Metal composite modified perovskite type zirconium oxide catalyst as well as preparation method and application thereof
By doping La and Cr elements into the zirconia catalyst, the perovskite zirconia catalyst is formed, which solves the problem of poor catalytic effect of traditional zirconia catalysts, improves the CO conversion rate and isobutene selectivity, and achieves a stable and economical Catalytic effect.
Patent Information
- Application Number
- CN202411051616.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The catalytic effect of zirconia catalysts prepared by traditional hydrothermal method is poor, and the CO conversion and isobutene selectivity are low.
By doping La and Cr elements in ZrO2, a metal composite modified perovskite zirconium oxide catalyst is formed, increasing the number of oxygen vacancies of the catalyst, and providing an alkaline environment and a redox reaction of the acid oxide CrO3 through alkaline liquid. Improve the redox performance and CO conversion rate of the catalyst.
It significantly improves the CO conversion rate and isobutene selectivity, has stable chemical properties, simple process, low cost, and is suitable for industrial production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthesis gas chemical industry and catalyst preparation, and specifically relates to a metal composite modified perovskite type zirconium oxide catalyst and a preparation method and application thereof. Background Art
[0002] Low-carbon olefins mainly include ethylene, propylene and butene, which are important basic chemical raw materials and are widely used in synthetic plastics, fibers, rubber and other fields. Ethylene can be used in the synthesis of polyethylene, polyvinyl chloride and other fields, and propylene is mainly used to prepare acrylonitrile and synthetic rubber. Isobutylene (i-C4 = ) has a wide range of uses. The methyl tert-butyl ether prepared by its reaction with methanol is a good gasoline additive and anti-knock agent. At the same time, high-purity isobutylene can be used as a polymerization monomer or intermediate to prepare fine chemicals such as butyl rubber, polyisobutylene, and methyl methacrylate. However, the traditional method for preparing isobutylene mainly relies on the C4 product of petroleum cracking, which has high separation costs and cannot meet industrial needs. With the expansion of the isobutylene market demand and the contradiction between petroleum resources, exploring clean, efficient, and low-cost isobutylene preparation processes has gradually become a hot topic of increasing concern.
[0003] Synthesis gas is mainly composed of CO and H2, and can be produced from non-petroleum carbon resources such as coal, natural gas and biomass. Synthesis gas can be highly selectively converted into isobutylene and isobutane under the action of a catalyst, a process called isomerization reaction. This route alleviates the dependence of traditional methods for preparing isobutylene on petroleum resources to a certain extent, and constructs a feasible energy development route with simple process. It is currently believed that the isomerization reaction achieves chain growth through CO insertion reaction and condensation reaction, promoting the formation of branched C4 products.
[0004] ZrO2 has the properties of high melting point, high hardness, high resistivity and low thermal expansion coefficient, and is widely used in the fields of glass industry, refractory materials and inorganic coatings. ZrO2 has a variety of phase structures and is rich in oxygen vacancies and acid-base sites. Among them, oxygen vacancies are the active sites for the formation of methoxy intermediates between CO and the surface of ZrO2. At the same time, oxygen vacancies and acidic sites jointly promote the condensation reaction in the isomerization reaction, which is beneficial to improve the CO conversion rate. The basic sites in the ZrO2 catalyst can enhance the CO insertion reaction, which is beneficial to improve the selectivity of isobutylene in the product. Therefore, under the joint constraints of oxygen vacancies and acidic and basic sites, the ZrO2 catalyst exhibits good catalytic performance in the CO hydrogenation isomerization reaction and is considered to be one of the most promising materials in the 21st century.
[0005] However, the catalytic effect of the zirconium oxide catalyst prepared by the traditional hydrothermal method is poor, and there are problems of low CO conversion rate and isobutylene selectivity. Based on this, the present application is proposed. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects of the prior art and provide a metal composite modified perovskite type zirconium oxide catalyst and its preparation method and application, which effectively solves the problems of poor catalytic effect of traditionally prepared zirconium oxide, low CO conversion rate and isobutylene selectivity.
[0007] The present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a metal composite modified perovskite type zirconium oxide catalyst, comprising the following steps:
[0009] (1) mixing a soluble zirconium salt, citric acid and deionized water in a certain proportion to obtain a mixed solution A;
[0010] (2) adding alkali solution dropwise into mixed solution A to obtain mixed solution B;
[0011] (3) placing the mixed solution B in a water bath and stirring at a constant temperature until it becomes a transparent gel, cooling the gel to room temperature, and drying to obtain a precursor C;
[0012] (4) calcining the precursor C to obtain ZrO2 powder;
[0013] (5) ZrO2 powder is dissolved in deionized water to obtain a solution, and appropriate amounts of La(NO3)3·6H2O and CrO3 are poured into the solution and stirred, followed by drying and calcining to obtain a metal composite modified perovskite-type zirconium oxide catalyst.
[0014] The oxygen vacancy content in the zirconium oxide catalyst prepared by the traditional hydrothermal method is relatively low. Considering the influence of the oxygen vacancy content on the isomerization reaction, the present invention doped La and Cr elements in ZrO2, resulting in lattice distortion of the catalyst, which promoted the lattice energy of the perovskite catalyst to increase, and at the same time, the lattice oxygen was activated and migrated to the crystal surface, increasing the number of oxygen vacancies in the catalyst. In addition, the alkaline environment provided by the alkali solution is conducive to improving the selectivity of isobutylene in the product, but excessive alkaline conditions are not conducive to improving the CO conversion rate. The acidic CrO3 can react with the alkali solution, and the acidic oxide CrO3 undergoes a redox reaction under alkaline conditions, which can improve the redox performance of the catalyst. At the same time, the alkalinity in the preparation process can be appropriately adjusted, which is conducive to improving the CO conversion rate and isobutylene selectivity.
[0015] Furthermore, in step (1), the soluble zirconium salt is any one of zirconium sulfate, zirconium acetate or zirconium nitrate pentahydrate.
[0016] Furthermore, in step (1), the ratio of the soluble zirconium salt, citric acid and deionized water is (8-10) g: (5-10) g: (60-90) mL.
[0017] Furthermore, in step (2), the solute in the alkali solution is any one of sodium hydroxide, potassium hydroxide, and calcium hydroxide.
[0018] Furthermore, in step (2), the ratio of the solute to the deionized water in the alkali solution is (5-10) g: (20-50) mL.
[0019] Furthermore, in step (2), the ratio of the solute to the deionized water in the alkali solution is (5-10) g: (20-50) mL.
[0020] Furthermore, in step (3), the stirring temperature of the mixed solution B in a water bath is preferably 80 to 120°C.
[0021] Furthermore, in step (3), the transparent gel-like substance is placed in an oven for drying, and the oven temperature is controlled to be 60-100° C. and the drying time is 9-20 hours.
[0022] Furthermore, in step (4), the precursor C is placed in a muffle furnace and calcined at 400-500° C. in an air atmosphere for 3-6 hours. The purpose of calcination is to convert the precursor C into ZrO2, and the particle size of the ZrO2 powder is 30-80 nm.
[0023] Furthermore, in step (5), the molar ratio of La(NO3)3·6H2O and CrO3 to ZrO2 powder is 1:1:(20-200).
[0024] Furthermore, in step (5), the stirring time is 20-40 min.
[0025] The second object of the present invention is to provide a metal composite modified perovskite-type zirconium oxide catalyst prepared by the above preparation method.
[0026] The third object of the present invention is to provide the use of the metal composite modified perovskite-type zirconium oxide catalyst prepared above in catalyzing CO hydrogenation isomerization synthesis reaction.
[0027] The preparation method of the metal composite modified perovskite type zirconium oxide catalyst of the present invention can simultaneously improve the CO conversion rate and the selectivity of isobutylene. The mechanism is as follows:
[0028] ZrO2 interacts with CO to form formate species and methoxyl groups, wherein the site for generating methoxyl groups is considered to be an oxygen vacancy. Formate can form methoxyl groups by hydrogenation. Methoxyl groups combine with water to generate methanol, and achieve chain growth through aldehyde condensation, ultimately forming 2-methylpropanal. 2-methylpropanal forms isobutylene by hydrogenation or dehydration. However, the oxygen vacancy content on the surface of the ZrO2 catalyst not doped with lanthanide metals is low, the number of methoxyl intermediates generated is small, and its CO conversion rate is low. The metal composite modified perovskite zirconium oxide catalyst of the present invention promotes the content of oxygen vacancies, forms methoxyl intermediates in the isomerization reaction, and improves the CO conversion rate and isobutylene selectivity. At the same time, the added CrO3 is an acidic oxide that can properly neutralize the alkali solution in the raw material, and undergoes a reduction reaction to become +4 valence, which promotes the increase of the oxygen vacancy content. Along with the improvement of the redox property of the catalyst, CO forms methoxyl intermediates with the hydroxyl groups on the surface of ZrO2, and achieves chain growth through CO insertion and condensation reaction, further promoting the progress of the isomerization reaction.
[0029] The present invention has the following beneficial effects:
[0030] 1. The metal composite modified perovskite-type zirconia catalyst prepared by the present invention effectively solves the problem of low CO conversion rate in isomerization synthesis reaction. The introduction of La and Cr elements causes the lattice to be distorted, increases the migration capacity of lattice oxygen, and the formation of a large number of oxygen vacancies is conducive to improving the redox property of the catalyst;
[0031] 2. The present invention adds alkaline solution as a precipitant, which is beneficial to improving the yield of the catalyst precursor, and the alkaline environment constructed is also beneficial to improving the selectivity of isobutylene;
[0032] 3. The metal composite modified perovskite-type zirconia catalyst prepared by the present invention has stable chemical properties, simple process, low cost and is suitable for industrial production. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The embodiment of the present invention provides a method for preparing a metal composite modified perovskite type zirconium oxide catalyst, comprising the following steps:
[0035] (1) mixing a soluble zirconium salt, citric acid and deionized water in a certain proportion to obtain a mixed solution A;
[0036] (2) adding alkali solution dropwise into mixed solution A to obtain mixed solution B;
[0037] (3) placing the mixed solution B in a water bath and stirring at a constant temperature until it becomes a transparent gel, cooling the gel to room temperature, and drying to obtain a precursor C;
[0038] (4) calcining the precursor C to obtain ZrO2 powder;
[0039] (5) ZrO2 powder is dissolved in deionized water to obtain a solution, and appropriate amounts of La(NO3)3·6H2O and CrO3 are poured into the solution and stirred, followed by drying and calcining to obtain a metal composite modified perovskite-type zirconium oxide catalyst.
[0040] The lanthanide metal La and the acidic metal oxide CrO3 are introduced into the ZrO2 catalyst to form a perovskite catalyst. The catalyst satisfies the perovskite structure formed by the combination of rare earth metals and transition metals in the traditional sense, and the structure is conducive to weakening the metal-oxygen bond inside the catalyst. The introduction of the two metals causes the lattice to be distorted, increases the mobility of lattice oxygen, and is conducive to oxygen loading and storage. The perovskite structure of LaCrZrOz is conducive to electron conduction and provides abundant adsorption sites for CO. At the same time, the added CrO3 is an acidic oxide that can properly neutralize the alkali solution in the raw material, and undergoes a reduction reaction to become +4 valence, which promotes the increase of oxygen vacancy content. With the improvement of the redox property of the catalyst, CO forms a methoxy intermediate with the hydroxyl group on the surface of ZrO2, and achieves chain growth through CO insertion and condensation reaction, further promoting the isomerization reaction.
[0041] The oxygen vacancy content in the zirconium oxide catalyst prepared by the traditional hydrothermal method is relatively low. Considering the influence of the oxygen vacancy content on the isomerization reaction, the present invention doped La and Cr elements in ZrO2, resulting in lattice distortion of the catalyst, which promoted the lattice energy of the perovskite catalyst to increase, and at the same time, the lattice oxygen was activated and migrated to the crystal surface, increasing the number of oxygen vacancies in the catalyst. In addition, the alkaline environment provided by the alkali solution is conducive to improving the selectivity of isobutylene in the product, but excessive alkaline conditions are not conducive to improving the CO conversion rate. The acidic CrO3 can react with the alkali solution, and the acidic oxide CrO3 undergoes a redox reaction under alkaline conditions, which can improve the redox performance of the catalyst. At the same time, the alkalinity in the preparation process can be appropriately adjusted, which is conducive to improving the CO conversion rate and isobutylene selectivity.
[0042] Compared with the ZrO2 catalyst prepared by the traditional hydrothermal method, the catalyst prepared by the sol-gel method of the present invention has a larger specific surface area and the number of active sites, and can improve the CO conversion rate and isobutylene selectivity.
[0043] The present invention will be further described below by means of specific examples.
[0044] Example 1
[0045] The preparation method of the metal composite modified perovskite type zirconium oxide catalyst in this example specifically comprises the following steps:
[0046] (1) Preparation of soluble nitrate mixed solution A: Weigh 9.22 g of zirconium nitrate pentahydrate (Zr(NO3)4·5H2O) and 6.64 g of citric acid (C6H8O7), dissolve them in 100 mL of deionized water at 600 rad / min, and mechanically stir for 20 min to obtain mixed solution A.
[0047] (2) Preparation of mixed solution B: Weigh 3 g of sodium hydroxide (NaOH) and dissolve it in 30 mL of deionized water. Add the prepared alkali solution drop by drop into mixed solution A at 400 rad / min until the pH of mixed solution A reaches 10. Stir continuously at 400 rad / min for 30 min to obtain mixed solution B.
[0048] (3) Place the mixed solution B obtained in step (2) in a 100°C water bath and continue stirring at 400 rad / min until it becomes a transparent gel. Place the gel in an oven at 80°C and dry for 12 hours to obtain a ZrO2 precursor C.
[0049] (4) The precursor obtained in step (3) is placed in a muffle furnace and calcined at 450° C. for 4 h in an air atmosphere to obtain white ZrO2 powder.
[0050] (5) The ZrO2 powder obtained in step (4) was stirred and dissolved in 30 mL of deionized water, and La(NO3)3·6H2O and CrO3 powder were added to the solution (the molar ratio of La(NO3)3·6H2O and CrO3 powder to ZrO2 powder was 1:1:20), and the mixture was stirred for 30 min at 500 rad / min to obtain a mixed solution D. The obtained mixed solution D was placed in an oven at 80°C and dried for 12 h, and the dried solid was placed in a muffle furnace and calcined at 450°C for 4 h in an air atmosphere to obtain a product, which was recorded as LaCrZr 20 O z .
[0051] Example 2
[0052] The preparation method of the metal composite modified perovskite type zirconium oxide catalyst in this example is basically the same as that in Example 1, except that La(NO3)3·6H2O and CrO3 powder are added in step (5), and the molar ratio of La(NO3)3·6H2O and CrO3 powder to ZrO2 powder is 1:1:50. Therefore, the metal composite modified perovskite type zirconium oxide catalyst prepared in this example is marked as LaCrZr 50 O z .
[0053] Example 3
[0054] The preparation method of the metal composite modified perovskite type zirconium oxide catalyst in this example is basically the same as that in Example 1, except that La(NO3)3·6H2O and CrO3 powder are added in step (5), and the molar ratio of La(NO3)3·6H2O and CrO3 powder to ZrO2 powder is 1:1:100. Therefore, the metal composite modified perovskite type zirconium oxide catalyst prepared in this example is marked as LaCrZr 100 O z .
[0055] Example 4
[0056] The preparation method of the metal composite modified perovskite type zirconium oxide catalyst in this example is basically the same as that in Example 1, except that La(NO3)3·6H2O and CrO3 powder are added in step (5), and the molar ratio of La(NO3)3·6H2O and CrO3 powder to ZrO2 powder is 1:1:200. Therefore, the metal composite modified perovskite type zirconium oxide catalyst prepared in this example is marked as LaCrZr 200 O z .
[0057] Comparative Example 1
[0058] The method for preparing the zirconium oxide catalyst in this example specifically comprises the following steps:
[0059] (1) Preparation of soluble nitrate mixed solution A: Weigh 9.22 g of zirconium nitrate pentahydrate (Zr(NO3)4·5H2O) and 6.64 g of citric acid (C6H8O7), dissolve them in 100 mL of deionized water at 600 rad / min, and mechanically stir for 20 min to obtain mixed solution A.
[0060] (2) Preparation of mixed solution B: Weigh 3 g of sodium hydroxide (NaOH) and dissolve it in 30 mL of deionized water. Add the prepared alkali solution drop by drop into mixed solution A at 400 rad / min until the pH of mixed solution A reaches 10. Stir continuously at 400 rad / min for 30 min to obtain mixed solution B.
[0061] (3) Place the mixed solution B obtained in step (2) in a 100°C water bath and continue stirring at 400 rad / min until it becomes a transparent gel. Place the gel in an oven at 80°C and dry for 12 hours to obtain a ZrO2 precursor C.
[0062] (4) The precursor obtained in step (3) is placed in a muffle furnace and calcined at 450° C. for 4 h in an air atmosphere to obtain a white ZrO2 powder, which is a zirconium oxide catalyst.
[0063] Comparative Example 2
[0064] The preparation method of the metal-modified zirconium oxide catalyst in this example specifically comprises the following steps:
[0065] (1) Preparation of soluble nitrate mixed solution A: Weigh 9.22 g of zirconium nitrate pentahydrate (Zr(NO3)4·5H2O) and 6.64 g of citric acid (C6H8O7), dissolve them in 100 mL of deionized water at 600 rad / min, and mechanically stir for 20 min to obtain mixed solution A.
[0066] (2) Preparation of mixed solution B: Weigh 3 g of sodium hydroxide (NaOH) and dissolve it in 30 mL of deionized water. Add the prepared alkali solution drop by drop into mixed solution A at 400 rad / min until the pH of mixed solution A reaches 10. Stir continuously at 400 rad / min for 30 min to obtain mixed solution B.
[0067] (3) Place the mixed solution B obtained in step (2) in a 100°C water bath and continue stirring at 400 rad / min until it becomes a transparent gel. Place the gel in an oven at 80°C and dry for 12 hours to obtain a ZrO2 precursor C.
[0068] (4) The precursor obtained in step (3) is placed in a muffle furnace and calcined at 450° C. for 4 h in an air atmosphere to obtain white ZrO2 powder.
[0069] (5) The ZrO2 powder obtained in step (4) was stirred and dissolved in 30 mL of deionized water, and La(NO3)3·6H2O powder was added to the solution (the molar ratio of La(NO3)3·6H2O to ZrO2 powder was 1:20), and the mixture was stirred for 30 min at 500 rad / min to obtain a mixed solution. The obtained mixed solution was placed in an oven at 80°C and dried for 12 h, and the dried solid was placed in a muffle furnace and calcined at 450°C for 4 h in an air atmosphere to obtain a product, which was recorded as LaZr 20 O z .
[0070] The catalyst performance tests and characterizations were performed on the catalysts prepared in the above Examples 1 to 4 and Comparative Examples 1 to 2:
[0071] When evaluating the performance of the catalyst, in order to make the catalyst particles uniform in size and not to block the reaction tube, the catalysts prepared in the above Examples 1 to 4 and Comparative Examples 1 to 2 of the present invention should be made into catalyst particles of 20 to 40 meshes.
[0072] The catalysts prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were evaluated in a micro fixed reactor. The process conditions were: 0.5 to 3 mL of 20 to 50 mesh catalyst, 300 to 500° C. reaction temperature, 0.5 to 5 MPa reaction pressure, H2 / CO as feed gas = 1 or 2, and a space velocity of 500 to 5000·h -1 .
[0073] For example, the LaCr prepared in Example 1 was subjected to 20 ZrO z The performance of the catalyst was evaluated. The specific operation steps were as follows: 1 mL of the perovskite-type zirconium oxide catalyst prepared in Example 2 was weighed and loaded into the constant temperature zone in the middle of the reaction tube. The raw gas was H2 / CO=2, the temperature was 400°C, the pressure was 3 MPa, and the space velocity (GHSV) was 700 h -1 After reaching a stable state, sampling and analysis were carried out at intervals of 3 hours. Gas chromatography was used to perform quantitative and qualitative analysis on the raw gas and products. The CO conversion rate and the selectivity of each component were calculated using the methane correlation method of "Determination and gas chromatography of H2, N2, CO, CO2 and C1-C8 hydrocarbons in coal-based Fischer-Tropsch synthesis tail gas". The specific results are shown in Table 1.
[0074] Table 1 Comparison of process parameters and performance test results of CO-adding hydrogenation isomerization reaction of catalysts prepared in Examples 1 to 4 and Comparative Examples 1 to 2
[0075]
[0076] It can be seen from Table 1 that in the distribution of hydrogenation products of the metal composite modified perovskite zirconia catalyst, the CO2 selectivity is maintained at about 50%. Compared with the perovskite catalyst prepared by the traditional hydrothermal method, the LaCrZrO prepared by the sol-gel method in this method is z The catalyst powder particle size is smaller, which is conducive to the dispersion of active components. Compared with unmodified ZrO2, metal composite modified LaZr 20 O z and LaCrZrO z CO conversion rate of catalyst and i-C4 = The selectivity ratio has been improved. Compared with LaZr, which only introduces La element 20 O z Compared with the catalysts, the catalytic performance of the series of catalysts introduced with CrO3 is more obvious. = The significant improvement in selectivity is attributed to the lattice distortion of the catalyst formed by the doping of La and Cr. In addition, CrO3 undergoes a redox reaction with the alkali solution in the raw material, which makes the oxygen atom mobility higher. The more abundant oxygen vacancies inside the catalyst are conducive to the formation of methoxy intermediates, which promotes the isomerization reaction and increases the i-C4 = The acidic oxide CrO3 reacts with the alkali solution in the raw material to neutralize. Therefore, the pH value of the solution can be adjusted during the catalyst preparation process by changing the CrO3 content. The design has both high CO conversion rate and high i-C4 = Selective reaction conditions.
[0077] Four composite modified ZrO2 catalysts with different La(NO3)3·6H2O and CrO3 contents were compared, among which LaCrZr 100 The Oz catalyst has the best catalytic effect, with a selectivity of 80.2% for low-carbon olefins, 65.4% for isobutylene, and an olefin-to-alkane ratio (O / P) of 10.8. This indicates that the introduction of appropriate amounts of La(NO3)3·6H2O and CrO3 causes the catalyst lattice to distort, which is beneficial to increasing the oxygen vacancy content of the catalyst. The increase in the number of oxygen vacancies is beneficial to the interaction between CO and the catalyst surface to generate more methoxy intermediates, which is beneficial to improving the CO conversion rate and i-C4 = Moreover, the acidic oxide CrO3 undergoes redox reaction under alkaline conditions, which increases the oxygen vacancy content of the catalyst and can also appropriately adjust the pH value of the catalyst, thus maintaining a high CO conversion rate while having a high i-C4 = Selective.
[0078] The metal composite modified perovskite-type zirconia catalyst prepared by the present invention effectively solves the problem of low CO conversion rate in isomerization synthesis reaction. The introduction of La and Cr elements causes the lattice to be distorted, increases the migration capacity of lattice oxygen, and the formation of a large number of oxygen vacancies is beneficial to improving the redox property of the catalyst.
[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a metal composite modified perovskite-type zirconium oxide catalyst, characterized in that: The following steps are involved: (1) mixing a soluble zirconium salt, citric acid and deionized water in a certain proportion to obtain a mixed solution A; (2) adding alkali solution dropwise into mixed solution A to obtain mixed solution B; (3) placing the mixed solution B in a water bath and stirring at a constant temperature until it becomes a transparent gel, cooling the gel to room temperature, and drying to obtain a precursor C; (4) calcining the precursor C to obtain ZrO2 powder; (5) ZrO2 powder is dissolved in deionized water to obtain a solution, and appropriate amounts of La(NO3)3·6H2O and CrO3 are poured into the solution and stirred, followed by drying and calcining to obtain a metal composite modified perovskite-type zirconium oxide catalyst.
2. The method for preparing the metal composite modified perovskite type zirconium oxide catalyst according to claim 1, characterized in that: In step (1), the soluble zirconium salt is any one of zirconium sulfate, zirconium acetate or zirconium nitrate pentahydrate.
3. The method for preparing the metal composite modified perovskite type zirconium oxide catalyst according to claim 1, characterized in that: In step (1), the ratio of the soluble zirconium salt, citric acid and deionized water is (8-10) g: (5-10) g: (60-90) mL.
4. The method for preparing the metal composite modified perovskite type zirconium oxide catalyst according to claim 1, characterized in that: In step (2), the solute in the alkali solution is any one of sodium hydroxide, potassium hydroxide and calcium hydroxide.
5. The method for preparing the metal composite modified perovskite type zirconium oxide catalyst according to claim 1, characterized in that: In step (2), the ratio of solute to deionized water in the alkali solution is (5-10) g: (20-50) mL.
6. The method for preparing the metal composite modified perovskite type zirconium oxide catalyst according to claim 1, characterized in that: In step (2), the alkali solution is added dropwise to the mixed solution A to control the pH value of the mixed solution B to be 8-10.
7. The method for preparing the metal composite modified perovskite type zirconium oxide catalyst according to claim 1, characterized in that: In step (4), the precursor C is calcined at 400-500° C. in an air atmosphere for 3-6 hours.
8. The method for preparing the metal composite modified perovskite type zirconium oxide catalyst according to claim 1, characterized in that: In step (5), the molar ratio of La(NO3)3·6H2O and CrO3 to ZrO2 powder is 1:1:(20-200).
9. A metal composite modified perovskite type zirconium oxide catalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the metal composite modified perovskite type zirconium oxide catalyst according to claim 9 in catalyzing CO hydrogenation isomerization synthesis reaction.
Citation Information
Patent Citations
Process for the conversion of syngas to oxygenates
CN101646641A
Core-shell type catalyst for directional catalytic conversion of biomass synthesis gas, and preparation of core-shell type catalyst
CN108906070A
Reaction catalyst for converting isoparaffin into n-alkane and preparation method thereof
CN111569861A
Metal composite modified nano zirconium oxide catalyst as well as preparation method and application thereof
CN111644169A
Preparation method and application of Gd-modified nano-zirconia catalyst
CN116272951A