Titanium-copper composite photocatalyst and preparation method thereof
Preparation of titanium-copper composite photocatalysts by one-step hydrothermal method solves the high cost and low efficiency of precious metal cocatalysts in traditional photocatalyst technology, and achieves efficient and stable photocatalytic hydrogen production performance, which is suitable for solar energy conversion and clean energy fields. .
Patent Information
- Application Number
- CN202411037166.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The use of precious metal cocatalysts in traditional photocatalytic hydrogen production technology leads to high costs, environmental pollution and low light utilization efficiency. The catalyst structure and composition limit the effective separation and migration of photogenerated carriers, resulting in low photocatalytic efficiency.
A one-step hydrothermal method is used to prepare titanium-copper composite photocatalyst. By magnetic stirring, urea and copper chloride are added to deionized water, titanium tetrachloride is added slowly, and hydrothermal treatment is carried out to form a titanium-copper composite photocatalyst with excellent performance, simplifying Preparation process, reduce production costs, and achieve large-scale production.
Without the use of precious metal cocatalysts, the titanium-copper composite photocatalyst exhibits excellent photocatalytic hydrogen production performance, up to 64mmol/g/h, and has excellent stability, and has no significant decline in performance for 30 hours. It is suitable for solar energy Convert and clean energy production.
Smart Images

Figure CN118976491A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photocatalysts, and in particular to a titanium-copper composite photocatalyst and a preparation method thereof. Background Art
[0002] In traditional photocatalytic hydrogen production technology, precious metals such as platinum (Pt), palladium (Pd) or gold (Au) are usually used as co-catalysts to improve the photocatalytic efficiency. Although these precious metal co-catalysts can significantly improve the photocatalytic activity, their high cost and scarcity limit the widespread application and commercialization of photocatalytic technology. In addition, the mining and refining processes of these precious metals are often accompanied by serious environmental pollution and resource consumption problems. In addition, many existing photocatalytic materials exhibit low light utilization efficiency and catalytic stability in the process of photocatalytic hydrogen production, which is mainly due to the fact that the structure and composition of the catalyst limit the effective separation and migration of photogenerated carriers. These problems lead to low efficiency of photocatalytic hydrogen production and limit its performance in practical applications. Summary of the invention
[0003] In order to overcome the above defects of the prior art, the present invention provides a method for preparing a titanium-copper composite photocatalyst. The preparation method is simple and quick, and a large amount of powder catalyst can be produced in one reactor. It has the advantages of high cost-effectiveness and easy large-scale production.
[0004] The invention provides a method for preparing a titanium-copper composite photocatalyst, which specifically comprises the following steps: adding urea and copper chloride to deionized water in sequence while magnetically stirring, slowly adding a titanium tetrachloride solution dropwise after a primary stirring treatment, then performing a secondary stirring treatment, performing a hydrothermal treatment after the treatment, and obtaining a precipitate by centrifugation after the hydrothermal treatment, performing a drying treatment, and finally obtaining the titanium-copper composite photocatalyst.
[0005] Compared with the prior art, the present invention adopts a one-step hydrothermal method to directly prepare a titanium-copper composite photocatalyst with excellent performance. This method simplifies the preparation process, reduces production costs, and can achieve large-scale production.
[0006] In a possible implementation manner, the molar ratio of Cu:Ti is (0.5-2.5):1.
[0007] Compared with the prior art, the present invention adopts the above-mentioned molar ratio of Cu:Ti because different Cu:Ti ratios will affect the electronic structure of the composite material, thereby affecting the separation efficiency of photogenerated electrons and holes, and further affecting the catalytic activity. Too much or too little copper may cause the catalyst to be structurally unstable during use, affecting its life.
[0008] In a possible implementation manner, the stirring treatment lasts for 5-10 minutes.
[0009] Compared with the prior art, the present invention adopts the above stirring treatment time mainly to ensure that urea and copper chloride can be fully dissolved and evenly dispersed in deionized water during the preparation of the titanium-copper composite photocatalyst.
[0010] In a possible implementation manner, the specific dropwise addition parameters of the titanium tetrachloride are: 100-120 ul is added each time, with an interval of 5-10 seconds between each addition.
[0011] Compared with the prior art, the present invention first uses a magnetic stirrer to dissolve urea and copper chloride in deionized water. The magnetic stirring can ensure that the reactants are fully mixed, accelerate the dissolution process, and keep the solution uniform. Subsequently, the present invention adopts the method of slowly adding titanium tetrachloride solution after the urea and copper chloride are completely dissolved. This dropping method helps to control the reaction rate, avoid violent reaction or local overheating, and is also conducive to generating a more uniform composite material precursor.
[0012] In a possible implementation manner, the secondary stirring treatment lasts for 30 minutes, and the stirring speed is 400-600 r / min.
[0013] Compared with the prior art, the secondary stirring treatment of the present invention adopts a vigorous stirring method, which can further accelerate the uniform dispersion of the reaction mixture, promote sufficient contact and reaction between the reactants, and help form smaller and more uniform particles or a tighter composite structure.
[0014] In a possible implementation, the parameters of the hydrothermal treatment are as follows: temperature is 90° C., and time is 12 h.
[0015] Compared with the prior art, the hydrothermal treatment using the above parameters is beneficial to promoting the in-depth reaction, completing the necessary chemical bonding and structural transformation, and forming the target titanium-copper composite photocatalyst structure.
[0016] In a possible embodiment, the centrifugation is performed 2-3 times.
[0017] In a possible implementation, the temperature of the drying process is 60°C.
[0018] Compared with the prior art, the present invention subsequently removes moisture from the collected precipitate by drying to obtain a dry composite photocatalyst powder. The temperature of the drying treatment used in the present invention can prevent material deterioration or structural damage.
[0019] The second object of the present invention is to provide a titanium-copper composite photocatalyst, which is prepared by the above-mentioned preparation method and has a crystal grain size of ≤30nm.
[0020] Compared with the prior art, the grain size of the titanium-copper composite photocatalyst of the present invention is controlled to be less than 30 nanometers. Such nanometer-scale size helps to increase the specific surface area and light absorption capacity of the photocatalyst, thereby enhancing its photocatalytic activity.
[0021] The titanium-copper composite photocatalyst prepared by the preparation method of the present invention exhibits excellent photocatalytic hydrogen production performance of up to 64 mmol / g / h without the need for precious metal co-catalysts, and has excellent stability. There is no obvious decline in performance after continuous hydrogen production reaction for 30 hours. At the same time, the titanium-copper composite photocatalyst of the present invention has broad application prospects in the fields of solar energy conversion and clean energy production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The hydrogen production efficiency result diagram of the samples prepared in Example 2 and Examples 5-7; Figure 2 The hydrogen production efficiency result diagram of the samples prepared in Examples 2 to 4; Figure 3 XRD characterization diagrams of samples prepared in Examples 1 to 4; Figure 4 XRD characterization diagrams of samples prepared in Example 2 and Examples 5-7; Figure 5 This is a SEM characterization image of CuTi-2 prepared in Example 2; Figure 6 This is the TEM characterization image of CuTi-2 prepared in Example 2. DETAILED DESCRIPTION
[0023] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. It should be noted that the following embodiments are only used to illustrate the implementation method and typical parameters of the present invention, and are not used to limit the parameter range described in the present invention. Reasonable changes derived therefrom are still within the scope of protection of the claims of the present invention.
[0024] It should be noted that the endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.
[0025] Unless otherwise defined, all terms, symbols and other scientific terms used herein are intended to have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. In some cases, terms with conventionally understood meanings are defined herein for the purpose of clarification or ease of reference, and such definitions herein should not be construed as indicating significant differences from conventional understandings in the art. The technical methods described or cited herein are generally well understood by those skilled in the art and are adopted by conventional methods. Unless otherwise stated, the use of commercially available kits, reagents and instruments is carried out in accordance with the protocols and parameters given by the manufacturer.
[0026] The technical effects of the present invention are described below in conjunction with specific embodiments.
[0027] Example 1 The present embodiment provides a titanium-copper composite photocatalyst, which is prepared by the following preparation method: 50-70 mL of deionized water is added to the inner tank of a reactor, 3 g of urea and 1.8 g of copper chloride are added successively under magnetic stirring, and the stirring time is 10 min. When the color of the solution is uniform, 1.2 mL of titanium tetrachloride solution is slowly added dropwise, followed by vigorous stirring for 30 min, and the solution is placed in an oven at 90° C. for 12 h, centrifuged 2 to 3 times, and dried at 60° C. to obtain a titanium-copper composite photocatalyst, which is marked as CuTi-1.
[0028] Example 2 The present embodiment provides a titanium-copper composite photocatalyst, which is prepared by the following preparation method: 50-70 mL of deionized water is added to the inner tank of a reactor, 3 g of urea and 2.4 g of copper chloride are added successively under magnetic stirring, and the stirring time is about 10 min. When the color of the solution is uniform, 1.2 mL of titanium tetrachloride solution is slowly added dropwise, followed by vigorous stirring for 30 min, and the solution is placed in an oven at 90° C. for 12 h, centrifuged 2 to 3 times, and dried at 60° C. to obtain a titanium-copper composite photocatalyst, which is marked as CuTi-2.
[0029] Example 3 The present embodiment provides a titanium-copper composite photocatalyst, which is prepared by the following preparation method: 50-70 mL of deionized water is added to the inner tank of a reactor, 3 g of urea and 3.4 g of copper chloride are added successively under magnetic stirring, and the stirring time is about 10 min. When the color of the solution is uniform, 1.2 mL of titanium tetrachloride solution is slowly added dropwise, followed by vigorous stirring for 30 min, and the solution is placed in an oven at 90° C. for 12 h, centrifuged 2 to 3 times, and dried at 60° C. to obtain a titanium-copper composite photocatalyst, which is marked as CuTi-3.
[0030] Example 4 The present embodiment provides a titanium-copper composite photocatalyst, which is prepared by the following preparation method: 50-70 mL of deionized water is added to the inner tank of a reactor, 3 g of urea and 5.4 g of copper chloride are added successively under magnetic stirring, and the stirring time is about 10 min. When the color of the solution is uniform, 1.2 mL of titanium tetrachloride solution is slowly added dropwise, followed by vigorous stirring for 30 min, and the solution is placed in an oven at 90° C. for 12 h, centrifuged 2 to 3 times, and dried at 60° C. to obtain a titanium-copper composite photocatalyst, which is marked as CuTi-4.
[0031] Example 5 This embodiment provides a titanium-zinc composite photocatalyst, which is prepared by the following preparation method: 50-70 mL of deionized water is added to the inner tank of the reactor, and 3 g of urea, 1.189 g of Zn(NO 3 ) 2 6H 2 O, stirring time is about 10 minutes, wait until the solution color is uniform, slowly add 1.2 mL of titanium tetrachloride solution, then stir vigorously for 30 minutes, place in an oven at 90 ° C for 12 hours, centrifuge 2 to 3 times, and dry at 60 ° C to obtain a titanium-zinc composite photocatalyst, marked as ZnTi.
[0032] Example 6 This embodiment provides a titanium-cerium composite photocatalyst, which is prepared by the following preparation method: 50-70 mL of deionized water is added to the inner tank of the reaction kettle, and 3 g of urea, 8.68 g of Ce(NO 3 ) 3 6H 2 O. Stir for about 10 min, wait until the solution color is uniform, slowly add 1.2 mL of titanium tetrachloride solution, then stir vigorously for 30 min, place in an oven at 90 ° C for 12 h, centrifuge 2 to 3 times, and dry at 60 ° C to obtain a titanium-cerium composite photocatalyst, marked as CeTi.
[0033] Example 7 This embodiment provides a titanium-aluminum composite photocatalyst, which is prepared by the following preparation method: 50-70 mL of deionized water is added to the inner tank of the reaction kettle, and 3 g of urea, 7.5 g of Al(NO 3 ) 3 9H 2 O. Stir for about 10 min, wait until the solution color is uniform, slowly add 1.2 mL of titanium tetrachloride solution, then stir vigorously for 30 min, place in an oven at 90 ° C for 12 h, centrifuge 2 to 3 times, and dry at 60 ° C to obtain a titanium-aluminum composite photocatalyst, marked as AlTi.
[0034] The present invention performs performance tests on the samples obtained in Examples 1 to 7 respectively. Figure 1 The hydrogen production efficiency result diagram of the samples prepared in Example 2 and Examples 5-7 is shown in FIG. Figure 2 The hydrogen production efficiency result diagram of the samples prepared in Example 2-Example 4; Figure 1-Figure 2 It can be seen that without additional loading of precious metals (such as Au, Pt, etc.), with methanol as the sacrificial agent, the hydrogen production efficiency is as high as 64mmol / g / h. The titanium-copper composite photocatalyst prepared by the preparation method of the present invention has long-term performance stability, and the performance does not decrease significantly after continuous hydrogen production reaction for 30 hours.
[0035] Figure 3 The XRD characterization diagrams of the samples prepared in Examples 1 to 4 are as follows: Figure 4 From the XRD characterization diagrams of the samples prepared in Example 2 and Examples 5-7, it can be seen that the titanium-copper composite photocatalyst prepared by the present invention has anatase titanium dioxide as the main phase, followed by impurities containing copper hydroxide and copper chloride. In the phase with the best performance (Example 2), the corresponding diffraction peaks do not appear due to the diffuse distribution of copper hydroxide, copper chlorine and copper chloride.
[0036] Figure 5 This is the SEM characterization picture of CuTi-2 prepared in Example 2. Figure 5 It can be seen that the titanium-copper composite photocatalyst prepared by the present invention has fine grains.
[0037] Figure 6 TEM characterization diagram of CuTi-2 prepared in Example 2. Figure 6 It can be seen that the titanium-copper composite photocatalyst prepared by the present invention has ultra-fine grains, about 10 nm.
[0038] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for preparing a titanium-copper composite photocatalyst, characterized in that: The preparation method specifically comprises the following steps: adding urea and copper chloride to deionized water in sequence while magnetic stirring, slowly adding titanium tetrachloride solution after a stirring treatment, then performing a secondary stirring treatment, performing a hydrothermal treatment after the treatment, and obtaining a precipitate by centrifugation after the hydrothermal treatment, and performing a drying treatment to finally obtain a titanium-copper composite photocatalyst.
2. The method for preparing the titanium-copper composite photocatalyst according to claim 1, characterized in that: The molar ratio of Cu:Ti is (0.5-2.5):
1.
3. The method for preparing the titanium-copper composite photocatalyst according to claim 1, characterized in that: The time of the stirring treatment is 5-10 minutes.
4. The method for preparing the titanium-copper composite photocatalyst according to claim 1, characterized in that: The specific dropping parameters of the titanium tetrachloride are: 100-120ul is added each time, and the interval between each addition is 5-10 seconds.
5. The method for preparing the titanium-copper composite photocatalyst according to claim 1, characterized in that: The secondary stirring treatment lasts for 30 minutes, and the stirring speed is 400-600 r / min.
6. The method for preparing the titanium-copper composite photocatalyst according to claim 1, characterized in that: The parameters of the hydrothermal treatment are as follows: temperature is 90° C. and time is 12 h.
7. The method for preparing the titanium-copper composite photocatalyst according to claim 1, characterized in that: The number of centrifugation is 2-3 times.
8. The method for preparing the titanium-copper composite photocatalyst according to claim 1, characterized in that: The temperature of the drying process is 60°C.
9. A titanium-copper composite photocatalyst, prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The crystal grains of the titanium-copper composite photocatalyst are ≤30nm.
Citation Information
Patent Citations
Titanium dioxide low-temperature hydrothermal synthesis method
CN102992394A
3D morphology CeO2 / TiO2 catalyst preparation method
CN107597092A
Composite photocatalyst for treating organic pollutants in wastewater as well as preparation method and application of composite photocatalyst
CN114471586A
Preparation method of wood-based composite material, wood-based composite material and application of wood-based composite material
CN115318289A
Hydrothermal crystallization preparation method of high activity ball shaped nano-crystal titanium dioxide powder photocatalyst