Zirconium-based metal organic framework supported cobalt ferrite magnetic dephosphorization material as well as preparation method and application thereof
The magnetic phosphorus removal material of cobalt ferrite is supported by the zirconium-based metal organic framework, and the spinel cobalt ferrite CoFe2O4 nanoparticles are loaded, which solves the problem of efficient removal of phosphate and glyphosate in water, and realizes the removal of multi-form phosphorus. And the secondary pollution of inorganic phosphorus is avoided through the recyclability of magnetic materials.
Patent Information
- Application Number
- CN202411199464.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-19
AI Technical Summary
The existing phosphorus removal technology is difficult to efficiently remove phosphate and organic phosphorus pesticide glyphosate in water at the same time, and the inorganic phosphorus produced during advanced oxidation needs to be further removed to prevent secondary contamination.
The zirconium-based metal organic framework is used to support the magnetic phosphorus removal material of cobalt ferrite, and spinel cobalt ferrite CoFe2O4 nanoparticles are loaded on the zirconium-based metal organic framework MOF-808, and the material preparation is achieved through ultrasonic stirring and high-temperature reaction. and used to remove phosphate and activate peracetic acid to degrade glyphosate while adsorbing the resulting phosphate.
It realizes efficient removal of multi-form phosphorus in water, with both adsorption and catalytic functions, the material is magnetic and easy to recover, avoids secondary pollution of inorganic phosphorus, and is suitable for large-scale promotion and application.
Smart Images

Figure CN118976476A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sewage treatment, more specifically, to the technical field of removal of organic phosphorus and inorganic phosphorus, and in particular to a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material and a preparation method and application thereof. Background Art
[0002] Excess phosphorus is the main cause of eutrophication of water bodies.
[0003] Traditional phosphorus removal methods, such as chemical precipitation and bio-enhanced phosphorus removal, are difficult to meet increasingly stringent emission standards. In addition, while the world is working to eliminate existing pollutants, the continuous introduction of new pollutants poses a major threat to humans and the environment. New pollutants in water include organophosphorus pesticides represented by glyphosate. Due to the rapid development of modern agriculture, organophosphorus pesticides have been widely used around the world. However, the excessive use of organophosphorus pesticides has led to their frequent detection in groundwater and surface water, posing a potential threat to human life and safety. Therefore, the effective removal of polymorphic phosphorus in water is crucial for environmental protection and human health.
[0004] For the selective removal of phosphates, efficient phosphorus removal materials can be designed and prepared through the mechanism that metal-based materials and phosphates can form inner layer complexes. For the removal of organophosphorus, many researchers focus on advanced oxidation methods to produce strong oxidative free radicals to degrade and mineralize organophosphorus pesticides. In addition to commonly used oxidants such as hydrogen peroxide and persulfate, peracetic acid (PAA) is used to degrade new pollutants in water due to its high oxidation potential, such as endocrine disruptors, disinfection by-products, and drugs. It is worth noting that organophosphorus compounds in the advanced oxidation process will be converted into inorganic phosphorus. In order to prevent secondary pollution, the generated inorganic phosphorus products need to be effectively removed.
[0005] Therefore, it is hoped to provide a phosphorus removal material that can remove phosphates and activate peracetic acid to degrade glyphosate while adsorbing the generated phosphates, thereby achieving efficient removal of polymorphic phosphorus in water. Summary of the invention
[0006] In order to overcome the shortcomings of the above-mentioned prior art, an object of the present invention is to provide a method for preparing a zirconium-based metal-organic framework supported cobalt ferrite magnetic phosphorus removal material. The zirconium-based metal-organic framework supported cobalt ferrite magnetic phosphorus removal material prepared thereby can remove phosphate and activate peracetic acid to degrade glyphosate, while adsorbing the generated phosphate, thereby achieving efficient removal of polymorphic phosphorus in water, and is suitable for large-scale promotion and application.
[0007] Another object of the present invention is to provide a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material, which can remove phosphates and activate peracetic acid to degrade glyphosate, while adsorbing the generated phosphates to achieve efficient removal of polymorphic phosphorus in water, and is suitable for large-scale promotion and application.
[0008] Another object of the present invention is to provide an application of a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material, which is used to remove phosphates and activate peracetic acid to degrade glyphosate, while adsorbing the generated phosphates to achieve efficient removal of polymorphic phosphorus in water, and is suitable for large-scale promotion and application.
[0009] To achieve the above objectives, in the first aspect of the present invention, a method for preparing a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material is provided, wherein the spinel cobalt ferrite CoFe 2 O 4 Nanoparticles are loaded on the zirconium-based metal organic framework MOF-808 to prepare MOF-808 / CoFe 2 O 4 Phosphorus removal material, the MOF-808 / CoFe 2 O 4 The phosphorus removal material is the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material.
[0010] Preferably, the spinel cobalt ferrite CoFe 2 O 4 The steps of loading the nanoparticles on the zirconium-based metal organic framework MOF-808 specifically include:
[0011] (1) The spinel cobalt ferrite CoFe 2 O 4 The nanoparticles, the zirconium-based metal organic framework MOF-808 and trisodium citrate are added into deionized water, and reacted at high temperature after ultrasonic stirring to obtain a reaction product;
[0012] (2) The reaction product is subjected to magnetic separation, washing and drying to obtain the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material.
[0013] More preferably, in the step (1), the spinel cobalt ferrite CoFe 2 O 4 The ratio of the nanoparticles, the zirconium-based metal organic framework MOF-808, the trisodium citrate and the deionized water is 20mg-30mg: 50mg-60mg: 100mg-150mg: 50mL-80mL; the ultrasonic stirring time is 30min; the temperature of the high temperature reaction is 100°C-150°C, and the high temperature reaction time is 2h-4h.
[0014] Preferably, the spinel cobalt ferrite CoFe 2 O 4 The nanoparticles were prepared by the following steps:
[0015] (A1) FeCl 3 6H 2 O、CoCl 2 6H 2 O is added into ethylene glycol and ultrasonically stirred to obtain a precursor solution;
[0016] (A2) adding anhydrous sodium acetate and polyethylene glycol to the precursor solution to obtain a mixed solution, and reacting the mixed solution under high temperature and high pressure to obtain a reaction product;
[0017] (A3) The reaction product is subjected to magnetic separation, washing and drying to obtain the spinel cobalt ferrite CoFe 2 O 4 Nanoparticles.
[0018] More preferably, in the step (A1), the FeCl 3 6H 2 O, the CoCl 2 6H 2 The ratio of O to the ethylene glycol is 50mmol-100mmol:25mmol-50mmol:1L; and the ultrasonic stirring time is 30min.
[0019] More preferably, in the step (A2), the anhydrous sodium acetate, the polyethylene glycol and the FeCl 3 6H 2 The ratio of O is 200mmol~300mmol:6g~15g:50mmol; the step of reacting the mixed solution under high temperature and high pressure specifically includes: sealing the mixed solution in an autoclave, and then placing the autoclave in an oven, reacting at 180℃~200℃ for 18h~20h.
[0020] Preferably, the zirconium-based metal organic framework MOF-808 is prepared by the following steps:
[0021] (B1) ZrOCl 2 8H 2 O is added into a precursor solution consisting of deionized water, trimesic acid, acetic acid and concentrated hydrochloric acid, and heated and stirred to obtain a reaction product;
[0022] (B2) Soaking the reaction product in ethanol and then drying it to obtain the zirconium-based metal organic framework MOF-808.
[0023] More preferably, in the step (B1), the ZrOCl 2 8H 2 The ratio of O to the trimesic acid is 30mmol-90mmol:10mmol-30mmol, the ratio of the acetic acid, the deionized water, the concentrated hydrochloric acid and the trimesic acid is 0.3L-0.6L:0.3L-0.6L:3mL-6mL:10mmol-30mmol; the heating and stirring temperature is 100°C-120°C.
[0024] In a second aspect of the present invention, a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material is provided, wherein the material is prepared by the above-mentioned method for preparing the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material.
[0025] In a third aspect of the present invention, there is provided a use of the above-mentioned zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material in removing phosphorus from water.
[0026] In a fourth aspect of the present invention, there is provided a use of the above-mentioned zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material for removing phosphate and glyphosate from water.
[0027] In a fifth aspect of the present invention, there is provided a use of the above-mentioned zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material in activating peracetic acid.
[0028] The beneficial effects of the present invention are:
[0029] 1. The preparation method of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material of the present invention is to prepare spinel cobalt ferrite CoFe 2 O 4 Nanoparticles are loaded on the zirconium-based metal organic framework MOF-808 to prepare
[0030] MOF-808 / CoFe 2 O 4 Phosphorus removal material, MOF-808 / CoFe 2 O 4 The phosphorus removal material is a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material, which can remove phosphates and activate peracetic acid to degrade glyphosate, while adsorbing the produced phosphates, thereby achieving efficient removal of polymorphic phosphorus in water and is suitable for large-scale promotion and application.
[0031] 2. The zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material of the present invention is prepared by the above-mentioned zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material preparation method. It can remove phosphates and activate peracetic acid to degrade glyphosate, while adsorbing the generated phosphates, thereby achieving efficient removal of polymorphic phosphorus in water, and is suitable for large-scale promotion and application.
[0032] 3. The application of the above-mentioned zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material of the present invention is used to remove phosphates and activate peracetic acid to degrade glyphosate, while adsorbing the generated phosphates to achieve efficient removal of polymorphic phosphorus in water, and is suitable for large-scale promotion and application.
[0033] These and other objects, features and advantages of the present invention will be more fully reflected in the following detailed description and claims, and may be achieved by the means, devices and combinations thereof particularly pointed out in the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a transmission electron microscope TEM image of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material prepared in Example 1 of the present invention.
[0035] Figure 2 This is the XPS graph of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material prepared in Example 1 of the present invention.
[0036] Figure 3 This is the hysteresis curve of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0037] In order to effectively remove polymorphic phosphorus in water and protect the environment and human health, the inventors have proposed a method for preparing a zirconium-based metal-organic framework supported cobalt ferrite magnetic phosphorus removal material through in-depth and extensive research. The zirconium-based metal-organic framework supported cobalt ferrite magnetic phosphorus removal material prepared by the method can remove phosphate and activate peracetic acid to degrade glyphosate, while adsorbing the generated phosphate, thereby achieving efficient removal of polymorphic phosphorus in water.
[0038] The preparation method of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material of the present invention is to prepare spinel cobalt ferrite CoFe 2 O 4 Nanoparticles are loaded on the zirconium-based metal organic framework MOF-808 to prepare MOF-808 / CoFe 2 O 4 Phosphorus removal material, the MOF-808 / CoFe 2 O 4The phosphorus removal material is the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material.
[0039] The spinel cobalt ferrite CoFe 2 O 4 The step of loading the nanoparticles on the zirconium-based metal organic framework MOF-808 may specifically include any suitable steps. Preferably, the spinel cobalt ferrite CoFe 2 O 4 The steps of loading the nanoparticles on the zirconium-based metal organic framework MOF-808 specifically include:
[0040] (1) The spinel cobalt ferrite CoFe 2 O 4 The nanoparticles, the zirconium-based metal organic framework MOF-808 and trisodium citrate are added into deionized water, and reacted at high temperature after ultrasonic stirring to obtain a reaction product;
[0041] (2) The reaction product is subjected to magnetic separation, washing and drying to obtain the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material.
[0042] In the step (1), the spinel cobalt ferrite CoFe 2 O 4 The ratio of the nanoparticles, the zirconium-based metal organic framework MOF-808, the trisodium citrate and the deionized water can be determined as needed. More preferably, in the step (1), the spinel cobalt ferrite CoFe 2 O 4 The ratio of the nanoparticles, the zirconium-based metal organic framework MOF-808, the trisodium citrate and the deionized water is 20 mg to 30 mg: 50 mg to 60 mg: 100 mg to 150 mg: 50 mL to 80 mL.
[0043] In the step (1), the time of the ultrasonic stirring can be determined as needed. More preferably, in the step (1), the time of the ultrasonic stirring is 30 minutes.
[0044] In the step (1), the temperature and time of the high temperature reaction can be determined as needed. More preferably, in the step (1), the temperature of the high temperature reaction is 100° C. to 150° C., and the time of the high temperature reaction is 2 h to 4 h.
[0045] In the step (2), the washing may specifically include any suitable steps. More preferably, in the step (2), the washing specifically includes: washing with methanol and another deionized water for 5 times respectively.
[0046] In the step (2), the drying may specifically include any suitable steps. More preferably, in the step (2), the drying specifically includes: vacuum drying in a vacuum drying oven at 40° C. to 60° C. for 8 h to 12 h.
[0047] The spinel cobalt ferrite CoFe 2 O 4 The nanoparticles are prepared by any suitable steps. Preferably, the spinel cobalt ferrite CoFe 2 O 4 The nanoparticles were prepared by the following steps:
[0048] (A1) FeCl 3 6H 2 O、CoCl 2 6H 2 O is added into ethylene glycol and ultrasonically stirred to obtain a precursor solution;
[0049] (A2) adding anhydrous sodium acetate and polyethylene glycol to the precursor solution to obtain a mixed solution, and reacting the mixed solution under high temperature and high pressure to obtain a reaction product;
[0050] (A3) The reaction product is subjected to magnetic separation, washing and drying to obtain the spinel cobalt ferrite CoFe 2 O 4 Nanoparticles.
[0051] In the step (A1), the FeCl 3 6H 2 O, the CoCl 2 6H 2 O and the ratio of ethylene glycol can be determined as needed. More preferably, in the step (A1), the FeCl 3 6H 2 O, the CoCl 2 6H 2 The ratio of O to the ethylene glycol is 50mmol-100mmol:25mmol-50mmol:1L.
[0052] In the step (A1), the time of the ultrasonic stirring can be determined as needed. More preferably, in the step (A1), the time of the ultrasonic stirring is 30 minutes.
[0053] In the step (A2), the anhydrous sodium acetate, the polyethylene glycol and the FeCl 3 6H 2 O ratio can be determined as needed. More preferably, in the step (A2), the anhydrous sodium acetate, the polyethylene glycol and the FeCl3 6H 2 The ratio of O is 200mmol~300mmol:6g~15g:50mmol.
[0054] In the step (A2), the step of reacting the mixed solution under high temperature and high pressure may specifically include any suitable steps. More preferably, in the step (A2), the step of reacting the mixed solution under high temperature and high pressure specifically includes: sealing the mixed solution in an autoclave, and then placing the autoclave in an oven, and reacting at 180°C to 200°C for 18h to 20h.
[0055] In the step (A2), the autoclave may be any suitable autoclave. Furthermore, in the step (A2), the autoclave is a stainless steel autoclave lined with Teflon.
[0056] In the step (A3), the washing may specifically include any suitable steps. More preferably, in the step (A3), the washing specifically includes: washing with methanol and another deionized water for 5 times respectively.
[0057] In the step (A3), the drying may specifically include any suitable steps. More preferably, in the step (A3), the drying specifically includes: vacuum drying in a vacuum drying oven at 40° C. to 60° C. for 8 h to 10 h.
[0058] The zirconium-based metal organic framework MOF-808 is prepared by any suitable steps. Preferably, the zirconium-based metal organic framework MOF-808 is prepared by the following steps:
[0059] (B1) ZrOCl 2 8H 2 O is added into a precursor solution consisting of deionized water, trimesic acid, acetic acid and concentrated hydrochloric acid, and heated and stirred to obtain a reaction product;
[0060] (B2) Soaking the reaction product in ethanol and then drying it to obtain the zirconium-based metal organic framework MOF-808.
[0061] In the step (B1), the ZrOCl 2 8H 2 The ratio of ZrOCl to trimesic acid and the ratio of acetic acid, deionized water, concentrated hydrochloric acid and trimesic acid can be determined as needed. More preferably, in step (B1), the ZrOCl 2 8H 2The ratio of O to the trimesic acid is 30mmol-90mmol:10mmol-30mmol, and the ratio of the acetic acid, the deionized water, the concentrated hydrochloric acid and the trimesic acid is 0.3L-0.6L:0.3L-0.6L:3mL-6mL:10mmol-30mmol.
[0062] In the step (B1), the temperature of the heating and stirring can be determined as needed. More preferably, in the step (B1), the temperature of the heating and stirring is 100°C to 120°C.
[0063] In the step (B2), the number of soaking times can be determined as needed. More preferably, in the step (B2), the number of soaking times is 3 times.
[0064] In the step (B2), the drying may specifically include any suitable steps. More preferably, in the step (B2), the drying specifically includes: vacuum drying in a vacuum drying oven at 40° C. to 60° C. for 8 h to 10 h.
[0065] The present invention also provides a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material, which is prepared by adopting the preparation method of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material.
[0066] The present invention also provides the use of the above-mentioned zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material in removing phosphorus from water.
[0067] The present invention also provides the use of the above-mentioned zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material in removing phosphate and glyphosate from water.
[0068] When verifying the use of zirconium-based metal-organic framework-supported cobalt ferrite magnetic phosphorus removal material for removing phosphate and glyphosate from water, specifically, the zirconium-based metal-organic framework-supported cobalt ferrite magnetic phosphorus removal material and peracetic acid (PAA) are added to a phosphorus-contaminated aqueous solution containing phosphate and glyphosate, and the reaction is carried out at 25°C to 35°C for 30min to 120min, wherein the concentration of the phosphate solution is 10mg / L to 50mg / L, the concentration of the glyphosate aqueous solution is 20mg / L to 80mg / L, the ratio of the zirconium-based metal-organic framework-supported cobalt ferrite magnetic phosphorus removal material to the phosphorus-contaminated aqueous solution is 0.3g to 1.0g:1L, the initial pH value of the reaction is 3 to 9, and the ratio of peracetic acid (PAA) to the phosphorus-contaminated aqueous solution is 0.3mmol to 1.5mmol:1L.
[0069] The present invention also provides the use of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material in activating peracetic acid.
[0070] In order to more clearly understand the technical content of the present invention, the following embodiments are given in detail.
[0071] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards. If there are no corresponding national standards, they are carried out according to the general international standards, conventional conditions, or conditions recommended by the manufacturer.
[0072] Unless otherwise defined or indicated, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the method of the present invention.
[0073] Example 1
[0074] In this example, the zirconium-based metal organic framework-supported cobalt ferrite magnetic phosphorus removal material I was prepared by the following scheme
[0075] S1, FeCl in the ratio of 50mmol:25mmol:1L 3 6H 2 O、CoCl 2 6H 2 O was added into ethylene glycol and stirred for 30 min to obtain a precursor solution;
[0076] S2, according to anhydrous sodium acetate, polyethylene glycol and FeCl 3 6H 2 O in a ratio of 200mmol:6g:50mmol; anhydrous sodium acetate and polyethylene glycol are added to the precursor solution obtained in step S1 to obtain a mixed solution; the mixed solution is sealed in a stainless steel autoclave lined with Teflon; the autoclave is then placed in an oven, reacted at 200°C for 18h, and naturally cooled to room temperature to obtain reactant 1;
[0077] S3, after magnetic separation, the reactant obtained in step S2 was washed with anhydrous ethanol and deionized water for 5 times respectively, and then placed in a vacuum drying oven at 50°C for 10 hours to obtain CoFe 2 O 4 Nanoparticles;
[0078] S4, ZrOCl in a ratio of 90mmol:10mmol 2 8H 2 O and trimesic acid are mixed, and acetic acid, deionized water and concentrated hydrochloric acid are added to the above mixture in a ratio of trimesic acid: acetic acid: deionized water: concentrated hydrochloric acid of 10mmol: 0.3L: 0.45L: 6mL, and heated and stirred at 100°C to obtain reactant 2;
[0079] S5, soaking the reactant obtained in step S4 in ethanol for three times, and then placing it in a vacuum drying oven at 60° C. for 8 h to obtain MOF-808;
[0080] S6, the CoFe obtained in step S3 2 O 4 The nanoparticles, the MOF-808 metal organic framework material obtained in step S5, and trisodium citrate were added to 60 mL of deionized water in a ratio of 20 mg: 50 mg: 100 mg, and the mixture was ultrasonically stirred for 30 min and reacted at 150° C. for 3 h to obtain reactant three;
[0081] S7. After magnetic separation, the reactants obtained in step S6 are washed with methanol and deionized water for 5 times respectively, and then placed in a vacuum drying oven at 40° C. for 10 h to obtain a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material I.
[0082] The transmission electron microscope TEM image of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material Ⅰ is shown in Figure 1 As shown by Figure 1 It can be seen that the surface of the composite material is rough, indicating that MOF-808 is loaded with a lot of CoFe 2 O 4 Nanoparticles.
[0083] XPS analysis of the elements on the surface of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material Ⅰ is shown in Figure 2 As shown in the figure, the characteristic peaks corresponding to Co 2p, Fe 2p, Zr 3d and O1s can be clearly found, indicating that the phosphorus removal material prepared in Example 1 contains CoFe 2 O 4 and the main elements of MOF-808.
[0084] The hysteresis curve of the Zr-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material Ⅰ is shown in Figure 3 As shown, its saturation magnetization (Ms) is 53.86emu / g. Figure 3 It can be seen that the phosphorus removal material prepared in Example 1 has good superparamagnetic properties, which is conducive to recycling from the solution in practical applications.
[0085] Take 100 mL of phosphorus-contaminated aqueous solution containing phosphate (15 mg / L) and glyphosate (20 mg / L), add 0.05 g of the phosphorus removal material prepared in Example 1, adjust the pH to 7, add PAA (concentration of 0.5 mmol / L), place it in a constant temperature oscillator for oscillation reaction for 30 minutes, and the oscillator temperature and speed are 35°C and 180 r / min, respectively.
[0086] The wastewater after the reaction was filtered with a water filter membrane with a pore size of 0.45 μm; the concentrations of glyphosate and total phosphorus in the supernatant were determined, and the results showed that the glyphosate removal rate could reach 93.4%; the total phosphorus removal rate could reach 91.2%. Glyphosate and total phosphorus were determined by liquid chromatography and ammonium molybdate spectrophotometry, respectively.
[0087] Example 2
[0088] In this example, the following scheme is used to prepare the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material Ⅱ
[0089] S1, FeCl in the ratio of 75mmol:50mmol:1L 3 6H 2 O、CoCl 2 6H 2 O was added into ethylene glycol and stirred for 30 min to obtain a precursor solution;
[0090] S2, according to anhydrous sodium acetate, polyethylene glycol and FeCl 3 6H 2 O in a ratio of 250mmol:10g:50mmol; anhydrous sodium acetate and polyethylene glycol are added to the precursor solution obtained in step S1 to obtain a mixed solution; the mixed solution is sealed in a stainless steel autoclave lined with Teflon; the autoclave is then placed in an oven, reacted at 180°C for 19h, and naturally cooled to room temperature to obtain reactant 1;
[0091] S3, the reactant obtained in step S2 was subjected to magnetic separation, washed with anhydrous ethanol and deionized water for 5 times respectively, and then placed in a vacuum drying oven at 60°C for 8h to obtain CoFe 2 O 4 ;
[0092] S4, ZrOCl in a ratio of 30mmol:30mmol 2 8H 2 O and trimesic acid are mixed, and acetic acid, deionized water and concentrated hydrochloric acid are added into the mixture in a ratio of 30 mmol: 0.45 L: 0.6 L: 3 mL of trimesic acid: acetic acid: deionized water: concentrated hydrochloric acid, and the mixture is heated and stirred at 110° C. to obtain a reactant 2;
[0093] S5, soaking the second product obtained in step S4 in ethanol for three times, and then placing it in a vacuum drying oven at 50° C. for 9 h to obtain MOF-808;
[0094] S6, the CoFe obtained in step S3 2 O 4The nanoparticles, the MOF-808 metal organic framework material obtained in step S5, and trisodium citrate were added into 50 mL of deionized water in a ratio of 25 mg: 60 mg: 150 mg, and the mixture was ultrasonically stirred for 30 min and reacted at 120° C. for 4 h to obtain reactant three;
[0095] S7. After magnetic separation, the reactants obtained in step S6 are washed with methanol and deionized water for 5 times respectively, and then placed in a vacuum drying oven at 60° C. for 12 hours to obtain the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material II.
[0096] The transmission electron microscope TEM image of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material Ⅱ is similar to Figure 1 As shown, the XPS pattern of the zirconium-based metal organic framework-supported cobalt ferrite magnetic phosphorus removal material Ⅱ is similar to Figure 2 As shown in Figure 2, the hysteresis curve of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material ⅡI is similar to Figure 3 shown.
[0097] Take 100 mL of phosphorus-contaminated aqueous solution containing phosphate (10 mg / L) and glyphosate (80 mg / L), add 0.03 g of the phosphorus removal material prepared in Example 2, adjust the pH to 9, add PAA (concentration of 1.5 mmol / L), place it in a constant temperature oscillator for oscillation reaction for 120 minutes, and the oscillator temperature and speed are 30°C and 180 r / min, respectively.
[0098] The wastewater after the reaction was filtered with a water filter membrane with a pore size of 0.45 μm; the concentrations of glyphosate and total phosphorus in the supernatant were determined, and the results showed that the glyphosate removal rate could reach 96.1%; the total phosphorus removal rate could reach 93.4%. Glyphosate and total phosphorus were determined by liquid chromatography and ammonium molybdate spectrophotometry, respectively.
[0099] Example 3
[0100] In this example, the following scheme is used to prepare the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material III
[0101] S1, FeCl in the ratio of 100mmol:35mmol:1L 3 6H 2 O、CoCl 2 6H 2 O was added into ethylene glycol and stirred for 30 min to obtain a precursor solution;
[0102] S2, according to anhydrous sodium acetate, polyethylene glycol and FeCl 3 6H 2O in a ratio of 300mmol:15g:50mmol; anhydrous sodium acetate and polyethylene glycol are added to the precursor solution obtained in step S1 to obtain a mixed solution; the mixed solution is sealed in a stainless steel autoclave lined with Teflon; the autoclave is then placed in an oven, reacted at 190°C for 20h, and naturally cooled to room temperature to obtain reactant 1;
[0103] S3, the reactant obtained in step S2 was subjected to magnetic separation, washed with anhydrous ethanol and deionized water for 5 times respectively, and then placed in a vacuum drying oven at 40°C for 9 hours to obtain CoFe 2 O 4 ;
[0104] S4, ZrOCl in a ratio of 60mmol:20mmol 2 8H 2 O and trimesic acid are mixed, and acetic acid, deionized water and concentrated hydrochloric acid are added into the mixture in a ratio of 20 mmol: 0.6 L: 0.3 L: 4.5 mL of trimesic acid: acetic acid: deionized water: concentrated hydrochloric acid, and the mixture is heated and stirred at 120° C. to obtain a reactant 2;
[0105] S5, soaking the second product obtained in step S4 in ethanol for three times, and then placing it in a vacuum drying oven at 40° C. for 10 h to obtain MOF-808;
[0106] S6, the CoFe obtained in step S3 2 O 4 The nanoparticles, the MOF-808 metal organic framework material obtained in step S5, and trisodium citrate were added into 80 mL of deionized water in a ratio of 30 mg: 55 mg: 120 mg, and the mixture was ultrasonically stirred for 30 min and reacted at 100° C. for 2 h to obtain reactant three;
[0107] S7. After magnetic separation, the reactant III obtained in step S6 is washed with methanol and deionized water for 5 times respectively, and then placed in a vacuum drying oven at 50° C. for 8 hours to obtain a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material III.
[0108] The transmission electron microscope TEM images of zirconium-based metal organic framework-supported cobalt ferrite magnetic phosphorus removal materials Ⅰ and Ⅱ are similar Figure 1 As shown, the XPS patterns of the zirconium-based metal organic framework-supported cobalt ferrite magnetic phosphorus removal materials Ⅰ and Ⅱ are similar Figure 2 As shown in Figure 2, the hysteresis curves of the zirconium-based metal organic framework-supported cobalt ferrite magnetic phosphorus removal materials I and II are similar Figure 3 shown.
[0109] Take 100 mL of phosphorus-contaminated aqueous solution containing phosphate (50 mg / L) and glyphosate (50 mg / L), add 0.1 g of the phosphorus removal material prepared in Example 3, adjust the pH to 3, add PAA (concentration of 0.3 mmol / L), place it in a constant temperature oscillator for 60 minutes of oscillation reaction, and the oscillator temperature and speed are 25°C and 180 r / min, respectively.
[0110] The wastewater after the reaction was filtered with a water filter membrane with a pore size of 0.45 μm; the concentrations of glyphosate and total phosphorus in the supernatant were determined, and the results showed that the glyphosate removal rate could reach 88.6%; the total phosphorus removal rate could reach 89.3%. Glyphosate and total phosphorus were determined by liquid chromatography and ammonium molybdate spectrophotometry, respectively.
[0111] Comparative Example 1:
[0112] The same steps as in Example 1 were used to prepare CoFe 2 O 4 The magnetic nanoparticles are different from those in Example 1 in that the magnetic nanoparticles are not loaded on the surface of MOF-808. The other steps are the same, and then the steps in Example 1 are followed to remove glyphosate and phosphate from water.
[0113] Comparative Example 2:
[0114] The metal organic framework MOF-808 was prepared by the same steps as in Example 1, except that CoFe was not loaded. 2 O 4 Magnetic nanoparticles, other steps are the same, and then the steps of Example 1 are followed to remove glyphosate and phosphate in water.
[0115] Comparative Examples
[0116] The removal rates of glyphosate and total phosphorus by the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal materials prepared in Examples 1 to 3 and the products obtained in Comparative Examples 1 to 2 are summarized as follows, as shown in Table 1 below:
[0117] Table 1. Comparison of phosphorus removal effects of different phosphorus removal materials in the present invention
[0118] Material Glyphosate removal rate (%) Total phosphorus removal rate (%) Example 1 95.7 91.2 Example 2 96.1 93.4 Example 3 93.6 89.3 <![CDATA[Comparative Example 1 CoFe 2 O 4 > 85.2 66.3 Comparative Example 2MOF-808 78.4 54.9
[0119] It can be seen from the removal rates of Example 1 and Comparative Example 1 in Table 1 that, on the basis of Comparative Example 1, Example 1 also has a Zr-based metal organic framework material, which can enhance the removal effect of the composite material on inorganic phosphorus produced after oxidative degradation reaction, thereby improving the removal rate of total phosphorus.
[0120] It can be seen from the removal rates of Example 1 and Comparative Example 2 in Table 1 that on the basis of Comparative Example 2, Example 1 also loaded CoFe 2O 4 , which can significantly enhance the catalytic activity of the composite material and improve the degradation efficiency of glyphosate.
[0121] The present invention firstly uses a solvothermal method to convert FeCl 3 6H 2 O and CoCl 2 6H 2 O reaction to obtain spinel cobalt ferrite CoFe 2 O 4 Nanoparticles, then ZrOCl 2 8H 2 O and trimesic acid were used to synthesize the zirconium-based metal organic framework MOF-808, and finally the magnetic nanoparticles were loaded on the zirconium-based metal organic framework MOF-808 to prepare MOF-808 / CoFe 2 O 4 Phosphorus removal material. The magnetic phosphorus removal material prepared by the present invention can selectively capture inorganic phosphorus in water through the complexation of metal zirconium and phosphate, and can also activate peracetic acid (PAA) to degrade the new pollutant glyphosate in water, while in situ adsorbing the generated phosphate. In addition, the phosphorus removal material has magnetism and is easy to separate and recycle from the solution. The zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material provided by the present invention has excellent adsorption performance and catalytic activity, and can be used for the efficient removal of polymorphic phosphorus in water.
[0122] Compared with the prior art, the present invention has the following beneficial effects:
[0123] 1. The phosphorus removal material has both adsorption and catalytic functions, which can adsorb phosphates in water and catalytically degrade organic phosphorus;
[0124] 2. The phosphorus removal material has a certain magnetic property, which makes it easy to separate from water and shows excellent recyclability;
[0125] 3. MOF-808 contains Zr-OH groups with high affinity for phosphate groups, which can efficiently adsorb inorganic phosphorus produced by degradation reactions to avoid secondary pollution.
[0126] Therefore, the present invention comprises the following steps: 2 O 4 Nanoparticles and Zr 6 O 4 (OH) 4The metal organic framework MOF-808 with clusters as nodes is combined to obtain a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material. The magnetic composite material prepared by the present invention can not only efficiently adsorb phosphate in water, but also effectively activate PAA, degrade the organophosphorus pesticide glyphosate in water, and at the same time in situ adsorb inorganic phosphorus produced by the reaction. In addition, the phosphorus removal material has magnetic properties and is easy to separate solids and liquids for recycling.
[0127] In summary, the zirconium-based metal-organic framework supported cobalt ferrite magnetic phosphorus removal material prepared by the preparation method of the zirconium-based metal-organic framework supported cobalt ferrite magnetic phosphorus removal material of the present invention can remove phosphate and activate peracetic acid to degrade glyphosate, while adsorbing the generated phosphate, thereby achieving efficient removal of polymorphic phosphorus in water, and is suitable for large-scale promotion and application.
[0128] In this specification, the present invention has been described with reference to specific embodiments thereof. However, it is apparent that various modifications and variations may be made without departing from the spirit and scope of the present invention. Therefore, the description should be regarded as illustrative rather than restrictive.
Claims
1. A method for preparing a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material, characterized in that: The spinel cobalt ferrite CoFe2O4 nanoparticles are loaded on the zirconium-based metal organic framework MOF-808 to prepare the MOF-808 / CoFe2O4 dephosphorization material, and the MOF-808 / CoFe2O4 dephosphorization material is the zirconium-based metal organic framework supported cobalt ferrite magnetic dephosphorization material.
2. The method for preparing the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to claim 1, characterized in that: The step of loading spinel cobalt ferrite CoFe2O4 nanoparticles on zirconium-based metal organic framework MOF-808 specifically includes: (1) adding the spinel cobalt ferrite CoFe2O4 nanoparticles, the zirconium-based metal organic framework MOF-808 and trisodium citrate into deionized water, and reacting them at high temperature after ultrasonic stirring to obtain a reaction product; (2) The reaction product is subjected to magnetic separation, washing and drying to obtain the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material.
3. The method for preparing the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to claim 2, characterized in that: In the step (1), the ratio of the spinel cobalt ferrite CoFe2O4 nanoparticles, the zirconium-based metal organic framework MOF-808, the trisodium citrate and the deionized water is 20mg-30mg: 50mg-60mg: 100mg-150mg: 50mL-80mL; the ultrasonic stirring time is 30min; the temperature of the high temperature reaction is 100°C-150°C, and the high temperature reaction time is 2h-4h.
4. The method for preparing the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to claim 1, characterized in that: The spinel cobalt ferrite CoFe2O4 nanoparticles are prepared by the following steps: (A1) adding FeCl3·6H2O and CoCl2·6H2O into ethylene glycol and stirring with ultrasonic to obtain a precursor solution; (A2) adding anhydrous sodium acetate and polyethylene glycol to the precursor solution to obtain a mixed solution, and reacting the mixed solution under high temperature and high pressure to obtain a reaction product; (A3) The reaction product is subjected to magnetic separation, washing and drying to obtain the spinel cobalt ferrite CoFe2O4 nanoparticles.
5. The method for preparing the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to claim 4, characterized in that: In the step (A1), the ratio of the FeCl3·6H2O, the CoCl2·6H2O and the ethylene glycol is 50mmol-100mmol:25mmol-50mmol:1L; the ultrasonic stirring time is 30min; or, in the step (A2), the ratio of the anhydrous sodium acetate, the polyethylene glycol and the FeCl3·6H2O is 200mmol-300mmol:6g-15g:50mmol; the step of reacting the mixed solution under high temperature and high pressure specifically comprises: sealing the mixed solution in an autoclave, then placing the autoclave in an oven, and reacting at 180°C-200°C for 18h-20h.
6. The method for preparing the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to claim 1, characterized in that: The zirconium-based metal organic framework MOF-808 is prepared by the following steps: (B1) adding ZrOCl2·8H2O to a precursor solution consisting of deionized water, trimesic acid, acetic acid and concentrated hydrochloric acid, and heating and stirring to obtain a reaction product; (B2) Soaking the reaction product in ethanol and then drying it to obtain the zirconium-based metal organic framework MOF-808.
7. The method for preparing the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to claim 6, characterized in that: In the step (B1), the ratio of the ZrOCl2·8H2O to the trimesic acid is 30mmol-90mmol:10mmol-30mmol, the ratio of the acetic acid, the deionized water, the concentrated hydrochloric acid and the trimesic acid is 0.3L-0.6L:0.3L-0.6L:3mL-6mL:10mmol-30mmol; and the temperature of the heating and stirring is 100°C-120°C.
8. A zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material, characterized in that: The material is prepared by the method for preparing a zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to any one of claims 1 to 7.
9. Use of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to claim 8 in removing phosphorus from water or activating peracetic acid.
10. Use of the zirconium-based metal organic framework supported cobalt ferrite magnetic phosphorus removal material according to claim 8 in removing phosphate and glyphosate from water.
Citation Information
Patent Citations
Preparation method of modified zirconium-based metal-organic framework material MOF-808
CN113368824A
Method for degrading and detecting organophosphorus pesticide by using Fe-CDs and MOF-808 composite material
CN113736095A
Method for degrading carbamazepine by activating peracetic acid with carbon nanotube supported catalyst
CN116002842A
Method for treating antibiotics in water body through advanced oxidation method of activating peracetic acid by cobalt ferrite
CN117263359A
Ferromagnetic metal particles and preparation process thereof
US5188898A
Cited By
Preparation method of zirconium-cobalt bimetal phthalocyanine and application of zirconium-cobalt bimetal phthalocyanine in degradation of glyphosate in water body
CN120094648A