Nickel-based catalyst, preparation method thereof and application of nickel-based catalyst in methane dry gas reforming reaction

Through the core-shell domain structure of nickel-based catalyst, the problems of metal sintering and carbon deposition of nickel-based catalysts in methane dry gas reforming reaction are solved, and high-efficiency reaction and long-life catalysts under low temperature conditions are achieved, which significantly improves stability and anti-carbon properties.

CN118976530APending Publication Date: 2024-11-19NANCHANG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411064358.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Nickel-based catalysts are prone to metal sintering and carbon deposition during methane dry gas reforming reaction, resulting in catalyst deactivation, affecting reaction efficiency and product H2/CO ratio.

Method used

Using the preparation method of nickel-based catalyst, through the core-shell domain effect, a nickel precursor is used to combine with the porous support S-1 molecular sieve and silicon compound to form a base core and shell structure, inhibit the migration of metal particles and the growth of carbon nanotubes, and improve the The stability and resistance to carbon deposits of the catalyst.

Benefits of technology

The methane dry gas reforming reaction is realized under low temperature conditions, which significantly improves the stability and carbon deposit resistance of the catalyst, extends the service life of the catalyst, and maintains an efficient methane conversion rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976530A_ABST
    Figure CN118976530A_ABST
Patent Text Reader

Abstract

The invention provides a nickel-based catalyst, a preparation method thereof and application of the nickel-based catalyst in a methane dry gas reforming reaction, and relates to the technical field of catalyst preparation. The nickel-based catalyst with excellent stability and carbon deposition resistance is prepared by using the core-shell confinement effect and wrapping the nickel precursor with the silicon layer and the porous carrier wrapping the surface of the nickel precursor. The catalyst effectively inhibits migration and aggregation of metal particles, hinders growth of carbon nanotubes, improves the problems of metal sintering and carbon deposition of a nickel-based catalyst, can realize a methane dry gas reforming reaction at a relatively low temperature, and promotes energy conversion and low-carbon development.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to a nickel-based catalyst and a preparation method thereof and application thereof in a methane dry gas reforming reaction. Background Art

[0002] Fossil fuel shortages and greenhouse gas emissions are major challenges today. Methane dry gas reforming reactions convert two greenhouse gases, methane and carbon dioxide, into synthesis gas (H2 and CO), providing new ideas for greenhouse gas governance and global low-carbon development. Synthesis gas can be used in Fischer-Tropsch synthesis reactions to produce liquid fuels and high-value-added chemicals. Methane dry gas reforming reactions can efficiently utilize greenhouse gases and alleviate energy shortages, and have good application prospects in carbon dioxide emission reduction, environmental friendliness, and high-value-added products.

[0003] Methane dry gas reforming reaction CH4(g)+CO2(g)→2H2(g)+2CO(g)

[0004] Methane cracking reaction CH4(g)→C(s)+2H2(g)

[0005] Carbon monoxide disproportionation reaction 2C0(g)→C(s)+CO2(g)

[0006] Reverse water gas reaction CO2(g)+H2(g)→H2O(g)+CO(g)

[0007] During the methane dry gas reforming reaction, there are problems of high-temperature metal sintering and carbon deposition leading to catalyst deactivation. First, the methane dry gas reforming reaction is a strong endothermic reaction. In order to obtain a high conversion rate, the reaction temperature needs to be maintained at 800℃-1000℃, but this will increase energy consumption and the problem of high-temperature metal sintering; secondly, side reactions cause carbon to be deposited on the catalyst surface, thereby affecting the performance and life of the catalyst. Carbon deposition mainly comes from methane cracking reaction and carbon monoxide disproportionation reaction, and the occurrence of reverse water gas reaction will convert H2 and CO2 into CO and H2O, seriously affecting the product H2 / CO ratio.

[0008] Currently, nickel-based catalysts have become a research hotspot due to their low cost and high activity. However, nickel-based catalysts are prone to metal sintering and carbon deposition, resulting in catalyst deactivation. Therefore, it is urgent to provide a solution to improve the above problems. Summary of the invention

[0009] The present invention aims to provide a nickel-based catalyst and a preparation method thereof and application in a methane dry gas reforming reaction. The catalyst utilizes a core-shell confinement effect to inhibit the migration and aggregation of metal particles and hinder the growth of carbon nanotubes, thereby effectively improving the stability and anti-carbon deposition performance of the catalyst.

[0010] In a first aspect, the present invention provides a nickel-based catalyst, comprising a base core and a shell layer coated on the surface of the base core, wherein the base core comprises a nickel precursor and a porous carrier wrapped on the surface of the nickel precursor, and the shell layer comprises a silicon compound.

[0011] Optionally, the porous carrier wraps and / or supports nickel, an active component in the catalyst.

[0012] Optionally, the nickel precursor includes a nickel salt and a chelating agent, wherein the nickel salt includes at least one of nickel nitrate, nickel chloride, nickel acetate and nickel sulfate, and the chelating agent is ethylenediamine.

[0013] Optionally, the nickel element in the nickel precursor accounts for 0.6wt%-1.0wt% of the total mass of the catalyst.

[0014] Optionally, the porous carrier comprises S-1 molecular sieve.

[0015] Optionally, the S-1 molecular sieve comprises a silicon compound, a structure directing agent and H2O, wherein the silicon compound comprises at least one of silica sol and an organosilicon compound, and the structure directing agent comprises TPAOH.

[0016] Optionally, the molar ratio of the silicon compound, the structure directing agent and H2O is 1:(1 / 4-2 / 5):(1 / 40-1 / 10).

[0017] Optionally, the silica sol includes SiO2, and the organic silicon compound includes TEOS.

[0018] Optionally, the shell thickness is controlled by changing the mass ratio of the base core to the silicon compound. Specifically, the shell thickness is positively correlated with the content of the silicon compound, and the shell thickness affects the stability and anti-carbon deposition performance of the catalyst.

[0019] In a second aspect, the present invention provides a method for preparing the above catalyst, comprising the following steps:

[0020] The nickel precursor and S-1 molecular sieve are subjected to hydrothermal crystallization reaction to obtain the base core;

[0021] In an alkaline solvent environment, the base core is surface activated and then a silicon compound is added to react to generate a catalyst precursor; the catalyst precursor is reduced to obtain a nickel-based catalyst.

[0022] The catalyst preparation method provided by the present invention effectively inhibits the migration and aggregation of metal particles in the catalyst and hinders the growth of carbon nanotubes, thereby increasing the service life of the catalyst.

[0023] Optionally, when the nickel precursor and the S-1 molecular sieve are subjected to a hydrothermal crystallization reaction, the process includes: mixing a nickel salt and a chelating agent in a molar ratio of (0.4-2):1, and then ultrasonically treating the mixture for 30 min-40 min to obtain a nickel precursor; stirring a structure directing agent in water until it is clear, and then slowly dropping a silicon compound and stirring the mixture at room temperature for 3.5 h-4.5 h to obtain an S-1 molecular sieve; mixing the nickel precursor and the S-1 molecular sieve and stirring the mixture for 1 h-2 h, pouring the mixture into a reactor, and placing the mixture in an oven at 170°C-180°C for reaction for 3d-4d.

[0024] Optionally, when the silicon compound is added for reaction after the surface activation of the base core, the alkaline solvent environment includes NH3·H2O, and the pH of the system is adjusted to 8-11.

[0025] Optionally, when the silicon compound is added to react after the core base is surface activated, the alkaline solvent environment is ethanol.

[0026] Optionally, when the silicon compound is added for reaction after the core base is surface activated, the reagent used for the surface activation includes CTAB.

[0027] Optionally, when the silicon compound is added to react after the surface activation of the base core, the reagent used for the surface activation is set in excess compared to the base core.

[0028] Optionally, when reducing the catalyst precursor, the reaction atmosphere is a reducing atmosphere.

[0029] Optionally, when adding the silicon compound to react after surface activation of the base core, the base core is ultrasonically treated for 30 min-40 min and then mixed with a surfactant in an alkaline solution environment and stirred for 25 min-35 min, the silicon compound is slowly added dropwise until the system becomes milky white colloid and then reacted at 25°C-80°C for 8h-16h.

[0030] Optionally, after the nickel precursor is subjected to a hydrothermal crystallization reaction with the S-1 molecular sieve and the base core is surface activated and then a silicon compound is added to react, the obtained base core and catalyst need to be washed, dried and calcined. Specifically, the washing includes washing with pure water and ethanol for 3 to 5 times, the drying includes drying in an oven at 80°C to 100°C for 4h to 6h, and the calcination includes calcining in a muffle furnace at 550°C to 650°C for 4h to 6h.

[0031] In a third aspect, the present invention provides use of a catalyst prepared by any of the above optional preparation methods in a methane dry gas reforming reaction.

[0032] The catalyst provided by the present invention can realize the methane dry gas reforming reaction under relatively low temperature conditions, and compared with other catalysts, has excellent stability and anti-carbon deposition performance.

[0033] Optionally, at 500°C-800°C, methane and carbon dioxide generate carbon monoxide and hydrogen under the action of a nickel-based catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly introduce the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments.

[0035] Figure 1 This is a TEM image of the Ni@S-1@SiO2 catalyst after reduction prepared in Example 1 of the present invention;

[0036] Figure 2 Thermogravimetric analysis results of the nickel-based catalysts prepared in Example 1 and Comparative Example 1 of the present invention for methane dry gas reforming reaction at 30° C. to 800° C. for 25 hours;

[0037] Figure 3 The methane conversion rates of the nickel-based catalysts prepared in Example 1 of the present invention and Comparative Example 1 were respectively measured at 650° C. for 0 h to 25 h of methane dry gas reforming reaction. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described through the following embodiments in conjunction with the accompanying drawings. However, the following embodiments are illustrative and are only used to specifically describe the present invention rather than to limit the present invention.

[0039] The present invention provides a nickel-based catalyst, which comprises a base core and a shell layer coated on the surface of the base core, wherein the base core comprises a nickel precursor and a porous carrier coated on the surface of the nickel precursor, and the shell layer comprises a silicon compound.

[0040] In some embodiments, the porous carrier wraps and / or supports nickel, an active component in the catalyst.

[0041] In some embodiments, the nickel precursor includes a nickel salt and a chelating agent, wherein the nickel salt includes at least one of nickel nitrate, nickel chloride, nickel acetate and nickel sulfate, and the chelating agent includes ethylenediamine.

[0042] In some embodiments, the nickel element in the nickel precursor accounts for 0.6 wt%-1.0 wt% of the total mass of the catalyst.

[0043] In some embodiments, the porous support comprises S-1 molecular sieve.

[0044] In some embodiments, the S-1 molecular sieve includes a silicon compound, a structure directing agent and H2O. Specifically, the silicon compound includes at least one of silica sol and an organic silicon compound, and the structure directing agent includes TPAOH.

[0045] In some embodiments, the molar ratio of the silicon compound, the structure directing agent, and H2O is 1:(1 / 4-2 / 5):(1 / 40-1 / 10).

[0046] In some embodiments, the silica sol includes SiO2, and the organic silicon compound includes TEOS.

[0047] In some embodiments, the shell thickness is controlled by changing the mass ratio of the base core to the silicon compound. Specifically, the shell thickness is positively correlated with the content of the silicon compound, and the shell thickness affects the stability and anti-carbon deposition performance of the catalyst.

[0048] The present invention also provides a method for preparing a nickel-based catalyst, comprising the following steps:

[0049] The base core is prepared by hydrothermal crystallization reaction of S1, nickel precursor and S-1 molecular sieve;

[0050] S2. In an alkaline solvent environment, the base core is surface activated and then a silicon compound is added to react to generate a catalyst precursor; the catalyst precursor is reduced to obtain a nickel-based catalyst.

[0051] In fact, when executing step S1, the following sub-steps are included:

[0052] S1.1. Mix nickel salt and chelating agent in a molar ratio of (0.4-2):1 and ultrasonically treat for 30 min-40 min to obtain a nickel precursor; first stir the structure directing agent in water until it is clear, then slowly dropwise add the silicon compound and stir at room temperature for 3.5 h-4.5 h to obtain the S-1 molecular sieve;

[0053] S1.2. Mix the nickel precursor and S-1 molecular sieve and stir for 1h-2h, pour into a reactor and place in an oven, react at 170℃-180℃ for 3d-4d to obtain a base core, wash, dry and calcine the base core to obtain a base core powder.

[0054] In some embodiments, when performing step S2, the alkaline solvent environment includes NH3·H2O, and the pH of the system is adjusted to 8-11.

[0055] In some embodiments, when performing step S2, the alkaline solvent environment includes ethanol.

[0056] In some embodiments, when performing step S2, the reagent used for surface activation includes CTAB.

[0057] In some embodiments, when executing step S2, the reagent used for activation is set in excess compared to the base core.

[0058] In some embodiments, when executing step S2, the reaction atmosphere during reduction is a reducing atmosphere, specifically, including hydrogen and argon.

[0059] In fact, when executing step S2, the following sub-steps are included:

[0060] S2.1, ultrasonically treat the core for 30 min-40 min, and then mix and stir with a surfactant in an alkaline solvent environment for 25 min-35 min;

[0061] S2.2. Slowly add silicon compound to the mixed solution obtained in S2.1 until the system becomes milky white colloid, then react at 25°C-80°C for 8h-16h to obtain a catalyst precursor, reduce the catalyst precursor, wash, dry and calcine to obtain a catalyst powder.

[0062] In some embodiments, when performing step S1.2 and step S2.2, washing includes washing with pure water and ethanol for 3-5 times, drying includes drying in an oven at 80°C-100°C for 4h-6h, and calcining includes calcining in a muffle furnace at 550°C-650°C for 4h-6h.

[0063] The present invention also provides an application of the catalyst in a methane dry gas reforming reaction, comprising:

[0064] At 500℃-800℃, methane and carbon dioxide generate carbon monoxide and hydrogen over the action of nickel-based catalysts.

[0065] Example 1

[0066] Embodiment 1 of the present invention provides a method for preparing a nickel-based catalyst, comprising the following steps:

[0067] S1.1. Mix 0.1 g Ni(NO3)2·6H2O (CAS: 13478-00-7) with 2 mL ethylenediamine (CAS: 107-15-3) and treat in an ultrasonic pool for 30 min to obtain a nickel precursor; mix 43.3 g TPAOH (CAS: 4499-86-9) with 48 mL pure water and stir until the solution is clear, slowly drop 28.3 g TEOS (CAS: 78-10-4) and stir at room temperature for 4 h to obtain S-1 molecular sieve;

[0068] S1.2, pour the nickel precursor into the S-1 molecular sieve and stir for 1 hour, transfer the mixture to the reactor and place it in an oven, and let it stand for reaction at 170°C for 3 days to obtain a solid base core, wash the solid base core with pure water and ethanol by centrifugation three times, and then put it in an oven at 80°C for 6 hours, grind the dried solid sample into powder, put it into a crucible, and calcine it in a muffle furnace at 550°C for 6 hours to obtain the purified Ni@S-1 base core powder;

[0069] S2.1. Dissolve 2.0 g CTAB (CAS: 57-09-0) in 360 mL anhydrous ethanol and 300 mL deionized water, stir at room temperature until the solution is clear, mix 1.0 g of the base core powder with 180 mL pure water, and disperse by ultrasonic for 30 min.

[0070] S2.2, respectively, adding the solutions containing CTAB and the base core powder into a three-necked flask and mixing, adding 7mL 28wt% NH3·H2O and stirring vigorously for 30min, slowly dropping TEOS until the system becomes milky white colloid, and reacting at 25℃ for 9h to obtain a solid catalyst, washing the solid catalyst three times with pure water and ethanol by centrifugation, and drying it in an oven at 80℃ for 6h, grinding the dried solid sample into powder, loading it into a crucible, and calcining it in a muffle furnace at 550℃ for 5h to obtain a purified nickel-based catalyst (Ni@S-1@SiO 2-33 ).

[0071] In a fixed bed reactor, the nickel-based catalyst was reduced in situ at 75°C for 2 h with a 10% H2-Ar mixed gas at a flow rate of 30 mL / min. Figure 1 As shown: SiO2 grows directionally on the surface of the S-1 molecular sieve, and the thickness of the SiO2 shell is about 33nm. Some nickel nanoparticles are inside the S-1 shell, and some are covered by the SiO2 shell, proving that the core-shell confined catalyst was successfully prepared.

[0072] Comparative Example 1

[0073] Comparative Example 1 of the present invention provides a method for preparing a nickel-based catalyst. Compared with Example 1, Comparative Example 1 only performs the reactions of steps S1.1 to S1.4 to finally prepare a nickel-based catalyst (Ni@S-1).

[0074] Stability test

[0075] The catalysts prepared in Example 1 and Comparative Example 1 were respectively used for methane dry gas reforming reaction:

[0076] First, Ni@S-1@SiO 2-33 Catalyst powder and Ni@S-1 catalyst powder were pressed and sieved to 60 mesh to prepare granular catalysts. 50 mg of catalyst was taken and loaded into a quartz tube with an inner diameter of 6 mm, and both ends were blocked with quartz wool. The two catalysts were heated from room temperature to 750 ° C in a 10% H2 / Ar atmosphere with a space velocity of 30 mL / min and maintained for 2 h. After the reduction was completed, the reaction gas (CH4:CO2=1:1, WHSV=18,000 mL gcat -1 h -1 , p = 1 atm), during the cooling process from 800 °C to 400 °C, the methane conversion rate and thermogravimetry of the two catalysts were tested every 50 °C.

[0077] Figure 2 Thermogravimetric analysis results of two catalysts for methane dry gas reforming reaction at 30℃ to 800℃ for 25h. The results show that with the increase of reaction temperature, Ni@S-1@SiO 2-33 The stability of the catalyst showed no downward trend and no carbon deposition was observed by thermogravimetric analysis, while the carbon deposition content of the Ni@S-1 catalyst reached 46% at 800°C.

[0078] Figure 3 The methane conversion rates of the two catalysts for methane dry gas reforming reaction at 650℃ from 0h to 25h are shown in Table 1. 2-33 Under the action of the catalyst, the methane conversion rate was stable at around 61.7% and did not decrease with the increase of reaction time, indicating that Ni@S-1@SiO 2-33 The catalyst was not deactivated and had a certain stability. However, under the action of Ni@S-1 catalyst, the conversion rate of methane continued to decrease with the increase of reaction time. After 25 hours of reaction, it decreased by 54.84% compared with the initial value, which proved that the activity of Ni@S-1 catalyst decreased and its stability was poor.

[0079] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A nickel-based catalyst, characterized in that The catalyst comprises a base core and a shell layer coated on the surface of the base core, the base core comprises a nickel precursor and a porous carrier coated on the surface of the nickel precursor, and the shell layer comprises a silicon compound.

2. The catalyst according to claim 1, characterized in that The nickel precursor comprises a nickel salt and a chelating agent; the nickel element in the nickel precursor accounts for 0.6wt%-1.0wt% of the total mass of the catalyst; the porous carrier comprises an S-1 molecular sieve; the silicon compound comprises at least one of silica sol and organosilicon; and the shell thickness is controlled by changing the mass ratio of the base core to the silicon compound.

3. The catalyst according to any one of claims 1 to 2, characterized in that The nickel salt includes at least one of nickel nitrate, nickel chloride, nickel acetate and nickel sulfate; and / or the chelating agent is ethylenediamine; and / or the structure directing agent includes TPAOH; and / or the S-1 molecular sieve includes a silicon compound, a structure directing agent and H2O, and the molar ratio of the silicon compound, the structure directing agent and H2O is 1:(1 / 4-2 / 5):(1 / 40-1 / 10); and / or the organosilicon includes TEOS.

4. A method for preparing the catalyst according to any one of claims 1 to 3, characterized in that: The following steps are involved: The nickel precursor and S-1 molecular sieve are subjected to hydrothermal crystallization reaction to obtain the base core; In an alkaline solvent environment, the base core is surface activated and then a silicon compound is added to react to generate a catalyst precursor; the catalyst precursor is reduced to obtain a nickel-based catalyst.

5. The preparation method according to claim 4, characterized in that: The nickel precursor and the S-1 molecular sieve are subjected to a hydrothermal crystallization reaction, which includes: mixing the nickel salt and the chelating agent in a molar ratio of (0.4-2):1, and then ultrasonically treating for 30 minutes to 40 minutes to obtain the nickel precursor; mixing the nickel precursor and the S-1 molecular sieve and stirring for 1 hour to 2 hours, pouring into a reaction kettle, and placing in an oven, and reacting at 170°C to 180°C for 3 days to 4 days.

6. The preparation method according to claim 4, characterized in that: When the silicon compound is added to the base core after surface activation: the alkaline solvent environment includes NH3·H2O, and the pH of the system is adjusted to 8-11; and / or, the alkaline solvent environment includes ethanol; and / or, the reagent used for surface activation includes CTAB; and / or, the reagent used for surface activation is set in excess compared to the base core; and / or, the reaction atmosphere during reduction is a reducing atmosphere.

7. The preparation method according to claim 4, characterized in that: When the silicon compound is added to the base core after surface activation, the reaction includes: ultrasonically treating the base core for 30 minutes to 40 minutes, mixing and stirring with a surfactant in an alkaline solution environment for 25 minutes to 35 minutes, slowly dropping the silicon compound until the system becomes milky white colloid, and reacting at 25°C to 80°C for 8 hours to 16 hours.

8. The preparation method according to claim 4, characterized in that: After the nickel precursor is subjected to a hydrothermal crystallization reaction with the S-1 molecular sieve and the base core is surface activated and then a silicon compound is added to react, the base core and the catalyst need to be washed, dried and calcined, including: washing the prepared base core and the catalyst with pure water and ethanol for 3 to 5 times, placing them in an oven at 80°C to 100°C to dry for 4h to 6h and calcining them in a muffle furnace at 550°C to 650°C for 4h to 6h.

9. A catalyst according to any one of claims 1 to 3, or a catalyst prepared by the preparation method according to any one of claims 4 to 8, characterized in that: Application in methane dry gas reforming reaction.

10. The use according to claim 9, characterized in that: At 500℃-800℃, methane and carbon dioxide generate carbon monoxide and hydrogen under the action of catalyst.

Citation Information

Patent Citations

  • SiO2 Ni-loaded double-layer core-shell catalyst as well as preparation method and application thereof

    CN113578326A

  • Preparation method and application of nickel-based molecular sieve catalyst for methane dry reforming

    CN116786153A

  • Manufacture method of catalyst for the carbon dioxide reforming of methane, and its reforming reaction

    KR1020100011687A