for 1h. After heating, the solution was poured into a mold and frozen into gel at a low temperature of minus 30 degrees Celsius. After gelation, it was freeze-dried at a temperature of -100°C and a pressure of 25Pa for 12h to obtain magnetic aerogel.
[0057] Octadecyltrimethoxysilane was added to a mixed solution of ethanol / deionized water in a volume ratio of 1:20 so that the volume concentration of octadecyltrimethoxysilane in the final solution was 1%. The prepared magnetic aerogel was immersed in the above solution to react for 1 hour. The sample was taken out, cleaned, and dried at 60°C for 1.5 hours to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel.
[0058] Example 4
[0059] Ferroferric oxide nanoparticles and water were taken at a mass ratio of 10:100, respectively, and dispersed for 20 minutes using an ultrasonic cell crusher with a power of 10 W to obtain a mixed solution.
[0060] 20g of the mixed solution, 2g of cellulose, 10g of polyvinyl alcohol with a molecular weight of 9000-10000 and 3g of tannic acid were stirred and heated at 90°C for 1h. After heating, the solution was poured into a mold and frozen into gel at a low temperature of minus 30 degrees Celsius. After gelation, it was freeze-dried at a temperature of -100°C and a pressure of 25Pa for 12h to obtain magnetic aerogel.
[0061] Octadecyltrimethoxysilane was added to a mixed solution of ethanol / deionized water in a volume ratio of 1:20 so that the volume concentration of octadecyltrimethoxysilane in the final solution was 1%. The prepared magnetic aerogel was immersed in the above solution to react for 1 hour. The sample was taken out, cleaned, and dried at 60°C for 1.5 hours to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel.
[0062] The cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 was analyzed using a scanning electron microscope, and its scanning electron microscope SEM photograph was obtained as shown in FIG. Figure 1 shown.
[0063] The magnetic properties of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 were analyzed, and its magnetization curve was obtained as shown in the figure: Figure 2 shown.
[0064] The mechanical properties of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 were analyzed, and the cyclic compression curve thereof was obtained as shown in FIG. Figure 3 shown.
[0065] The hydrophobic properties of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 were tested, and the optical photograph of its water contact angle was obtained as shown in FIG. Figure 4 shown.
[0066] The cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 was placed in oily wastewater with different pH values to detect its adsorption performance, and the adsorption efficiency diagram at different pH values was obtained, as shown in FIG. Figure 5 shown.
[0067] The cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 was placed in oily wastewater containing pump oil for adsorption, and its cyclic adsorption diagram was obtained as shown in FIG. Figure 6 shown.
[0068] The cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 is shown in the following figure: Figure 7 shown.
[0069] Comparative Example 1
[0070] Take ferroferric oxide nanoparticles and water in a mass ratio of 0:100 respectively.
[0071] 20g of aqueous solution, 2g of cellulose, 10g of polyvinyl alcohol with a molecular weight of 9000-1000 and 3g of tannic acid were stirred and heated at 90°C for 1h. After heating, the solution was poured into a mold and frozen into gel at a low temperature of minus 30 degrees Celsius. After gelation, it was freeze-dried at a temperature of -100°C and a pressure of 25Pa for 12h to obtain magnetic aerogel.
[0072] Octadecyltrimethoxysilane was added to a mixed solution of ethanol / deionized water in a volume ratio of 1:20 so that the volume concentration of octadecyltrimethoxysilane in the final solution was 1%. The prepared magnetic aerogel was immersed in the above solution to react for 1 hour. The sample was taken out, cleaned, and dried at 60°C for 1.5 hours to obtain a cellulose polyvinyl alcohol composite porous aerogel.
[0073] The magnetic adsorption process photos of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 and the cellulose polyvinyl alcohol composite porous aerogel obtained in Comparative Example 1 are shown in FIG. Figure 8 shown.
[0074] Comparative Example 2
[0075] Ferroferric oxide nanoparticles and water were taken at a mass ratio of 10:100, respectively, and dispersed for 20 minutes using an ultrasonic cell crusher with a power of 10 W to obtain a mixed solution.
[0076] 20g of the mixed solution, 2g of cellulose, 10g of polyvinyl alcohol with a molecular weight of 9000-10000 and 3g of tannic acid were stirred and heated at 90°C for 1h. After heating, the solution was poured into a mold and frozen into gel at a low temperature of minus 30 degrees Celsius. After gelation, it was freeze-dried at a temperature of -100°C and a pressure of 25Pa for 12h to obtain cellulose polyvinyl alcohol magnetic porous aerogel.
[0077] The photos of the cellulose polyvinyl alcohol composite magnetic porous aerogel obtained in Example 4 and the cellulose polyvinyl alcohol magnetic porous aerogel obtained in Comparative Example 2 showing the effect of oil adsorption in water are shown in Figure 2. Fig. 9 As shown, the left figure is Example 4 and the right figure is Comparative Example 2.
[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a cellulose polyvinyl alcohol composite magnetic porous aerogel, characterized in that: The following steps are involved: S1) mixing ferroferric oxide nanoparticles, cellulose, polyvinyl alcohol and a cross-linking agent in water and heating them, then forming a gel under low temperature conditions, and freeze-drying them to obtain a magnetic aerogel; S2) immersing the magnetic aerogel in a solution containing a long-chain alkyl silane coupling agent to obtain a cellulose polyvinyl alcohol composite magnetic porous aerogel.
2. The preparation method according to claim 1, characterized in that: The cellulose is selected from one or more of cellulose nanocrystals, cellulose nanofibers and microcrystalline cellulose; The molecular weight of the polyvinyl alcohol is 9000 to 50000; The cross-linking agent is selected from tannic acid; The long-chain alkylsilane coupling agent is selected from octadecyltrimethoxysilane.
3. The preparation method according to claim 1, characterized in that: In the step S1), the ferrosoferric oxide nanoparticles are first dispersed in water, and then mixed with cellulose, polyvinyl alcohol and a cross-linking agent and heated; the dispersion method is ultrasound; and the dispersion time is 5 to 20 minutes.
4. The preparation method according to claim 1, characterized in that: The mass ratio of the ferrosoferric oxide nanoparticles to water is 1:100 to 15:
100.
5. The preparation method according to claim 1, characterized in that: The mass ratio of the total mass of the ferrosoferric oxide nanoparticles and water to the mass ratio of the polyvinyl alcohol is 100:10 to 100:
25.
6. The preparation method according to claim 1, characterized in that: The mass ratio of the cellulose to the polyvinyl alcohol is 1:3 to 1:
10.
7. The preparation method according to claim 1, characterized in that: The mass ratio of the cross-linking agent to polyvinyl alcohol is 1:3 to 1:
10.
8. The preparation method according to claim 1, characterized in that: The temperature of the mixed heating is 90°C to 120°C; the time of the mixed heating is 2 to 3 hours; The volume ratio of the long-chain alkyl silane coupling agent to the solution containing the long-chain alkyl silane coupling agent is 0.5:100 to 1.5:100; The cellulose polyvinyl alcohol composite magnetic porous aerogel has loose 3D pores; the pore size of the 3D pores is 10-80 nm.
9. The cellulose polyvinyl alcohol composite magnetic porous aerogel prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The cellulose polyvinyl alcohol composite magnetic porous aerogel comprises ferroferric oxide nanoparticles; the ferroferric oxide nanoparticles are dispersed inside and on the surface of the cellulose polyvinyl alcohol composite magnetic porous aerogel; and the surface and pore surfaces of the cellulose polyvinyl alcohol composite magnetic porous aerogel are coated with a long-chain alkyl silane coupling agent.
10. Use of the cellulose polyvinyl alcohol composite magnetic porous aerogel prepared by the preparation method of any one of claims 1 to 8 or the cellulose polyvinyl alcohol composite magnetic porous aerogel according to claim 9 as an adsorbent for oil-water separation.
Citation Information
Patent Citations
A preparing method of acetylated nanometer cellulose-based magnetic oil-absorbing aerogel
CN106496642A
Method for preparing aerogel through freezing and thawing cycle method
CN107365427A
Preparation method of polyvinyl alcohol / bagasse nano-cellulose aerogel
CN108752623A
Underwater elastic cellulose aerogel and preparation method and application thereof
CN112898625A
Preparation method of nanocellulose hydrophobic aerogel and application of food system
CN116444852A
Cited By
Photoelectric thermomagnetic control biomass composite material with simple wettability switching prepared by water-phase one-pot method and application of photoelectric thermomagnetic control biomass composite material