Pt monatomic and nano-particle coexisting catalyst, preparation method and application of Pt monatomic and nano-particle coexisting catalyst
By supporting Pt single atoms and nanoparticles on cobalt tetroxide, the problems of low efficiency and poor stability of existing catalysts in the oxidation of gaseous pollutants such as toluene are solved, and efficient catalytic oxidation effect is achieved.
Patent Information
- Application Number
- CN202411119425.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
AI Technical Summary
In the process of catalyzing the oxidation of gaseous pollutants such as toluene, existing catalysts have problems such as high manufacturing cost, low catalytic efficiency, poor selectivity and poor thermal stability, and it is difficult to continue to work stably under different environmental conditions.
Using a catalyst for coexistence of Pt single atoms and nanoparticles, the Pt single atoms and nanoparticles supported on tricobalt tetoxide are mixed and calcined. The active components are achieved by mixing the platinum source with ZIF-67 and calcining it. Evenly dispersed and synergistically enhanced.
It improves the catalytic activity and stability of the catalyst, achieves efficient oxidation of gaseous pollutants, provides good activation sites and electronic structure regulation, and improves catalytic efficiency.
Smart Images

Figure CN118976514A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst materials, and in particular to a Pt single atom and nanoparticle coexistence catalyst, a preparation method and application thereof. Background Art
[0002] With the acceleration of industrialization, the impact of gaseous pollutants such as toluene, propane, propylene, etc. on the environment and human health is becoming increasingly serious. As an effective pollutant treatment technology, catalytic oxidation is of great significance for reducing the emission of these harmful gases. Toluene catalytic oxidation is one of the key reactions in the fields of petrochemicals and fine chemicals. It is not only related to the production of chemical products, but also closely related to environmental governance and energy utilization. As a widely existing organic compound, the catalytic oxidation process of toluene is of great significance for the synthesis of high value-added chemicals. The types of catalysts currently used include precious metal catalysts, non-precious metal catalysts, and composite oxide catalysts. Catalysts for industrial use need to have low manufacturing costs, high catalytic efficiency, and good thermal and chemical stability to withstand long-term high temperature and chemical corrosion environments, thereby reducing replacement costs and maintenance difficulties.
[0003] However, the catalysts in the prior art still have the disadvantages of high manufacturing cost, low catalytic efficiency, poor selectivity and poor thermal stability. Therefore, how to improve the catalytic activity of the catalyst and ensure that the catalyst can continue to work stably under different environmental conditions (such as high space velocity) has become a problem that needs to be solved urgently. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a Pt single atom and nanoparticle coexistence catalyst and its preparation method and use. The Pt single atom and nanoparticle coexistence catalyst of the present invention has high metal dispersion and redox ability, and has very high efficiency and stability in catalytic oxidation of gaseous pollutants.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a catalyst in which a single Pt atom and nanoparticles coexist, the method comprising the following steps: mixing ZIF-67 and water to obtain a suspension; uniformly mixing a platinum source with the suspension to obtain a platinum aqueous solution, and heating, rotary evaporating, first drying and calcining the obtained platinum aqueous solution to obtain the catalyst in which a single Pt atom and nanoparticles coexist;
[0007] The prepared Pt single atom and nanoparticle coexistence catalyst comprises cobalt tetroxide and an active component Pt;
[0008] The active component Pt is supported on the cobalt tetroxide in the form of single atoms and nanoparticles.
[0009] The Pt single atom and nanoparticle coexistence catalyst prepared by the present invention has a high specific surface area and rich pore structure, so that the platinum source is first loaded on ZIF-67, and then the ZIF-67 is converted into cobalt tetroxide through calcination, so that part of the platinum species loaded on ZIF-67 before calcination enters the lattice of cobalt tetroxide generated after calcination to form Pt single atoms, and the rest of the platinum species are loaded on the surface of cobalt tetroxide in the form of Pt nanoparticles.
[0010] The preparation method of the present invention is simple and efficient, and the active components can be evenly dispersed on cobalt tetroxide without agglomeration. Conventional catalysts prepared by directly using cobalt tetroxide as a raw material can only obtain catalysts in which platinum species are loaded on cobalt tetroxide in the form of nanoparticles, and the catalytic activity is average. The preparation method of the present invention can realize that the active components exist on the carrier in the form of single atoms and nanoparticles coexisting, thereby further improving the catalytic efficiency.
[0011] The active component Pt in the present invention can be loaded on the lattice and surface of cobalt tetroxide generated by calcining ZIF-67 in the form of coexistence of single atoms and nanoparticles. On the one hand, the introduction of Pt single atoms not only provides a good VOCs activation site, but also regulates the electronic structure of adjacent Pt nanoparticles and promotes the activation of molecular oxygen. In addition, the introduction of Pt single atoms distorts the Co3O4 lattice, promotes the activation of adjacent lattice oxygen, realizes the dual activation of lattice oxygen and molecular oxygen, and further improves the catalytic efficiency. On the other hand, Pt nanoparticles themselves have certain catalytic activity. The coexistence of active components in two loading forms can play a synergistic role and improve the catalytic efficiency of the catalyst.
[0012] The "first drying" and "second drying" mentioned in the present invention are only to distinguish different steps and do not represent the order in which the steps are performed.
[0013] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0014] Preferably, the ZIF-67 has a hexagonal structure.
[0015] Preferably, the specific surface area of ZIF-67 is 200-450m 2 / g, for example, it can be 200m 2 / g, 230m 2 / g, 250m 2 / g, 270m 2 / g、300m 2 / g, 340m 2 / g, 350m 2 / g, 380m 2 / g, 400m 2 / g, 410m 2 / g, 430m 2 / g or 450m 2 / g, but not limited to the listed values, other values not listed in the numerical range are also applicable, preferably 340m 2 / g.
[0016] Preferably, the solid content of the suspension is 12.2-16.3 g / L, for example, it can be 12.2 g / L, 12.4 g / L, 12.6 g / L, 12.8 g / L, 13.0 g / L, 13.5 g / L, 13.7 g / L, 14.2 g / L, 14.5 g / L, 15.0 g / L, 15.4 g / L, 15.6 g / L, 15.8 g / L, 16.0 g / L or 16.3 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0017] Preferably, the ZIF-67 is mixed with water and then ultrasonically mixed to obtain the suspension.
[0018] Preferably, the ultrasonic time is 5-20 min, for example, 5 min, 10 min, 15 min or 20 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the platinum source comprises tetraammine platinum nitrate or platinum nitrate.
[0020] The present invention does not specifically limit the Pt concentration in the platinum aqueous solution, as long as the molar content of Pt in the final product satisfies that the content of the active component Pt is 0.3-6wt% based on the total mass of the Pt single atom and nanoparticle coexisting catalyst as 100wt%.
[0021] Preferably, the heating temperature is 40-80°C, for example, it can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the heating process is accompanied by stirring.
[0023] Heating and stirring can make the active components dispersed more evenly on ZIF-67 without agglomeration, ensuring the full utilization of the active components and the carrier.
[0024] Preferably, the heating time is 1-3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, the vacuum degree of the rotary evaporation is 50-200 Pa, for example, 50 Pa, 100 Pa or 200 Pa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] Preferably, the rotary evaporation temperature is 25-60°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the first drying temperature is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C or 80°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the first drying time is 12-24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the calcination temperature is 350-550°C, for example, it can be 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C or 550°C, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0030] In the present invention, the calcination temperature is further regulated within the range of 350-550°C. Calcination within this temperature range can obtain a Pt single atom and nanoparticle coexistence catalyst with better performance. The calcination temperature affects the dispersion of the active sites. If the calcination temperature is too low, the calcination product of ZIF-67 cannot exist in the form of Co3O4, affecting the formation of Pt single atoms. If the calcination temperature is too high, the grain size of the ZIF calcination product Co3O4 will become larger, which is not conducive to the dispersion of the active components.
[0031] Preferably, the calcination time is 1-3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0032] Preferably, the preparation method of ZIF-67 comprises:
[0033] The cobalt source is dissolved in methanol to obtain solution A, dimethylimidazole is dissolved in methanol to obtain solution B, solution A and solution B are mixed and ultrasonicated, and then a hydrothermal reaction is performed, and the ZIF-67 is obtained after centrifugation, washing and a second drying.
[0034] Preferably, the cobalt source comprises cobalt nitrate hexahydrate or cobalt acetate tetrahydrate.
[0035] Preferably, the concentration of solution A is 0.1-0.25 mol / L, for example, 0.1 mol / L, 0.2 mol / L or 0.25 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] Preferably, the concentration of solution B is 0.1-0.55 mol / L, for example, 0.1 mol / L, 0.25 mol / L or 0.55 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] Preferably, the ultrasonic time is 5-10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] Preferably, the temperature of the hydrothermal reaction is 110-130°C, for example, 110°C, 115°C, 120°C, 125°C or 130°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] In the preparation method of ZIF-67 of the present invention, the temperature of the hydrothermal reaction is controlled to be 110-130° C., so that ZIF-67 with a more uniform grain size can be prepared, and the catalyst effect obtained thereby is further improved.
[0040] Preferably, the hydrothermal reaction time is 3-5 h, for example, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0041] Preferably, the washing solvent comprises ethanol.
[0042] Preferably, the second drying temperature is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C or 80°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, the second drying time is 12-24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] Preferably, the preparation method comprises the following steps:
[0045] (1) dissolving a cobalt source in methanol to obtain a solution A with a concentration of 0.1-0.25 mol / L, dissolving dimethyl imidazole in methanol to obtain a solution B with a concentration of 0.1-0.55 mol / L, mixing solution A and solution B, ultrasonicating for 5-10 min, and then hydrothermally reacting at 110-130° C. for 3-5 h, centrifuging, washing with ethanol, and second drying at 60-80° C. for 12-24 h to obtain the ZIF-67;
[0046] (2) ZIF-67 is added to water and ultrasonicated for 5-20 minutes to obtain a suspension with a solid content of 12.2-16.3 g / L, an appropriate amount of platinum source is added to the suspension to obtain a Pt aqueous solution, and the suspension is heated and stirred at 40-80°C for 1-3 hours, and then rotary evaporated at a vacuum degree of 50-200 Pa and a temperature of 25-60°C, and first dried at 60-80°C for 12-24 hours, and then calcined at 350-550°C for 1-3 hours to obtain the Pt single atom and nanoparticle coexistence catalyst.
[0047] In a second aspect, the present invention provides a Pt single atom and nanoparticle coexistence catalyst prepared according to the preparation method described in the first aspect.
[0048] The active component Pt in the present invention can be loaded in the lattice and surface of cobalt tetroxide generated by calcining ZIF-67 in the form of coexistence of single atoms and nanoparticles. On the one hand, the introduction of Pt single atoms not only provides a good VOCs activation site, but also regulates the electronic structure of adjacent Pt nanoparticles and promotes the activation of molecular oxygen. In addition, the introduction of Pt single atoms distorts the Co3O4 lattice, promotes the activation of adjacent lattice oxygen, realizes the dual activation of lattice oxygen and molecular oxygen, and further improves the catalytic efficiency. On the other hand, Pt nanoparticles themselves have certain catalytic activity. The coexistence of active components in two loading forms can play a synergistic role and improve the catalytic efficiency of the catalyst.
[0049] Preferably, based on the total mass of the catalyst in which Pt single atoms and nanoparticles coexist as 100wt%, the content of the active component Pt is 0.3-6wt%, preferably 4wt%-6wt%, for example, it can be 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt% or 6wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, and the balance is cobalt tetroxide.
[0050] The platinum content in the present invention affects the dispersibility of the subsequently loaded Pt and the effect of the catalyst. By controlling the platinum content within the range of 0.3-6wt%, preferably within the range of 4wt%-6wt%, a catalyst with a more excellent effect can be prepared. If the platinum content is too low, the platinum species will be loaded on the catalyst surface only in the form of single atoms, and there will be no platinum species in the form of nanoparticles, thereby reducing the oxidation performance of the catalyst. If the platinum content is too high, the active component Pt will be aggregated, which is not only not conducive to the catalyst functioning, but also leads to an increase in manufacturing costs.
[0051] In a third aspect, the present invention provides a use of the Pt single atom and nanoparticle coexistence catalyst according to the second aspect, wherein the Pt single atom and nanoparticle coexistence catalyst is used for catalytic oxidation of gaseous pollutants.
[0052] The Pt single atom and nanoparticle coexistence catalyst of the present invention has excellent catalytic oxidation efficiency for the catalytic oxidation of gaseous pollutants, can provide sufficient and effective activation sites for the activation of pollutants and molecular oxygen, and accelerate the catalytic purification efficiency of pollutants.
[0053] Preferably, the gaseous pollutant includes any one of toluene, propane or propylene, or a combination of at least two of them.
[0054] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0055] Compared with the prior art, the present invention has at least the following beneficial effects:
[0056] (1) The content of the active component Pt in the catalyst of coexistence of Pt single atoms and nanoparticles in the present invention is 0.3-6wt%. The active component can achieve excellent catalytic activity at a very low content, which is mainly attributed to the fact that the introduction of Pt single atoms not only provides a good VOCs activation site, but also regulates the electronic structure of adjacent Pt nanoparticles and promotes the activation of molecular oxygen. In addition, the introduction of Pt single atoms distorts the cobalt tetroxide lattice of the ZIF-67 calcined product, promotes the activation of adjacent lattice oxygen, realizes the dual activation of lattice oxygen and molecular oxygen, and further improves the catalytic efficiency.
[0057] (2) The present invention adopts a heating impregnation method to prepare the catalyst without adding other reducing agents. The present invention utilizes a high specific surface area and rich pore structure to first load the platinum source on ZIF-67, and then undergoes a calcination procedure to allow part of the Pt species loaded on ZIF-67 to enter the lattice of the ZIF-67 calcined product cobalt oxide to form Pt single atoms, and the remaining Pt species are loaded on the surface of the ZIF-67 calcined product cobalt oxide in the form of Pt nanoparticles. The preparation method is simple and efficient, and the active components can be evenly dispersed on ZIF-67 without agglomeration, and a catalyst in which Pt single atoms and nanoparticles coexist is obtained after calcination.
[0058] (3) The Pt single atom and nanoparticle coexistence catalyst of the present invention has excellent catalytic oxidation efficiency, a wide range of applications, and high catalytic activity for the catalytic oxidation of gaseous pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 This is a spherical aberration electron microscope image of the Pt single atom and nanoparticle coexistence catalyst prepared in Example 1 of the present invention;
[0060] Figure 2 This is a spherical aberration electron microscope image of the Pt single atom catalyst prepared in Comparative Example 1 of the present invention;
[0061] Figure 3 This is a spherical aberration electron microscope image of the nanoparticle Pt / Co3O4 catalyst prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0062] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0063] In the following examples, unless otherwise specified, all reagents and consumables were purchased from conventional reagent manufacturers in the field; unless otherwise specified, the experimental methods and technical means used were conventional methods and means in the field.
[0064] Example 1
[0065] This embodiment provides a Pt single atom and nanoparticle coexistence catalyst, wherein the Pt single atom and nanoparticle coexistence catalyst comprises cobalt tetroxide and an active component Pt supported on the cobalt tetroxide; the active component Pt is supported on the cobalt tetroxide in the form of single atoms and nanoparticles;
[0066] Based on the total mass of the Pt single atom and nanoparticle coexisting catalyst being 100wt%, the content of the active component Pt is 1wt%, and the remainder is cobalt tetroxide;
[0067] The preparation method of the Pt single atom and nanoparticle coexistence catalyst provided in this embodiment comprises the following steps:
[0068] (1) dissolving cobalt nitrate hexahydrate in methanol to obtain a solution A with a concentration of 0.1511 mol / L, dissolving dimethylimidazole in methanol to obtain a solution B with a concentration of 0.500 mol / L, mixing solution A and solution B, ultrasonicating for 10 min, and then hydrothermally reacting at 120° C. for 4 h, centrifuging, washing with ethanol, and second drying at 70° C. for 12 h to obtain the ZIF-67;
[0069] (2) ZIF-67 was added to water and ultrasonicated for 10 minutes to obtain a suspension with a solid content of 16.3 g / L. An appropriate amount of tetraammine platinum nitrate was added to the suspension to obtain a Pt aqueous solution with a Pt concentration of 0.0592 g / L. The suspension was heated and stirred at 60°C for 2 hours, and then rotary evaporated at a vacuum degree of 100 Pa and a temperature of 60°C, and first dried at 70°C for 12 hours. Thereafter, the suspension was calcined at 350°C for 2 hours to obtain the Pt single atom and nanoparticle coexistence catalyst.
[0070] The spherical aberration electron microscopy image of the prepared Pt single atom and nanoparticle coexistence catalyst is shown in Figure 1 As shown, the red circle marks the Pt single atom, and the particles with 0.23nm lattice fringes are metal Pt nanoparticles. It can be seen that the active components thereon exist in the form of coexistence of single atoms and nanoparticles.
[0071] Example 2
[0072] This embodiment provides a Pt single atom and nanoparticle coexistence catalyst, wherein the Pt single atom and nanoparticle coexistence catalyst comprises cobalt tetroxide and an active component Pt supported on the cobalt tetroxide; the active component Pt is supported on the cobalt tetroxide in the form of single atoms and nanoparticles;
[0073] Based on the total mass of the Pt single atom and nanoparticle coexisting catalyst being 100wt%, the content of the active component Pt is 6wt%, and the remainder is cobalt tetroxide;
[0074] The preparation method of the Pt single atom and nanoparticle coexistence catalyst provided in this embodiment comprises the following steps:
[0075] (1) dissolving cobalt acetate tetrahydrate in methanol to obtain a solution A with a concentration of 0.25 mol / L, dissolving dimethylimidazole in methanol to obtain a solution B with a concentration of 0.550 mol / L, mixing solution A and solution B, ultrasonicating for 5 min, and then hydrothermally reacting at 110° C. for 5 h, centrifuging, washing with ethanol, and second drying at 60° C. for 24 h to obtain the ZIF-67;
[0076] (2) ZIF-67 was added to water and ultrasonicated for 5 minutes to obtain a suspension with a solid content of 12.2 g / L. An appropriate amount of tetraammine platinum nitrate was added to the suspension to obtain a Pt aqueous solution with a Pt concentration of 0.355 g / L. The suspension was heated and stirred at 40°C for 3 hours, and then rotary evaporated at a vacuum degree of 50 Pa and a temperature of 60°C, and first dried at 60°C for 24 hours. Thereafter, the suspension was calcined at 400°C for 2 hours to obtain the Pt single atom and nanoparticle coexistence catalyst.
[0077] Example 3
[0078] This embodiment provides a Pt single atom and nanoparticle coexistence catalyst, wherein the Pt single atom and nanoparticle coexistence catalyst comprises cobalt tetroxide and an active component Pt supported on the cobalt tetroxide; the active component Pt is supported on the cobalt tetroxide in the form of a single atom;
[0079] Based on the total mass of the Pt single atom and nanoparticle coexisting catalyst being 100wt%, the content of the active component Pt is 0.3wt%, and the remainder is cobalt tetroxide;
[0080] The preparation method of the Pt single atom and nanoparticle coexistence catalyst provided in this embodiment comprises the following steps:
[0081] (1) dissolving cobalt nitrate hexahydrate in methanol to obtain a solution A with a concentration of 0.25 mol / L, dissolving dimethylimidazole in methanol to obtain a solution B with a concentration of 0.35 mol / L, mixing solution A and solution B, ultrasonicating for 10 min, and then hydrothermally reacting at 130° C. for 3 h, centrifuging, washing with ethanol, and second drying at 80° C. for 12 h to obtain the ZIF-67;
[0082] (2) ZIF-67 was added to water and ultrasonicated for 20 minutes to obtain a suspension with a solid content of 16.3 g / L. An appropriate amount of platinum nitrate was added to the suspension to obtain a Pt aqueous solution with a Pt concentration of 0.01775 g / L. The suspension was heated and stirred at 80°C for 1 hour, and then rotary evaporated at a vacuum degree of 50 Pa and a temperature of 60°C, and first dried at 80°C for 12 hours. Thereafter, the suspension was calcined at 350°C for 2 hours to obtain the Pt single atom and nanoparticle coexistence catalyst.
[0083] Example 4
[0084] This embodiment provides a Pt single atom and nanoparticle coexistence catalyst, which is different from Example 1 only in that when preparing the Pt single atom and nanoparticle coexistence catalyst, the calcination temperature in step (2) is 600°C.
[0085] Example 5
[0086] This embodiment provides a Pt single atom and nanoparticle coexistence catalyst, which is different from Example 1 only in that when preparing the Pt single atom and nanoparticle coexistence catalyst, the calcination temperature in step (2) is 300°C.
[0087] Comparative Example 1
[0088] This comparative example provides a Pt single-atom catalyst, which differs from Example 1 only in that, based on the total mass of the Pt single-atom catalyst being 100wt%, the content of the active component Pt is 0.25wt%, and the remainder is cobalt tetroxide; the active component Pt is supported on the cobalt tetroxide in the form of a single atom; when preparing the Pt single-atom catalyst, the concentration of Pt in the Pt aqueous solution is ensured to be 0.01479g / L in step (2).
[0089] The spherical aberration electron microscopy image of the prepared Pt single atom catalyst is shown in Figure 2 As shown, the red circle marks the Pt single atom, which does not contain nanoparticles.
[0090] Comparative Example 2
[0091] This comparative example provides a nano-particle Pt / Co3O4 catalyst. Taking the total mass of the nano-particle Pt / Co3O4 catalyst as 100wt%, the content of the active component Pt is 1wt%. The preparation method of the nano-particle Pt / Co3O4 catalyst provided in this comparative example comprises the following steps:
[0092] (1) dissolving cobalt nitrate hexahydrate in methanol to obtain a solution A with a concentration of 0.1511 mol / L, dissolving dimethylimidazole in methanol to obtain a solution B with a concentration of 0.500 mol / L, mixing solution A and solution B and ultrasonicating for 10 min, then hydrothermally reacting at 120° C. for 4 h, centrifuging, washing with ethanol and second drying at 70° C. for 12 h to obtain the ZIF-67, and calcining the ZIF-67 obtained in step (1) at 350° C. for 2 h in an air atmosphere to obtain a Co3O4 carrier;
[0093] (2) Add the Co3O4 carrier obtained in step (1) to water and ultrasonicate for 10 minutes to obtain a suspension with a solid content of 16.3 g / L, add an appropriate amount of tetraammine platinum nitrate to the suspension to obtain a Pt aqueous solution with a Pt concentration of 0.1667 g / L, heat and stir at 60°C for 2 hours, then rotary evaporate at a vacuum degree of 50 Pa and a temperature of 60°C, and first dry at 70°C for 12 hours. Take 0.9 g of the dried product and place it in a 1.259 g / L NaBH4 solution, grind it until no bubbles are generated, wash it, dry it at 60-90°C for 8h-12h, and then place it in a muffle furnace at 200°C for 2h to obtain a 1% Pt / Co3O4 catalyst;
[0094] The spherical aberration electron microscopy image of the prepared nanoparticle Pt / Co3O4 catalyst is shown in Figure 3 As shown, the particles with 0.23 nm lattice fringes are metal Pt nanoparticles, that is, the active component Pt in the prepared Pt / Co3O4 catalyst exists in the form of nanoparticles, and no Pt single atoms are found.
[0095] Comparative Example 3
[0096] This comparative example provides a nano-particle Pt / Co3O4 catalyst. Taking the total mass of the nano-particle Pt / Co3O4 catalyst as 100wt%, the content of the active component Pt is 0.25wt% (the content is the same as that in comparative example 1). The preparation method of the nano-particle Pt / Co3O4 catalyst provided in this comparative example comprises the following steps:
[0097] (1) dissolving cobalt nitrate hexahydrate in methanol to obtain a solution A with a concentration of 0.125 mol / L, dissolving dimethylimidazole in methanol to obtain a solution B with a concentration of 0.427 mol / L, mixing solution A and solution B and subjecting them to ultrasonic treatment for 10 min, and then subjecting them to hydrothermal reaction at 120° C. for 4 h, and subjecting them to centrifugation, washing with ethanol, and second drying at 70° C. for 12 h to obtain the ZIF-67, and calcining the ZIF-67 obtained in step (1) at 350° C. for 2 h in an air atmosphere to obtain a Co3O4 carrier;
[0098] (2) The Co3O4 carrier obtained in step (1) is added to water and ultrasonicated for 10 minutes to obtain a suspension with a solid content of 16.3 g / L. An appropriate amount of tetraammine platinum nitrate is added to the suspension to obtain a Pt aqueous solution with a Pt concentration of 0.0417 g / L. The suspension is heated and stirred at 60°C for 2 hours, and then rotary evaporated at a vacuum degree of 100 Pa and a temperature of 60°C, and first dried at 70°C for 12 hours. 0.9 g of the dried product is placed in a 1.259 g / L NaBH4 solution and ground until no bubbles are generated. The product is washed and dried at 60-90°C for 8-12 hours, and then calcined in a muffle furnace at 200°C for 2 hours to obtain a 0.25% Pt / Co3O4 catalyst.
[0099] Test method:
[0100] 0.1 g of the prepared catalyst was placed in a fixed bed reactor, and appropriate concentrations of pollutants (e.g., 500 ppm toluene, 1000 ppm propane, 1000 ppm propylene, etc.) were introduced at a space velocity of 2,4000 h -1 , under the condition of reaction temperature of 100-250°C, online testing is carried out using a gas chromatograph equipped with a hydrogen flame detector and a thermal conductivity detector.
[0101] After the pollutant concentration is stabilized, the conversion rate of the pollutant is calculated according to (initial pollutant concentration-real-time pollutant concentration) / (initial pollutant concentration)×100%. The test results are shown in Table 1.
[0102] Table 1
[0103]
[0104] The test results show that:
[0105] (1) It can be seen from Examples 1-3 that the content of the active component Pt in the catalyst of coexistence of Pt single atoms and nanoparticles in the present invention is 0.3-6wt%, and the catalyst has excellent catalytic activity for catalyzing gaseous pollutants. When catalyzing toluene, T 90% When catalyzing propane, T 90% When propylene is catalyzed at 220°C, T 90% The temperature of the catalyst was 128℃, which was mainly attributed to the fact that the introduction of Pt single atoms not only provided good activation sites, but also regulated the electronic structure of adjacent Pt nanoparticles, promoting the activation of molecular oxygen. In addition, the introduction of Pt single atoms distorted the Co3O4 lattice, promoting the activation of adjacent lattice oxygen, achieving dual activation of lattice oxygen and molecular oxygen, and further improving the catalytic efficiency.
[0106] (2) By comparing Example 1 with Examples 4-5, it can be seen that the present invention can achieve better pollutant degradation efficiency by further controlling the calcination temperature. The calcination temperature affects the dispersion of active sites. If the calcination temperature is too low, the calcination product of ZIF-67 cannot exist in the form of Co3O4, affecting the formation of Pt single atoms; if the calcination temperature is too high, the grain size of the ZIF calcination product Co3O4 will become larger, which is not conducive to the dispersion of active components.
[0107] (3) It can be seen from Example 1 and Comparative Example 1 that when the content of the active component Pt is 0.25wt%, Pt is supported on the cobalt tetroxide in the form of a single atom, and no Pt nanoparticles are contained. At this time, the catalytic activity of the catalyst is greatly reduced. The present invention controls the content of the active component Pt within the range of 0.3-6wt%, and the active component Pt can be supported on the cobalt tetroxide in the form of a single atom and nanoparticles coexisting, thereby obtaining a technical effect of excellent catalytic effect.
[0108] (4) It can be seen from Example 1 and Comparative Example 2 that when the Pt loading amount is the same, different Pt loading forms will also affect the reaction activity of the catalyst. Comparative Example 3 adopts the NaBH4 solution reduction method to prepare Pt in the form of nanoparticles loaded on a Co3O4 carrier, and its catalytic activity is far less than that of Example 1. It can be seen that the catalyst of the present invention, in which the Pt source is first loaded on ZIF-67 and then the Pt single atom and nanoparticles coexist, has a better degradation efficiency for pollutants.
[0109] (5) It can be seen from Comparative Examples 1 and 3 that, when the Pt loading is the same, the degradation efficiency of the pollutants by the single-atom Pt catalyst prepared in Comparative Example 1 is lower than that of the pure nanoparticle Pt-loaded Co3O4 catalyst prepared in Comparative Example 3, which further illustrates that Pt in the form of nanoparticles has a beneficial effect on the activity of the catalyst, thereby further proving that the coexistence of single Pt atoms and nanoparticles in the present invention can effectively improve the degradation efficiency of pollutants.
[0110] In summary, the Pt single atom and nanoparticle coexistence catalyst prepared by the present invention, due to the high specific surface area and rich pore structure of ZIF-67, the platinum source is first loaded on ZIF-67, and then after calcination, ZIF-67 is converted into cobalt tetraoxide, so that part of the platinum species loaded on ZIF-67 before calcination enters the cobalt tetraoxide lattice generated after calcination to form Pt single atoms, and the remaining part of the platinum species is loaded on the surface of cobalt tetraoxide in the form of Pt nanoparticles. The content of the active component Pt in the Pt single atom and nanoparticle coexistence catalyst of the present invention is 0.3-6wt%, and the catalytic gaseous pollutants have excellent catalytic activity, which is mainly attributed to the introduction of Pt single atoms not only providing good VOCs activation sites, but also regulating the electronic structure of adjacent Pt nanoparticles, and promoting the activation of molecular oxygen. In addition, the introduction of Pt single atoms distorts the Co3O4 lattice, promotes the activation of adjacent lattice oxygen, realizes the dual activation of lattice oxygen and molecular oxygen, and further improves the efficiency of catalytic oxidation.
[0111] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a catalyst containing coexistence of Pt single atoms and nanoparticles. It is characterized in that The preparation method comprises the following steps: Mixing ZIF-67 and water to obtain a suspension; uniformly mixing a platinum source with the suspension to obtain a platinum aqueous solution, heating, rotary evaporating, first drying and calcining the obtained platinum aqueous solution to obtain the Pt single atom and nanoparticle coexistence catalyst; The prepared Pt single atom and nanoparticle coexistence catalyst comprises cobalt tetroxide and active component Pt; the active component Pt is loaded on the cobalt tetroxide in the form of single atom and nanoparticle coexistence.
2. The preparation method according to claim 1, It is characterized in that The ZIF-67 has a hexagonal structure and a specific surface area of 200-450 m 2 / g; Preferably, the ZIF-67 is mixed with water and ultrasonically mixed to obtain the suspension; Preferably, the solid content of the suspension is 12.2-16.3 g / L; Preferably, the ultrasonic time is 5-20 min; Preferably, the platinum source comprises tetraammine platinum nitrate or platinum nitrate; Preferably, the heating temperature is 40-80°C; Preferably, the heating process is accompanied by stirring; Preferably, the heating time is 1-3h; Preferably, the vacuum degree of the rotary evaporation is 50-200 Pa; Preferably, the temperature of the rotary evaporation is 25-60°C.
3. The preparation method according to claim 1 or 2, It is characterized in that The first drying temperature is 60-80°C; Preferably, the first drying time is 12-24h; Preferably, the calcination temperature is 350-550°C; Preferably, the calcination time is 1-3 hours.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that The preparation method of ZIF-67 comprises: The cobalt source is dissolved in methanol to obtain solution A, dimethylimidazole is dissolved in methanol to obtain solution B, solution A and solution B are mixed and ultrasonicated, and then a hydrothermal reaction is performed, and the ZIF-67 is obtained after centrifugation, washing and a second drying.
5. The preparation method according to claim 4, It is characterized in that The cobalt source includes cobalt nitrate hexahydrate or cobalt acetate tetrahydrate; Preferably, the concentration of solution A is 0.1-0.25 mol / L; Preferably, the concentration of solution B is 0.1-0.55 mol / L; Preferably, the ultrasonication time is 5-10 min.
6. The preparation method according to claim 4 or 5, It is characterized in that The temperature of the hydrothermal reaction is 110-130°C; Preferably, the hydrothermal reaction time is 3-5h; Preferably, the washing solvent comprises ethanol; Preferably, the second drying temperature is 60-80°C; Preferably, the second drying time is 12-24 hours.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: (1) dissolving a cobalt source in methanol to obtain a solution A with a concentration of 0.1-0.25 mol / L, dissolving dimethyl imidazole in methanol to obtain a solution B with a concentration of 0.1-0.55 mol / L, mixing solution A and solution B, ultrasonicating for 5-10 min, and then hydrothermally reacting at 110-130° C. for 3-5 h, centrifuging, washing with ethanol, and second drying at 60-80° C. for 12-24 h to obtain the ZIF-67; (2) ZIF-67 is added to water and ultrasonicated for 5-20 minutes to obtain a suspension with a solid content of 12.2-16.3 g / L, an appropriate amount of platinum source is added to the suspension to obtain a Pt aqueous solution, and the suspension is heated and stirred at 40-80°C for 1-3 hours, and then rotary evaporated at a vacuum degree of 50-200 Pa and a temperature of 25-60°C, and first dried at 60-80°C for 12-24 hours, and then calcined at 350-550°C for 1-3 hours to obtain the Pt single atom and nanoparticle coexistence catalyst.
8. A Pt single atom and nanoparticle coexistence catalyst, It is characterized in that The Pt single atom and nanoparticle coexistence catalyst is prepared according to the preparation method according to any one of claims 1-7.
9. The Pt single atom and nanoparticle coexistence catalyst according to claim 8, It is characterized in that Taking the total mass of the Pt single atom and nanoparticle coexisting catalyst as 100wt%, the content of the active component Pt is 0.3-6wt%, preferably 4wt%-6wt%, and the balance is cobalt tetroxide.
10. Use of the Pt single atom and nanoparticle coexistence catalyst according to claim 8 or 9, It is characterized in that The Pt single atom and nanoparticle coexistence catalyst is used for catalytic oxidation of gaseous pollutants.
Citation Information
Patent Citations
Pt / CoO monatomic catalyst as well as preparation method and applications thereof
CN110252337A
Preparation method and application of nanoscale Co3O4 (at) Pt
CN114160155A
Platinum group metal catalyst and preparation and application thereof
CN114917927A
Platinum-loaded honeycomb carbon catalyst as well as preparation method and application thereof
CN117913298A
Cited By
A trace ruthenium modified cobalt-based nanocage catalyst and preparation and application thereof
CN120250065B
Platinum monatomic-platinum nanoparticle synergistic dispersion catalyst as well as preparation method and application thereof
CN120914271A