Carbon material composite Co-M bimetallic catalyst and preparation method and application thereof

By combining Co-M bimetallic catalysts on carbon materials, the problem of insufficient catalytic performance of a single Co-based catalyst is solved, efficient and stable hydrogen production is achieved, and the stability and activity of the catalyst are improved.

CN118976509APending Publication Date: 2024-11-19ZHONGBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411041067.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the production of catalytic hydrogen, a single Co-based catalyst has problems such as insufficient catalytic performance, poor stability and prone to agglomeration, which limits its application in the field of hydrogen energy.

Method used

Using carbon material composite Co-M bimetallic catalyst, through acidification treatment and liquid phase reduction reaction, cobalt and a second metal source (such as molybdenum) are combined with carbon material to form a catalyst with nanostructures, increasing catalytic active sites and inhibiting agglomeration. .

Benefits of technology

The catalytic activity and stability of the catalyst are improved, the contact area between the catalyst and the reactants is increased, and efficient hydrogen production is achieved, and the raw materials are easy to obtain and easy to prepare.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976509A_ABST
    Figure CN118976509A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalysts, in particular to a carbon material composite Co-M bimetallic catalyst and a preparation method and application thereof. In view of the defects of few active sites, high possibility of agglomeration after hydrolysis reaction and poor cycling stability of the existing Co-based catalyst, the catalyst of a second-phase metal doped composite carbon material, namely a carbon material composite Co-M bimetallic catalyst, is prepared by adopting a relatively simple process, M is selected from copper, iron, nickel, molybdenum, tungsten or chromium, and the Co-M bimetallic catalyst is a metal-based catalyst. The catalyst has the advantages of large specific surface area, multiple active sites, high catalytic activity, cheap and easily available raw materials and wide practical application, the preparation method is simple and convenient, NaBH4 hydrolysis can be catalyzed to produce hydrogen, and the technical defects of a traditional Co-based catalyst are effectively overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, in particular to a carbon material composite Co-M bimetallic catalyst and a preparation method and application thereof. Background Art

[0002] In order to overcome the problems of energy shortage and environmental pollution in the future, finding renewable green energy is an important issue that needs to be solved urgently in the world. Hydrogen is a clean and environmentally friendly secondary energy source with a wide range of sources, so hydrogen is considered to be one of the most important energy sources in the future energy structure. The main sources of hydrogen are obtained through natural gas reforming, coal gasification, bio-cracking and gasification, electrolysis and photohydrolysis, and hydrolysis of chemical hydrides and borohydrides. However, the actual application of hydrogen energy is still limited by two key factors: the preparation of hydrogen energy and the storage of hydrogen energy. Among them, the theoretical hydrogen storage capacity of sodium borohydride is as high as 10.6wt%. At the same time, it has the advantages of being able to exist stably in an alkaline environment, easy to store, and good controllability. Therefore, the use of sodium borohydride has received more and more attention.

[0003] However, the hydrolysis rate of sodium borohydride is relatively slow in the absence of a catalyst, so a catalyst must be added. Commonly used catalysts include precious metals such as Ru and Pt, but their high prices and low reserves limit their practical applications. Therefore, non-precious metal-based catalysts have attracted the attention of researchers, and Co-based catalysts have been widely studied due to their low prices and abundant reserves.

[0004] However, single Co-based catalysts have the characteristics of few active sites, easy agglomeration after hydrolysis reaction, and poor cyclic stability, which greatly reduce their catalytic activity and hydrogen production rate. At present, single Co-based catalysts still have disadvantages such as poor catalytic performance and weak stability. Therefore, it is particularly important to develop a high-performance catalyst with high catalytic activity and strong stability. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a carbon material composite Co-M bimetallic catalyst and its preparation method and application. In order to overcome the problem of insufficient catalytic performance of current Co-based catalysts, the purpose of this application is to provide a carbon material composite Co-M bimetallic catalyst with easy raw material acquisition, easy synthesis, high catalytic efficiency and reusability, and use the carbon material composite Co-M bimetallic catalyst to catalyze the hydrolysis of sodium borohydride to produce hydrogen.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] The preparation method of the carbon material composite Co-M bimetallic catalyst comprises the following steps:

[0008] The carbon material is subjected to an acid treatment to obtain a treated carbon material; the method of the acid treatment is: placing the carbon material in aqua regia and subjecting it to an acid treatment at 80° C. for 2 hours, then centrifugally washing with a large amount of deionized water until the pH reaches 6.0-7.0, and drying to a constant weight, wherein the acid treatment causes a large amount of carboxyl groups to be present on the surface of the carbon material;

[0009] A soluble cobalt source, a soluble metal source and a treated carbon material are mixed and dispersed in a dispersant to form a dispersion, and then a modifier is added to the dispersion to perform electronegativity modification on the treated carbon material to obtain a mixed solution; the modifier is used to drive away hydrogen on the carboxyl group of the treated carbon material, so that the treated carbon material is electronegative and is convenient for complexing with metal cations of the cobalt source and the metal source; the dispersant is a mixed solution of water and ethanol;

[0010] At 0-50° C., a NaBH4 aqueous solution is added to the mixed solution to carry out a liquid-phase reduction reaction, and after the bubbles stop, a carbon material composite Co-M bimetallic catalyst is obtained; in the liquid-phase reduction reaction, NaBH4 reacts with a cobalt source and a metal source to load cobalt nanoparticles and metal nanoions on the carbon material;

[0011] The soluble metal source is selected from a copper source, an iron source, a nickel source, a molybdenum source, a tungsten source or a chromium source. The present application takes a molybdenum source as an example to review the technical solution. Of course, after the copper source, the iron source, the nickel source, the tungsten source or the chromium source replaces the molybdenum source, a catalyst with excellent catalytic performance for catalyzing the hydrolysis of sodium borohydride to produce hydrogen can also be obtained.

[0012] Preferably, the molar ratio of the total amount of Co ions and M ions in the mixed solution to NaBH4 is 1:3-5; too low an amount of NaBH4 will lead to incomplete reduction reaction, reduced specific surface area of ​​the prepared catalyst, and reduced number of active sites; too high an amount of NaBH4 may cause excessive NaBH4 to cover the active sites of the catalyst, causing agglomeration and reducing the catalytic activity of the catalyst.

[0013] Preferably, the cobalt source is a soluble cobalt salt selected from CoNO3, CoCl2 or Co3(PO4)2.

[0014] Preferably, the carbon material is selected from carbon nanotubes, activated carbon, graphene or expanded graphite; further, the carbon material is selected from carbon nanotubes.

[0015] Preferably, the modifier is triethylamine, which is mainly used to modify the carbon material, improve the surface state, and enable the metal ions to better adhere to the carbon material carrier; in order to achieve better improvement, the amount of triethylamine added in the present application is higher than the amount of carbon material, and the amount of triethylamine can not be limited.

[0016] Preferably, the carbon material is dispersed in ethyl acetate, acetone, tetramethylethylenediamine, tetrahydrofuran or ethanol.

[0017] Preferably, the molybdenum source is selected from Mo(NO3)2, Mo3(PO4)2, MoCl2, Na2MoO4; the chromium source is selected from CrCl2 or Cr(NO3)2; the tungsten source is selected from Na2WO4; the copper source is selected from copper chloride, copper sulfate or copper nitrate; the iron source is selected from ferric chloride, ferric sulfate or ferric nitrate; and the nickel source is selected from nickel sulfate or nickel chloride.

[0018] The present invention also protects a carbon material composite Co-M bimetallic catalyst prepared by the above preparation method. In the carbon material composite Co-M bimetallic catalyst, the molar ratio of Co ions to M ions is 50-95:5-50, and the addition of the second metal source is equivalent to the modification of the single Co-based catalyst, thereby improving its catalytic activity. Only a small amount of the second metal source needs to be added to greatly improve the catalytic activity of the catalyst; further, the molar ratio of Co ions to M ions is 95:5, and the ratio of 95:5 is obtained through experimental screening, which is equivalent to an optimal ratio. Increasing or decreasing the ratio of Mo will reduce the catalytic activity of the catalyst; the mass ratio of the total amount of Co ions and M ions to the carbon material is 80-95:5-20, and further, the mass ratio of the total amount of Co ions and M ions to the carbon material is 80:20, 85:15, 90:10, and 95:5, respectively; more preferably, the mass ratio of the total amount of Co ions and M ions to the carbon material is 85:15 or 95:5, respectively, and this condition is obtained through experimental screening.

[0019] The present invention also protects the use of a carbon material composite Co-M bimetallic catalyst in the preparation of a NaBH4 hydrolysis hydrogen production catalyst, and the application method is: NaBH4 and the carbon material composite Co-M bimetallic catalyst are mixed and ball-milled to obtain a mixture, the mixture is added to water, and then the generated hydrogen is collected, and the collection method can be a drainage method;

[0020] The mass ratio of NaBH4 to carbon material composite Co-M bimetallic catalyst is 2-10:1.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention provides a carbon material composite Co-M bimetallic catalyst. Co and M are dual active center catalysts, which catalyze the decomposition of NaBH4 and the dissociation of H2O respectively. The synergistic effect of the two promotes hydrolysis and rapid hydrogen production. The carbon-based material is used as a carrier to disperse the catalyst, increase the specific surface area of ​​the catalyst, effectively inhibit the agglomeration of Co, and increase the contact area between the catalyst and the reactant, thereby accelerating the reaction. The B element is introduced during the catalyst preparation process to stabilize the active metal of the catalyst.

[0023] 2. In the carbon material composite Co-M bimetallic nanocatalyst of the present invention, metal nanoparticles are simultaneously composited on the surface and between layers (pores) of the nanocarbon material, so that electrons are transferred from the surface of the carbon material to the active metal surface, increasing its surface electron cloud density. At the same time, the nanocarbon material effectively increases the specific surface area of ​​the catalyst. The two synergistically catalyze and improve the catalytic activity of the catalyst. At the same time, the magnetism of Co is conducive to the recovery of raw materials, which is convenient for practical use.

[0024] 3. The preparation principle of the carbon material composite Co-M bimetallic catalyst of the present application is: a certain proportion of metal Co source, second phase metal source and nano-carbon material are formulated into a suspension, the suspension is first subjected to electronegativity modification treatment to allow the carbon material to complex with the metal cations of the cobalt source and the metal source, and then the active metal ions are in situ reduced on the surface of the nano-carbon material by dripping reduced NaBH4 solution to obtain a highly active and highly dispersed bimetallic composite catalyst. The raw materials of the present invention are easy to obtain and the preparation is simple, and the carbon material composite Co-M bimetallic catalyst is easy to synthesize. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The SEM, TEM and HRTEM images of Co-5Mo-B-15CNT prepared in Example 1 of the present invention, wherein a is the SEM image of Co-5Mo-B-15CNT, b is the TEM image of Co-5Mo-B-15CNT, c is the HRTEM image of Co-5Mo-B-15CNT, and d is an enlarged image of b;

[0026] Figure 2 This is a graph of the hydrogen production rate of Co-5Mo-B-15CNT prepared in Example 1 of the present invention;

[0027] Figure 3 This is a graph of the hydrogen production rate of Co-5Mo-B-15AC prepared in Example 2 of the present invention;

[0028] Figure 4 This is a graph of the hydrogen production rate of Co-5Mo-B-15Go prepared in Example 3 of the present invention;

[0029] Figure 5 The SEM image and corresponding EDS element spectrum of the mixture obtained by mechanically ball-milling NaBH4 and Co-5Mo-B-15CNT of Example 1;

[0030] Figure 6 A comparison chart of the rates of catalytic hydrogen production using samples of Example 1, Examples 4-6 and Comparative Example 1 of the present invention;

[0031] Figure 7A comparison chart of the rates of catalytic hydrogen production using samples of Examples 1-3, Comparative Example 1 and Comparative Example 4 of the present invention;

[0032] Figure 8 The figure is a comparison chart of the rates of catalytic hydrogen production using samples of comparative examples 1-4 of the present invention. DETAILED DESCRIPTION

[0033] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.

[0034] Taking into account the current single Co-based catalyst has the characteristics of few active sites, easy agglomeration after hydrolysis reaction, and poor cycle stability, the present invention adopts a relatively simple process to prepare a catalyst of a second-phase metal-doped composite carbon material; at this time, the Co source and the second-phase metal source are stably attached to the surface of the carbon material, which increases the active sites of the catalytic reaction. The carbon material has the characteristics of a large specific surface area. After stably complexing with Co ions, the agglomeration problem of Co ions in the hydrolysis process is effectively avoided. By compounding the catalyst particles at the surface interface of the nano-carbon material, the structural stability of the catalyst is increased, the agglomeration phenomenon of the catalyst in the reaction process is reduced, and the stability of the catalyst is increased; then a catalyst with a large specific surface area, more active sites, high catalytic activity, cheap raw materials, easy to obtain, and wide practical application is obtained to catalyze the hydrolysis of NaBH4 to produce hydrogen, which effectively solves the shortcomings of poor catalytic performance of traditional Co-based catalysts.

[0035] The following examples and comparative examples are used to further illustrate the technical solution of the present application, as shown below:

[0036] Example 1

[0037] The preparation method of the carbon material composite Co-Mo bimetallic catalyst comprises the following steps:

[0038] S1, placing the carbon nanotubes in aqua regia and acidifying them at 80°C for 2h, then washing them by centrifugation with a large amount of deionized water until the pH reaches 6.0, and drying them to a constant weight to obtain treated carbon nanotubes;

[0039] At room temperature, 30 mg of the treated carbon nanotubes were dispersed in 60 mL of anhydrous ethanol to obtain solution a;

[0040] S2, disperse 345.0 mg of CoCl2 and 28.8 mg of Na2MoO4 in 60 mL of deionized water, and sonicate until completely dissolved to obtain solution b;

[0041] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0042] S4. In an ice-water bath, 10 mL of 15 mmol NaBH4 solution was added dropwise to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stopped, the mixture was washed with a large amount of deionized water and ethanol, and then vacuum-dried at 60°C for 6 h to obtain a product named Co-5Mo-B-15CNT. At this time, the mass ratio of the total amount of Co ions and M ions to the treated carbon nanotubes was 85:15, the molar ratio of Co ions to Mo ions was 95:5, and the molar ratio of the total amount of Co ions and M ions to NaBH4 was 1:5.

[0043] Example 2

[0044] The preparation method of the carbon material composite Co-Mo bimetallic catalyst comprises the following steps:

[0045] S1. Place the activated carbon in aqua regia and acidify at 80°C for 2h, then wash by centrifugation with a large amount of deionized water until the pH reaches 6.0, and dry to constant weight to obtain treated activated carbon;

[0046] At room temperature, 30 mg of the treated activated carbon was dispersed in 60 mL of anhydrous ethanol to obtain solution a;

[0047] S2, disperse 345.0 mg of CoCl2 and 28.8 mg of Na2MoO4 in 60 mL of deionized water, and sonicate until completely dissolved to obtain solution b;

[0048] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0049] S4. In an ice-water bath, add 10 mL of 15 mmol NaBH4 solution to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stop, wash with a large amount of deionized water and ethanol, and then vacuum dry at 60°C for 6 hours to obtain a product named Co-5Mo-B-15AC. At this time, the mass ratio of the total amount of Co ions and M ions to the treated activated carbon is 85:15, the molar ratio of Co ions to Mo ions is 95:5, and the molar ratio of the total amount of Co ions and M ions to NaBH4 is 1:5.

[0050] Example 3

[0051] The preparation method of the carbon material composite Co-Mo bimetallic catalyst comprises the following steps:

[0052] S1, placing graphene in aqua regia and acidifying at 80°C for 2h, then washing by centrifugation with a large amount of deionized water until the pH reaches 6.0, and drying to constant weight to obtain treated graphene;

[0053] 30 mg of the treated graphene was dispersed in 60 mL of anhydrous ethanol at room temperature to obtain solution a;

[0054] S2, disperse 345.0 mg of CoCl2 and 28.8 mg of Na2MoO4 in 60 mL of deionized water, and sonicate until completely dissolved to obtain solution b;

[0055] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0056] S4. In an ice-water bath, 10 mL of 15 mmol NaBH4 solution was added dropwise to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stopped, the mixture was washed with a large amount of deionized water and ethanol, and then vacuum-dried at 60°C for 6 h to obtain a product named Co-5Mo-B-15Go. At this time, the mass ratio of the total amount of Co ions and M ions to the treated graphene was 85:15, the molar ratio of Co ions to Mo ions was 95:5, and the molar ratio of the total amount of Co ions and M ions to NaBH4 was 1:5.

[0057] Example 4

[0058] The preparation method of the carbon material composite Co-Mo bimetallic catalyst comprises the following steps:

[0059] S1, placing the carbon nanotubes in aqua regia and acidifying them at 80°C for 2h, then washing them by centrifugation with a large amount of deionized water until the pH reaches 6.0, and drying them to a constant weight to obtain treated carbon nanotubes;

[0060] At room temperature, 10 mg of the treated carbon nanotubes were dispersed in 60 mL of anhydrous ethanol to obtain solution a;

[0061] S2, disperse 385.6 mg of CoCl2 and 32.2 mg of Na2MoO4 in 60 mL of deionized water, and sonicate until completely dissolved to obtain solution b;

[0062] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0063] S4. In an ice-water bath, add 10 mL of 15 mmol NaBH4 solution to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stop, wash with a large amount of deionized water and ethanol, and then vacuum dry at 60°C for 6 hours to obtain a product named Co-5Mo-B-5CNT. At this time, the mass ratio of the total amount of Co ions and M ions to the treated carbon nanotubes is 95:5, the molar ratio of Co ions to Mo ions is 95:5, and the molar ratio of the total amount of Co ions and M ions to NaBH4 is 1:5.

[0064] Example 5

[0065] The preparation method of the carbon material composite Co-Mo bimetallic catalyst comprises the following steps:

[0066] S1, placing the carbon nanotubes in aqua regia and acidifying them at 80°C for 2h, then washing them by centrifugation with a large amount of deionized water until the pH reaches 6.0, and drying them to a constant weight to obtain treated carbon nanotubes;

[0067] At room temperature, 20 mg of the treated carbon nanotubes were dispersed in 60 mL of anhydrous ethanol to obtain solution a;

[0068] S2, disperse 365.3 mg of CoCl2 and 30.5 mg of Na2MoO4 in 60 mL of deionized water, and sonicate until completely dissolved to obtain solution b;

[0069] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0070] S4. In an ice-water bath, 10 mL of 15 mmol NaBH4 solution was added dropwise to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stopped, the mixture was washed with a large amount of deionized water and ethanol, and then vacuum-dried at 60°C for 6 h to obtain a product named Co-5Mo-B-10CNT. At this time, the mass ratio of the total amount of Co ions and M ions to the treated carbon nanotubes was 90:10, the molar ratio of Co ions to Mo ions was 95:5, and the molar ratio of the total amount of Co ions and M ions to NaBH4 was 1:5.

[0071] Example 6

[0072] The preparation method of the carbon material composite Co-Mo bimetallic catalyst comprises the following steps:

[0073] S1, placing the carbon nanotubes in aqua regia and acidifying them at 80°C for 2h, then washing them by centrifugation with a large amount of deionized water until the pH reaches 6.0, and drying them to a constant weight to obtain treated carbon nanotubes;

[0074] At room temperature, 40 mg of the treated carbon nanotubes were dispersed in 60 mL of anhydrous ethanol to obtain solution a;

[0075] S2, 324.7 mg of CoCl2 and 27.2 mg of Na2MoO4 were dispersed in 60 mL of deionized water and ultrasonicated until completely dissolved to obtain solution b;

[0076] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0077] S4. In an ice-water bath, 10 mL of 15 mmol NaBH4 solution was added dropwise to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stopped, the mixture was washed with a large amount of deionized water and ethanol, and then vacuum-dried at 60°C for 6 h to obtain a product named Co-5Mo-B-20CNT. At this time, the mass ratio of the total amount of Co ions and M ions to the treated carbon nanotubes was 80:20, the molar ratio of Co ions to Mo ions was 95:5, and the molar ratio of the total amount of Co ions and M ions to NaBH4 was 1:5.

[0078] Example 7

[0079] The preparation method of the carbon material composite Co-Mo bimetallic catalyst comprises the following steps:

[0080] S1, placing the carbon nanotubes in aqua regia and acidifying them at 80°C for 2h, then washing them by centrifugation with a large amount of deionized water until the pH reaches 6.0, and drying them to a constant weight to obtain treated carbon nanotubes;

[0081] At room temperature, 30 mg of the treated carbon nanotubes were dispersed in 60 mL of anhydrous ethanol to obtain solution a;

[0082] S2, disperse 326.8 mg of CoCl2 and 57.6 mg of Na2MoO4 in 60 mL of deionized water, and sonicate until completely dissolved to obtain solution b;

[0083] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0084] S4. In an ice-water bath, 10 mL of 9 mmol NaBH4 solution was added dropwise to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stopped, the mixture was washed with a large amount of deionized water and ethanol, and then vacuum-dried at 60°C for 6 h to obtain a product named Co-10Mo-B-15CNT. At this time, the mass ratio of the total amount of Co ions and M ions to the treated carbon nanotubes was 85:15, the molar ratio of Co ions to Mo ions was 90:10, and the molar ratio of the total amount of Co ions and M ions to NaBH4 was 1:3.

[0085] Example 8

[0086] The preparation method of the carbon material composite Co-Cr bimetallic catalyst, the preparation steps of this embodiment are the same as those of embodiment 1, except that Mo is replaced by Cr, and comprises the following steps:

[0087] S1, placing the carbon nanotubes in aqua regia and acidifying them at 80°C for 2h, then washing them by centrifugation with a large amount of deionized water until the pH reaches 6.0, and drying them to a constant weight to obtain treated carbon nanotubes;

[0088] At room temperature, 30 mg of the treated carbon nanotubes were dispersed in 60 mL of anhydrous ethanol to obtain solution a;

[0089] S2, disperse 345.0 mg of CoCl2 and 25.4 mg of Cr(NO3)2 in 60 mL of deionized water, and sonicate until completely dissolved to obtain solution b;

[0090] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0091] S4. In an ice-water bath, add 10 mL of 15 mmol NaBH4 solution to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stop, wash with a large amount of deionized water and ethanol, and then vacuum dry at 60°C for 6 h to obtain a product named Co-5Cr-B-15CNT.

[0092] Example 9

[0093] The preparation method of the carbon material composite Co-W bimetallic catalyst, the preparation steps of this embodiment are the same as those of embodiment 1, except that Mo is replaced by W, and the steps include:

[0094] S1, placing the carbon nanotubes in aqua regia and acidifying them at 80°C for 2h, then washing them by centrifugation with a large amount of deionized water until the pH reaches 6.0, and drying them to a constant weight to obtain treated carbon nanotubes;

[0095] At room temperature, 30 mg of the treated carbon nanotubes were dispersed in 60 mL of anhydrous ethanol to obtain solution a;

[0096] S2, disperse 345.0 mg of CoCl2 and 41.1 mg of Na2WO4 in 60 mL of deionized water, and sonicate until completely dissolved to obtain solution b;

[0097] S3, slowly adding solution b into solution a, then dropping 240 μL of triethylamine, and then ultrasonicating for 1 h and magnetically stirring for 3 h at room temperature to obtain a mixed solution;

[0098] S4. In an ice-water bath, add 10 mL of 15 mmol NaBH4 solution to the mixed solution to carry out a liquid-phase reduction reaction. After the bubbles stop, wash with a large amount of deionized water and ethanol, and then vacuum dry at 60°C for 6 h to obtain a product named Co-5W-B-15CNT.

[0099] The applicant also conducted experiments using copper source, iron source and nickel source as raw materials. The results showed that the catalyst prepared using Mo source as raw material had the best catalytic performance. Therefore, Mo source was used as an example and compared with the comparative example. The comparative example is as follows:

[0100] Comparative Example 1

[0101] The preparation method of Co-5Mo-B catalyst, which is the same as the preparation steps of Example 1, except that carbon nanotubes are not compounded, comprises the following steps:

[0102] S1. Disperse 345.0 mg of CoCl2 and 28.8 mg of Na2MoO4 in 60 mL of deionized water and sonicate until completely dissolved to obtain solution a;

[0103] S2. In an ice-water bath, add 10 mL of 15 mmol NaBH4 solution to the mixed solution a to carry out a liquid-phase reduction reaction. After the bubbles stop, wash with a large amount of deionized water and ethanol, and then vacuum dry at 60°C for 6 h to obtain a product named Co-5Mo-B. At this time, the molar ratio of Co ions to Mo ions is 95:5.

[0104] Comparative Example 2

[0105] Preparation method of Co-3Mo-B catalyst, this comparative example has the same preparation steps as comparative example 1, except that the mass of CoCl2 and Na2MoO4 is recalculated so that the molar ratio of Co ion to Mo ion is 97:3, comprising the following steps:

[0106] S1. Disperse 352.3 mg of CoCl2 and 17.28 mg of Na2MoO4 in 60 mL of deionized water and sonicate until completely dissolved to obtain solution a;

[0107] S2. In an ice-water bath, add 10 mL of 15 mmol NaBH4 solution to the mixed solution a to carry out a liquid-phase reduction reaction. After the bubbles stop, wash with a large amount of deionized water and ethanol, and then vacuum dry at 60°C for 6 h to obtain a product named Co-3Mo-B. At this time, the molar ratio of Co ions to Mo ions is 97:3.

[0108] Comparative Example 3

[0109] Preparation method of Co-7Mo-B catalyst, this comparative example has the same preparation steps as comparative example 1, except that the mass of CoCl2 and Na2MoO4 is recalculated so that the molar ratio of Co ion to Mo ion is 93:7, comprising the following steps:

[0110] S1. Disperse 337.74 mg of CoCl2 and 40.32 mg of Na2MoO4 in 60 mL of deionized water and sonicate until completely dissolved to obtain solution a;

[0111] S2. In an ice-water bath, add 10 mL of 15 mmol NaBH4 solution to the mixed solution a to carry out a liquid-phase reduction reaction. After the bubbles stop, wash with a large amount of deionized water and ethanol, and then vacuum dry at 60°C for 6 h to obtain a product named Co-7Mo-B. At this time, the molar ratio of Co ions to Mo ions is 93:7.

[0112] Comparative Example 4

[0113] The preparation method of Co-B catalyst, which is the same as the preparation steps of Comparative Example 1, except that Mo is not compounded, comprises the following steps:

[0114] S1. Disperse 345.0 mg of CoCl2 in 60 mL of deionized water and sonicate until completely dissolved to obtain a CoCl2 solution;

[0115] S2. In an ice-water bath, add 10 mL of 15 mmol of NaBH4 solution to the CoCl2 solution to carry out a liquid-phase reduction reaction. After the bubbles stop, wash with a large amount of deionized water and ethanol, and then vacuum dry at 60°C for 6 hours to obtain a product named Co-B.

[0116] Carbon material composite Co-Mo bimetallic catalysts were prepared in Examples 1-7 of the present invention. The samples of Examples 1-6 and Comparative Examples 1-4 were studied below. The specific research methods and results are as follows:

[0117] Figure 1 The results show that the catalyst particles are dispersed relatively evenly on the surface of carbon nanotubes, effectively inhibiting agglomeration. At the same time, some catalyst particles are compounded into the interlayers and ports of carbon nanotubes, and the loosely cross-linked tubular structure forms a fast and convenient electron conduction channel.

[0118] The operation of the hydrolysis hydrogen production experiment is as follows: first, the samples of Examples 1-6 and Comparative Examples 1-4 are respectively mechanically ball-milled with NaBH4 to form a mixture, and then 0.25 g of the mixture is placed in a 250 mL three-necked flask, and the flask is placed in a 298k water bath. Subsequently, 5 mL of deionized water is pumped into the three-necked flask at a rate of 50 mL / min by a peristaltic pump. The generated hydrogen is collected by the drainage method and connected to a computer to record the changes in the quality of the water in a timely manner.

[0119] Figure 2-4 The results show that the three Co-based bimetallic composite carbon material catalysts obtained in Examples 1-3 all have high hydrogen production rates and good catalytic performance, among which Co-5Mo-B-15CNT has the highest hydrogen production rate and the best catalytic performance.

[0120] Figure 5 The results showed that NaBH4 and Co-5Mo-B-15CNT were evenly mixed in the mixture prepared after ball milling, which made the hydrolysis rate stable and controllable, facilitating the determination of hydrogen production.

[0121] Figure 6 The results show that after adding carbon nanotubes, the hydrogen production rate is greatly improved, and it reaches the best at 15wt%. The catalytic performance is 2.51 times higher than that of Co-5Mo-B. The higher catalytic performance can be attributed to the strong interaction between different components in the catalyst. The appropriate ratio of Mo and CNT greatly increases the specific surface area of ​​the catalyst, exposing more active sites while forming a fast and convenient conduction channel, accelerating the mass transfer and diffusion of reactants.

[0122] Figure 7 The results show that with the addition of the second metal source and different carbon materials, the catalytic performance has been improved to varying degrees, among which Co-5Mo-B-15CNT has the shortest hydrogen production time and the highest hydrogen production rate.

[0123] Figure 8 The results show that after screening, Co-5Mo-B has the shortest hydrogen production time and the highest hydrogen production rate. Therefore, when Co is compounded with the second metal source, the more the second metal source, the better the performance.

[0124] Those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a carbon material composite Co-M bimetallic catalyst, characterized in that: The steps include: acidifying the carbon material to obtain a treated carbon material; A soluble cobalt source, a soluble metal source and a treated carbon material are mixed and dispersed in a dispersant to form a dispersion liquid, and then a modifier is added to the dispersion liquid to perform electronegativity modification on the treated carbon material to obtain a mixed liquid; A NaBH4 aqueous solution is added to the mixed solution to carry out a liquid phase reduction reaction, and after the bubbles stop, a carbon material composite Co-M bimetallic catalyst is obtained; Wherein, the soluble metal source is selected from a copper source, an iron source, a nickel source, a molybdenum source, a tungsten source or a chromium source.

2. The method for preparing the carbon material composite Co-M bimetallic catalyst according to claim 1, characterized in that: The modifier is triethylamine.

3. The method for preparing the carbon material composite Co-M bimetallic catalyst according to claim 1, characterized in that: The molar ratio of Co ions to metal ions is 50-95:5-50, and the mass ratio of the total amount of Co ions and metal ions to the treated carbon material is 80-95:5-20.

4. The method for preparing the carbon material composite Co-M bimetallic catalyst according to claim 3, characterized in that: The molar ratio of Co ions to metal ions is 95:5, and the mass ratio of the total amount of Co ions and metal ions to the treated carbon material is 85:15 or 95:

5.

5. The method for preparing the carbon material composite Co-M bimetallic catalyst according to claim 1, characterized in that: The molar ratio of the total amount of Co ions and metal ions in the mixed solution to NaBH4 is 1:3-5.

6. The method for preparing the carbon material composite Co-M bimetallic catalyst according to claim 1, characterized in that: The carbon material is selected from carbon nanotubes, graphene, activated carbon or expanded graphite.

7. The method for preparing a carbon material composite Co-M bimetallic catalyst according to claim 1, characterized in that: The carbon material is placed in aqua regia and subjected to acidification treatment under heating conditions.

8. A carbon material composite Co-M bimetallic catalyst prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the carbon material composite Co-M bimetallic catalyst according to claim 8 in the preparation of a NaBH4 hydrolysis hydrogen production catalyst.

10. The use according to claim 9, characterized in that: The mass ratio of NaBH4 to carbon material composite Co-M bimetallic catalyst is 2-10:1.